A high-toughness modified PS foam floor protective film underlayment material and its preparation method

By adjusting the formulation and process of PS foam material and using chemical and butane physical foaming methods, a modified PS foam padding material with high toughness and compressive strength was prepared. This solved the brittleness and compatibility problems of existing materials, and enabled continuous winding and thermal bonding of the material, thus improving the floor protection effect on construction sites.

CN123107261APending Publication Date: 2026-11-17HEBEI DAI SI DECORATION MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611453938.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PS foam materials, when used as a protective film layer for ground surfaces, suffer from high brittleness, poor resistance to trampling, crushing, and bending, making them unsuitable for rolling and incompatible with continuous thermal composite roll production processes for protective films. This results in materials that are prone to cracking, crumbling, and rapid aging under sunlight.

Method used

By adjusting the formula and optimizing the preparation process, using chemical foaming and butane physical foaming methods, and employing GPPS/HIPS polystyrene, POE/EVA elastomer toughening agent, reinforcing filler and functional additives, and controlling the cell structure and foaming parameters, a high-toughness modified PS foamed floor protective film underlayment material was prepared, ensuring the material's toughness, compressive strength and compatibility.

Benefits of technology

The material exhibits high toughness, excellent pressure resistance and cushioning performance, and a uniform and dense cell structure, making it suitable for continuous winding and thermal lamination. This solves the problem of material use on construction sites, reduces costs, and improves performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to a high-toughness modified PS foam floor protective film underlayment material and its preparation method, including two formulations and preparation methods: chemical foaming and butane physical foaming. The basic formulation consists of: GPPS / HIPS polystyrene, POE / EVA elastomer toughening agent, reinforcing filler, AC chemical foaming agent (physical nucleating agent), lubricant / dispersant, and functional additives. The preparation method includes: (1) raw material pretreatment and mixing; (2) extrusion melt plasticizing; (3) pressure foaming process; (4) extrusion molding process; and (5) post-treatment and composite process. This invention improves traditional brittle PS foam materials by optimizing the formulation and adjusting the preparation process, developing a modified PS foam buffer underlayment substrate suitable for floor protective films. It improves the toughness and mechanical strength of the foam material, enhances the structure, and results in a uniform underlayment thickness. This invention optimizes the processing technology, leading to a wide range of product applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical production technology and relates to a high-toughness modified PS foamed floor protective film material and its preparation method. Background Technology

[0002] Currently, EPE (Expanded Polyethylene) foam is the mainstream cushioning material used for floor protection on construction sites. While EPE foam has excellent toughness and cushioning resilience, its stiffness is relatively low, making it prone to wrinkling and shifting when laid, and its raw material cost is relatively high. KT board is a PS closed-cell foam board with fine and uniform cells, but the matrix is ​​not toughened or modified, making the material hard and brittle. It is extremely easy to crack and crumble when bent or crushed, and as a rigid board, it cannot be rolled up and cannot be used directly as a protective film layer.

[0003] Ordinary unmodified PS foam materials have a rigid pore structure and poor molecular chain toughness after molding, resulting in high rigidity and poor flexibility. They are prone to cracking, brittle fracture, and crumbling under external forces such as stepping, bending, and rolling, and have poor impact resistance and resistance to cyclic rolling. Currently, there is a lack of PS-based foam padding materials that can be continuously rolled and thermally laminated, which cannot simultaneously meet the requirements of stiffness, cushioning, cost, and subsequent lamination processing, thus limiting the application of PS foam materials in the field of floor protection films. This is the industry pain point that this project needs to address.

[0004] The technical defects that need to be addressed in the floor protective film underlayment material for construction sites are: ① Pure PS substrate is brittle, with poor resistance to trampling, crushing, and bending; it crumbles and sheds debris under stress, polluting the construction site. ② It cannot be rolled up, making it unsuitable for continuous thermal lamination roll production processes. ③ Its surface energy is incompatible with the thermal lamination process of PE film and woven fabric, easily leading to delamination and peeling. ④ It is prone to excessively thin cell walls and unreasonable expansion ratios, resulting in permanent cell collapse under load and loss of cushioning capacity. ⑤ Short-term storage at construction sites exposes it to sunlight, causing rapid aging and brittleness. Summary of the Invention

[0005] The purpose of this invention is to provide a high-toughness modified PS foam floor protective film cushioning material and its preparation method. By adjusting the formula modification and optimizing the preparation process, the traditional brittle PS foam material is improved, and a modified PS foam buffer cushioning substrate suitable for floor protective films is developed, overcoming the shortcomings of existing floor protective film cushioning materials.

[0006] The technical solution of this invention is: a high-toughness modified PS foamed floor protective film underlayment material, comprising two types: a chemical foaming formula and a butane physical foaming formula. (i) Chemical foaming formulation, by parts: GPPS / HIPS polystyrene 70-75, POE / EVA elastomer toughening agent 9-14, reinforcing filler (talc / nano calcium carbonate) 1-6, AC chemical foaming agent 1.7-2.2, lubricant / dispersant 0.8-1.3, functional additives 0.5-1.

[0007] (ii) Butane physical foaming formula GPPS / HIPS polystyrene 76-80, POE / EVA elastomer toughening agent 14-18, reinforcing filler 6-10, physical nucleating agent 1.2-1.6, lubricant / dispersant (EBS, zinc stearate) 0.8-1.3, functional additives 0.5-0.9.

[0008] GPPS / HIPS polystyrene serves as the foaming resin matrix, providing a stiffening skeleton for the padding layer; its grade is GP-525. POE / EVA elastomer toughening agent improves PS brittleness, enhances bending resistance and trampling resistance, and prevents flaking; its grade is POE-8150. Reinforcing fillers enhance compressive and crush resistance, assist in cell nucleation, and control costs; the grade used is 1250-mesh talc. Lubricants / dispersants ensure uniform mixing and dispersion, prevent die accumulation, control precipitation, and guarantee thermal bonding effects; they are a blend of BS and zinc stearate in a ratio of BS:zinc stearate = 0.6–1.0:0.2–0.4. Functional additives include nucleating agents, antioxidants, and UV additives, used to stabilize cells, inhibit short-term aging at construction sites, and refine cell structure. The nucleating agent is NA-108, the antioxidant is Antioxidant 1010, and the UV additive is UV-531. The ratio of NA-108, Antioxidant 1010, and UV-531 is 0.2-0.4:0.1-0.2:0.1-0.2. AC chemical foaming agent decomposes upon heating to produce gas; it is specifically designed for chemical foaming and its grade is AC-3000. Physical nucleating agents are used for butane foaming cell nucleation and refinement; specifically, talc-based physical foaming nucleation masterbatches.

[0009] Another aspect of this invention is: a method for preparing a high-toughness modified PS foamed floor protective film underlay material, including a chemical foaming process and a butane physical foaming process, the preparation process of which is as follows: (1) Raw material pretreatment and mixing Raw material weighing and proportioning: Weigh GPPS / HIPS polystyrene, POE / EVA elastomer toughening agent, reinforcing filler, AC chemical foaming agent (or physical nucleating agent), lubricant / dispersant, and functional additives precisely according to the required proportions and put them into high-speed mixing equipment.

[0010] High-speed premixing: Mixing temperature controlled at 85℃, mixing speed at 800 r / min, and mixing time at 6 min. This ensures thorough dispersion of all components, preventing agglomeration and segregation, and eliminating potential localized brittleness. The mixing parameters are the same for both chemical foaming and butane physical foaming.

[0011] (2) Extrusion Melt Plasticization A. Melting and plasticizing process of chemical foaming route: The mixed material is fed into a twin-screw extruder, and the temperature is controlled in stages: Zone 1 165℃, Zone 2 175℃, Zone 3 182℃, and the screw speed is 220r / min; the material is fully melted and plasticized to establish a stable melt pressure and avoid premature decomposition of the foaming agent.

[0012] B. Butane Physical Foaming Route: Melting and Plasticizing Process (Refer to EPE Gas Injection Foaming Mode): The mixed material is fed into a twin-screw extruder with a high-pressure gas injection port. Temperature is controlled in stages: Zone 1 160℃, Zone 2 170℃, Zone 3 176℃, screw speed 200 r / min. The melt is fully plasticized and possesses high sealing and pressure-bearing capacity, suitable for high-pressure butane injection.

[0013] (3) Pressure foaming process A: Process parameters for chemical foaming process • Foaming temperature: 160~180℃; • Foaming pressure: 6.5~7.5MPa; • Foaming ratio: 3 to 8 times, preferably 5 to 8 times; • Insulation and foaming time: 25s; • Bubble control requirements: fine closed pores, uniform pore size, pore diameter 0.1~0.4mm, no large voids, and no continuous broken bubbles.

[0014] Foaming principle: The AC foaming agent decomposes upon heating inside the extruder, releasing gas that is evenly dispersed within the modified PS melt to form cells. The product thickness is 1-4mm, and residual gas is released rapidly, requiring no curing process. The expansion ratio should not be too high to prevent permanent collapse of the cells due to trampling.

[0015] B: Butane physical foaming process parameters • Melt temperature in the gas injection section: 168~174℃; • Extrusion melt pressure: 9.~11.0MPa; • Butane injection pressure: 10–12 MPa; • Butane injection ratio: 4-7% of material mass; • Foaming ratio: 3 to 7 times, preferably 4 to 5.5 times; • Depressurization and foaming time: 12–18 seconds; • Bubble control requirements: fine closed pores, pore diameter 0.08~0.35mm, fine pores, no broken bubbles, no cross-pores or large voids.

[0016] Foaming principle: Liquid butane is injected into high-temperature modified PS melt under high pressure, and the butane dissolves in the melt. The pressure is released instantaneously when the melt is extruded from the die, causing the butane to vaporize and expand, forming fine closed-cell bubbles. The padding layer is 1-4mm thin, and a small amount of residual butane escapes quickly, eliminating the need for a long curing process on the KT board.

[0017] (4) Extrusion molding process (two sets of foaming molding sections share the same molding section): extrusion of foam pad blank by flat die head → cooling roller locks in the foam and shapes.

[0018] Molding method: Extrusion flat film foaming molding.

[0019] Specific molding parameters: die head temperature 178℃, traction speed 4.5m / min, cooling roller temperature 42℃, padding thickness control range 1.0~4.0mm, width 1200~2000mm.

[0020] Molding requirements: The padding layer surface must be flat and of uniform thickness, with a thickness tolerance of ±0.2mm. It must be free of scratches, bulges, holes, and brittle edges. The surface condition must meet the requirements for subsequent thermal lamination processing, and the entire roll must have uniform performance without any localized brittle areas.

[0021] (5) Post-processing and lamination processes Previous process: After foaming and molding, the material is cooled and shaped, pulled and leveled, trimmed, and then rolled up to obtain the modified PS foam padding master roll.

[0022] Subsequent process: The padding master roll is hot-pressed and laminated with PE film / woven fabric (adhesive lamination is not recommended). The hot lamination temperature is 145-155℃. Cut to order specifications and rewind to obtain the finished product. Simple surface protection treatment can be added as needed.

[0023] The high-toughness modified PS foam floor protective film underlayment material of this invention conforms to the standard GB / T10802-2017 Determination of Compression Permanent Deformation of Flexible Foam Polymer Materials. The performance indicators of the finished products from both foaming processes are consistent; butane physical foaming produces finer pores and exhibits slightly better compression rebound than chemical foaming.

[0024] This invention relates to a high-toughness modified PS foam floor protection film underlayment material. Through optimized formula modification and adjusted preparation process, it improves traditional brittle PS foam materials, developing a modified PS foam buffer underlayment substrate suitable for floor protection films. Specific effects include: ① Solving the problems of inherent PS brittleness, cracking under repeated bending and trampling, and the absence of foam debris, thus improving toughness. ② Possessing suitable pressure-resistant buffering performance, it is not prone to permanent collapse under load, improving mechanical strength. ③ Improving the structure, with uniform and dense closed-cell structure, stable foaming ratio, uniform underlayment thickness, and no voids, broken bubbles, or localized brittle points. ④ Optimizing the processing technology, producing continuous rolls that can be wound up, suitable for subsequent hot-pressing lamination with PE film / woven fabric without delamination or bulging. Supporting both chemical foaming and butane physical foaming production routes. ⑤ Widely applicable, replacing some pearl cotton underlayments for floor protection of ceramic tiles, marble, and flooring in construction sites, achieving a balance between cost and performance. Detailed Implementation

[0025] The present invention will now be described in detail with reference to the embodiments. The scope of protection of the present invention is not limited to the embodiments, and any modifications made by those skilled in the art within the scope defined by the claims also fall within the scope of protection of the present invention.

[0026] The production process of the high-toughness modified PS foamed floor protective film underlay material of this invention is as follows: raw material weighing and proportioning → high-speed mixing and premixing → extrusion melting and plasticizing → pressurized foaming → extrusion of foamed underlay blank by flat die → cooling roller foam locking and shaping → traction flattening → trimming → rewinding of foamed underlay master roll → subsequent thermal lamination of PE, PVC, OPP, CPE, film / non-woven fabric / EVA / EPE pearl cotton / EA environmentally friendly cotton / woven fabric surface layer → slitting and rewinding of finished floor protective film.

[0027] Example 1: Preparation of high-toughness modified PS foamed floor protective film underlay material by chemical foaming formulation process.

[0028] The chemical foaming formulation, by parts: GP-525: 73, POE-8150: 12, 1250 mesh talc: 3, AC-3000: 2, lubricant / dispersant: 1.0, functional additives: 0.8. The lubricant / dispersant is a blend of BS and zinc stearate, with a BS:zinc stearate ratio of 0.7:0.3. Functional additives include nucleating agents, antioxidants, and UV additives. The nucleating agent is NA-108, the antioxidant is Antioxidant 1010, and the UV additive is UV-531. The ratio of NA-108, Antioxidant 1010, and UV-531 is 0.4:0.2:0.2.

[0029] The preparation process of a chemically foamed high-toughness modified PS foam floor protective film underlayment material is as follows: 1. Raw material pretreatment and mixing (1) Raw material weighing and proportioning: Weigh GPPS / HIPS polystyrene, POE / EVA elastomer toughening agent, reinforcing filler, AC chemical foaming agent, lubricant / dispersant and functional additives accurately according to the required proportions and put them into high-speed mixing equipment.

[0030] (2) High-speed mixing and premixing: Control the mixing temperature at 85℃, the mixing speed at 800 r / min, and the mixing time at 6 min. Ensure that all components are fully dispersed, without agglomeration or segregation, and eliminate the potential for localized brittleness.

[0031] 2. Extrusion melt plasticizing Melting and plasticizing process: The mixed material is fed into a twin-screw extruder with segmented temperature control: Zone 1 165℃, Zone 2 175℃, Zone 3 182℃, and screw speed 220 r / min. The material is fully melted and plasticized to establish a stable melt pressure and prevent premature decomposition of the foaming agent.

[0032] 3. The process parameters for the pressurized foaming process are as follows: • Foaming temperature: 170±5℃; • Foaming pressure: 7±0.2MPa; • Foaming ratio: 5 to 6 times, preferably 6 to 7 times; • Insulation and foaming time: 25s; • Bubble control requirements: fine closed pores, uniform pore size, pore diameter 0.2-0.3mm, no large voids, and no continuous broken bubbles.

[0033] Requirements: fine closed pores, uniform pore size, pore diameter 0.2-0.3mm, no large voids, and no continuous broken bubbles.

[0034] 4. Extrusion molding process: Extrusion of foam pad preform by flat die → Cooling roller locks in the foam and shapes it.

[0035] Molding method: Extrusion flat film foaming molding.

[0036] Specific molding parameters: die head temperature 178℃, traction speed 4.5m / min, cooling roller temperature 42℃, padding thickness control range 1.0~4.0mm, width 1200~2000mm.

[0037] Molding requirements: The padding layer surface must be flat and of uniform thickness, with a thickness tolerance of ±0.2mm. It must be free of scratches, bulges, holes, and brittle edges. The surface condition must meet the requirements for subsequent thermal lamination processing, and the entire roll must have uniform performance without any localized brittle areas.

[0038] (5) Post-processing and lamination processes Previous process: After foaming and molding, the modified PS foam padding layer master roll is obtained by cooling and shaping, traction and leveling, trimming and winding.

[0039] Subsequent process: The padding master roll is hot-pressed and laminated with PE film / woven fabric (adhesive lamination is not recommended), with a hot lamination temperature of 15±2℃; the finished product is then cut and rewound according to order specifications. Simple surface protection treatment can be added as needed.

[0040] The product was tested according to GB / T10802-2017, "Determination of Compression Set of Flexible Foam Polymer Materials". The specific test items and test results are shown in Table 1.

[0041] Table 1. Measurement data of compression set of chemically foamed flexible polymeric foam materials

[0042] Example 2: Preparation of high-toughness modified PS foamed floor protective film underlay material by butane physical foaming process.

[0043] The formulation for the butane physical foaming process, by parts: GP-525: 78, POE-8150: 16, 1250 mesh talc: 8, talc-based physical foaming nucleating masterbatch: 1.4, lubricant / dispersant (EBS + zinc stearate): 1.1, where BS:zinc stearate = 0.8: 0.3. Functional additives: 0.8, with the ratio of functional additives NA-108, antioxidant 1010, and UV-531 being 0.4:0.2:0.2.

[0044] The process for producing high-toughness modified PS foamed floor protective film underlayment material using a butane physical foaming formulation includes the following preparation steps: 1. Raw material pretreatment and mixing (1) Raw material weighing and proportioning: Weigh GPPS / HIPS polystyrene, POE / EVA elastomer toughening agent, reinforcing filler, physical nucleating agent, lubricant / dispersant, and functional additives accurately according to the required proportions and put them into high-speed mixing equipment.

[0045] (2) High-speed mixing and premixing: Control the mixing temperature at 85℃, the mixing speed at 800 r / min, and the mixing time at 6 min. Ensure that all components are fully dispersed, without agglomeration or segregation, and eliminate the potential for localized brittleness.

[0046] 2. Extrusion melt plasticizing Melt plasticizing process (referencing EPE foaming mode): The mixed material is fed into a twin-screw extruder with a high-pressure gas injection port. Segmented temperature control: Zone 1 160℃, Zone 2 170℃, Zone 3 176℃, screw speed 200 r / min. The melt is fully plasticized and possesses high sealing and pressure-bearing capacity for high-pressure butane injection.

[0047] 3. Pressure foaming process Butane physical foaming process parameters • Melt temperature in the gas injection section: 168~174℃; • Extrusion melt pressure: 9.~11.0MPa; • Butane injection pressure: 10–12 MPa; • Butane injection ratio: 5-6% of material mass; • Foaming ratio: 3 to 7 times, preferably 4 to 5.5 times; • Depressurization and foaming time: 14–16 seconds; • Bubble control requirements: fine closed pores, pore diameter 0.18~0.30mm, fine pores, no broken bubbles, no cross-pores or large voids.

[0048] Safety reminder: Butane is flammable and explosive. The entire set of equipment must be equipped with explosion-proof motors, static grounding, exhaust ventilation, and combustible gas alarm devices.

[0049] 4. Extrusion molding process: Extrusion of foam pad preform by flat die → Cooling roller locks in the foam and shapes it.

[0050] (1) Molding method: Extrusion flat film foaming molding.

[0051] Specific molding parameters: die head temperature 178℃, traction speed 4.5m / min, cooling roller temperature 42℃, padding thickness control range 1.0~4.0mm, width 1200~2000mm.

[0052] (2) Molding requirements: The padding layer surface should be flat and of uniform thickness, with a thickness tolerance of ±0.2mm. It should be free of scratches, bulges, holes, and brittle edges. The surface condition should meet the requirements for subsequent thermal lamination processing, and the entire roll should have uniform performance without any localized brittle areas.

[0053] Note: Butane physical foaming is more sensitive to die head pressure fluctuations, so the die head pressure must be strictly controlled to prevent melt gushing and bubble bursting.

[0054] 5. Post-processing and lamination processes (1) Pre-process: After foaming and molding, the modified PS foam padding layer master roll is obtained by cooling and shaping, traction and leveling, trimming and winding.

[0055] (2) Subsequent process: The padding master roll is hot-pressed and laminated with PE film / woven fabric (adhesive lamination is not recommended). The hot lamination temperature is 145-155℃. The finished product is then cut and rewound according to the order specifications. Simple surface protection treatment can be added as needed.

[0056] The high-toughness modified PS foam floor protective film underlayment material of this invention conforms to the standard GB / T10802-2017 Determination of compression set of flexible foam polymer materials. Specific test items and indicators are shown in Table 1.

[0057] Table 2. Measurement data of compression set of butane physically foamed flexible foam polymer materials

[0058] Tests show that modified PS foam padding outperforms ordinary PS foam. Its compression cushioning and bending resistance are close to those of pearl cotton padding. It also exhibits better stiffness, meeting the requirements for floor protection on construction sites. The butane physically foamed version has finer cell structure and a feel even closer to pearl cotton.

[0059] This invention relates to a high-toughness modified PS foam floor protective film underlay material with a wide range of applications, primarily including home and commercial construction sites: cushioning and protection for tile, marble, wood flooring, and slab flooring, preventing bumps, scratches, and foot traffic, as well as temporary floor protection for short-term indoor areas. The end product of this invention is a modified PS foam cushioning underlay master roll. The finished floor protective film, after thermal lamination with a PE / woven fabric surface layer, replaces some EPE pearl cotton-type floor protective materials.

[0060] Chemical foaming: Low equipment modification cost, can be produced using a regular twin-screw extruder, but the cell uniformity is slightly lower than that of butane physical foaming, suitable for small to medium batch production. Butane physical foaming: Fine cell structure, better cushioning and rebound, the finished product is closer to the texture of pearl cotton, but requires explosion-proof high-pressure gas injection extrusion equipment, with high safety control requirements, suitable for mass production.

Claims

1. A high-toughness modified PS foam floor protective film underlayment material, characterized in that: Including chemical foaming formulations and butane physical foaming formulations: (i) Chemical foaming formulation, by parts: GPPS / HIPS polystyrene 70-75, POE / EVA elastomer toughening agent 9-14, reinforcing filler 1-6, AC chemical foaming agent 1.7-2.2, lubricant / dispersant 0.8-1.3, functional additives 0.5-1; (ii) Butane physical foaming formulation, by parts: GPPS / HIPS polystyrene 76-80, POE / EVA elastomer toughening agent 14-18, reinforcing filler 6-10, physical nucleating agent 1.2-1.6, lubricant / dispersant 0.8-1.3, functional additives 0.5-0.

9.

2. The high-toughness modified PS foamed floor protective film underlayment material according to claim 1, characterized in that: The grade of the GPPS / HIPS polystyrene is GP-525; the toughening agent of the POE / EVA elastomer is POE-8150; the reinforcing filler is 1250 mesh talc powder; the lubricant / dispersant is a compound of BS and zinc stearate, with a compounding ratio of BS:zinc stearate = 0.8~1.2:0.3~0.

6.

3. The high-toughness modified PS foamed floor protective film underlayment material according to claim 1, characterized in that: The AC chemical foaming agent is designated AC-3000; the butane physical nucleating agent is a talc-based physical foaming nucleating masterbatch.

4. The high-toughness modified PS foamed floor protective film underlayment material according to claim 1, characterized in that: The functional additives include nucleating agents, antioxidants, and UV additives; the nucleating agent is NA-108, the antioxidant is antioxidant 1010, and the UV additive is UV-531; the ratio of NA-108, antioxidant 1010, and UV-531 is 0.2-0.5:0.1-0.3:0.1-0.

3.

5. A method for preparing a high-toughness modified PS foamed floor protective film underlayment material according to claim 1, characterized in that: The preparation process is as follows: (1) Raw material pretreatment and mixing Raw material weighing and proportioning: Weigh GPPS / HIPS polystyrene, POE / EVA elastomer toughening agent, reinforcing filler, AC chemical foaming agent (or physical nucleating agent), lubricant / dispersant, and functional additives precisely according to the required proportions and put them into the high-speed mixing equipment. High-speed mixing premixing: control the mixing temperature at 85℃, the mixing speed at 800r / min, and the mixing time at 6min; the mixing parameters for chemical foaming and butane physical foaming are the same; (2) Extrusion Melt Plasticization A. Melting and plasticizing process of chemical foaming route: The mixed material is fed into a twin-screw extruder, with segmented temperature control: Zone 1 165℃, Zone 2 175℃, Zone 3 182℃, and screw speed 220r / min; the material is fully melted and plasticized to avoid premature decomposition of the foaming agent; B. Melting and plasticizing process of butane physical foaming route: The mixed material is fed into a twin-screw extruder with a high-pressure gas injection port; Segmented temperature control: Zone 1 160℃, Zone 2 170℃, Zone 3 176℃, screw speed 200r / min; the melt is fully plasticized and has high sealing and pressure resistance, used for high-pressure injection of butane; (3) Pressure foaming process A: Process parameters for chemical foaming process • Foaming temperature: 160~180℃; • Foaming pressure: 6.5~7.5MPa; • Foaming ratio: 3 to 8 times, preferably 5 to 8 times; • Insulation and foaming time: 25s; • Bubble control requirements: fine closed pores, uniform pore size, pore diameter 0.1~0.4mm, no large voids, no continuous broken bubbles; B: Butane physical foaming process parameters • Melt temperature in the gas injection section: 168~174℃; • Extrusion melt pressure: 9.0~11.0MPa; • Butane injection pressure: 10–12 MPa; • Butane injection ratio: 4-7% of material mass; • Foaming ratio: 3 to 7 times, preferably 4 to 5.5 times; • Depressurization and foaming time: 12–18 seconds; • Bubble control requirements: fine closed pores, pore diameter 0.08~0.35mm, fine pores, no broken bubbles, no cross-pores or large voids; (4) Extrusion molding process Molding method: Extrusion flat film foaming molding; Specific molding parameters: die head temperature 178℃, traction speed 4.5m / min, cooling roller temperature 42℃, padding thickness control range 1.0~4.0mm, width 1200~2000mm; Molding requirements: The padding layer surface should be flat and uniform in thickness, with a thickness tolerance of ±0.2mm; free from scratches, bulges, holes, and brittle edges; the surface condition should meet the requirements of subsequent thermal bonding processing, and the entire roll should have uniform performance without localized brittle areas; (5) Post-processing and lamination processes Previous process: After foaming and molding, the modified PS foam padding layer master roll is obtained by cooling and shaping, traction and leveling, trimming and winding. Subsequent process: The padding master roll is hot-pressed with PE film / woven fabric at a temperature of 145-155℃; the finished product is obtained by cutting and rewinding according to the order specifications.

6. The preparation method of the high-toughness modified PS foamed floor protective film underlayment material according to claim 5, characterized in that: The high-toughness modified PS foam floor protective film underlay material conforms to the standard GB / T10802-2017 Determination of compression set of flexible foam polymer materials.