A propyltrimethoxysilane oligomer additive for use in rubber compounding and its application method
By preparing propyltrimethoxysilane oligomer additives, controlling the water-silicon molar ratio and octyl molar ratio, and using volatile glacial acetic acid as a catalyst and hexamethyldisilazane for end-capping, the problems of high methanol release and poor dispersion of silica during the compounding process were solved, achieving stable vulcanization and improved performance of the compounded rubber.
Patent Information
- Application Number
- CN202611344251.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to achieve controlled condensation and full end-capping of oligomers without introducing residual non-volatile strong acids. Furthermore, there is a lack of systematic solutions for the hydrophobic modification effect of propyl non-reactive alkyl oligomer additives in rubber compounds, resulting in high methanol release, poor dispersion of silica, and unstable performance of vulcanized rubber during the compounding process.
By using propyltrimethoxysilane oligomer additives, controlling the water-silicon molar ratio, octyl molar ratio, and using volatile glacial acetic acid as a catalyst, combined with hexamethyldisilazane end-capping, and controlling pH and temperature during the preparation process, the controllable condensation and full end-capping of oligomers are achieved, reducing methanol release during the mixing stage and improving the hydrophobic modification of silica.
It significantly reduces methanol release during the mixing process, improves the dispersibility of silica, enhances the mechanical and processing properties of vulcanized rubber, ensures the stability and batch consistency of the vulcanization system, and reduces rolling resistance and the Payne effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of rubber additives technology, specifically to a propyltrimethoxysilane oligomer additive for use in rubber compounds and its application method. Background Technology
[0002] Silica, as a core reinforcing filler for green tires, can significantly reduce tire rolling resistance, improve wet skid resistance, and maintain wear resistance, and has been widely used in passenger tire tread compounds. However, the surface of silica is rich in hydrophilic silanol groups, which have poor compatibility with hydrophobic rubber matrices. Particles easily aggregate spontaneously through hydrogen bonding, forming filler networks, leading to high Mooney viscosity, poor filler dispersion, and deterioration of extrusion and calendering performance in the compound. Simultaneously, it significantly increases the Payne effect and dynamic hysteresis of the vulcanized rubber. Therefore, organic modification of the silica surface is usually necessary.
[0003] A common method for modifying the surface of silica is to introduce silane coupling agents. Traditional sulfur-containing silane coupling agents improve the interfacial bonding between silica and rubber by condensing the alkoxy group at one end of the molecule with the silanol group on the silica surface and coupling the sulfur bond at the other end with the rubber. However, these monomeric silanes undergo in-situ hydrolysis and condensation at high mixing temperatures, releasing large amounts of volatile organic compounds (VOCs) such as alcohols. For example, a silane containing three methoxy groups releases 3 moles of methanol per mole upon complete hydrolysis, which translates to a mass fraction of over 50%, posing significant environmental and occupational health challenges to tire and rubber product manufacturing.
[0004] To reduce VOC emissions from alcohols, existing technologies attempt to prepolymerize silanes into oligomers, allowing some alkoxy groups to undergo pre-hydrolysis and condensation during the preparation stage and recovering the released alcohols, thereby reducing alcohol release during the compounding stage. However, existing oligomeric silanes mostly focus on coupling functions, and the introduced alkyl chains are mostly reactive functional groups containing sulfur, amino, and vinyl groups. There is still a lack of systematic technical solutions for oligomer additives that use non-reactive alkyl groups such as propyl to achieve hydrophobic modification of silica, and their application methods in compounded rubber.
[0005] Furthermore, the preparation of silane oligomers typically uses strong acids as hydrolysis condensation or end-capping catalysts. These strong acids have high boiling points and are non-volatile; if they remain in the finished product, they can neutralize zinc oxide in the rubber formulation, delay sulfur vulcanization, and interfere with amine accelerators such as DPG and CBS, affecting the vulcanization characteristics and batch consistency of the vulcanized rubber. Current technology also lacks a clear solution for achieving controlled condensation and sufficient end-capping of oligomers without introducing non-volatile strong acid residues.
[0006] Therefore, how to provide a silane oligomer additive that can significantly reduce methanol release during the mixing process and effectively improve the dispersion of silica, as well as its application method, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a propyltrimethoxysilane oligomer additive for use in rubber compounds and its application method, which solves the problem that existing oligosilanes mainly focus on coupling functions, and there is a lack of methods for addressing the hydrophobic modification effect of propyl nonfunctional silane oligomers in rubber compounds and their application methods.
[0008] To achieve the above objectives, the present invention provides the following technical solution: A propyltrimethoxysilane oligomer additive is prepared by reacting the following raw materials in parts by weight: 15-18 parts by weight of propyltrimethoxysilane, 6-10 parts by weight of octyltrimethoxysilane, 2.6-3.2 parts by weight of deionized water, 45-55 parts by weight of anhydrous methanol, 14-18 parts by weight of hexamethyldisilazane, 0.05-0.1 parts by weight of glacial acetic acid, and 0.1-0.5 parts by weight of antioxidant.
[0009] Furthermore, the propyltrimethoxysilane oligomer additive is prepared by reacting the following raw materials in parts by weight: 16 parts propyltrimethoxysilane, 8 parts octyltrimethoxysilane, 2.9 parts deionized water, 50 parts anhydrous methanol, 16 parts hexamethyldisilazane, 0.07 parts glacial acetic acid, and 0.3 parts antioxidant.
[0010] A method for preparing the propyltrimethoxysilane oligomer additive includes the following steps: Step 1: Rinse the reactor equipped with a stirrer with anhydrous methanol, add propyltrimethoxysilane and octyltrimethoxysilane, and then add anhydrous methanol to dissolve them. Add glacial acetic acid to adjust the pH of the system to 3.6-3.9; Nitrogen gas was bubbled for 10 minutes to remove oxygen, and the nitrogen pressure was maintained at a slight positive pressure. The temperature was then raised to 35°C. Step 2: Dilute deionized water with anhydrous methanol and add it dropwise continuously at 35-45℃ for 60-90 minutes; after the addition is complete, keep the temperature at 30-60 minutes, and the temperature of the reaction vessel should not exceed 45℃. Step 3: Heat the reactor to 50-60℃ and react for 3-4 hours, then perform central control monitoring. Step 4: The reactor is heated to 80°C under nitrogen protection, and hexamethyldisilazane is slowly added over 30 minutes. The reactor was then heated to 90-110℃ and held for 2-3 hours. Ammonia was then slowly purged with nitrogen and subjected to secondary central control testing. Step 5: Adjust the temperature of the reactor to 80-90℃, and remove methanol, water, residual end-capping agent, ammonia and residual glacial acetic acid under reduced pressure until no distillate is produced; Cool down, add antioxidant 1010, stir well, and pass through a 200-mesh sieve to obtain the propyltrimethoxysilane oligomer additive.
[0011] Furthermore, in step 1, the anhydrous methanol used to rinse the reaction vessel accounts for 5%-10% of the total anhydrous methanol, and the anhydrous methanol used for miscibility accounts for 30%-40%; In step 2, the anhydrous methanol used to dilute the deionized water accounts for 50%-60% of the total anhydrous methanol.
[0012] Furthermore, in step 3, during the controlled detection: the rotational viscosity is 20-60 mPa·s; the Si—O—Si absorption peak in the Fourier transform infrared spectrum is located at 1130 cm⁻¹. -1 With 1030cm -1 The methoxy C-H absorption peak is located at 2830-2850 cm⁻¹. -1 .
[0013] Furthermore, step 4, the secondary central control detection, uses Fourier transform infrared spectroscopy at 3400 cm⁻¹. -1 The disappearance of the silanol hydroxyl absorption peak is taken as the end point of the capping process.
[0014] A method for using the propyltrimethoxysilane oligomer additive in a rubber compound includes the following steps: Rubber, silica, aluminum hydroxide, magnesium hydroxide, talc, and the propyltrimethoxysilane oligomer additive are put into a mixer for mixing; the amount of the propyltrimethoxysilane oligomer additive is 4%-8% of the amount of silica; the mixing temperature is 140-155℃, and the mixture is discharged after maintaining the temperature for 2-3 minutes to complete the silanization reaction.
[0015] Furthermore, the amount of the propyltrimethoxysilane oligomer additive is 5.7% of the amount of silica, the mixing temperature is 145-150℃, and the holding time is 2 minutes.
[0016] Furthermore, after the rubber compound is discharged, it is sheeted on an open mill and vulcanizing agent is added for vulcanization to obtain the finished rubber product.
[0017] This invention provides a propyltrimethoxysilane oligomer additive for use in rubber compounding and its application method, which has the following beneficial effects: First, traditional monomeric trialkoxysilanes undergo in-situ hydrolysis and condensation at high temperatures during mixing, releasing 3 moles of alcohol per silicon atom. For example, propyltrimethoxysilane releases approximately 58.5 g of methanol per 100 g of monomer upon complete hydrolysis. This invention, by locking the water-silicon molar ratio R at 1.15-1.25, completes the hydrolysis and condensation of approximately 2 / 3 of the methoxy groups during the preparation stage, resulting in a residual methoxy group of approximately 1.0 per Si in the finished product. Methanol release during the mixing stage is reduced to approximately 19.5 g / 100 g, a reduction of approximately 66.7%. Furthermore, methanol can be condensed and recovered during the preparation stage, further amplifying environmental benefits.
[0018] Second, it enhances the hydrophobicity of silica, improves dispersion, and reduces Mooney viscosity and the Payne effect. Increasing the octyl molar content to approximately 26% allows the C8 long chains to form a dense, thicker hydrophobic coating layer on the silica surface, shielding silanol groups, weakening the filler-filler hydrogen bond network, and improving compatibility with the rubber matrix. This can reduce the Mooney viscosity of the compound by approximately 10%-20%, and the Payne effect ΔG′ by approximately 40%-60%.
[0019] Third, it reduces rolling resistance and improves wear resistance and mechanical properties. The more uniform dispersion of silica and the weakened filler network result in a 20%-30% decrease in tanδ of the vulcanized rubber at 60℃, reduced DIN abrasion, and increased tensile strength. It also has a coating modification effect on flame-retardant fillers such as aluminum hydroxide / magnesium hydroxide, improving their dispersion and flame retardant / mechanical balance.
[0020] Fourth, eliminate acid residues and protect the vulcanization system. Non-volatile methanesulfonic acid is removed and replaced with volatile glacial acetic acid as a catalyst, which is then removed under reduced pressure in step 5. The finished product has no strong acid residues, avoiding neutralization of zinc oxide, delaying sulfur vulcanization, and interference with DPG / CBS amine accelerators. The vulcanization rate and crosslinking density are stable and controllable.
[0021] Fifth, the molecular weight, degree of condensation, and residual methoxy groups are controllable, and the process is stable and reproducible. Continuous addition instead of segmented addition, narrowing the pH to 3.6-3.9, combined with precise temperature-time windows and intermediate control parameters, ensures that the degree of condensation, molecular weight distribution, and number of residual methoxy groups of the oligomers are stable and controllable, facilitating industrial scale-up.
[0022] Sixth, thorough end-capping enhances storage stability and hydrophobic durability. Residual silanols are end-capped with hexamethyldisilazane at a 1:2 molar ratio, and then capped at 3400 cm⁻¹. -1 The disappearance of the hydroxyl peak in silanols marks the end-capping endpoint. Dynamic control of the feed amount results in a product with stronger and more durable hydrophobicity, and less susceptibility to self-polymerization and thickening during storage. Detailed Implementation
[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example
[0024] The formulation of propyltrimethoxysilane oligomer additives is as follows: 16 parts by weight of propyltrimethoxysilane, 8 parts by weight of octyltrimethoxysilane, 2.9 parts by weight of deionized water, 50 parts by weight of anhydrous methanol, 16 parts by weight of hexamethyldisilazane, 0.07 parts by weight of glacial acetic acid, and 0.3 parts by weight of antioxidant 1010. This ratio corresponds to a water-silicon molar ratio R≈1.22 and an octyl molar percentage≈26%.
[0025] Preparation process of propyltrimethoxysilane oligomer additives: Step 1: Rinse the inner wall of the reactor with anhydrous methanol accounting for 8.3% of the total anhydrous methanol, add propyltrimethoxysilane and octyltrimethoxysilane, and then add anhydrous methanol accounting for 33.4% of the total to dissolve them. Add glacial acetic acid to adjust the pH to 3.8; purge with nitrogen gas for 10 minutes to remove oxygen, maintain a slight positive pressure, and heat the reactor to 35°C; Step 2: Dilute the deionized water with 58.3% anhydrous methanol, and continuously add it dropwise for 75 minutes while heating the reaction vessel to 35-45℃; after the addition is completed, keep the temperature at this temperature for 45 minutes, during which time the temperature inside the reaction vessel shall not exceed 45℃. Step 3: The temperature inside the reactor is raised to 55℃, and the reaction is carried out for 3.5 hours. The reactants are monitored and tested under the following standards: viscosity 32 mPa·s, and the Si-O-Si peak in FTIR is located at 1130 / 1030 cm⁻¹. -1 The methoxy peak is located at 2830-2850 cm⁻¹ -1 ; Step 4: Under nitrogen protection, heat the reactor to 80°C, slowly add hexamethyldisilazane over 30 minutes, then heat the reactor to 100°C and hold for 2.5 hours. Purge the reactor with nitrogen to remove ammonia, and bring the FTIR to 3400 cm⁻¹. -1 The disappearance of the silanol hydroxyl peak serves as the end point for capping. Step 5: Adjust the temperature to 85℃, remove methanol, water, residual end-capping agent, ammonia and residual glacial acetic acid under reduced pressure until no distillation occurs, which takes about 2.5 hours; cool down, add antioxidant 1010, stir well, and pass through a 200-mesh sieve to obtain the propyltrimethoxysilane oligomer additive.
[0026] Application of propyltrimethoxysilane oligomer additives in rubber compounds: The compound rubber formulation by weight is: solution-polymerized styrene-butadiene rubber 100, silica 70, propyltrimethoxysilane oligomer additive 4, zinc oxide 3, stearic acid 2, antioxidant 1.5, accelerator DPG 1.5, accelerator CBS 1.5, and sulfur 1.4. The internal mixer has a filling coefficient of 0.7, a rotor speed of 60 r / min, an initial temperature of 80℃, and mixes the rubber compound to 145-150℃ for 2 minutes to complete silanization before discharging the compound. The rubber compound is then sheeted from the open mill, vulcanizing agent is added, and vulcanization is carried out at 160℃.
[0027] II. Comparative Example Comparative Example 1: The compounding formula did not contain silane additives, and the rest was the same as in Example 1.
[0028] Comparative Example 2: The additive was replaced with monomer propyltrimethoxysilane in the same molar amount as in Example 1, and the rest was the same as in Example 1.
[0029] Comparative Example 3: In the additive formulation, deionized water was reduced to 2.6 parts by weight, and propyl / octyltrimethoxysilane was taken to the upper limit of 21.3 / 9.9 parts by weight, i.e., R≈0.84, and the rest was the same as in Example 1.
[0030] Comparative Example 4: The amount of octyltrimethoxysilane in the additive formulation was reduced to 3.4 parts by weight, i.e., the molar percentage of octyl was approximately 8.4%, and the rest was the same as in Example 1.
[0031] Comparative Example 5: The amount of propyltrimethoxysilane oligomer additive used in the method of use was increased to 12% of the amount of silica, and the rest was the same as in Example 1.
[0032] Performance testing and data Test methods: Mooney viscosity ML(1+4) at 100℃ according to GB / T1232; Payne effect ΔG′ using a rubber processing analyzer (RPA) strain scan (0.28%-100%, 60℃, 1Hz) to obtain the difference in storage modulus; tanδ at 60℃ using dynamic mechanical analysis; DIN abrasion according to GB / T9867; tensile strength according to GB / T528; scorch time t 10 , positive vulcanization time t 90 A rotorless vulcanizing apparatus (160℃) was used. Table 1 Physicochemical properties of samples with different additives
[0033]
[0034] Table 2 Processing properties and vulcanization characteristics of different sample rubber compounds
[0035]
[0036] Table 3 Effect of additive dosage on the properties of the compound (Example 1: Additives)
[0037]
[0038] In summary, Example 1 (the optimal embodiment of the present invention) is superior to Comparative Examples 1–5 in terms of residual methoxy groups (1.0 nucleotides / Si), methanol release from the compound (19.5 g / 100g, a 66.7% reduction compared to the monomer), Mooney viscosity (77), Payne effect ΔG′ (320 kPa, a 62.4% reduction compared to the blank), tanδ at 60 ℃ (0.105, a 26.1% reduction compared to the blank), DIN abrasion (95 mm³), and tensile strength (20.2 MPa); moreover, the finished product has no acid residue (acid value 0.05 mg KOH / g) and exhibits normal vulcanization characteristics. 6.5 min (12.8 min). The above data verify the necessity and synergistic effect of the four technical features: water-to-silicon molar ratio, octyl content, volatile acid catalysis, and dynamic end-capping with hexamethyldisilazane.
[0039] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. A propyltrimethoxysilane oligomer additive, characterized in that, It is prepared by reacting the following raw materials in parts by weight: 15-18 parts by weight of propyltrimethoxysilane, 6-10 parts by weight of octyltrimethoxysilane, 2.6-3.2 parts by weight of deionized water, 45-55 parts by weight of anhydrous methanol, 14-18 parts by weight of hexamethyldisilazane, 0.05-0.1 parts by weight of glacial acetic acid, and 0.1-0.5 parts by weight of antioxidant.
2. The propyltrimethoxysilane oligomer additive according to claim 1, characterized in that, It is prepared by reacting the following raw materials in parts by weight: 16 parts propyltrimethoxysilane, 8 parts octyltrimethoxysilane, 2.9 parts deionized water, 50 parts anhydrous methanol, 16 parts hexamethyldisilazane, 0.07 parts glacial acetic acid, and 0.3 parts antioxidant.
3. A method for preparing the propyltrimethoxysilane oligomer additive as described in claim 1, characterized in that, Includes the following steps: Step 1: Rinse the reactor equipped with a stirrer with anhydrous methanol, add propyltrimethoxysilane and octyltrimethoxysilane, and then add anhydrous methanol to dissolve them. Add glacial acetic acid to adjust the pH of the system to 3.6-3.9; Nitrogen gas was bubbled for 10 minutes to remove oxygen, and the nitrogen pressure was maintained at a slight positive pressure. The temperature was then raised to 35°C. Step 2: Dilute deionized water with anhydrous methanol and add it dropwise continuously at 35-45℃ for 60-90 minutes; after the addition is complete, keep the temperature at 30-60 minutes, and the temperature of the reaction vessel should not exceed 45℃. Step 3: Heat the reactor to 50-60℃ and react for 3-4 hours, then perform central control monitoring. Step 4: The reactor is heated to 80°C under nitrogen protection, and hexamethyldisilazane is slowly added over 30 minutes. The reactor was then heated to 90-110℃ and held for 2-3 hours. Ammonia was then slowly purged with nitrogen and subjected to secondary central control testing. Step 5: Adjust the temperature of the reactor to 80-90℃, and remove methanol, water, residual end-capping agent, ammonia and residual glacial acetic acid under reduced pressure until no distillate is produced; Cool down, add antioxidant 1010, stir well, and pass through a 200-mesh sieve to obtain the propyltrimethoxysilane oligomer additive.
4. The method for preparing the propyltrimethoxysilane oligomer additive according to claim 3, characterized in that, In step 1, the anhydrous methanol used to rinse the reaction vessel accounts for 5%-10% of the total anhydrous methanol, and the anhydrous methanol used for miscibility accounts for 30%-40%. In step 2, the anhydrous methanol used to dilute the deionized water accounts for 50%-60% of the total anhydrous methanol.
5. The method for preparing the propyltrimethoxysilane oligomer additive according to claim 3, characterized in that, In step 3 of the controlled detection: the rotational viscosity is 20-60 mPa·s; the Si—O—Si absorption peak in the Fourier transform infrared spectrum is located at 1130 cm⁻¹. -1 With 1030cm -1 The methoxy C-H absorption peak is located at 2830-2850 cm⁻¹. -1 .
6. The method for preparing the propyltrimethoxysilane oligomer additive according to claim 3, characterized in that, Step 4, the secondary central control detection, uses Fourier transform infrared spectroscopy at 3400 cm⁻¹. -1 The disappearance of the silanol hydroxyl absorption peak is taken as the end point of the capping process.
7. A method of using the propyltrimethoxysilane oligomer additive of claim 1 in a rubber compound, characterized in that, Includes the following steps: Rubber, silica, aluminum hydroxide, magnesium hydroxide, talc, and the propyltrimethoxysilane oligomer additive are put into a mixer for mixing; the amount of the propyltrimethoxysilane oligomer additive is 4%-8% of the amount of silica; the mixing temperature is 140-155℃, and the mixture is discharged after maintaining the temperature for 2-3 minutes to complete the silanization reaction.
8. The method of using the propyltrimethoxysilane oligomer additive according to claim 7 in the compound rubber, characterized in that, The amount of the propyltrimethoxysilane oligomer additive is 5.7% of the amount of the silica, the mixing temperature is 145-150℃, and the holding time is 2 minutes.
9. The method of using the propyltrimethoxysilane oligomer additive according to claim 7 in a rubber compound, characterized in that, After the rubber compound is discharged, it is sheeted on an open mill and vulcanizing agent is added for vulcanization to obtain the finished rubber product.