A low compression set TPE-TPU composite elastomer and its preparation method

By employing low-temperature pre-crystallization and dynamic blending processes, combined with acylhydrazone compatibilizers and highly branched α-olefins, a three-level anti-deformation network is constructed. This solves the problem of easy deformation of styrene-based TPE and TPU blends under long-term pressure, resulting in a high-performance composite elastomer suitable for automotive sealing and electronic damping applications.

CN123107293APending Publication Date: 2026-11-17GUANGDONG HONGCHAO RUBBER & PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611571993.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, styrene-based TPE and TPU blends are prone to permanent deformation and interfacial debonding under long-term pressure, which cannot meet the requirements of high-precision, long-life pressure-bearing components, and traditional compatibilizers cannot effectively reduce permanent deformation.

Method used

By employing low-temperature pre-crystallization treatment and low-temperature dynamic blending process, combined with a bifunctional compatibilizer containing acylhydrazone bonds and a highly branched α-olefin block copolymer, a three-level anti-deformation network is constructed to enhance interfacial compatibility and molecular entanglement, forming a regular nanocrystalline structure and reducing compression set.

Benefits of technology

It significantly reduces the compression set of composite materials, improves the creep resistance and thermoplastic processability of the materials, and is suitable for high-end pressure-bearing applications such as automotive sealing and electronic damping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of polymer material modification technology, specifically to a low compression set TPE-TPU composite elastomer and its preparation method. The composite elastomer, by weight, comprises a styrene-based thermoplastic elastomer, a polyester-type thermoplastic polyurethane, an α-olefin block copolymer of highly branched polyolefin, a bifunctional compatibilizer containing acylhydrazone bonds, amino-β-cyclodextrin, and additives. This invention first synthesizes three core raw materials, pre-crystallizes the TPU at low temperature, and then pre-grafts the interface, blends with the matrix, and extrudes at low temperature to obtain the finished product. This invention constructs a three-level anti-deformation network, combined with the entanglement reinforcement effect of the highly branched polyolefin, reducing compression set. The material possesses both elasticity and thermoplastic processability, making it suitable for high-end pressure-bearing applications such as automotive sealing and electronic vibration damping.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer material modification technology, specifically to a low compression set TPE-TPU composite elastomer and its preparation method. Background Technology

[0002] Styrene-based thermoplastic elastomers (TPEs, such as SEBS and SEEPS) combine the high elasticity of rubber with the thermoplastic processing properties of plastics. Due to their excellent weather resistance and comfortable feel, they are widely used in automotive seals, electronic shock absorbers, and medical device components. However, pure styrene-based TPEs have limited physical cross-linking strength in the hard segments, and under long-term pressure, the soft segment molecular chains are prone to irreversible slippage, resulting in high compression set and insufficient high-temperature creep resistance, failing to meet the requirements of high-precision, long-life pressure-bearing components. Thermoplastic polyurethane (TPU) has high microcrystalline cross-linking density in the hard segments and excellent mechanical strength and creep resistance. Blending it with styrene-based TPEs is currently the main method to improve the overall performance of composite elastomers. However, the significant difference in polarity between the two leads to severe phase separation and weak interfacial bonding when directly blended, making them prone to interfacial debonding under pressure, which in turn exacerbates permanent deformation and reduces mechanical properties. Existing technologies often employ conventional graft compatibilizers such as SEBS-g-MAH to improve interfacial bonding. However, these compatibilizers only achieve compatibilization through static covalent bonds or physical entanglement, failing to dissipate sustained stress under long-term compressive loads. Irreversible interface damage still easily occurs, failing to fundamentally reduce permanent deformation. On the other hand, TPU's creep resistance highly depends on the well-ordered microcrystalline network formed by its hard segments. However, in traditional high-temperature melt blending processes, strong shear and high temperatures of 180-200°C completely destroy the ordered microcrystalline structure of TPU hard segments. After cooling, only disordered hard segment agglomerates form, significantly reducing physical crosslinking efficiency and preventing TPU from fully realizing its creep resistance. Furthermore, the high flexibility of polyolefin soft segments in the TPE matrix means that long-range irreversible slippage under long-term pressure is the core cause of permanent deformation. Existing technologies often restrict molecular chain movement by adding inorganic fillers and increasing crosslinking degree, often accompanied by side effects such as increased material hardness, decreased elasticity, and deteriorated processing fluidity.

[0003] Therefore, inventing a low-compression-permanent TPE-TPU composite elastomer is very promising. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a low-compression-permanent TPE-TPU composite elastomer and its preparation method. The composite elastomer, by weight, comprises a styrene-based thermoplastic elastomer, a polyester-type thermoplastic polyurethane, an α-olefin block copolymer of highly branched polyolefin, a bifunctional compatibilizer containing acylhydrazone bonds, amino-β-cyclodextrin, and additives. This invention first synthesizes three core raw materials, pre-crystallizes the TPU at low temperature, and then pre-grafts the interface, blends with the matrix, and extrudes at low temperature to obtain the finished product. This invention constructs a three-level anti-deformation network, combined with the entanglement reinforcement effect of the highly branched polyolefin, reducing compression set. The material possesses both elasticity and thermoplastic processability, making it suitable for high-end pressure-bearing applications such as automotive sealing and electronic vibration damping.

[0005] This invention discloses a low compression set TPE-TPU composite elastomer, which is composed of the following components in parts by weight: 50-60 parts of styrene-based thermoplastic elastomer; 20-30 parts of thermoplastic polyurethane (TPU); 5-15 parts of α-olefin block copolymer highly branched polyolefin; 2-7 parts of bifunctional compatibilizer containing acylhydrazone bonds; 1-6 parts of amino-β-cyclodextrin; 0.2-0.7 parts of antioxidant; 0.3-0.8 parts of lubricant.

[0006] Preferably, the styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% by mass and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system.

[0007] Preferably, the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70~95A and a hard segment melting point of 150~170℃.

[0008] Preferably, the α-olefin block copolymerized highly branched polyolefin is ethylene and C4~C 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 .

[0009] Preferably, the specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; wherein, G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups.

[0010] Preferably, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0011] Preferably, the lubricant is zinc stearate; the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0012] This invention also discloses a method for preparing a low compression set TPE-TPU composite elastomer, the method comprising the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the mass ratio of styrene segments controlled at 18-35%; then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%, and styrene-based thermoplastic elastomers were obtained after devolatilization and drying. Preparation of S2 α-olefin block copolymer highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers were introduced in stages in a series reactor for block copolymerization. The branching degree of the polymer was controlled to be 25~45 branches / 1000 main chain carbon atoms by adjusting the monomer feed ratio, polymerization temperature and polymerization pressure. The polymerization product was devolatilized and granulated to obtain the α-olefin block copolymer highly branched polyolefin. Preparation of S3 acylhydrazone-containing bifunctional compatibilizer: C1~C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazide condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1~C6 alkylene groups, and Ar is a phenyl group; S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 110~120℃ for 4~5 hours to remove moisture; then the drying oven is heated to a temperature 5~15℃ below the melting point of TPU hard segments and heat-treated for 2~3 hours to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the oven, sealed and stored for later use to obtain precrystallized TPU. S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 90~100℃ and the rotation speed is set to 800~1300rpm. The mixture is mixed for 3~8min to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture. Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in a weight ratio and mixed at 1000~1500 rpm for 5~10 min at room temperature until all components are evenly dispersed to obtain the matrix mixture; S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 130~140℃, plasticizing section 140~150℃, homogenizing section 150~160℃, and die head temperature 155~165℃. The screw speed is controlled at 150~300rpm, and the residence time of the material in the barrel is 2~3min. After the extruded strip is cooled by a cooling water bath, it is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

[0013] Preferably, in step S1, the reaction temperature of the anionic polymerization is 60°C, the hydrogenation reaction temperature is 70°C, and the hydrogen pressure is 1.5 MPa; in step S2, the polymerization temperature is 80°C, and the polymerization pressure is 1.5 MPa.

[0014] Preferably, in step S3, the aldehyde-hydrazine condensation reaction takes 5 hours, the end-group modification is performed by diisocyanate addition, the reaction temperature is 55°C, and the reaction time is 2.5 hours.

[0015] Compared with the prior art, the beneficial effects of the present invention are: This invention provides a low compression set TPE-TPU composite elastomer and its preparation method, which has the following characteristics: (1) The acylhydrazone-containing bifunctional compatibilizer used in this invention has an isocyanate group as the reaction end, a phenyl group as the affinity end, and an acylhydrazone bond as the dynamic unit. The isocyanate group can undergo a highly efficient addition reaction with the terminal hydroxyl groups of polyester TPU to form a stable covalent bond at the phase interface; the phenyl end generates a strong π-π stacking effect with the styrene hard segment in styrene thermoplastic elastomer, driving the compatibilizer to be directionally enriched at the two-phase interface, and the compatibilization efficiency is significantly better than that of traditional non-directional compatibilizers such as SEBS-g-MAH. During the compression process, the dynamic covalent bond of the acylhydrazone can dissipate the stress at the interface through reversible fracture-recombination, avoiding irreversible peeling of the interface under long-term pressure, and greatly reducing the permanent deformation caused by phase separation at the interface level.

[0016] (2) The α-olefin block copolymer with high branching degree of polyolefin introduced in this invention is a block copolymer obtained by coordination polymerization of ethylene and 1-butene. Its short branched chain structure has excellent compatibility with the hydrogenated butadiene soft segments of styrene thermoplastic elastomers and can be uniformly dispersed in the matrix phase. The high branching degree of 25~45 branches / 1000 main chain carbons can provide a large number of molecular entanglement points and improve the physical crosslinking density of the matrix. At the same time, its non-polar polyolefin segments can be encapsulated by the hydrophobic cavities of amino-β-cyclodextrin, increasing the anchoring points of host-guest interaction and further strengthening the soft segment confinement effect at the molecular scale. While inhibiting irreversible slippage of the chain segments, it improves the toughness of the system and avoids the material embrittlement defects that accompany the improvement of creep resistance.

[0017] (3) This invention synthesizes styrene-butadiene block copolymers by sequential anionic polymerization, and then obtains styrene thermoplastic elastomers by highly selective hydrogenation. The styrene mass content is precisely controlled in the range of 18-35% and the degree of hydrogenation is ≥98%, which makes the distribution of hard segment micro-regions more uniform and the soft segment phase structure more regular. This not only ensures the basic high elasticity of the composite elastomer, but also provides a uniform working environment for interfacial π-π interaction and host-guest inclusion interaction. It has better compatibility with compatibilizers and highly branched polyolefins, and can effectively avoid performance fluctuations caused by batch differences of commercial general-purpose materials.

[0018] (4) In view of the characteristics of strong crystallinity and high structural stability of polyester-type TPU hard segments, this invention first induces the TPU hard segment molecular chains to arrange in an orderly manner through low-temperature heat treatment at 5~15℃ below the melting point of the hard segments, forming regular nanocrystals with uniform size and high crystallinity; then, through a low-temperature dynamic blending extrusion process, the pre-formed microcrystalline structure is preserved to the greatest extent, so that it is uniformly dispersed in the system as a high-strength physical crosslinking point, and a stable anti-creep skeleton is constructed. This process completely avoids the destructive effect of traditional high-temperature blending on TPU microcrystals, fully releases the anti-creep performance advantage of polyester-type TPU, and significantly improves the shape recovery ability under long-term pressure.

[0019] (5) This invention constructs a three-level anti-deformation network, which, together with the entanglement reinforcement effect of highly branched polyolefins, synergistically suppresses permanent deformation at three scales: aggregated structure, phase interface, and molecular chain. Tests show that the permanent deformation of the composite elastomer at room temperature (23°C) can be reduced to below 6.5%, and at high temperature (70°C) to below 12%, while maintaining excellent tensile strength, elongation at break, and thermoplastic processing fluidity. It can be widely applied to applications requiring high long-term pressure resistance and resilience, such as automotive seals, electronic shock absorbers, and flexible medical components. Detailed Implementation

[0020] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0021] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0022] Example 1: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 50 parts of styrene-based thermoplastic elastomer; 20 parts of thermoplastic polyurethane (TPU); 5 parts of α-olefin block copolymer highly branched polyolefin; 2 parts of a bifunctional compatibilizer containing acylhydrazone bonds; 1 part of amino-β-cyclodextrin; 0.2 parts of antioxidant; and 0.3 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is a mixture of ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0023] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0024] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0025] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0026] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 110°C for 4 hours to remove moisture; then the drying oven is heated to a temperature 5°C below the melting point of the TPU hard segments and heat-treated for 2 hours to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the furnace, sealed and stored for later use to obtain precrystallized TPU.

[0027] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 90℃ and the rotation speed is 800rpm. The mixture is mixed for 3 minutes to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0028] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in the weight ratio and mixed at 1000 rpm for 5 minutes at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0029] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 130℃, plasticizing section 140℃, homogenizing section 150℃, and die head temperature 155℃. The screw speed is controlled at 150 rpm, and the residence time of the material in the barrel is 2 min. After the extruded strip is cooled by a cooling water bath, it is fed into a pelletizer for pelleting to obtain the low compression set TPE-TPU composite elastomer.

[0030] Example 2: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 52 parts of styrene-based thermoplastic elastomer; 22 parts of thermoplastic polyurethane (TPU); 7 parts of α-olefin block copolymer highly branched polyolefin; 3 parts of a bifunctional compatibilizer containing acylhydrazone bonds; 2 parts of amino-β-cyclodextrin; 0.3 parts of antioxidant; and 0.4 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is a mixture of ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0031] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0032] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0033] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0034] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 112℃ for 4.2h to remove moisture; then the drying oven is heated to a temperature 7℃ below the melting point of TPU hard segments and heat-treated for 2.2h to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the furnace, sealed and stored for later use to obtain precrystallized TPU.

[0035] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 92℃ and the rotation speed is 900rpm. The mixture is mixed for 4min to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0036] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in the weight ratio and mixed at 1100 rpm for 6 minutes at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0037] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 132℃, plasticizing section 142℃, homogenizing section 152℃, and die head temperature 157℃. The screw speed is controlled at 170 rpm, and the residence time of the material in the barrel is 2.2 min. After being cooled in a cooling water bath, the extruded strip is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

[0038] Example 3: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 54 parts of styrene-based thermoplastic elastomer; 24 parts of thermoplastic polyurethane (TPU); 9 parts of α-olefin block copolymer highly branched polyolefin; 4 parts of a bifunctional compatibilizer containing acylhydrazone bonds; 3 parts of amino-β-cyclodextrin; 0.4 parts of antioxidant; and 0.5 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is a mixture of ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0039] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0040] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0041] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0042] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 114℃ for 4.4h to remove moisture; then the drying oven is heated to a temperature 9℃ below the melting point of TPU hard segments and heat-treated for 2.4h to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the furnace, sealed and stored for later use to obtain precrystallized TPU.

[0043] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 94℃ and the rotation speed is 1000rpm. The mixture is mixed for 5 minutes to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0044] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in the weight ratio and mixed at 1200 rpm for 7 minutes at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0045] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 134℃, plasticizing section 144℃, homogenizing section 154℃, and die head temperature 159℃. The screw speed is controlled at 190 rpm, and the residence time of the material in the barrel is 2.4 min. After being cooled in a cooling water bath, the extruded strip is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

[0046] Example 4: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 56 parts of styrene-based thermoplastic elastomer; 26 parts of thermoplastic polyurethane (TPU); 11 parts of α-olefin block copolymer highly branched polyolefin; 5 parts of bifunctional compatibilizer containing acylhydrazone bonds; 4 parts of amino-β-cyclodextrin; 0.5 parts of antioxidant; and 0.6 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is a mixture of ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0047] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0048] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0049] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0050] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 116℃ for 4.6h to remove moisture; then the drying oven is heated to a temperature 11℃ lower than the melting point of TPU hard segments and heat-treated for 2.6h to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the furnace, sealed and stored for later use to obtain precrystallized TPU.

[0051] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 96℃ and the rotation speed is 1100rpm. The mixture is mixed for 6 minutes to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0052] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in the weight ratio and mixed at 1300 rpm for 8 minutes at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0053] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 136℃, plasticizing section 146℃, homogenizing section 156℃, and die head temperature 161℃. The screw speed is controlled at 230 rpm, and the residence time of the material in the barrel is 2.6 min. After being cooled in a cooling water bath, the extruded strip is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

[0054] Example 5: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 58 parts of styrene-based thermoplastic elastomer; 28 parts of thermoplastic polyurethane (TPU); 13 parts of α-olefin block copolymer highly branched polyolefin; 6 parts of bifunctional compatibilizer containing acylhydrazone bonds; 5 parts of amino-β-cyclodextrin; 0.6 parts of antioxidant; and 0.7 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18-35% and a Shore hardness of 50-80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is a mixture of ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0055] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0056] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0057] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0058] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 118°C for 4.8 hours to remove moisture; then the drying oven is heated to a temperature 13°C below the melting point of the TPU hard segments and heat-treated for 2.8 hours to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature in the oven, sealed and stored for later use to obtain precrystallized TPU.

[0059] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 98℃ and the rotation speed is 1200rpm. The mixture is mixed for 7min to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0060] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in the weight ratio and mixed at 1400 rpm for 9 minutes at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0061] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 138℃, plasticizing section 148℃, homogenizing section 158℃, and die head temperature 163℃. The screw speed is controlled at 260 rpm, and the residence time of the material in the barrel is 2.8 min. After being cooled in a cooling water bath, the extruded strip is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

[0062] Example 6: A low compression set TPE-TPU composite elastomer, composed of the following parts by weight: 60 parts of styrene-based thermoplastic elastomer; 30 parts of thermoplastic polyurethane (TPU); 15 parts of α-olefin block copolymer highly branched polyolefin; 7 parts of a bifunctional compatibilizer containing acylhydrazone bonds; 6 parts of amino-β-cyclodextrin; 0.7 parts of antioxidant; and 0.8 parts of lubricant. The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 35% by mass and a Shore hardness of 80A, serving as the continuous phase matrix of the composite system; the thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70-95A and a hard segment melting point of 150-170℃; the α-olefin block copolymer highly branched polyolefin is ethylene and C4-C4... 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 The specific structural formula of the bifunctional compatibilizer containing acylhydrazone bonds is G-L1-CO-NH-N=CH-L2-Ar; where G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups; the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the lubricant is zinc stearate; and the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

[0063] A method for preparing a low compression set TPE-TPU composite elastomer includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the styrene segment mass ratio controlled at 18-35%. Then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%. After devolatilization and drying, styrene-based thermoplastic elastomers were obtained. The reaction temperature for the anionic polymerization was 60℃, the hydrogenation reaction temperature was 70℃, and the hydrogen pressure was 1.5 MPa.

[0064] Preparation of S2 α-olefin block copolymerized highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers are introduced in stages in a series reactor for block copolymerization. By adjusting the monomer feed ratio, polymerization temperature, and polymerization pressure, the branching degree of the polymer is controlled to be 25~45 branches / 1000 main chain carbon atoms. The polymerization product is devolatilized and granulated to obtain the α-olefin block copolymerized highly branched polyolefin. In step S2, the polymerization temperature is 80℃ and the polymerization pressure is 1.5MPa.

[0065] Preparation of S3 Bifunctional Compatibilizer Containing Acylhydrazone Bonds: C1-C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazone condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then, the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1-C6 alkylene groups, and Ar is a phenyl group; wherein the aldehyde-hydrazone condensation reaction time was 5 h, and the end group modification was carried out by diisocyanate addition method, the reaction temperature was 55℃, and the reaction time was 2.5 h.

[0066] S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 120°C for 5 hours to remove moisture; then the drying oven is heated to a temperature 15°C below the melting point of the TPU hard segments and heat-treated for 3 hours to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the furnace, sealed and stored for later use to obtain precrystallized TPU.

[0067] S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 100℃ and the rotation speed is 1300rpm. The mixture is mixed for 8 minutes to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture.

[0068] Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant and lubricant are added to a mixer in the weight ratio and mixed at 1500 rpm for 10 min at room temperature until all components are evenly dispersed to obtain the matrix mixture.

[0069] S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 140℃, plasticizing section 150℃, homogenizing section 160℃, and die head temperature 165℃. The screw speed is controlled at 300 rpm, and the residence time of the material in the barrel is 3 min. After the extruded strip is cooled by a cooling water bath, it is fed into a pelletizer for pelleting to obtain the low compression set TPE-TPU composite elastomer.

[0070] Example 7: The bifunctional compatibilizer containing acylhydrazone bonds was replaced with maleic anhydride-grafted SEBS, and step S3 was omitted. The remaining raw materials and preparation methods were the same as in Example 6.

[0071] Example 8: The amino-β-cyclodextrin was removed, and the remaining raw materials and preparation method were the same as in Example 6.

[0072] Example 9: The α-olefin block copolymer of highly branched polyolefin was replaced with ethylene-1-octene random copolymer, and step S3 was omitted. The remaining raw materials and preparation methods were the same as in Example 6.

[0073] Example 10: The low-temperature pre-crystallization treatment of S4 TPU was omitted and replaced with high-temperature blending at 200℃. The other raw materials and preparation methods were the same as in Example 6.

[0074] The performance of the TPE-TPU composite elastomers prepared in Examples 1-10 was tested, and the test results are shown in the table below:

[0075] The data in the table above shows that: (1) In Examples 1-6, as the amount of acylhydrazone-containing bifunctional compatibilizer, amino-β-cyclodextrin, and α-olefin block copolymerized highly branched polyolefin was gradually increased, and with the simultaneous optimization of low-temperature pre-crystallization process parameters, the compression set of the composite elastomer at normal and high temperatures showed a continuous downward trend, the tensile strength steadily increased, and the elongation at break remained at a relatively high level of over 500%. This indicates that the synergistic effect of the three-level anti-deformation network is gradually strengthened with the increase of the amount of core components. The compatibilized structure constructed by dynamic covalent bonds and π-π stacking at the interface is more compact, and the stress dissipation capacity is enhanced. At the molecular scale, the number of host-guest inclusion anchor points of cyclodextrin increases, and the irreversible slip of soft segments is more effectively constrained. The physical cross-linking skeleton of TPU regular microcrystals fully exerts its anti-creep effect, and the molecular entanglement strengthening effect of highly branched polyolefin is superimposed, which together achieves a significant reduction in compression set.

[0076] (2) Examples 7-10 served as control groups. After replacing or removing a single core innovative element, the compressive permanent deformation resistance of the composite elastomers deteriorated to varying degrees. Example 7 replaced the dynamic compatibilizer with conventional SEBS-g-MAH, lacking the reversible fracture-recombination stress dissipation mechanism of acylhydrazone bonds. The interface only has static covalent bonding, which easily leads to irreversible debonding under long-term pressure. The compression set at normal and high temperatures increased significantly compared to Example 6, verifying the core role of the dynamic double cross-linking compatibilization system. Example 8 removed amino-β-cyclodextrin, and the molecular-level host-guest confinement anchoring effect disappeared. The long-range slip of the polyolefin soft segments could not be effectively constrained, and the compression set increased significantly, proving that the supramolecular confinement mechanism is the key link in improving creep resistance. Example 9 replaced the highly branched block polyolefin with ordinary random POE. The branching degree and the additional entanglement points and inclusion sites brought by the block structure decreased, the synergistic strengthening effect weakened, and the compression set increased. Example 10 canceled the low-temperature precrystallization process and used high-temperature blending, which caused the TPU hard segment microcrystals to be destroyed, the high-strength physical cross-linking skeleton to fail, and the creep resistance to deteriorate significantly.

[0077] In summary, this invention successfully constructs a three-level synergistic anti-deformation network of aggregated state, interface, and molecular chain by custom-preparing a styrene-based thermoplastic elastomer matrix, α-olefin block copolymerization of highly branched polyolefin, and a bifunctional compatibilizer containing acylhydrazone bonds, combined with TPU low-temperature pre-crystallization and low-temperature blending processes. This network can significantly reduce the compression set of TPE-TPU composite elastomers while maintaining excellent mechanical elasticity and thermoplastic processability. The innovative mechanisms support each other and synergistically enhance each other, and the prepared materials can meet the long-term use requirements of high-end pressure-bearing elastic components such as automotive seals, electronic damping, and medical flexible parts.

[0078] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A low compression set TPE-TPU composite elastomer, characterized in that, It is composed of the following components by weight: 50-60 parts of styrene-based thermoplastic elastomer; 20-30 parts of thermoplastic polyurethane (TPU); 5-15 parts of α-olefin block copolymer highly branched polyolefin; 2-7 parts of bifunctional compatibilizer containing acylhydrazone bonds; 1-6 parts of amino-β-cyclodextrin; 0.2-0.7 parts of antioxidant; and 0.3-0.8 parts of lubricant.

2. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The styrene-based thermoplastic elastomer is a hydrogenated product of styrene-butadiene-styrene block copolymer, with a styrene content of 18%~35% by mass and a Shore hardness of 50A~80A, serving as the continuous phase matrix of the composite system.

3. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The thermoplastic polyurethane (TPU) is a polyester-type TPU with a Shore hardness of 70A~95A and a hard segment melting point of 150~170℃.

4. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The α-olefin block copolymer of highly branched polyolefin is ethylene and C4~C 12 A block copolymer prepared by coordination polymerization of an α-olefin, wherein the α-olefin is 1-butene; the polyolefin has a branching degree of 25-45 branches per 1000 main chain carbon atoms, a crystallinity of ≤15%, and a density of 0.860-0.885 g / cm³. 3 .

5. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The specific structural formula of the bifunctional compatibilizer containing acylhydrazone is G-L1-CO-NH-N=CH-L2-Ar; wherein, G is a reactive end group that can covalently react with the terminal hydroxyl group of TPU and is selected from isocyanate groups; L1 and L2 are linking groups and are C1~C6 alkylene groups; Ar is an aromatic end group and is selected from phenyl groups.

6. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:

1.

7. The low compression set TPE-TPU composite elastomer according to claim 1, characterized in that, The lubricant is zinc stearate; the amino-β-cyclodextrin is mono-(6-amino-6-deoxy)-β-cyclodextrin.

8. A method for preparing a low compression set TPE-TPU composite elastomer, characterized in that, Includes the following steps: Preparation of S1 styrene-based thermoplastic elastomers: Styrene-butadiene-styrene triblock copolymers were synthesized by sequential anionic polymerization using cyclohexane as the reaction solvent and n-butyllithium as the initiator, with the mass ratio of styrene segments controlled at 18%~35%; then, selective hydrogenation was carried out using a supported nickel catalyst, with the degree of hydrogenation controlled at ≥98%, and styrene-based thermoplastic elastomers were obtained after devolatilization and drying. Preparation of S2 α-olefin block copolymer highly branched polyolefin: Using a metallocene coordination catalysis system, ethylene and 1-butene monomers were introduced in stages in a series reactor for block copolymerization. The branching degree of the polymer was controlled to be 25~45 branches / 1000 main chain carbon atoms by adjusting the monomer feed ratio, polymerization temperature and polymerization pressure. The polymerization product was devolatilized and granulated to obtain the α-olefin block copolymer highly branched polyolefin. Preparation of S3 acylhydrazone-containing bifunctional compatibilizer: C1~C6 alkyl monohydrazides and benzyl aldehydes were added to anhydrous ethanol solvent at a molar ratio of 1:1, and an aldehyde-hydrazide condensation reaction was carried out under reflux to obtain a terminal alkyl acylhydrazone intermediate; then the alkyl end of the intermediate was modified to introduce isocyanate reactive end groups, and after purification, a bifunctional compatibilizer containing acylhydrazone bonds with the structural formula G-L1-CO-NH-N=CH-L2-Ar was obtained, wherein G is an isocyanate group, L1 and L2 are C1~C6 alkylene groups, and Ar is a phenyl group; S4 TPU Low-Temperature Precrystallization Treatment: Polyester TPU is placed in a vacuum drying oven and dried at 110~120℃ for 4~5 hours to remove moisture; then the drying oven is heated to a temperature 5~15℃ below the melting point of TPU hard segments and heat-treated for 2~3 hours to induce the TPU hard segment molecular chains to arrange in an orderly manner to form a regular nanocrystalline structure; after the heat treatment is completed, it is cooled to room temperature with the oven, sealed and stored for later use to obtain precrystallized TPU. S5 Interface Pre-grafting Mixing: The pre-crystallized TPU from step S4 and the bifunctional compatibilizer containing acylhydrazone bonds obtained in step S3 are added to a mixer. The mixing temperature is set to 90~100℃ and the rotation speed is set to 800~1300rpm. The mixture is mixed for 3~8min to allow the isocyanate end groups of the compatibilizer to undergo a pre-grafting reaction with the terminal hydroxyl groups on the TPU surface, thus obtaining a pre-grafted TPU mixture. Preparation of S6 matrix mixture: The styrene thermoplastic elastomer obtained in step S1, the α-olefin block copolymer highly branched polyolefin obtained in step S2, and amino-β-cyclodextrin, antioxidant, and lubricant are added to a mixer in a weight ratio and mixed at 1000~1500 rpm for 5~10 min at room temperature until all components are evenly dispersed to obtain the matrix mixture; S7 Low-temperature dynamic blending extrusion granulation: The pre-grafted TPU mixture prepared in step S5 and the matrix mixture prepared in step S6 are simultaneously added to the main feed port of a twin-screw extruder. The temperatures of each section of the twin-screw extruder are set as follows: feeding section 130~140℃, plasticizing section 140~150℃, homogenizing section 150~160℃, and die head temperature 155~165℃. The screw speed is controlled at 150~300rpm, and the residence time of the material in the barrel is 2~3min. After the extruded strip is cooled by a cooling water bath, it is fed into a pelletizer for pelletizing to obtain the low compression set TPE-TPU composite elastomer.

9. The method for preparing a low compression set TPE-TPU composite elastomer according to claim 8, characterized in that, In step S1, the reaction temperature of the anionic polymerization is 60°C, the hydrogenation reaction temperature is 70°C, and the hydrogen pressure is 1.5 MPa; in step S2, the polymerization temperature is 80°C, and the polymerization pressure is 1.5 MPa.

10. The method for preparing a low compression set TPE-TPU composite elastomer according to claim 8, characterized in that, In step S3, the aldehyde-hydrazine condensation reaction takes 5 hours, and the end-group modification is performed using the diisocyanate addition method at a reaction temperature of 55°C for 2.5 hours.