A method for preparing pentagonal high-entropy metal-organic framework materials by ball milling and a method for modifying lithium-sulfur battery separators thereof.
The five-element high-entropy metal-organic framework material prepared by ball milling solves the shuttle effect problem of polysulfides in lithium-sulfur batteries by utilizing the unique effect of the high-entropy framework and lattice distortion, thereby improving the cycle stability and electrochemical performance of the battery and reducing the preparation cost.
Patent Information
- Application Number
- CN202611235341.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
During the charging and discharging process of lithium-sulfur batteries, the shuttle effect caused by the dissolution and leaching of soluble long-chain lithium polysulfides leads to the loss of positive electrode active material and the growth of lithium dendrites, affecting battery safety and cycle stability. In addition, the high-temperature treatment of traditional high-entropy metal-organic framework materials increases the preparation cost.
Five-element high-entropy metal-organic framework materials were prepared by ball milling. By introducing the "cocktail effect" and lattice distortion of the high-entropy framework, the chemical adsorption and catalytic conversion performance of polysulfides were improved. By combining conductivity and polysulfide adsorption capacity, the electron transfer rate of active sites was optimized, the shuttle effect was suppressed and the polysulfide conversion was accelerated.
It significantly improves the cycle stability and electrochemical utilization of lithium-sulfur batteries, reduces manufacturing costs, achieves high specific surface area and confinement effect, and enhances the long-term cycle performance and safety of batteries.
Smart Images

Figure CN123107101A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-sulfur battery separator modification technology, and particularly relates to a method for preparing pentagonal high-entropy metal-organic framework materials by ball milling and a method for modifying lithium-sulfur battery separators. Background Technology
[0002] Lithium-sulfur batteries possess significant advantages such as high theoretical specific capacity (1675 mAh / g), excellent energy density (2600 Wh / kg), low cost, and environmental friendliness, and are widely recognized as one of the most promising next-generation rechargeable battery systems. However, during actual charge-discharge cycles of lithium-sulfur batteries, the dissolution and leaching of soluble long-chain lithium polysulfides (LiPSs) in the electrolyte can trigger a severe "shuttle effect." This not only directly causes the loss of active sulfur material in the positive electrode and rapid capacity decay, but also further corrodes and passivates the metallic lithium anode, inducing the disordered growth of lithium dendrites, posing a significant safety hazard to the battery. In addition, the electronic insulation properties of elemental sulfur and its discharge products, short-chain lithium sulfides (Li2S2, Li2S), as well as the dramatic volume expansion and contraction of the electrodes during cycling, greatly limit the commercial application of lithium-sulfur batteries.
[0003] Surface functional modification of separators has proven to be an effective route to block lithium polysulfide shuttle and promote their in-situ catalytic conversion. However, the large pore structure of common separators cannot suppress lithium polysulfide shuttle, easily leading to battery capacity decay; their poor mechanical strength makes it difficult to suppress lithium dendrite penetration, causing battery short circuits. Studies have shown that metal-organic frameworks (MOFs) have a large specific surface area and highly ordered tunable nanopores, making them a promising separator modification material. MOFs, as a positive electrode side modification layer for separators, can effectively enhance the lithium polysulfide (Li) capacity. + The improved transport efficiency and electrolyte affinity not only inhibit the shuttle movement of soluble LiPSs in organic electrolytes and promote the conversion of lithium polysulfides, but also slow down the growth of lithium dendrites.
[0004] On the other hand, traditional high-entropy metal-organic frameworks (HE-MOFs) are highly temperature-dependent, typically requiring high-temperature treatment to induce polymetallic cations to occupy lattice sites, which significantly increases preparation costs and energy consumption. Therefore, finding an energy-efficient room-temperature synthesis method to prepare modified coating materials with synergistic effects, high specific surface area, and confinement capabilities offers significant advantages in improving the utilization rate of active materials, accelerating redox kinetics, and extending battery life, thus possessing broad practical application potential. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention proposes a method for preparing pentagonal high-entropy metal-organic framework materials via ball milling and a method for modifying lithium-sulfur battery separators. To overcome the limitation of traditional catalysts having only a single catalyst site, this invention introduces the unique "cocktail effect" and lattice distortion of the high-entropy framework, significantly improving the polar chemisorption and catalytic conversion performance for polysulfides. Simultaneously, it significantly reduces the loss of positive electrode active material and the rapid capacity decay.
[0006] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing a pentagonal high-entropy metal-organic framework material by ball milling, comprising the following steps: using 2,5-dihydroxyterephthalic acid as an organic ligand, and using metal acetates containing nickel, cobalt, and copper and metal oxides containing zinc and magnesium as metal sources, reacting by ball milling, and obtaining a pentagonal high-entropy metal-organic framework material with high crystallinity and ordered microporous structure after washing and drying.
[0007] This invention overcomes the limitations of traditional single / bimetallic catalysts by utilizing the unique cocktail effect of a high-entropy framework to achieve synergistic effects of atomically dispersed multiple active sites. The multi-metal synergy significantly reduces the nucleation overpotential of Li₂S, transforming the deposition path from two-dimensional growth to three-dimensional instantaneous nucleation. Simultaneously, the finite-domain effect of the high-entropy MOF ensures uniform Li₂S deposition, significantly improving sulfur dispersion and electrochemical utilization. The lattice distortion of the high-entropy MOF generates numerous unsaturated coordination metal sites, efficiently adsorbing polysulfides and accelerating their conversion. Furthermore, the excellent conductivity and polysulfide adsorption capacity further enhance battery performance.
[0008] This invention ensures the successful synthesis of high-entropy MOF materials while controlling preparation costs. Based on the unique "confined effect" and "multi-scale synergistic catalysis theory" of MOF materials, the synthesized five-member high-entropy metal-organic framework material (HMOF-NCCZM) maintains a highly ordered microporous MOF-74 framework, with an extremely high specific surface area (reaching 927.02 m²). 2 / g) effectively improves the wettability of the electrolyte.
[0009] During the operation of lithium-sulfur batteries, this multi-metal system exhibits its unique characteristics and works synergistically, primarily due to the excellent electrolyte wettability of the HMOF layer, its strong anchoring function for LiPS, and the acceleration of catalytic kinetics. High-entropy sites significantly lower the energy barriers for liquid-liquid transitions (Li₂S₈~Li₂S₄) and liquid-solid transitions (Li₂S₄~Li₂S₂ / Li₂S). The overlapping electron clouds of the high-entropy metal centers generate a "cocktail effect," optimizing the d-band centers of the active sites and thus accelerating the electron transfer rate. Because Mg and Co have a strong affinity for sulfur, they anchor polysulfides to the surface of the MOF spheres through strong chemical polarity interactions, suppressing the shuttle effect. Simultaneously, in the pentagonal high-entropy system, the different electronegativity of each metal forms directional catalytic ion channels.
[0010] Low electronegativity Mg and Zn act as electron donors, injecting electrons into Cu sites via a Ni / Co bridge. Ultimately, these electrons are precisely injected into the antibonding orbitals (SS*) of sulfur molecules. This multi-electron synergistic effect not only enhances the chemical anchoring of polysulfides but also significantly improves the cycle stability of the battery under high sulfur loads by lowering the activation energy of sulfur redox reactions.
[0011] Furthermore, the molar ratio of the 2,5-dihydroxyterephthalic acid, the metal acetate containing nickel, cobalt, and copper, and the metal oxide containing zinc and magnesium is 3:1:1:1:1:1.
[0012] Furthermore, the metal acetates containing nickel, cobalt, and copper are Ni(CH3COO)2·3H2O, Co(CH3COO)2·3H2O, and Cu(CH3COO)2·H2O; the metal oxides containing zinc and magnesium are ZnO and MgO.
[0013] Furthermore, the ball milling speed is 1000~1200 r / min, the ball-to-material ratio is 8:1~10:1, and the grinding balls are zirconium beads; preferably, the ball milling speed is 1200 r / min, the ball-to-material ratio is 10:1, wherein there are 5 zirconium beads with a diameter of 0.5 cm and 4 zirconium beads with a diameter of 0.85 cm.
[0014] Furthermore, water and methanol were added during ball milling.
[0015] The present invention also provides a pentagonal high-entropy metal-organic framework material prepared according to the above method.
[0016] The present invention also provides an application of the above-mentioned pentagonal high-entropy metal-organic framework material in the preparation of lithium-sulfur battery separators.
[0017] This invention also provides a method for modifying lithium-sulfur battery separators with the above-mentioned pentagonal high-entropy metal-organic framework material, comprising the following steps: A uniform slurry is prepared by mixing conductive materials, binders, organic solvents, and the pentagonal high-entropy metal-organic framework material. The uniform slurry was coated onto the surface of a polypropylene membrane and then vacuum dried to obtain a high-entropy metal-organic framework functional modified membrane.
[0018] Furthermore, the conductive material is conductive carbon; the binder is polyvinylidene fluoride; and the organic solvent is N-methylpyrrolidone.
[0019] The present invention also provides an application of the lithium-sulfur battery separator modified by the above method in the preparation of lithium-sulfur batteries.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects: 1. This invention constructs a high-entropy organometallic organic framework. Driven by the synergistic multi-metal "cocktail effect", the high-entropy framework combines coexisting Ni, Co, Cu, Zn and Mg centers with different electronegativity, causing lattice distortion and dynamic charge redistribution, thereby generating a large number of unsaturated active sites in the structure and establishing directional electron transport channels.
[0021] 2. This invention leverages a highly ordered microporous network to exert a powerful spatial confinement effect. Combined with the high specific surface area of high-entropy materials, it effectively guides the geometric evolution of phase transition from the traditional two-dimensional (2D) surface passivation to a three-dimensional (3D) instantaneous nucleation path, thereby promoting targeted charge injection into active reaction intermediates.
[0022] 3. The high-entropy material-modified membrane prepared in this invention exhibits excellent long-term cycling stability exceeding 2000 cycles, with an ultra-low capacity decay rate of 0.027% per cycle, and performs well even with a high sulfur loading (12.36 mg / cm³). 2 It operates stably under extreme conditions of electrolyte deficiency and low electrolyte concentration.
[0023] 4. The metal elements used in this invention are nickel, cobalt, copper, zinc, and magnesium. This is because, considering the practical difficulties faced by lithium-sulfur batteries—namely, the difficulty in converting lithium polysulfides and the challenge of converting "dead sulfur"—this method selects cobalt, an element with a highly active d-band center, to enhance the adsorption capacity of LiPs; nickel to lower the conversion energy barrier; and copper to direct electrons into the antibonding orbitals of SS, thereby improving catalytic efficiency. To support the structural stability of the material during long-term battery cycling, this method also introduces zinc and magnesium, whose low electronegativity allows them to act as electron donors and provide some structural support to the material.
[0024] 5. Element Selection: The different electronegativity of the five metals forms a directional catalytic ion channel. Low electronegativity Mg and Zn act as electron donors, directionally injecting electrons into Cu sites via the Ni / Co "electron bridge." Ultimately, these electrons are precisely injected into the antibonding orbitals (SS*) of sulfur molecules. This multi-electron synergistic effect not only enhances the chemical anchoring of polysulfides but also significantly improves the cycle stability of the battery under high sulfur loads by lowering the activation energy of sulfur redox reactions. Attached Figure Description
[0025] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The figures show the crystal structure and chemical composition characterization of the materials prepared in the embodiments and comparative examples of the present invention, where (a) is a Fourier transform infrared spectrum (FT-IR), (b) is an X-ray powder diffraction (XRD) pattern, and (c) is the pore size distribution of HMOF-NCCZM (the inset shows the N2 adsorption-desorption isotherm). Figure 2 The graphs show the electrochemical performance of the modified separator prepared in this invention in a lithium-sulfur battery. (a) shows the electrochemical performance after 2000 cycles at 1C. (b) shows the electrochemical performance of the modified separator prepared in this invention under different rate conditions (0.2C, 0.5C, 1C, 2C, 0.2C) in a lithium-sulfur battery. (c) shows the electrochemical test results of the modified separator prepared in Example 2 of this invention in a lithium-sulfur battery at different rates. (d) shows the impedance test graph of the modified separator prepared in this invention in a lithium-sulfur battery. Figure 3 This is a scanning electron microscope (SEM) image of the MOF-N prepared in Comparative Example 1 of this invention; Figure 4 This is a scanning electron microscope (SEM) image of the MOF-NCM prepared in Comparative Example 2 of this invention; Figure 5 The image shows a scanning electron microscope (SEM) image of the HMOF-NCCZM prepared in Example 1 of this invention. Figure 6 The energy dispersive spectroscopy (EDS) diagram of HMOF-NCCZM prepared in Example 1 of this invention is shown. Detailed Implementation
[0026] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0027] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0028] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0029] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0030] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0031] The present invention provides a method for preparing a pentagonal high-entropy metal-organic framework material by ball milling, comprising the following steps: using 2,5-dihydroxyterephthalic acid as an organic ligand, and using metal acetates containing nickel, cobalt, and copper and metal oxides containing zinc and magnesium as metal sources, reacting by ball milling, and obtaining a pentagonal high-entropy metal-organic framework material with high crystallinity and ordered microporous structure after washing and drying.
[0032] In a preferred embodiment of the present invention, the molar ratio of 2,5-dihydroxyterephthalic acid, a metal acetate containing nickel, cobalt, and copper, and a metal oxide containing zinc and magnesium is 3:1:1:1:1:1. The metals used in the five-element high-entropy metal-organic framework material of the present invention are nickel, cobalt, copper, zinc, and magnesium. The five metal ions are uniformly dispersed in the crystal lattice, and the configurational entropy of the high-entropy metal-organic framework material HMOF-NCCZM satisfies S... conf ≥ 1.5R, where R is the ideal gas constant.
[0033] In a preferred embodiment of the present invention, the metal acetates containing nickel, cobalt, and copper are Ni(CH3COO)2·3H2O, Co(CH3COO)2·3H2O, and Cu(CH3COO)2·H2O; and the metal oxides containing zinc and magnesium are ZnO and MgO.
[0034] In a preferred embodiment of the present invention, the ball milling speed is 1000~1200 r / min, the ball-to-material ratio is 8:1~10:1, and the grinding balls are zirconium beads; preferably, the ball milling speed is 1200 r / min, the ball-to-material ratio is 10:1, and the zirconium beads have diameters of 0.5 cm and 0.85 cm, wherein there are 5 zirconium beads with a diameter of 0.5 cm and 4 zirconium beads with a diameter of 0.85 cm. The present invention utilizes high-speed ball milling to generate mechanical energy and localized instantaneous high temperatures through intense friction and collision between the grinding balls and the material, driving a coordination reaction.
[0035] In a preferred embodiment of the invention, water and methanol (MeOH) are added during ball milling.
[0036] In a preferred embodiment of the present invention, the ball milling method is a mechanochemical ball milling method, which adopts a high-speed stepwise ball milling method. The specific process is as follows: in the first step, after adding the ligand (2,5-dihydroxyterephthalic acid) and nickel acetate, the ball milling time is 10 minutes and then paused; in the second step, after adding cobalt acetate, the ball milling time is 10 minutes and then paused; in the third step, after adding copper acetate, the ball milling time is 10 minutes and then paused; in the fourth step, after adding zinc oxide, the ball milling time is 10 minutes and then paused; in the fifth step, after adding magnesium oxide, the ball milling time is 20 minutes.
[0037] In a preferred embodiment of the present invention, a high-speed stepwise liquid-assisted ball mill is used. In the first step, 1000 μL of pure water is added to assist the milling; in the second and third steps, 320 μL of pure water is added to assist the milling in each step; and in the fourth step, 960 μL of methanol is added to assist the milling.
[0038] In a preferred embodiment of the present invention, the mixture after ball milling is centrifuged to collect the product, and the reactants are washed multiple times with methanol (washing times ≥ 3 times).
[0039] An exemplary method for preparing a pentagonal high-entropy metal-organic framework material by ball milling includes the following steps: 2,5-dihydroxyterephthalic acid (H4DHTA, 0.5944 g, 3.00 mmol) and Ni(CH3COO)2·3H2O (0.2484 g, 1.00 mmol) are placed in a ball mill, the mill speed is set to 1200 r / min, and zirconium beads (0.5 cm to 0.85 cm in diameter) are added at a ball-to-material ratio of 10:1. 1000 μL of H2O is added to the resulting reaction mixture, and after milling for 10 minutes, Co(CH3COO)2·3H2O (0.2491 g, 1.00 mmol) and 320 μL of H2O are added. After milling for 10 minutes, Cu(CH3COO)2·H2O (0.1997 g, 1.00 mmol) and 320 μL of H2O are added. After grinding for 10 minutes, ZnO (0.0814 g, 1.00 mmol) and 960 μL MeOH were added, and the resulting mixture was ground for another 10 minutes. Subsequently, MgO (0.040 g, 1.00 mmol) was added, and the entire mixture was ground for 20 minutes. The collected product was washed three times with MeOH and further dried overnight at 60 °C to obtain a high-entropy five-metal-organic framework material, denoted as HMOF-NCCZM.
[0040] The present invention also provides a pentagonal high-entropy metal-organic framework material (high-entropy MOF material) prepared according to the above method.
[0041] The embodiments of the present invention also provide an application of the above-mentioned pentagonal high-entropy metal-organic framework material in the preparation of lithium-sulfur battery separators (HMOF-NCCZM@PP).
[0042] Embodiments of the present invention also provide a method for modifying lithium-sulfur battery separators with the above-mentioned pentagonal high-entropy metal-organic framework material, comprising the following steps: A uniform slurry is prepared by mixing conductive materials, binders, organic solvents and a five-element high-entropy metal-organic framework material. A uniform slurry was coated onto the surface of a polypropylene (PP) membrane, and after vacuum drying, a high-entropy metal-organic framework functional modified membrane was obtained.
[0043] In a preferred embodiment of the present invention, the conductive material, binder, organic solvent, and pentagonal high-entropy metal-organic framework material are mixed and stirred for 8 hours. In a preferred embodiment of the present invention, the conductive material is conductive carbon; the binder is polyvinylidene fluoride; and the organic solvent is N-methylpyrrolidone (NMP).
[0044] In a preferred embodiment of the present invention, a pentagonal high-entropy metal-organic framework material, a conductive material and a binder are mixed in NMP at a mass ratio of 7:2:1.
[0045] In a preferred embodiment of the present invention, after the uniform slurry is coated on the surface of the PP diaphragm, the vacuum drying temperature is 60°C and the time is 12 hours.
[0046] For example, the method for modifying a lithium-sulfur battery separator with the above-mentioned pentagonal high-entropy metal-organic framework material includes the following steps: a. Preparation of slurry for modification materials: Take 0.035g of pentagonal high-entropy metal-organic framework material, 0.01g of conductive carbon and 0.005g of PVDF (polyvinylidene fluoride), add 0.8mL of NMP (N-methylpyrrolidone) and stir with a magnetic stirrer for 8h in a 25×25mm weighing bottle to prepare a uniform slurry.
[0047] b. Preparation of modified diaphragm: Fix the finished PP diaphragm on a glass plate, pour the above slurry onto the near end of the coater on the diaphragm, adjust the coater to a height of 100 micrometers, and uniformly scrape the slurry onto one side of the PP diaphragm. Place it in a vacuum oven and dry at 60°C for 12 hours. Use a cutter to cut out a 16mm diameter high-entropy metal-organic framework functional modified diaphragm.
[0048] Embodiments of the present invention also provide an application of the lithium-sulfur battery separator modified by the above method in the preparation of lithium-sulfur batteries.
[0049] In the preparation of lithium-sulfur batteries, the modified separator HMOF-NCCZM@PP is placed between the positive electrode and the lithium metal negative electrode of the lithium-sulfur battery, with the coating side facing the positive electrode.
[0050] An exemplary method for preparing a lithium-sulfur battery is as follows: A half-cell of a 2032 type button cell is assembled in a glove box. A high-entropy modified membrane with a diameter of 16 mm is used as the separator. A lithium metal disk with a diameter of 15.6 mm and a thickness of 450 μm is used as the counter electrode. The electrolyte consists of 1 mol L... -1 The battery consists of LiTFSI and 2wt% LiNO3 additive, dissolved in a 1:1 (v / v) mixture of 1,3-dioxolane (DOL) and dimethyl ethylene glycol (DME), with a total volume of 50 μL per cell. The prepared electrode sheets, along with positive / negative electrode shells, electrolyte, separator, spring, gasket, and lithium sheet, are assembled into CR-2032 button cells in an argon-filled ultrapure glove box.
[0051] This invention discloses a method for preparing a pentagonal high-entropy metal-organic framework (MOF) material using ball milling and its modification method for lithium-sulfur battery separators. The invention uses 2,5-dihydroxyterephthalic acid, acetate, and metal oxides as metal sources, and successfully prepares the pentagonal high-entropy metal-organic framework material HMOF-NCCZM (nickel-cobalt-copper-zinc-magnesium) using mechanical ball milling. A coater is then used to apply the material to the separator, preparing HMOF-NCCZM@PP to improve the performance of lithium-sulfur batteries. Nickel, cobalt, and copper provide a large number of catalytic active centers, while zinc and magnesium endow the material with excellent electrocatalytic conversion capabilities and maintain MOF framework stability under high specific surface area conditions. Magnesium has extremely strong chalcophilicity and can anchor polysulfides through chemisorption. This method overcomes the limitations of traditional single / bimetallic catalysts, utilizing the unique cocktail effect of the high-entropy framework to achieve synergistic effects of multiple active sites. The multi-metal synergy significantly reduces the Li2S nucleation overpotential, transforming the deposition path from two-dimensional growth to three-dimensional instantaneous nucleation. Meanwhile, the finite-domain effect of high-entropy MOF ensures uniform Li2S deposition, significantly improving sulfur dispersion and electrochemical utilization. The lattice distortion of high-entropy MOF generates a large number of unsaturated coordination metal sites, which efficiently adsorb polysulfides and accelerate their conversion. At the same time, the excellent conductivity and polysulfide adsorption capacity further improve the battery performance.
[0052] Unless otherwise specified, the room temperature in this invention is 25±2℃.
[0053] All raw materials used in the embodiments of the present invention were obtained through commercial purchase.
[0054] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0055] The technical solution of the present invention will be further illustrated by the following embodiments.
[0056] Example 1 This embodiment provides a method for preparing a high-entropy five-metal-organic framework material, the steps of which are as follows: 2,5-Dihydroxyterephthalic acid (H4DHTA, 0.5944 g, 3.00 mmol) and Ni(CH3COO)2·3H2O (0.2484 g, 1.00 mmol) were placed in a ball mill at 1200 r / min. Zirconium beads (0.5 cm and 0.85 cm in diameter, with 5 beads of 0.5 cm and 4 beads of 0.85 cm in diameter) were added at a ball-to-material ratio of 10:1. 1000 μL of H2O was added to the resulting reaction mixture, and after grinding for 10 minutes, Co(CH3COO)2·3H2O (0.2491 g, 1.00 mmol) and 320 μL of H2O were added. After grinding for 10 minutes, Cu(CH3COO)2·H2O (0.1997 g, 1.00 mmol) and 320 μL of H2O were added. After grinding for 10 minutes, ZnO (0.0814 g, 1.00 mmol) and 960 μL MeOH were added, and the resulting mixture was ground for another 10 minutes. Subsequently, MgO (0.040 g, 1.00 mmol) was added, and the entire mixture was ground for 20 minutes. The collected product was washed three times with MeOH and further dried overnight at 60 °C to obtain a high-entropy pentmetal-organic framework material (high-entropy MOF material), denoted as HMOF-NCCZM.
[0057] Example 2 This embodiment provides a method for modifying lithium-sulfur battery separators with high-entropy MOF materials prepared by ball milling, the steps of which are as follows: Preparation of the slurry for the modified material: Take 0.035g of MOF-NCCZM material from Example 1, 0.01g of conductive carbon and 0.005g of PVDF (polyvinylidene fluoride), add 0.8mL of NMP (N-methylpyrrolidone) and stir with a magnetic stirrer for 8h in a 25×25mm weighing bottle to prepare a uniform slurry.
[0058] Preparation of modified separators: The finished PP separator is fixed on a glass plate. The above slurry is poured onto the near end of the coater on the separator. The coater is adjusted to a height of 100 micrometers, and the slurry is uniformly coated onto one side of the PP separator. It is placed in a vacuum oven and dried at 60°C for 12 hours. A high-entropy metal-organic framework functional modified separator with a diameter of 16 mm is cut out using a cutter. This is the high-entropy modified separator.
[0059] Assembly of lithium-sulfur button cells: Half-cells of 2032 type button cells were assembled in a glove box. A high-entropy modified separator with a diameter of 16 mm was used as the battery separator. A lithium metal disk with a diameter of 15.6 mm and a thickness of 450 μm was used as the counter electrode. The electrolyte consisted of 1 mol L⁻¹ -1The battery consists of LiTFSI and 2wt% LiNO3 additive dissolved in a 1:1 (v / v) mixture of 1,3-dioxolane (DOL) and dimethyl ethylene glycol (DME), with a total volume of 50 μL per cell. The prepared electrode sheets, along with positive / negative electrode shells, electrolyte, separator, spring, gasket, and lithium sheet, are assembled into CR-2032 button cells in an argon-filled ultrapure glove box.
[0060] Comparative Example 1 This comparative example provides a method for preparing a medium-entropy trimetallic organic framework material, the steps of which are as follows: Ni(CH3COO)2·3H2O (0.2484 g, 1.00 mmol) and 2,5-dihydroxyterephthalic acid (H4DHTA, 0.5944 g, 3.00 mmol) were placed in a ball mill at 1200 r / min, and zirconium beads were added at a ball-to-material ratio of 10:1. 1000 μL of H2O was added to the resulting reaction mixture, and after milling for 10 minutes, Co(CH3COO)2·3H2O (0.2491 g, 1.00 mmol) and 320 μL of H2O were added to the milling jar. After milling for 10 minutes, MgO (0.040 g, 1.00 mmol) and 100 μL of MeOH were added. The entire mixture was then milled for 20 minutes. The collected product was washed three times with MeOH and further dried overnight at 60 °C to obtain a medium-entropy trimetallic organometallic framework material, denoted as MOF-NCM.
[0061] CR-2032 button batteries were assembled using the medium-entropy trimetallic organic framework material of this comparative example, following the method of Example 2.
[0062] Comparative Example 2 This comparative example provides a method for preparing a low-entropy single-metal organic framework material, the steps of which are as follows: Ni(CH3COO)2·3H2O (0.2484 g, 1.00 mmol) and 2,5-dihydroxyterephthalic acid (H4DHTA, 0.198 g, 1.00 mmol) were placed in a ball mill at 1200 r / min, and zirconium beads were added at a ball-to-material ratio of 10:1. 300 μL of H2O was added to the reaction mixture, and the entire mixture was then milled at 1200 r / min for 20 minutes. The collected product was washed three times with MeOH and further dried overnight at 60 °C to obtain a low-entropy monometallic organic framework material, denoted as MOF-N.
[0063] CR-2032 button batteries were assembled using the low-entropy single-metal organic framework material of this comparative example, following the method of Example 2.
[0064] Impedance and electrochemical performance testing: EIS testing was performed using a CHI660E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd., China), with an amplitude of 5 mV. CV measurements were performed within the potential range of 1.7–2.8 V, with a scan rate of 0.1–0.5 mV·s. -1 Electrochemical performance tests were conducted on a LAND multichannel battery testing system, with a voltage range of 1.7–2.8 V.
[0065] Test Example 1: Physicochemical Property Characterization and Structural Verification Experiment of HMOF Material This test case aims to verify the crystal structure, chemical composition, and microstructure of the materials prepared in the examples and comparative examples, and to confirm the construction of the high-entropy metal framework through specific instrumental characterization data.
[0066] Experimental steps: The solid powder samples of metal-organic framework materials prepared in Example 1 and Comparative Examples 1-2 were placed in a vacuum drying oven and dried at 60°C for 12 hours to remove physically adsorbed moisture and solvent. Then, the dried samples were ground into fine powder of more than 200 mesh using an agate mortar.
[0067] The ground powder was tested using an X-ray powder diffractometer (XRD). The radiation source was set to Cu-Kα rays (λ=0.15406nm), the tube voltage was 40kV, the tube current was 40mA, the scanning range 2θ was 10° to 80°, and the scanning speed was set to 10° / min. The position and intensity of the diffraction peaks of each sample were recorded.
[0068] The tests were performed using Fourier transform infrared spectroscopy (FT-IR). 2 mg of the sample powder was mixed with 200 mg of dry potassium bromide powder, ground, and pressed into a tablet. The tablet was then heated at 500 cm⁻¹. -1 ~4000cm -1 Transmission scanning was performed within the wavenumber range, with a resolution set to 4 cm⁻¹. -1 A total of 32 scans were performed, and the infrared absorption spectra were recorded.
[0069] The surface morphology of the samples was observed using scanning electron microscopy (SEM). The sample powder was dispersed on a conductive adhesive, sputtered with gold, and then placed in the microscope vacuum chamber. Morphological images were captured at different magnifications under an accelerating voltage of 5–10 kV.
[0070] Accurately weigh 10 mg of sample powder and add it to a mixed acid solution of 3 mL concentrated nitric acid (68% by mass) and 5 mL hydrofluoric acid (45% by mass). Completely digest the solution in a microwave digester and bring the volume to 100 mL. Analyze the solution using inductively coupled plasma optical emission spectrometry (ICP-OES). Record the concentrations of nickel (Ni), cobalt (Co), copper (Cu), zinc (Zn), and magnesium (Mg) in Preparation Example 1, and calculate the configuration entropy S. conf .
[0071] The ICP test and configuration entropy calculation results of the materials in Example 1 and Comparative Example 1 are shown in Table 1.
[0072] Table 1. ICP test and configuration entropy calculation results of materials in Example 1 and Comparative Example 1 Figure 1 In (a), the horizontal axis represents the wavenumber, and the unit is cm. -1 The numerical range is from 500 to 4000; the vertical axis represents transmittance.
[0073] Figure 1 In (b), the horizontal axis is 2θ, the unit is degree, and the value ranges from 10 to 50; the vertical axis is intensity (au).
[0074] Figure 1 In the graph (c), the horizontal axis represents the pore width in nanometers (nm), ranging from 1 to 33; the vertical axis represents the density function of the pore size distribution (dV / dD, cm). 3 / g / nm); The inset shows the N2 adsorption-desorption isotherm, with the horizontal axis representing relative pressure (P / P0) and the vertical axis representing nitrogen uptake (cm). 3 / g).
[0075] Conclusion Analysis: Fourier transform infrared spectroscopy (FTIR) Figure 1 (a) Confirms that all three types of MOFs exhibit ligand-specific functional group signals. Compared with the pure ligand infrared spectra, the synthesized MOF-N, MOF-NCM, and HMOF-NCCZM show signals at 3300 cm⁻¹. -1 The OH stretching vibration has a broad peak at 1189 cm⁻¹. -1The complete disappearance of the in-plane bending vibration characteristic peak at the OH group indicates coordination between the metal ion and the ligand carboxyl group, confirming the successful synthesis of the target MOF material. HMOF-NCCZM shows a peak at 586 cm⁻¹. -1 The absorption peak intensity attributable to MO (M=Ni, Co, Cu, Zn, Mg) bonds is significantly higher than that of MOF-N and MOF-NCM, proving the formation of a stable multi-metal coordination framework.
[0076] X-ray diffraction pattern (XRD) Figure 1 (b) shows that the main peak positions of the three samples are basically consistent, indicating that despite the introduction of five metal ions with different radii and electronic structures, HMOF-NCCZM still maintains the MOF-74 crystal framework; the diffraction peaks match the standard Ni-MOF-74 card. During the ball milling synthesis process, the increase in the number of metal types did not destroy the long-range ordered structure of the high-entropy component; on the contrary, the crystallinity was better. This is attributed to the fact that the added Zn and Mg elements provided a certain degree of support for the structure. High crystallinity is conducive to the construction of stable channels, providing a structural basis for the physical interception and catalytic conversion of lithium polysulfides.
[0077] Nitrogen adsorption-desorption isotherms and pore size distribution ( Figure 1 (c) Analysis of the pore structure and specific surface area of HMOF-NCCZM confirmed that this MOF-74 derivative possesses a highly ordered microporous framework; the weak hysteresis loop in the high-pressure region (P / P0 > 0.4) indicates the presence of a small number of mesopores in the material. The micropores rely on the "molecular sieve effect" to physically trap long-chain lithium polysulfides (Li2S). n With n=2~8, the lithium sulfide conversion process is Li2S8→Li2S6→Li2S4+Li2S2), which confines it to the positive electrode side to alleviate the shuttle effect; the mesopores serve as ion transport channels to ensure the battery rate performance under high current.
[0078] Test Example 2: Assemble a button cell for cycle testing and mechanism verification. This test case aims to analyze the chemical anchoring of polysulfides and the cycle stability of the battery by the separator modified with high-entropy MOF material through actual testing.
[0079] Experimental steps: All electrochemical characterizations were performed in a half-cell configuration of a 2032 coin cell. Celgard 2500 polyolefin porous membranes were used as separators. A 15.6 mm diameter, 450 μm thick lithium metal disk was used as the counter electrode, while a 16 mm diameter polyethylene (PP) membrane or MOF@PP membrane was used as the separator. The electrolyte consisted of 1 mol L⁻¹ -1The battery consists of LiTFSI and 2% LiNO3 additives, dissolved in a 1:1 (v / v) mixture of 1,3-dioxolane (DOL) and dimethyl ethylene glycol (DME), with a total volume of approximately 50 μL per cell. In an argon-filled ultrapure glove box, the prepared electrode sheets were assembled with positive / negative electrode shells, electrolyte, separator, spring, gasket, and lithium foil to form a CR-2032 button cell.
[0080] After assembly, 1C rate cycling tests were performed on a LAND multichannel battery testing system, with a voltage range of 1.7–2.8 V. EIS testing was conducted using a CHI660E electrochemical workstation with an amplitude of 5 mV. CV measurements were performed within the 1.7–2.8 V potential range at scan rates of 0.1–0.5 mV s. -1 .
[0081] Lithium polysulfide deposition was tested on the LAND multi-channel battery testing system. The system discharged at a constant current of 0.112mA to 2.06V, and then discharged at a constant voltage of 2.05V until the current was 0.01mA, at which point the polysulfide deposition was complete.
[0082] Experimental data: Figure 2 In (a), the horizontal axis represents the cycle number, ranging from 1 to 2000; the vertical axis represents the specific capacity (mAh·g). -1 Coulombic efficiency (%)
[0083] Figure 2 In (b), the horizontal axis represents the cycle number, ranging from 1 to 26; the vertical axis represents the specific capacity (mAh·g). -1 Its sulfur loading is 12.36 mg / cm³. -2 .
[0084] Figure 2 In the graph (c), the horizontal axis represents the cycle number, ranging from 1 to 50; the vertical axis represents the specific capacity (mAh·g). -1 )).
[0085] Figure 2 In the diagram (d), the horizontal axis represents the real impedance (Z', hom), and the vertical axis represents the negative imaginary impedance (-Z'', hom).
[0086] Conclusion Analysis: At a rate of 1C ( Figure 2In (a), the initial discharge capacity of the LSB based on HMOF-NCCZM@PP reached 998.8 mAh / g. After 2000 cycles, at a relatively high current density of 1 C, the battery equipped with the HMOF-NCCZM@PP modified separator exhibited an extremely high initial discharge specific capacity (998.8 mAh / g), and the capacity retention curve remained extremely stable during long-term cycling, with the coulombic efficiency remaining close to 100%. In contrast, the capacity of the traditional PP separator or the single-metal / trimetallic control group showed rapid decay. The large number of unsaturated open metal sites (especially chalcophile Mg, Ni, etc.) exposed by the high-entropy MOF-74 lattice distortion efficiently adsorb long-chain lithium polysulfides (LiPSs) through MS bonds (metal-sulfur bonds). The unique confinement effect of MOF materials firmly fixes the intermediate state of lithium polysulfides and catalyzes their redox reaction, effectively suppressing the shuttle effect, thus giving the battery excellent long-cycle electrochemical stability (single-cycle decay rate of only 0.027%).
[0087] Under extreme operating conditions of high loading and lean electrolyte, the pentagonal high-entropy material induces the three-dimensional instantaneous nucleation and growth of the discharge product Li2S through multi-electron synergistic effects. This uniform micro-nano particle deposition releases the active space on the cathode surface, preventing uneven passivation of the insulating layer. The HMOF layer exhibits excellent electrolyte wettability, strong anchoring function for LiPS, and accelerated catalytic kinetics. The high-entropy sites significantly reduce the energy barriers of liquid-liquid conversion (Li2S8 ~ Li2S4) and liquid-solid conversion (Li2S4 ~ Li2S2 / Li2S), which not only enhances the chemical anchoring of polysulfides but also significantly improves the cycle stability of the battery under high sulfur loading by reducing the activation energy of sulfur redox reactions.
[0088] Electrochemical tests at different magnifications ( Figure 2 In the middle (c), as the charge / discharge rate gradually increases from low to high (2C), the battery equipped with the high-entropy modified separator exhibits extremely smooth capacity decay, maintaining a high proportion of capacity output even at the high current of 2C; when the current density returns to the low rate, the capacity achieves near 100% perfect recovery. This is attributed to the highly dispersed and synergistic interaction of transition metal sites such as Ni, Co, and Cu at the atomic level, constructing a high-flux "directional catalytic ion channel," significantly reducing the reaction energy barrier of liquid-solid and solid-liquid phase transitions, enabling the battery to maintain extremely fast redox reaction kinetics even at high currents. Simultaneously, HMOF-NCCZM possesses a very large specific surface area (927.02 m²). 2 / g) and highly ordered sub-nanometer micropores, while ensuring the physical confinement of polysulfides, promote the development of Li + Ion transport reduces concentration polarization.
[0089] Impedance spectra are typically composed of a semicircle in the high-frequency region (representing charge transfer impedance R). ct It consists of the slanted lines in the low-frequency region (representing the Warburg impedance of lithium-ion diffusion). Figure 2 As shown in (d), the battery using the HMOF-NCCZM@PP modified separator exhibits a significantly smaller semi-circular diameter in the high-frequency region compared to the pure PP separator and other control groups, both before and after cycling. Furthermore, the slope of the low-frequency curve is steeper, confirming that the multi-metal synergistic catalytic sites within the high-entropy framework effectively accelerate the electron exchange and interfacial charge transfer processes between the liquid polysulfide and the solid phase (Li2S2 / Li2S). The steeper low-frequency curve indicates that the excellent wettability between the modified layer and the electrolyte, along with the ordered open pore structure, effectively reduces the mass transfer resistance of the system, thereby significantly improving the lithium-ion diffusion kinetics.
[0090] The above results indicate that the high-entropy metal-organic framework (HMOF-NCCZM) modified separator (HMOF-NCCZM@PP) placed between the positive electrode and the lithium metal anode in a lithium-sulfur battery not only effectively reduces electrochemical polarization but also significantly improves the redox reaction rate of LiPS. It constructs a directional catalytic ion channel, lowers the liquid-solid phase transition energy barrier, and its unique confinement effect and multi-metal catalytic sites can regulate the Li2S growth path to accelerate the stepwise redox conversion of lithium polysulfides, thereby optimizing the battery's cycle performance.
[0091] The test results of Test Example 2 fully demonstrate that the high-entropy MOF material synthesized by ball milling optimizes the key electrochemical indicators of lithium-sulfur batteries through "active catalysis + physical / chemical dual confinement".
[0092] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a quinary high-entropy metal-organic framework material by a ball milling method, characterized in that, Includes the following steps: Using 2,5-dihydroxyterephthalic acid as an organic ligand, and metal acetates containing nickel, cobalt, and copper, and metal oxides containing zinc and magnesium as metal sources, the reaction was carried out by ball milling. After washing and drying, the five-element high-entropy metal-organic framework material was obtained.
2. The method for preparing pentagonal high-entropy metal-organic framework materials by ball milling according to claim 1, characterized in that, The molar ratio of the 2,5-dihydroxyterephthalic acid, the metal acetate containing nickel, cobalt, and copper, and the metal oxide containing zinc and magnesium is 3:1:1:1:1:
1.
3. The method for preparing pentagonal high-entropy metal-organic framework materials by ball milling according to claim 2, characterized in that, The metal acetates containing nickel, cobalt, and copper are Ni(CH3COO)2·3H2O, Co(CH3COO)2·3H2O, and Cu(CH3COO)2·H2O; The metal oxides containing zinc and magnesium are ZnO and MgO.
4. The method for preparing pentagonal high-entropy metal-organic framework materials by ball milling according to claim 1, characterized in that, The ball milling speed is 1000~1200 r / min, the ball-to-material ratio is 8:1~10:1, and the grinding balls are zirconium beads.
5. The method for preparing pentagonal high-entropy metal-organic framework materials by ball milling according to claim 1, characterized in that, Water and methanol were added during ball milling.
6. A pentagonal high-entropy metal-organic framework material, characterized in that, It is prepared according to any one of claims 1 to 5.
7. The application of the pentagonal high-entropy metal-organic framework material as described in claim 6 in the preparation of lithium-sulfur battery separators.
8. A method for modifying a lithium-sulfur battery separator using the pentagonal high-entropy metal-organic framework material as described in claim 6, characterized in that, Includes the following steps: A uniform slurry is prepared by mixing conductive materials, binders, organic solvents, and the pentagonal high-entropy metal-organic framework material. The uniform slurry was coated onto the surface of a polypropylene membrane and then vacuum dried to obtain a high-entropy metal-organic framework functional modified membrane.
9. The method for modifying a lithium-sulfur battery separator according to claim 8, characterized in that, The conductive material is conductive carbon; the binder is polyvinylidene fluoride; and the organic solvent is N-methylpyrrolidone.
10. The application of a lithium-sulfur battery separator modified according to any one of claims 8 to 9 in the preparation of lithium-sulfur batteries.