A high puncture degradable film bag and a preparation method thereof

By adding a multi-component composite reinforcement system of whiskers and inorganic fillers to PBAT resin, combined with interface modification of coupling agents and compatibilizers, the problems of low puncture strength and poor mechanical properties of PBAT membrane bags were solved, and the mechanical properties and full degradation characteristics of high-puncture biodegradable membrane bags were improved.

CN123107315APending Publication Date: 2026-11-17ZHEJIANG YINCHUANGXIN MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611311773.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

PBAT biodegradable film bags have low puncture strength and poor mechanical properties. Traditional granular inorganic fillers have limited modification effects and easily lead to a decrease in flexibility, making it difficult to meet the needs of heavy-duty packaging and outdoor packaging. At the same time, existing modification schemes may affect the degradation performance of the material.

Method used

By adding specific types, sizes, and proportions of whiskers to the PBAT resin system, along with calcium carbonate, talc, and compatibilizers, and then melt-blending and blow molding using a twin-screw extruder, a fibrous-spherical-flaky multi-component reinforced system is constructed. Coupling agents and compatibilizers are used for interface modification to ensure good bonding between the whiskers and the PBAT matrix.

Benefits of technology

It significantly improves the puncture strength, tensile properties, and tear resistance of the film bag, while taking into account both flexibility and rigidity, ensuring the material's fully degradable characteristics, making it suitable for various packaging scenarios, and completely degrading in the natural environment without causing white pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention belongs to the field of biodegradable materials and discloses a high-puncture biodegradable film bag and its preparation method. The film bag is blow-molded from a modified biodegradable resin composition, which includes PBAT resin, whiskers, calcium carbonate, talc, compatibilizer, and processing aids. The preparation method includes whisker pretreatment, component premixing, melt blending granulation, and blow molding. This invention selects whiskers of specific sizes and aspect ratios and combines them with calcium carbonate and talc to construct a fibrous-spherical-plate synergistic reinforcing network. Dual interface modification is implemented through coupling agents and compatibilizers, allowing the whiskers to be uniformly dispersed in the PBAT matrix and form a strong interfacial bond. The resulting film bag exhibits significantly improved puncture strength, tensile strength, and tear strength, while retaining the material's fully degradable characteristics. It can be widely used in food packaging, daily necessities packaging, agricultural packaging, and industrial packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biodegradable materials technology, specifically relating to a highly puncture-resistant biodegradable membrane bag and its preparation method. Background Technology

[0002] Biodegradable polymer materials are gradually replacing traditional non-biodegradable plastics, becoming the mainstream development direction in the packaging industry. Among them, polybutylene terephthalate (PBAT) is widely used in the production of biodegradable bags and packaging films due to its excellent biodegradability, flexibility, and processing performance. However, bags made from PBAT resin have significant performance shortcomings. Their puncture strength is low, making them susceptible to puncture by sharp objects (such as angular objects, branches, or hard particles) in practical applications, leading to leakage of the packaging contents and thus limiting their reliability. Furthermore, the tensile strength and tear strength of pure PBAT are insufficient to meet the requirements of heavy-duty packaging and outdoor packaging applications.

[0003] To improve the mechanical properties of PBAT, existing technologies often modify it by adding inorganic fillers such as calcium carbonate and talc. However, these traditional fillers are mostly in particulate form, resulting in poor interfacial bonding with the PBAT resin matrix. This not only fails to effectively enhance puncture resistance but may also lead to decreased flexibility and brittleness of the PBAT bag. Some technical approaches have attempted to introduce polymeric materials such as ethylene-vinyl acetate copolymer (EVA) and thermoplastic polyurethane (TPU) for toughening modification, but studies show that simply adding these materials often fails to significantly improve puncture strength and may instead increase material costs and affect degradation performance.

[0004] Whiskers, as high-purity single-crystal short fibers at the micro- and nanoscale, possess high strength, high modulus, and high aspect ratio. Their highly oriented crystal structure gives them mechanical strength close to the theoretical value of interatomic bonding forces. If whiskers can be rationally applied to the modification of PBAT resin, it is expected to solve the problem of insufficient puncture performance in existing PBAT film bags. Currently, whiskers have been used in the modification of some polymer materials to improve their shrinkage and flexural modulus properties. However, a technical solution specifically applying whiskers to the PBAT film bag system, aiming to synergistically improve puncture performance and other mechanical properties while ensuring complete biodegradability, has not yet been reported in the literature. Summary of the Invention

[0005] This invention addresses the technical challenges of traditional PBAT biodegradable membrane bags, such as low puncture strength, poor mechanical properties, and limited modification effects of traditional granular inorganic fillers that easily lead to decreased flexibility. It provides a high-puncture biodegradable membrane bag and its preparation method.

[0006] The main objective of this invention is: 1. A high-puncture biodegradable membrane bag is provided, which improves the puncture strength of the membrane bag and significantly reduces the breakage rate during use by adding specific types, sizes and proportions of whiskers as a modifying and reinforcing component to the PBAT resin system. Second, it achieves a synergistic improvement in the puncture resistance, tensile strength, and tear resistance of the film bag, while taking into account both flexibility and rigidity, to meet the usage needs of various packaging scenarios. Third, while improving mechanical properties, the material retains its fully degradable characteristics. After the membrane bag is discarded, it can be completely degraded in the natural environment, without white pollution, which meets the requirements of environmental protection policies.

[0007] To achieve the above objectives, the present invention adopts the following technical solution.

[0008] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 60-80 parts of PBAT resin, 5-20 parts of whiskers, 10-20 parts of calcium carbonate, 2-5 parts of talc, 1-3 parts of compatibilizer, and 0.3-1.5 parts of processing aid.

[0009] The preparation method includes: 1) Dry the whiskers to remove surface moisture; mix the dried whiskers with a coupling agent to coat the surface of the whiskers with the coupling agent, thus obtaining pretreated whiskers. 2) Mix PBAT resin, pretreated whiskers, compatibilizer, talc, calcium carbonate and processing aids to prepare a premix; 3) The premixed material is fed into a twin-screw extruder for melt blending, extruded and pelletized to obtain modified biodegradable resin particles; 4) The modified biodegradable resin particles are dried and then fed into a blow molding machine for blow molding to obtain a biodegradable film. After cutting and heat sealing, a high-puncture biodegradable film bag is made.

[0010] Preferred, Step 1) The whiskers are one or more of calcium sulfate whiskers, calcium carbonate whiskers, and magnesium sulfate whiskers, with a particle size ≤20 μm and an aspect ratio of 1 to 5.

[0011] The drying in step 1) is carried out in a forced-air drying oven at a temperature of 80-100 ℃ for 2-4 hours. The moisture content of the whiskers after drying is ≤0.3%.

[0012] Step 1) The mixing and stirring are carried out in a high-speed mixer at a speed of 800-1200 r / min for 10-20 min.

[0013] Step 1) The coupling agent is one of γ-aminopropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane, and the amount of coupling agent added is 0.5 to 2% of the weight of the whiskers.

[0014] Preferred, Step 2) The melt index of the PBAT resin at 190 °C and 2.16 kg is 3–10 g / 10 min; Step 2) The calcium carbonate is light calcium carbonate or heavy calcium carbonate, with a fineness of 1000-8000 mesh.

[0015] Step 2) The particle size D50 of the talc powder is 1.0 to 5.0 μm.

[0016] Step 2) The compatibilizer is one or more of styrene-acrylonitrile-glycidyl methacrylate and ethylene-acrylate-glycidyl methacrylate copolymer.

[0017] Step 2) The processing aid is one or more of stearic acid, zinc stearate, and polyethylene wax.

[0018] Step 2) The mixing is carried out in a high-speed mixer at a speed of 1000-1500 r / min and a temperature of 40-60 ℃ for 5-10 min.

[0019] Preferred, Step 3) The length-to-diameter ratio of the twin-screw extruder is (32-48):1, the temperature of each section is set as follows: feed section 140-160 ℃, melt section 160-175 ℃, die head section 170-180 ℃, screw speed is 100-150 r / min, and internal melt pressure of the extruder is 0.2-0.6 MPa.

[0020] Step 3) The particle size of the modified biodegradable resin particles after pelleting is 2-4 mm.

[0021] Preferred, Step 4) The drying process is carried out in a forced-air drying oven at a temperature of 80-90°C for 1-2 hours.

[0022] Step 4) The temperatures of each section of the blow molding machine are set as follows: feeding section 150-165 ℃, melting section 165-175 ℃, die head section 170-180 ℃, die head gap 0.8-1.2 mm, blow-up ratio 2.5-3.5, traction speed 2-5 m / min, cooling air temperature 20-30 ℃, and internal pressure of blow molding machine 0.1-0.3 MPa.

[0023] Step 4) The temperature of the heat seal is 120-140 ℃, and the heat sealing time is 1-3 s.

[0024] A highly puncture-resistant biodegradable film bag is prepared by any of the methods described above. The film layer thickness of the highly puncture-resistant biodegradable film bag is 0.015–0.080 mm, preferably 0.020–0.050 mm. This range covers mainstream application scenarios such as supermarket shopping bags, takeaway flat bags (0.02–0.030 mm), brand retail bags, and express delivery bags (0.035–0.045 mm). For heavy-duty packaging requirements, the film layer thickness is preferably 0.050 mm–0.080 mm.

[0025] The core of the technical solution of this invention lies in the addition of special whiskers as a modified reinforcing component to the PBAT resin system, and the synergistic improvement of the puncture performance, tensile performance and tear resistance of the membrane bag through the accompanying preparation process.

[0026] This invention is based on the crystallographic characteristics of whisker materials, which endow them with a unique strengthening and toughening mechanism. Whiskers are fibrous materials grown in single crystal form under artificially controlled conditions. They have almost no lattice defects, highly ordered atomic arrangement, and mechanical strength close to the theoretical limit determined by the interatomic forces between adjacent atoms. When whiskers are uniformly dispersed in a PBAT matrix, the composite material exhibits a reinforcing effect through three interrelated micromechanical mechanisms during puncture by a sharp object: crack bridging mechanism, where whiskers straddle both sides of a propagating crack, using their high strength to establish a stress transfer bridge between the crack surfaces, hindering further crack opening and propagation; crack deflection mechanism, where the crack tip is forced to change its propagation direction when encountering high-modulus whiskers, deflecting along the interface between the whisker and the matrix, thus significantly increasing the tortuosity and total length of the fracture path. According to Griffith fracture theory, the extension of the fracture path directly means an increase in fracture energy dissipation; and pull-out effect mechanism, where interfacial frictional resistance does work over the whisker slippage distance during the process of whisker being pulled out of the matrix, and a large amount of fracture energy is dissipated in the form of frictional heat. The synergistic effect of the above three mechanisms is fundamentally different from that of traditional particulate fillers. Spherical or sheet-like fillers can only form stress concentration points in the matrix and passively bear loads by physically occupying space. They lack the ability to actively intervene in the crack propagation process. Therefore, their improvement in puncture strength is far less than that of fibrous whiskers.

[0027] This invention constructs a multi-component composite reinforcement system using three different geometric morphologies of inorganic fillers: fibrous, spherical, and lamellar. The mechanical functions of these fillers within the matrix exhibit clear division and complementarity: fibrous whiskers, with their high aspect ratio, provide load-bearing capacity, acting as the main load transfer path and constructing a puncture-resistant skeletal network in the composite material; spherical calcium carbonate particles fill the voids between the fibrous network and the matrix, enhancing overall toughness through stress dispersion at the spherical interface when the material is subjected to tearing or tensile loads; and lamellar talc powder, with its two-dimensional planar structure, strengthens the interlayer bonding of the matrix, inhibiting interlayer slippage and delamination. These three filler morphologies contribute reinforcement effects at zero, one, and two-dimensional scales, respectively, constructing a multi-scale, multi-dimensional spatial reinforcement network within the PBAT matrix. This network can rapidly transfer and disperse locally concentrated stress to a larger volume area, avoiding early failure caused by stress concentration, thereby achieving simultaneous optimization of puncture strength, tensile strength, and tear resistance.

[0028] This invention employs a dual interface modification strategy combining surface modification of coupling agents and the addition of reactive compatibilizers to address the interfacial compatibility issue between inorganic whiskers and the organic PBAT matrix from both chemical bonding and physical entanglement perspectives. The whisker surface contains abundant active functional groups such as hydroxyl groups. The alkoxy groups at one end of the silane coupling agent molecule can undergo hydrolysis-condensation reactions with these hydroxyl groups to form covalent bonds, while the organic functional groups at the other end can physically entangle or chemically bond with the PBAT molecular chains, constructing a "molecular bridge" structure between the inorganic and organic phases. Furthermore, the epoxy functional groups carried on the compatibilizer molecular chains can undergo ring-opening addition reactions with the carboxyl groups at the ends of the PBAT molecular chains, forming additional chemical crosslinking points and further enhancing the interfacial bonding strength. The coupling agent and compatibilizer act on the surface of the inorganic whisker and the interior of the organic matrix, respectively, forming a complementary and reinforced chemical bonding layer in the interface region. This allows stress to be efficiently transferred from the low-modulus PBAT matrix to the high-modulus whisker reinforcing phase, which is a prerequisite for the uniform dispersion of whiskers and the full utilization of reinforcing efficiency.

[0029] Furthermore, the calcium sulfate whiskers, calcium carbonate whiskers, and magnesium sulfate whiskers selected in this invention are all inorganic salt materials. Their degradation pathway in the natural environment is a synergistic effect of hydrolysis and microbial erosion, ultimately decomposing into environmentally friendly inorganic salt ions without producing persistent organic pollutants. Since the introduction of whiskers does not alter the ester bond structure in the PBAT molecular chain, the original biodegradation pathway of PBAT—namely, the hydrolysis and breakage of ester bonds and subsequent microbial mineralization—is completely preserved. This feature distinguishes it from existing technologies that use organic polymer toughening agents such as EVA and TPU for modification. While the latter can improve some mechanical properties, the introduced organic components may interfere with the crystallization behavior and degradation rate of PBAT, and may even degrade slowly under certain conditions, negatively impacting overall degradation performance.

[0030] In this invention, the crystallographic nature and fibrous geometry of whiskers form the physical basis for their multiple reinforcement and toughening mechanisms. This basis, in turn, determines the irreplaceable role of whiskers as the main load-bearing framework in the "three-morphology" composite system. For the "three-morphology" reinforcement network to achieve synergistic optimization of mechanical properties such as puncture, tensile, and tear resistance, sufficient interfacial bonding strength between the whiskers and the matrix is ​​essential; otherwise, the applied load cannot be effectively transferred to the reinforcing phase. This is precisely the core scientific problem that the dual-interface modification strategy aims to solve. Furthermore, the implementation of all the above technical solutions is based on the constraint of not altering the molecular structure and degradation mechanism of PBAT, thereby achieving a leapfrog improvement in mechanical properties while ensuring that the material's full degradation characteristics are not sacrificed. The complete technical solution constituted by the above-mentioned internal logical connections gives this invention both outstanding substantive features and significant progress compared to existing technologies.

[0031] Compared with the prior art, the present invention provides a highly puncture-resistant biodegradable membrane bag and its preparation method, which has the following beneficial effects: 1. This invention utilizes the synergistic effect of three micromechanical mechanisms—crack bridging, crack deflection, and pull-out effect of whiskers—in conjunction with a multi-scale spatial reinforcement network constructed from fillers of different morphologies, such as fibrous, spherical, and sheet-like structures, to improve the puncture strength of membrane bags compared to unmodified PBAT membrane bags. This significantly reduces the puncture and breakage rate of membrane bags during filling, transportation, and use, thereby significantly improving reliability. 2. This invention achieves a synergistic improvement in puncture resistance, tensile strength, and tear resistance by functional division and performance complementarity of fillers in different dimensions, while taking into account both flexibility and rigidity. It can adapt to the usage requirements of various packaging scenarios and has a wide range of applications. 3. The modification scheme of the present invention will not destroy the original biodegradable structure of PBAT resin. The selected whiskers and inorganic fillers can be decomposed into environmentally friendly substances in the end. While greatly improving the mechanical properties, the material's fully degradable characteristics are completely preserved. After the film bag is discarded, it can be completely degraded in the natural environment without white pollution residue, which meets the requirements of green and environmentally friendly development. 4. This invention employs a dual interface modification strategy combining coupling agent surface modification and reactive compatibilizer, which effectively solves the interface compatibility problem between inorganic whiskers and the PBAT organic matrix, ensures efficient stress transfer from the matrix to the reinforcing phase, fully utilizes the reinforcing efficiency of whiskers, and results in good product performance stability. Detailed Implementation

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1

[0033] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 72 parts of PBAT resin (melt index of 5 g / 10 min at 190 °C and 2.16 kg), 12 parts of calcium sulfate whiskers (particle size ≤ 12 μm, aspect ratio 3:1), 14 parts of light calcium carbonate (fineness 3000 mesh), 3.5 parts of talc (D50 particle size 2.5 μm), 2.2 parts of styrene-acrylonitrile-glycidyl methacrylate compatibilizer, and 0.9 parts of stearic acid processing aid.

[0034] Preparation methods include: 1) Place calcium sulfate whiskers in a forced-air drying oven and dry at 92 ℃ for 3 h to remove surface moisture until the moisture content is ≤0.3%; then add the dried whiskers and γ-aminopropyltriethoxysilane coupling agent into a high-speed mixer. The amount of coupling agent added is 1.1% of the weight of the whiskers. Stir at 1000 r / min for 15 min to coat the surface of the whiskers with the coupling agent, thus obtaining pretreated whiskers. 2) PBAT resin, pretreated whiskers, styrene-acrylonitrile-glycidyl methacrylate compatibilizer, talc, light calcium carbonate and stearic acid were added sequentially to a high-speed mixer and mixed for 7 min at 1300 r / min speed and 52 ℃ temperature to obtain a premix. 3) The premixed material is fed into a twin-screw extruder with a length-to-diameter ratio of 40:1 for melt blending. The temperature of each section is set as follows: feed section 152 ℃, melt section 168 ℃, die head section 175 ℃, screw speed 125 r / min, internal melt pressure of extruder 0.40 MPa, extruded and pelletized to obtain modified biodegradable resin particles with a particle size of 3 mm. 4) The modified biodegradable resin particles were placed in a forced-air drying oven and dried at 85 ℃ for 1.5 h; then fed into a blow molding machine for blow molding. The temperature of each section of the blow molding machine was set as follows: feeding section 158 ℃, melting section 170 ℃, die head section 176 ℃, die head gap 1.0 mm, blow-up ratio 3.0, traction speed 3.5 m / min, cooling air temperature 25 ℃, and internal pressure of blow molding machine 0.20 MPa to obtain a biodegradable film, which was then cut and heat-sealed at 130 ℃ for 2 s to produce a high-puncture biodegradable film bag.

[0035] The material prepared in Example 1 was subjected to performance testing. The puncture strength was determined according to GB / T 10004-2008, the tensile strength and elongation at break were determined according to GB / T 1040.3-2006, and the tear resistance was determined according to GB / T 16578.1-2008. The specific characterization results are as follows.

[0036]

[0037] Analysis of the above characterization results shows that the high-puncture biodegradable membrane bag prepared in Example 1 has improved puncture strength, tensile strength and tear strength compared with the pure PBAT membrane bag (puncture strength of about 5.2 N, tensile strength of about 18.5 MPa and tear strength of about 68 kN / m). It has excellent comprehensive mechanical properties, taking into account both strength and flexibility. Example 2

[0038] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 68 parts of PBAT resin (melt index of 7 g / 10 min at 190 °C and 2.16 kg), 15 parts of calcium carbonate whiskers (particle size ≤ 8 μm, aspect ratio 4:1), 12 parts of heavy calcium carbonate (fineness 5000 mesh), 4 parts of talc (D50 particle size 2.0 μm), 2.5 parts of ethylene-acrylate-glycidyl ester copolymer compatibilizer, and 1.0 part of zinc stearate processing aid.

[0039] Preparation methods include: 1) Place calcium carbonate whiskers in a forced-air drying oven and dry at 85 ℃ for 3.5 h to remove surface moisture until the moisture content is ≤0.3%; then add the dried whiskers and γ-glycidoxypropyltrimethoxysilane coupling agent into a high-speed mixer. The amount of coupling agent added is 1.4% of the weight of the whiskers. Stir at 1100 r / min for 12 min to coat the surface of the whiskers with the coupling agent, thus obtaining pretreated whiskers. 2) PBAT resin, pretreated whiskers, ethylene-acrylate-glycidyl ester copolymer compatibilizer, talc, heavy calcium carbonate and zinc stearate were added sequentially to a high-speed mixer and mixed for 8 min at 1400 r / min speed and 46 ℃ temperature to obtain a premix. 3) The premixed material is fed into a twin-screw extruder with a length-to-diameter ratio of 44:1 for melt blending. The temperature of each section is set as follows: feed section 146 ℃, melt section 164 ℃, die head section 172 ℃, screw speed 135 r / min, internal melt pressure of extruder 0.45 MPa, extruded and pelletized to obtain modified biodegradable resin particles with a particle size of 3 mm. 4) The modified biodegradable resin particles were placed in a forced-air drying oven and dried at 82 ℃ for 1.8 h; then fed into a blow molding machine for blow molding. The temperature of each section of the blow molding machine was set as follows: feeding section 154 ℃, melting section 167 ℃, die head section 172 ℃, die head gap 1.0 mm, blow-up ratio 3.3, traction speed 3.0 m / min, cooling air temperature 24 ℃, and internal pressure of blow molding machine 0.20 MPa to obtain a biodegradable film, which was then cut and heat-sealed at 127 ℃ for 2.5 s to produce a high-puncture biodegradable film bag.

[0040] The material prepared in Example 2 was subjected to performance testing. The puncture strength was determined according to GB / T 10004-2008, the tensile strength and elongation at break were determined according to GB / T 1040.3-2006, and the tear resistance was determined according to GB / T 16578.1-2008. The specific characterization results are as follows.

[0041]

[0042] Analyzing the above characterization results, the high-puncture biodegradable film bag prepared in Example 2 shows a more significant improvement in various mechanical properties compared to Example 1. The puncture strength, tensile strength, and tear strength are all improved compared to the pure PBAT film bag, while still maintaining a 488% elongation at break. This indicates that the compound modification scheme of the present invention can significantly improve the strength indicators without excessively sacrificing the flexibility and fracture toughness of the material. The final prepared film bag has excellent comprehensive mechanical properties and can meet the usage requirements of various heavy-duty biodegradable packaging scenarios for high puncture and high tear resistance. Example 3

[0043] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 78 parts of PBAT resin (melt index of 4 g / 10 min at 190 °C and 2.16 kg), 6 parts of magnesium sulfate whiskers (particle size ≤ 16 μm, aspect ratio 1.5:1), 19 parts of light calcium carbonate (fineness 2000 mesh), 2.5 parts of talc (D50 particle size 3.0 μm), 1.5 parts of styrene-acrylonitrile-glycidyl methacrylate compatibilizer, and 0.5 parts of polyethylene wax processing aid.

[0044] Preparation methods include: 1) Place magnesium sulfate whiskers in a forced-air drying oven and dry at 98 ℃ for 2.2 h to remove surface moisture until the moisture content is ≤0.3%; then add the dried whiskers and γ-aminopropyltriethoxysilane coupling agent into a high-speed mixer. The amount of coupling agent added is 0.7% of the weight of the whiskers. Stir at 850 r / min for 18 min to coat the surface of the whiskers with the coupling agent to obtain pretreated whiskers. 2) PBAT resin, pretreated whiskers, styrene-acrylonitrile-glycidyl methacrylate compatibilizer, talc, light calcium carbonate and polyethylene wax were added sequentially to a high-speed mixer and mixed for 6 min at 1050 r / min speed and 56 ℃ temperature to obtain a premix. 3) The premixed material is fed into a twin-screw extruder with a length-to-diameter ratio of 34:1 for melt blending. The temperatures of each section are set as follows: feed section 156 ℃, melt section 172 ℃, and die head section 178 ℃. The screw speed is 108 r / min, and the melt pressure inside the extruder is 0.32 MPa. After extrusion, the material is pelletized to obtain modified biodegradable resin particles with a particle size of 3 mm. 4) The modified biodegradable resin particles were placed in a forced-air drying oven and dried at 88 ℃ for 1.2 h; then fed into a blow molding machine for blow molding. The temperature of each section of the blow molding machine was set as follows: feeding section 162 ℃, melting section 173 ℃, die head section 178 ℃, die head gap 0.9 mm, blow-up ratio 2.7, traction speed 4.5 m / min, cooling air temperature 28 ℃, and internal pressure of the blow molding machine 0.28 MPa to obtain a biodegradable film. After cutting, the film was heat-sealed at 133 ℃ for 1.5 s to produce a high-puncture biodegradable film bag.

[0045] The material prepared in Example 3 was subjected to performance testing. The puncture strength was determined according to GB / T 10004-2008, the tensile strength and elongation at break were determined according to GB / T 1040.3-2006, and the tear resistance was determined according to GB / T 16578.1-2008. The specific characterization results are as follows.

[0046]

[0047] Analyzing the above characterization results, the high-puncture biodegradable film bag prepared in Example 3 still shows a significant improvement in various mechanical properties compared to the pure PBAT film bag. Although the strength index improvement is slightly smaller than that in Examples 1 and 2 due to the reduced amount of whiskers, the longitudinal elongation at break reaches 562%, which is higher than the previous two examples. This indicates that the material under this formulation system has better flexibility and can be adapted to conventional biodegradable packaging application scenarios with high flexibility requirements and moderate strength requirements. It also has good comprehensive performance and fully biodegradable environmental protection characteristics. Example 4

[0048] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 60 parts of PBAT resin (melt index of 8 g / 10 min at 190 °C and 2.16 kg), 5 parts of calcium sulfate whiskers (particle size ≤ 20 μm, aspect ratio 1:1), 10 parts of light calcium carbonate (fineness 8000 mesh), 2 parts of talc (D50 particle size 5.0 μm), 1 part of styrene-acrylonitrile-glycidyl methacrylate compatibilizer, and 0.3 parts of stearic acid processing aid.

[0049] Preparation methods include: 1) Place calcium sulfate whiskers in a forced-air drying oven and dry at 80 ℃ for 2 h to remove surface moisture until the moisture content is ≤0.3%; then add the dried whiskers and γ-aminopropyltriethoxysilane coupling agent into a high-speed mixer. The amount of coupling agent added is 0.5% of the weight of the whiskers. Stir at 800 r / min for 10 min to coat the surface of the whiskers with the coupling agent, thus obtaining pretreated whiskers. 2) PBAT resin, pretreated whiskers, styrene-acrylonitrile-glycidyl methacrylate compatibilizer, talc, light calcium carbonate and stearic acid were added sequentially to a high-speed mixer and mixed for 5 min at 1000 r / min speed and 40 ℃ temperature to obtain a premix. 3) The premixed material is fed into a twin-screw extruder with a length-to-diameter ratio of 32:1 for melt blending. The temperature of each section is set as follows: feed section 140 ℃, melt section 160 ℃, die head section 170 ℃, screw speed 100 r / min, internal melt pressure of extruder 0.20 MPa, extruded and pelletized to obtain modified biodegradable resin particles with a particle size of 2 mm. 4) The modified biodegradable resin particles were placed in a forced-air drying oven and dried at 80 ℃ for 1 h; then fed into a blow molding machine for blow molding. The temperature of each section of the blow molding machine was set as follows: feeding section 150 ℃, melting section 165 ℃, die head section 170 ℃, die head gap 0.8 mm, blow-up ratio 2.5, traction speed 2.0 m / min, cooling air temperature 20 ℃, and internal pressure of blow molding machine 0.10 MPa to obtain a biodegradable film. After cutting, it was heat-sealed at 120 ℃ for 1 s to produce a high-puncture biodegradable film bag.

[0050] The material prepared in Example 4 was subjected to performance testing. The puncture strength was determined according to GB / T 10004-2008, the tensile strength and elongation at break were determined according to GB / T 1040.3-2006, and the tear resistance was determined according to GB / T 16578.1-2008. The specific characterization results are as follows.

[0051]

[0052] Analyzing the above characterization results, the high-puncture biodegradable film bag prepared in Example 4 still shows a significant improvement in various mechanical properties compared to the pure PBAT film bag. The total amount of whiskers and inorganic fillers added in this formulation system is relatively low, while the proportion of PBAT resin is higher. Therefore, the raw material processing has better fluidity and is easier to process. At the same time, the overall raw material cost is lower. The resulting film bag still maintains qualified puncture, tensile and tear resistance properties, and the elongation at break is also maintained at a high level, which can meet the usage requirements of ordinary light-load biodegradable packaging scenarios. Example 5

[0053] A highly puncture-resistant biodegradable film bag is blow-molded from a modified biodegradable resin composition, wherein the modified biodegradable resin composition comprises the following components in parts by weight: 80 parts of PBAT resin (melt index of 3 g / 10 min at 190 °C and 2.16 kg), 20 parts of calcium carbonate whiskers (particle size ≤ 5 μm, aspect ratio 5:1), 20 parts of heavy calcium carbonate (fineness 1000 mesh), 5 parts of talc (D50 particle size 1.0 μm), 3 parts of ethylene-acrylate-glycidyl ester copolymer compatibilizer, and 1.5 parts of polyethylene wax processing aid.

[0054] Preparation methods include: 1) Place calcium carbonate whiskers in a forced-air drying oven and dry at 100 °C for 4 h to remove surface moisture until the moisture content is ≤0.3%; then add the dried whiskers and γ-glycidyl oxypropyltrimethoxysilane coupling agent into a high-speed mixer. The amount of coupling agent added is 2.0% of the weight of the whiskers. Stir at 1200 r / min for 20 min to coat the surface of the whiskers with the coupling agent and obtain pretreated whiskers. 2) PBAT resin, pretreated whiskers, ethylene-acrylate-glycidyl ester copolymer compatibilizer, talc, heavy calcium carbonate and polyethylene wax are added sequentially to a high-speed mixer and mixed for 10 min at 1500 r / min speed and 60 ℃ temperature to obtain a premix. 3) Melt blending and granulation: The premixed material is fed into a twin-screw extruder with a length-to-diameter ratio of 48:1 for melt blending. The temperatures of each section are set as follows: feed section 160 ℃, melt section 175 ℃, and die head section 180 ℃. The screw speed is 150 r / min, and the melt pressure inside the extruder is 0.60 MPa. After extrusion, the material is granulated to obtain modified biodegradable resin particles with a particle size of 4 mm. 4) The modified biodegradable resin particles were placed in a forced-air drying oven and dried at 90 ℃ for 2 h; then fed into a blow molding machine for blow molding. The temperature of each section of the blow molding machine was set as follows: feeding section 165 ℃, melting section 175 ℃, die head section 180 ℃, die head gap 1.2 mm, blow-up ratio 3.5, traction speed 5.0 m / min, cooling air temperature 30 ℃, and internal pressure of blow molding machine 0.30 MPa to obtain a biodegradable film, which was then cut and heat-sealed at 140 ℃ for 3 s to produce a high-puncture biodegradable film bag.

[0055] The material prepared in Example 5 was subjected to performance testing. The puncture strength was determined according to GB / T 10004-2008, the tensile strength and elongation at break were determined according to GB / T 1040.3-2006, and the tear resistance was determined according to GB / T 16578.1-2008. The specific characterization results are as follows.

[0056]

[0057] Analysis of the above characterization results shows that the high-puncture biodegradable film bag prepared in Example 5 still achieves significant improvement in various mechanical properties compared with the pure PBAT film bag. The formulation system has a high amount of whiskers. Under the reinforcement effect of the high aspect ratio whiskers, the puncture strength, tensile strength and tear strength of the film bag all meet the standards for medium and heavy-duty packaging. Although the high total amount of inorganic filler makes the longitudinal elongation at break slightly lower than that of other examples with low filler content, the elongation at break of 442% can still ensure that the film bag has sufficient flexibility and fracture toughness.

[0058] Comparative Example 1: Based on Example 2, this example only modifies the type and amount of whiskers; the remaining steps are the same as in Example 2. The specific settings are as follows:

[0059] The performance testing method for the comparative product was exactly the same as that for Example 2. Partial performance characterization was performed, and the specific characterization results are shown in the table below.

[0060]

[0061] Analysis of the above characterization results shows that the puncture strength of D1-1 is lower than that of Example 2, indicating that the addition of whiskers is a key factor in improving puncture performance. The improvement in puncture strength of D1-2 is limited, indicating that an effective fiber reinforcement network cannot be formed when the amount of whiskers added is too low. The puncture strength of D1-3 is sufficient, but the elongation at break is significantly reduced, and a slight grainy texture appears on the film surface, indicating that although an excessive amount of whiskers can improve puncture performance, it will damage the flexibility of the material and the surface quality of the processed material. Although the puncture strength of D1-4 is improved to some extent, the tear strength and elongation at break are significantly lower than those of Example 2, and the film surface shows obvious roughness and fiber floating phenomenon. This is due to the difficulty in uniformly dispersing glass fibers in complex molds, which easily leads to areas of fiber deficiency.

[0062] The highly puncture-resistant biodegradable membrane bag prepared by this invention uses fully biodegradable PBAT resin as the matrix, and is reinforced with modified inorganic whiskers and inorganic fillers. Compared with pure PBAT membrane bags, the puncture strength, tensile strength and tear resistance are all improved. At the same time, the formula can be adjusted according to different usage scenarios to ensure the fully biodegradable and environmentally friendly characteristics while taking into account performance requirements.

[0063] Comparative Example 2: Based on Example 2, this example only modifies the whisker size and aspect ratio; the remaining steps are the same as in Example 2. The specific settings are as follows:

[0064] The performance testing method for the comparative product is completely consistent with that of Example 2. Partial performance characterization was performed, and the specific characterization results are as follows.

[0065]

[0066] Analysis of the above characterization results shows that all strength indicators of D2-1 are significantly lower than those of Example 2, indicating that when the whisker particle size is too large, stress concentration defects are easily formed inside the PBAT matrix, and the one-dimensional fiber reinforcement effect of the whiskers cannot be fully utilized. Therefore, the improvement effect on the mechanical properties of the film bag is very limited. The whisker aspect ratio of D2-2 is too high. Although theoretically the reinforcement potential of a single whisker is higher, the excessively high aspect ratio will cause the whiskers to agglomerate and entangle more easily during processing and mixing, making it difficult to disperse evenly in the matrix resin. Instead, it will cause internal defects. Not only are all strength indicators lower than those of Example 2, but the elongation at break of the material also decreases significantly. D2-3 uses nearly granular whiskers with a low aspect ratio. At this time, the whiskers can only play the role of ordinary inorganic filler and cannot form an effective one-dimensional fiber reinforcement network structure. Therefore, the improvement in puncture strength, tensile strength and tear strength is far lower than that of Example 2, and only slightly better than that of pure PBAT film bags without whiskers.

[0067] The whisker particle size and aspect ratio range selected in this invention is a reasonable range for reinforcing the PBAT matrix. It can ensure that the whiskers maintain good dispersion in the matrix and give full play to the one-dimensional structural reinforcement effect of the whiskers, ultimately achieving a balance between the strength and flexibility of the membrane bag.

[0068] Comparative Example 3: Based on Example 2, this example only modifies the use of the coupling agent and compatibilizer; the remaining steps are the same as in Example 2. The specific settings are as follows:

[0069] The performance testing method for the comparative product is completely consistent with that of Example 2. Partial performance characterization was performed, and the specific characterization results are shown in the table below.

[0070]

[0071] Analysis of the above characterization results shows that D3-1 did not undergo coupling agent pretreatment of the whiskers. The whiskers themselves are highly polar, resulting in poor interfacial bonding with the hydrophobic PBAT resin matrix. Under external force, stress concentration and crack propagation easily occur at the interface between the whiskers and the matrix. Therefore, all mechanical properties are significantly lower than those of Example 2. Furthermore, poor whisker dispersibility leads to a slight grainy texture on the film surface. D3-2 only lacks a compatibilizer. Although coupling agent pretreatment improves the interfacial bonding between the whiskers and the matrix, the overall compatibility of various inorganic fillers with the PBAT matrix is ​​not optimized. Therefore, all mechanical properties are still significantly lower than those of Example 2, and the film surface also exhibits a slight grainy texture due to poor dispersion of some fillers. D3-3 neither underwent whisker coupling pretreatment nor added a compatibilizer. All inorganic fillers, including the whiskers, failed to form a good interfacial bond with the PBAT matrix. Severe filler agglomeration and numerous internal defects significantly reduced mechanical properties. Ultimately, the film surface exhibited obvious grainy and rough defects, failing to meet packaging requirements.

[0072] The technical solution of pretreating whiskers with coupling agent and combining them with system compatibilizer in this invention can effectively improve the interfacial bonding performance between inorganic fillers and PBAT matrix, enhance the uniformity of filler dispersion in matrix, ensure that whiskers fully play their reinforcing role, and ultimately guarantee the mechanical properties of the film bag and the surface quality after processing and molding.

[0073] Comparative Example 4: Based on Example 2, this example only modifies the types of inorganic seasonings used in the compound; the remaining steps are the same as in Example 2. The specific settings are as follows:

[0074] The performance testing method for the comparative product is completely consistent with that of Example 2. Partial performance characterization was performed, and the characterization results are shown in the table below.

[0075]

[0076] Analyzing the above characterization results, D4-1, without the addition of flake talc, exhibited lower mechanical strengths than Example 2. This is because the flake-structured talc forms a layered barrier inside the film bag, effectively hindering crack propagation under external force, thus improving puncture and tear resistance. Without talc, the system loses its layered reinforcement and crack-resistant effect, resulting in a significant decline in mechanical properties. D4-2, without the addition of spherical heavy calcium carbonate, retained only calcium carbonate whiskers and talc. In this case, the filler gradation was unreasonable, and the one-dimensional whiskers and flake talc could not achieve close packing, easily forming gap defects inside the film bag. Therefore, all strength indicators were lower than in Example 2. Although the elongation at break was slightly improved, the overall mechanical properties could not meet the requirements for medium- and heavy-duty packaging. D4-3, without the addition of calcium carbonate whiskers, relied solely on spherical calcium carbonate and flake talc for filling. Lacking the reinforcing effect of the one-dimensional fiber structure, it could not form an effective reinforcing network. Therefore, the puncture strength, tensile strength, and tear resistance were all far lower than in Example 2, consistent with the performance change pattern of the whisker-free system described above.

[0077] The composite filling system of fibrous whiskers, spherical heavy calcium carbonate and flake talc powder used in this invention can achieve optimal gradation through the synergistic effect of fillers with different morphologies. It not only gives full play to the reinforcing effect of fillers of different dimensions, but also controls the cost of raw materials through reasonable filler matching. Finally, it produces a high-puncture biodegradable film bag with excellent comprehensive performance, which is suitable for the use needs of different packaging scenarios.

[0078] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0079] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a highly puncture-resistant biodegradable membrane bag, characterized in that, Includes the following steps: (1) Dry the whiskers to remove surface moisture; The dried whiskers are mixed and stirred with a coupling agent to coat the surface of the whiskers, thus obtaining pretreated whiskers. (2) PBAT resin, pretreated whiskers, compatibilizer, talc, calcium carbonate and processing aids are mixed to prepare a premix; (3) The premixed material is fed into a twin-screw extruder for melt blending, extruded and then pelletized to obtain modified biodegradable resin particles; (4) The modified biodegradable resin particles are dried and then blow-molded in a blow molding machine to obtain a biodegradable film. After cutting and heat sealing, a high-puncture biodegradable film bag is made.

2. The method according to claim 1, characterized in that, In step (2), the weight parts of PBAT resin, pretreated whiskers, calcium carbonate, talc, compatibilizer and processing aid are as follows: 60-80 parts of PBAT resin, 5-20 parts of pretreated whiskers, 10-20 parts of calcium carbonate, 2-5 parts of talc, 1-3 parts of compatibilizer and 0.3-1.5 parts of processing aid.

3. The method according to claim 2, characterized in that, In step (1), the whiskers are one or more of calcium sulfate whiskers, calcium carbonate whiskers, and magnesium sulfate whiskers, with a particle size ≤20 μm and an aspect ratio of 1 to 5; the coupling agent is one of γ-aminopropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane, and the amount of coupling agent added is 0.5 to 2% of the weight of the whiskers.

4. The method according to claim 1, characterized in that, In step (1), the drying is carried out in a blower drying oven at a temperature of 80-100 ℃ for 2-4 h, and the moisture content of the whiskers after drying is ≤0.3%; the mixing is carried out in a high-speed mixer at a speed of 800-1200 r / min for 10-20 min.

5. The method according to claim 2, characterized in that, In step (2), the melt index of the PBAT resin at 190 °C and 2.16 kg is 3 to 10 g / 10 min; the calcium carbonate is light calcium carbonate or heavy calcium carbonate with a fineness of 1000 to 8000 mesh; and the particle size D50 of the talc powder is 1.0 to 5.0 μm.

6. The method according to claim 2, characterized in that, In step (2), the compatibilizer is one or more of styrene-acrylonitrile-glycidyl methacrylate and ethylene-acrylate-glycidyl methacrylate copolymer; the processing aid is one or more of stearic acid, zinc stearate and polyethylene wax; the mixing is carried out in a high-speed mixer at a speed of 1000-1500 r / min and a temperature of 40-60 ℃ for 5-10 min.

7. The method according to claim 1, characterized in that, In step (3), the length-to-diameter ratio of the twin-screw extruder is (32-48):1, the temperature of each section is set to 140-160 ℃ for the feeding section, 160-175 ℃ for the melting section, and 170-180 ℃ for the die head section, the screw speed is 100-150 r / min, the melt pressure inside the extruder is 0.2-0.6 MPa, and the particle size of the modified biodegradable resin particles after pelleting is 2-4 mm.

8. The method according to claim 1, characterized in that, In step (4), the drying process is carried out in a forced-air drying oven at a temperature of 80–90 °C for 1–2 h. The temperature of each section of the blow molding machine is set as follows: feeding section 150–165 °C, melting section 165–175 °C, die head section 170–180 °C, die head gap 0.8–1.2 mm, blow-up ratio 2.5–3.5, traction speed 2–5 m / min, cooling air temperature 20–30 °C, and internal pressure of the blow molding machine 0.1–0.3 MPa. The heat sealing temperature is 120–140 °C, and the heat sealing time is 1–3 s.

9. The highly puncture-resistant biodegradable membrane bag prepared according to the method in claim 1, characterized in that, The membrane bag is blow-molded from a modified biodegradable resin composition comprising PBAT resin, whiskers, calcium carbonate, talc, compatibilizer, and processing aids; the membrane thickness of the membrane bag is 0.015–0.080 mm.

10. The highly puncture-resistant biodegradable membrane bag according to claim 9, characterized in that, The whiskers are one or more of calcium sulfate whiskers, calcium carbonate whiskers, and magnesium sulfate whiskers, with a particle size ≤20 μm and an aspect ratio of 1 to 5; the compatibilizer is one or more of styrene-acrylonitrile-glycidyl methacrylate and ethylene-acrylate-glycidyl methacrylate copolymer.