A low-temperature resistant and crack-resistant cable material and its preparation method
By leveraging the synergistic effects of soybean oil-grafted polyisoprene, polyester plasticizer, and silane-grafted polyethylene wax, the problem of brittleness in polyethylene cable materials at low temperatures was solved, achieving the preparation of cable materials with high toughness and good processing performance.
Patent Information
- Application Number
- CN202611297285.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Polyethylene cable materials are prone to brittleness at low temperatures, and existing modification methods cannot simultaneously meet the requirements for low-temperature toughness, crack resistance, and processing fluidity.
Cable materials are prepared by melt extrusion using components such as soybean oil-grafted polyisoprene, polyester plasticizer, and silane-grafted polyethylene wax. The three-dimensional structure of the hyperbranched polyester plasticizer improves the interfacial wettability and dispersion uniformity, the soybean oil-grafted polyisoprene forms a rubber microphase to improve toughness, and the silane-grafted polyethylene wax provides lubrication and dispersion.
It significantly improves the low-temperature crack resistance and processing fluidity of cable materials, reduces the embrittlement temperature, and enhances overall flexibility and crack resistance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable material preparation technology, specifically a low-temperature resistant and crack-resistant cable material and its preparation method. Background Technology
[0002] Polyethylene (PE) is widely used as insulation and sheathing material for cables due to its excellent electrical insulation, chemical resistance, processability, and relatively low cost. However, PE has poor resistance to environmental stress cracking and is prone to brittleness and cracking at low temperatures, severely limiting its outdoor applications in cold regions. The fundamental reason for PE's low-temperature brittleness lies in the presence of numerous stress defects at the interface between its crystalline and amorphous regions. Under external forces, microcracks easily propagate rapidly along grain boundaries, leading to brittle fracture of the material at temperatures far above its glass transition temperature.
[0003] In existing technologies, the low-temperature crack resistance of polyethylene is generally improved by adding elastomers and plasticizers. When using small-molecule plasticizers for modification, migration and precipitation are prone to occur under long-term heating and external force, resulting in material performance deterioration. Although large-molecule plasticizers have a certain degree of migration resistance, their functions are relatively singular and it is difficult to simultaneously meet the multiple requirements of low-temperature toughness, crack resistance, and processing fluidity.
[0004] In summary, to solve the above problems, this invention proposes a low-temperature resistant and crack-resistant cable material and its preparation method. Summary of the Invention
[0005] The purpose of this invention is to provide a low-temperature resistant and crack-resistant cable material and its preparation method, so as to solve the problems mentioned in the background art.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: A low-temperature resistant and crack-resistant cable material comprises the following components by weight: 80-100 parts polyethylene, 5-10 parts soybean oil-grafted polyisoprene, 3-5 parts polyester plasticizer, 5-10 parts silane-grafted polyethylene wax, 5-10 parts polyolefin elastomer, 5-10 parts filler, 0.3-0.5 parts stabilizer, and 0.1-0.5 parts antioxidant.
[0007] A method for preparing a low-temperature resistant and crack-resistant cable material includes the following steps: Polyethylene, soybean oil-grafted polyisoprene, polyester plasticizer, silane-grafted polyethylene wax, polyolefin elastomer, filler, stabilizer, and antioxidant are mixed and melt-extruded at 160-200℃ to obtain cable material.
[0008] In a more optimized manner, polyester plasticizers are prepared by the following process: Step 1: Mix 2-carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane, add p-toluenesulfonic acid, and react at 155-165℃ for 8-10 h under nitrogen atmosphere protection; then continue the reaction at 0.095-0.098 MPa for 1-2 h to obtain carboxylated polyester. Step 2: Add the carboxylated polyester to n-butanol and reflux at 155-165℃ for 3-4 hours; then continue the reaction at 0.095-0.098MPa for 1-2 hours to obtain alkyl-linked branched polyester. Step 3: Add alkyl-linked polyester, 3-isocyanate-propyltriethoxysilane (IPTS), and dibutyltin dilaurate to anhydrous methyl ethyl ketone. Under nitrogen atmosphere protection, reflux reaction at 70-78℃ for 4-6 hours, followed by vacuum distillation to obtain polyester plasticizer.
[0009] In a more optimized manner, in step 1, the molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane is (1.4-1.6):1; The mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid is 1:(0.01-0.03).
[0010] In a more optimized manner, in step 2, the mass ratio of carboxylated polyester to n-butanol is 1:(0.28-0.32).
[0011] In a more optimized manner, in step 3, the mass ratio of alkyl-linked polyester to IPTS is 1:(0.05-0.1). The mass ratio of alkyl-linked polyester to dibutyltin dilaurate is 100:(0.1-0.3). The mass ratio of alkyl-linked polyester to anhydrous methyl ethyl ketone is 1:(4-6).
[0012] In a more optimized manner, soybean oil-grafted polyisoprene is prepared by the following steps: (1) 2,2'-thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene and di-tert-butyl peroxide are mixed and reacted for 12-16 h under nitrogen atmosphere protection, 120-130℃ and 500-600 rpm. After precipitation, centrifugation, dissolution and drying, carboxylated polyisoprene is obtained. (2) Carboxylated polyisoprene and epoxidized soybean oil were added to toluene, and triphenylphosphine was added. The mixture was reacted at 90-110℃ for 2-3 hours to obtain soybean oil grafted polyisoprene.
[0013] In a more optimized manner, in step (1), the mass ratio of 2,2'-thiocarbonyl (sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide is 1:(60-80):(100-120):(0.2-0.3).
[0014] In a more optimized manner, in step (2), the mass ratio of carboxylated polyisoprene to epoxidized soybean oil is 1:(0.5-1). The ratio of carboxylated polyisoprene to toluene was 1 g: (4-8) mL; The mass ratio of carboxylated polyisoprene to triphenylphosphine is 1:(0.01-0.02).
[0015] In a more optimized manner, silane-grafted polyethylene wax is prepared by the following process: polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 are mixed evenly and melt-extruded at 160-180°C to obtain silane-grafted polyethylene wax.
[0016] The optimal mass ratio of polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 is 100:(5-15):(0.5-2):(0.1-0.3).
[0017] Ideally, the filler should be one or a mixture of two of magnesium hydroxide and silicon dioxide; The stabilizer used is a calcium-zinc stabilizer; The antioxidant used is antioxidant 1010.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are: 1. The polyester plasticizer of this invention uses diacids and polyols as raw materials, synthesizing a hyperbranched polyester skeleton through a polycondensation reaction. Then, it undergoes alkyl chain end-capping modification with n-butanol to construct a non-polar alkyl chain shell around the hyperbranched polyester, solving the compatibility problem between polar groups and the polyethylene matrix. Finally, it undergoes end-silylation treatment with isocyanate-based silanes, resulting in a molecule with a n-propyl-containing triethoxysilane group at the molecule's end. The non-polar n-propyl segment forms van der Waals interactions with the polyethylene matrix to improve the plasticizer's interfacial wettability and dispersion uniformity. Simultaneously, increasing the end-group volume inhibits... The plasticizer exhibits a unique three-dimensional structure, providing excellent intermolecular lubrication in polyethylene melts, significantly reducing melt viscosity and improving processing fluidity. Simultaneously, its hyperbranched structure induces polyethylene crystallization, refining grains and increasing crystallinity, thereby improving the tensile strength of cable materials while reducing processing viscosity. Furthermore, grain refinement increases grain boundary density, makes crack propagation paths more tortuous, and improves stress distribution uniformity, effectively inhibiting the initiation and propagation of microcracks under low-temperature conditions and enhancing the low-temperature crack resistance of cable materials.
[0019] 2. The soybean oil-grafted polyisoprene of this invention is prepared by reacting carboxylated polyisoprene with epoxidized soybean oil. The polyisoprene backbone has excellent flexibility and a low glass transition temperature, which can form a rubber microphase inside the polyethylene matrix, giving the blend system high ductility. Under external force, it can dissipate fracture energy and improve the low-temperature crack resistance of cable materials. At the same time, the polar ester segments of epoxidized soybean oil are distributed at the interface between the rubber microphase and the polyethylene matrix, which significantly improves the interface wettability and bonding force, and inhibits premature debonding of the two-phase interface under stress. When microcracks extend to the rubber microphase region, the rubber phase can effectively passivate the crack tip and prevent the microcracks from developing into macroscopic cracks.
[0020] 3. In this invention, during the melting stage, the polyester plasticizer, with its hyperbranched three-dimensional structure, acts as a lubricant between polyethylene molecular chains, reducing inter-chain frictional resistance. During the cooling stage after melt extrusion, the polyester plasticizer induces grain refinement, reducing stress defects at the interfaces between crystalline and amorphous regions. This improves the intrinsic low-temperature mobility and crystal morphology of the polyethylene matrix at the molecular level, laying the structural foundation for the uniform dispersion and interfacial bonding of the soybean oil-grafted polyisoprene rubber microphase. The soybean oil-grafted polyisoprene then undergoes shearing under external force in the form of a polyisoprene rubber microphase. The yielding and creasing processes efficiently dissipate fracture energy, and the polar ester groups of the epoxidized soybean oil grafted segments improve the wettability and bonding force between the rubber microphase and the matrix. The polyester plasticizer reduces the intermolecular forces, making the cable material more flexible overall and delaying crack initiation. Once a crack initiates and extends to the rubber microphase region, the soybean oil-grafted polyisoprene terminates the crack through mechanisms such as creasing, shear yielding, and crack tip passivation. The synergistic effect of these two processes significantly reduces the embrittlement temperature of the cable material and greatly improves its resistance to environmental stress cracking.
[0021] 4. This invention compensates for the shortcomings of polyethylene in low-temperature toughness and crack resistance by synergistic compounding of various functional components. The silane-grafted polyethylene wax uses polyethylene wax as a skeleton and introduces vinyltrimethoxysilane into the side groups of the molecular chain through a melt grafting reaction. The polyethylene wax skeleton has good compatibility with the polyethylene matrix and can provide excellent lubrication and dispersion during processing, improve the dispersion uniformity of each component in the matrix, and enhance the overall cohesive strength and crack resistance of the cable material. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] It should be noted that the following quantities are by weight. There are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: the polyethylene grade is DFDA-7042; the polyolefin elastomer grade is DF740; the average particle size of magnesium hydroxide is 1 μm; the average particle size of silica is 1 μm; the CAS number of 2,2'-thiocarbonyl(thio)bis(2-methylpropionic acid) is 355120-40-0; and the remaining raw materials are commercially available.
[0024] Example 1: A method for preparing a low-temperature resistant and crack-resistant cable material, comprising the following steps: S1: Preparation of polyester plasticizer S1-1: 2-Carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane were mixed, and p-toluenesulfonic acid was added. The mixture was reacted at 160°C for 9 h under a nitrogen atmosphere. Then, the reaction was continued for 1.5 h at 0.096 MPa to obtain a carboxylated polyester. The molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane was 1.5:1; the mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid was 1:0.02. S1-2: The carboxylated polyester was added to n-butanol and refluxed at 160°C for 3.5 h; then the reaction was continued at 0.096 MPa for 1.5 h to obtain alkyl-linked polyester; the mass ratio of carboxylated polyester to n-butanol was 1:0.3. S1-3: Alkyl-linked polyester, IPTS, and dibutyltin dilaurate were added to anhydrous methyl ethyl ketone (MEK). The mixture was refluxed at 75°C for 5 hours under nitrogen atmosphere and then subjected to vacuum distillation to obtain a polyester plasticizer. The mass ratio of alkyl-linked polyester to IPTS was 1:0.08; the mass ratio of alkyl-linked polyester to dibutyltin dilaurate was 100:0.2; and the mass ratio of alkyl-linked polyester to anhydrous MEK was 1:5. S2: Preparation of soybean oil-grafted polyisoprene S2-1: 2,2'-Thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide were mixed and reacted at 125°C and 550 rpm for 14 h under nitrogen atmosphere protection. After precipitation, centrifugation, dissolution, and drying, carboxylated polyisoprene was obtained. The mass ratio of 2,2'-thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide was 1:60:110:0.25. S2-2: Carboxylated polyisoprene and epoxidized soybean oil were added to toluene, and triphenylphosphine was added. The mixture was reacted at 100℃ for 2.5 h to obtain soybean oil-grafted polyisoprene. The mass ratio of carboxylated polyisoprene to epoxidized soybean oil was 1:0.8; the ratio of carboxylated polyisoprene to toluene was 1 g:6 mL; and the mass ratio of carboxylated polyisoprene to triphenylphosphine was 1:0.015. S3: Preparation of silane-grafted polyethylene wax Polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 were mixed evenly and melt-extruded at 170°C to obtain silane-grafted polyethylene wax; the mass ratio of polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 was 100:10:1:0.2. S4: Preparation of cable materials Polyethylene, soybean oil-grafted polyisoprene, polyester plasticizer, silane-grafted polyethylene wax, polyolefin elastomer, magnesium hydroxide, calcium-zinc stabilizer, and antioxidant 1010 are mixed and melt-extruded at 180°C to obtain cable material. The cable material comprises the following components by weight: 90 parts polyethylene, 8 parts soybean oil-grafted polyisoprene, 4 parts polyester plasticizer, 8 parts silane-grafted polyethylene wax, 8 parts polyolefin elastomer, 8 parts magnesium hydroxide, 0.4 parts calcium-zinc stabilizer, and 0.3 parts antioxidant 1010.
[0025] Example 2: A method for preparing a low-temperature resistant and crack-resistant cable material, comprising the following steps: S1: Preparation of polyester plasticizer S1-1: 2-Carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane were mixed, and p-toluenesulfonic acid was added. The mixture was reacted at 155°C for 10 h under a nitrogen atmosphere. Then, the reaction was continued for 2 h at 0.095 MPa to obtain a carboxylated polyester. The molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane was 1.4:1; the mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid was 1:0.01. S1-2: The carboxylated polyester was added to n-butanol and refluxed at 155°C for 4 hours; then the reaction was continued at 0.095 MPa for 2 hours to obtain alkyl-linked polyester; the mass ratio of carboxylated polyester to n-butanol was 1:0.28. S1-3: Alkyl-linked polyester, IPTS, and dibutyltin dilaurate were added to anhydrous methyl ethyl ketone (MEK). The mixture was refluxed at 70°C for 6 hours under nitrogen atmosphere and then subjected to vacuum distillation to obtain a polyester plasticizer. The mass ratio of alkyl-linked polyester to IPTS was 1:0.05; the mass ratio of alkyl-linked polyester to dibutyltin dilaurate was 100:0.1; and the mass ratio of alkyl-linked polyester to anhydrous MEK was 1:4. S2: Preparation of soybean oil-grafted polyisoprene S2-1: 2,2'-Thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide were mixed and reacted at 120°C and 500 rpm for 16 h under nitrogen atmosphere protection. After precipitation, centrifugation, dissolution, and drying, carboxylated polyisoprene was obtained. The mass ratio of 2,2'-thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide was 1:60:100:0.2. S2-2: Carboxylated polyisoprene and epoxidized soybean oil were added to toluene, and triphenylphosphine was added. The mixture was reacted at 90°C for 3 hours to obtain soybean oil-grafted polyisoprene. The mass ratio of carboxylated polyisoprene to epoxidized soybean oil was 1:0.5; the ratio of carboxylated polyisoprene to toluene was 1 g:4 mL; and the mass ratio of carboxylated polyisoprene to triphenylphosphine was 1:0.01. S3: Preparation of silane-grafted polyethylene wax Polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 were mixed evenly and melt-extruded at 160°C to obtain silane-grafted polyethylene wax; the mass ratio of polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 was 100:5:0.5:0.1. S4: Preparation of cable materials Polyethylene, soybean oil-grafted polyisoprene, polyester plasticizer, silane-grafted polyethylene wax, polyolefin elastomer, silica, calcium-zinc stabilizer, and antioxidant 1010 are mixed and melt-extruded at 160°C to obtain cable material. The cable material comprises the following components by weight: 80 parts polyethylene, 5 parts soybean oil-grafted polyisoprene, 3 parts polyester plasticizer, 5 parts silane-grafted polyethylene wax, 5 parts polyolefin elastomer, 5 parts silica, 0.3 parts calcium-zinc stabilizer, and 0.1 parts antioxidant 1010.
[0026] Example 3: A method for preparing a low-temperature resistant and crack-resistant cable material, comprising the following steps: S1: Preparation of polyester plasticizer S1-1: 2-Carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane were mixed, and p-toluenesulfonic acid was added. The mixture was reacted at 165°C for 8 hours under a nitrogen atmosphere. Then, the reaction was continued for 2 hours at 0.098 MPa to obtain a carboxylated polyester. The molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane was 1.6:1; the mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid was 1:0.03. S1-2: The carboxylated polyester was added to n-butanol and refluxed at 165°C for 3 hours; then the reaction was continued at 0.098 MPa for 1 hour to obtain alkyl-linked polyester; the mass ratio of carboxylated polyester to n-butanol was 1:0.32. S1-3: Alkyl-linked polyester, IPTS, and dibutyltin dilaurate were added to anhydrous methyl ethyl ketone (MEK). The mixture was refluxed at 78°C for 4 hours under nitrogen atmosphere and then subjected to vacuum distillation to obtain a polyester plasticizer. The mass ratio of alkyl-linked polyester to IPTS was 1:0.1; the mass ratio of alkyl-linked polyester to dibutyltin dilaurate was 100:0.3; and the mass ratio of alkyl-linked polyester to anhydrous MEK was 1:6. S2: Preparation of soybean oil-grafted polyisoprene S2-1: 2,2'-Thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide were mixed and reacted at 130°C and 600 rpm for 12 h under nitrogen atmosphere protection. After precipitation, centrifugation, dissolution, and drying, carboxylated polyisoprene was obtained. The mass ratio of 2,2'-thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide was 1:80:120:0.3. S2-2: Carboxylated polyisoprene and epoxidized soybean oil were added to toluene, and triphenylphosphine was added. The mixture was reacted at 110℃ for 2 hours to obtain soybean oil-grafted polyisoprene. The mass ratio of carboxylated polyisoprene to epoxidized soybean oil was 1:1; the ratio of carboxylated polyisoprene to toluene was 1 g: 8 mL; and the mass ratio of carboxylated polyisoprene to triphenylphosphine was 1:0.02. S3: Preparation of silane-grafted polyethylene wax Polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 were mixed evenly and melt-extruded at 180°C to obtain silane-grafted polyethylene wax; the mass ratio of polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 was 100:15:2:0.3. S4: Preparation of cable materials Polyethylene, soybean oil-grafted polyisoprene, polyester plasticizer, silane-grafted polyethylene wax, polyolefin elastomer, filler, calcium-zinc stabilizer, and antioxidant 1010 are mixed and melt-extruded at 200°C to obtain cable material; the filler is magnesium hydroxide and silicon dioxide, with a mass ratio of magnesium hydroxide to silicon dioxide of 3:2. The cable material comprises the following components by weight: 100 parts polyethylene, 10 parts soybean oil-grafted polyisoprene, 5 parts polyester plasticizer, 10 parts silane-grafted polyethylene wax, 10 parts polyolefin elastomer, 10 parts filler, 0.5 parts calcium-zinc stabilizer, and 0.5 parts antioxidant 1010.
[0027] Comparative Example 1: No polyester plasticizer added; otherwise the same as Example 2; specific differences are as follows: The cable material comprises the following components by weight: 80 parts polyethylene, 5 parts soybean oil-grafted polyisoprene, 5 parts silane-grafted polyethylene wax, 5 parts polyolefin elastomer, 5 parts silica, 0.3 parts calcium-zinc stabilizer, and 0.1 parts antioxidant 1010.
[0028] Comparative Example 2: No soybean oil-grafted polyisoprene was added; otherwise, it was the same as Example 2; the specific differences are as follows: The cable material comprises the following components by weight: 80 parts polyethylene, 3 parts polyester plasticizer, 5 parts silane-grafted polyethylene wax, 5 parts polyolefin elastomer, 5 parts silica, 0.3 parts calcium-zinc stabilizer, and 0.1 parts antioxidant 1010.
[0029] Comparative Example 3: The preparation method of the polyester plasticizer was adjusted; the rest was the same as in Example 2; the specific differences are as follows: S1: Preparation of polyester plasticizer S1-1: 2-Carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane were mixed, and p-toluenesulfonic acid was added. The mixture was reacted at 155°C for 10 h under a nitrogen atmosphere. Then, the reaction was continued for 2 h at 0.095 MPa to obtain a carboxylated polyester. The molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane was 1.4:1; the mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid was 1:0.01. S1-2: Carboxylated polyester, IPTS, and dibutyltin dilaurate were added to anhydrous methyl ethyl ketone (MEK). The mixture was refluxed at 70°C for 6 hours under nitrogen atmosphere and then distilled under reduced pressure to obtain a polyester plasticizer. The mass ratio of carboxylated polyester to IPTS was 1:0.05; the mass ratio of carboxylated polyester to dibutyltin dilaurate was 100:0.1; and the mass ratio of carboxylated polyester to anhydrous MEK was 1:4.
[0030] Comparative Example 4: The preparation method of the polyester plasticizer was adjusted; the rest was the same as in Example 2; the specific differences are as follows: S1: Preparation of polyester plasticizer S1-1: 2-Carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane were mixed, and p-toluenesulfonic acid was added. The mixture was reacted at 155°C for 10 h under a nitrogen atmosphere. Then, the reaction was continued for 2 h at 0.095 MPa to obtain a carboxylated polyester. The molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane was 1.4:1; the mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid was 1:0.01. S1-2: Carboxylated polyester was added to n-butanol and refluxed at 155°C for 4 hours; then the reaction was continued at 0.095 MPa for 2 hours to obtain polyester plasticizer; the mass ratio of carboxylated polyester to n-butanol was 1:0.28.
[0031] Comparative Example 5: Soybean oil grafted with polyisoprene was replaced with polyisoprene and epoxidized soybean oil; the rest was the same as in Example 2; the specific differences are as follows: The cable material comprises the following components by weight: 80 parts polyethylene, 3 parts polyisoprene, 2 parts epoxidized soybean oil, 3 parts polyester plasticizer, 5 parts silane-grafted polyethylene wax, 5 parts polyolefin elastomer, 5 parts silica, 0.3 parts calcium-zinc stabilizer, and 0.1 parts antioxidant 1010.
[0032] Experiment: The cable materials prepared in the examples and comparative examples were used as samples for performance testing. Tensile strength and elongation at break test: The tensile strength and elongation at break of the sample were tested at a tensile speed of 20 mm / min, in accordance with the standard GB / T 2951.11-2008. Low-temperature impact embrittlement performance: According to the standard GB / T 5470-2008, the low-temperature impact embrittlement performance of the samples at -50℃ is tested, and the appearance of cracks on the sample surface is observed; for each group of 30 samples, the number of cracks should not exceed 15 to be considered qualified; Environmental stress cracking resistance: Referring to GB / T 2951.41-2008, the samples were placed in a 10% (v / v) nonylphenol polyoxyethylene ether aqueous solution and tested for environmental stress cracking resistance at 50°C. The time when 50% of the samples showed cracking was recorded, i.e., F. 50 Value; 10 samples per group.
[0033] Conclusion: The data in the table above shows that: The low-temperature resistant and crack-resistant cable materials prepared in Examples 1-3 exhibit excellent performance, indicating that the present invention achieves a significant improvement in the comprehensive performance of the cable materials through the synergistic effects of molecular lubrication and heterogeneous nucleation of polyester plasticizer, energy dissipation and crack passivation of the rubber microphase of soybean oil grafted polyisoprene, and lubrication and dispersion of silane grafted polyethylene wax.
[0034] Comparative Example 1, based on Example 2, did not include polyester plasticizer, and the overall performance of the cable material deteriorated. This indicates that the hyperbranched structure of the polyester plasticizer plays an intermolecular lubrication and heterogeneous nucleation role in the polyethylene matrix, and is a key component for improving the tensile strength, toughness and crack resistance of the cable material.
[0035] Comparative Example 2 is based on Example 2, without the addition of soybean oil-grafted polyisoprene. The overall performance of the cable material deteriorates, which illustrates the importance of the rubber microphase formed by soybean oil-grafted polyisoprene in dissipating fracture energy and blunting crack tips at low temperatures through shear yielding and creasing.
[0036] Comparative Example 3 is based on Example 2. The polyester plasticizer was not modified by n-butanol alkyl chain end-capping, resulting in a deterioration in the overall performance of the cable material. This is because the hyperbranched polyester without n-butanol end-capping contains a large number of polar carboxyl groups, which have poor compatibility with the polyethylene matrix. This leads to uneven dispersion of the plasticizer in the matrix, forming a large number of stress concentration points, which seriously degrades the performance of the cable material.
[0037] Comparative Example 4 is based on Example 2. The polyester plasticizer was not modified with IPTS end groups, that is, it was only capped with n-butanol without introducing triethoxysilane end groups. The overall performance of the cable material deteriorated. This is because the van der Waals interaction between the n-propyl nonpolar segment in the triethoxysilane end group and the polyethylene molecular chain was weakened. The volume of the plasticizer molecule end group was reduced, and it was easier to migrate and precipitate during long-term use, resulting in the degradation of material performance.
[0038] Comparative Example 5, based on Example 2, replaced soybean oil-grafted polyisoprene with a physical blend of polyisoprene and epoxidized soybean oil. The overall performance of the cable material deteriorated, indicating that when epoxidized soybean oil and polyisoprene are not chemically grafted, they are only physically blended. Epoxidized soybean oil cannot effectively improve the interfacial wettability between the polyisoprene rubber microphase and the polyethylene matrix. Under stress, the interface between the two phases is prone to debonding, and the long-term toughening effect brought by chemical bonding cannot be exerted.
[0039] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a low-temperature resistant and crack-resistant cable material, characterized in that: Includes the following steps: Polyethylene, soybean oil-grafted polyisoprene, polyester plasticizer, silane-grafted polyethylene wax, polyolefin elastomer, filler, stabilizer, and antioxidant are mixed and melt-extruded to obtain cable material. The polyester plasticizer is prepared by reacting 2-carboxyethylphenylphosphine with 1,1,1-trimethylolpropane, esterifying with n-butanol, and modifying with 3-isocyanate-propyltriethoxysilane end groups. The soybean oil-grafted polyisoprene is prepared by reacting carboxylated polyisoprene with epoxidized soybean oil.
2. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 1, characterized in that: The polyester plasticizer is prepared by the following process: Step 1: Mix 2-carboxyethylphenylphosphonic acid and 1,1,1-trimethylolpropane, add p-toluenesulfonic acid, and react at 155-165℃ for 8-10 h under nitrogen atmosphere protection; then continue the reaction at 0.095-0.098 MPa for 1-2 h to obtain carboxylated polyester. Step 2: Add the carboxylated polyester to n-butanol and reflux at 155-165℃ for 3-4 hours; then continue the reaction at 0.095-0.098MPa for 1-2 hours to obtain alkyl-linked branched polyester. Step 3: Add alkyl-linked polyester, 3-isocyanate-propyltriethoxysilane, and dibutyltin dilaurate to anhydrous butanone. Under nitrogen atmosphere protection, reflux reaction at 70-78℃ for 4-6 hours, followed by vacuum distillation to obtain polyester plasticizer.
3. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 1, characterized in that: The soybean oil-grafted polyisoprene is prepared by the following steps: (1) 2,2'-thiocarbonyl(sulfur)bis(2-methylpropionic acid), dioxane, isoprene and di-tert-butyl peroxide are mixed and reacted for 12-16 h under nitrogen atmosphere protection, 120-130℃ and 500-600 rpm. After precipitation, centrifugation, dissolution and drying, carboxylated polyisoprene is obtained. (2) Carboxylated polyisoprene and epoxidized soybean oil were added to toluene, and triphenylphosphine was added. The mixture was reacted at 90-110℃ for 2-3 hours to obtain soybean oil grafted polyisoprene.
4. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 2, characterized in that: In step 1, the molar ratio of 2-carboxyethylphenylphosphonic acid to 1,1,1-trimethylolpropane is (1.4-1.6):1; The mass ratio of 1,1,1-trimethylolpropane to p-toluenesulfonic acid is 1:(0.01-0.03).
5. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 2, characterized in that: In step 2, the mass ratio of the carboxylated polyester to n-butanol is 1:(0.28-0.32). In step 3, the mass ratio of the alkyl-linked branched polyester to 3-isocyanate-propyltriethoxysilane is 1:(0.05-0.1).
6. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 3, characterized in that: In step (1), the mass ratio of 2,2'-thiocarbonyl (sulfur)bis(2-methylpropionic acid), dioxane, isoprene, and di-tert-butyl peroxide is 1:(60-80):(100-120):(0.2-0.3).
7. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 3, characterized in that: In step (2), the mass ratio of carboxylated polyisoprene to epoxidized soybean oil is 1:(0.5-1).
8. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 1, characterized in that: The silane-grafted polyethylene wax is prepared by the following process: polyethylene wax, vinyltrimethoxysilane, dicumyl peroxide, and antioxidant 1010 are mixed evenly and then melt-extruded at 160-180°C to obtain silane-grafted polyethylene wax.
9. The method for preparing a low-temperature resistant and crack-resistant cable material according to claim 1, characterized in that: The filler is one or a mixture of two of magnesium hydroxide and silicon dioxide. The stabilizer used is a calcium-zinc stabilizer; The antioxidant used is antioxidant 1010.
10. The cable material prepared by the method for preparing a low-temperature resistant and crack-resistant cable material according to any one of claims 1-9, characterized in that: It includes the following components by weight: 80-100 parts polyethylene, 5-10 parts soybean oil-grafted polyisoprene, 3-5 parts polyester plasticizer, 5-10 parts silane-grafted polyethylene wax, 5-10 parts polyolefin elastomer, 5-10 parts filler, 0.3-0.5 parts stabilizer, and 0.1-0.5 parts antioxidant.