A PLA-modified material, its preparation method and application
By coating boron nitride and micron-sized silica with pyrrolidone and blending it with PLA resin, a continuous thermal conductivity pathway is constructed, which solves the problems of low thermal conductivity and weak interlayer bonding of PLA material in FDM printing, and achieves high-speed printing and high layer bonding strength.
Patent Information
- Application Number
- CN202611399806.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PLA materials suffer from problems such as low thermal conductivity, insufficient printing speed, and weak interlayer fusion during FDM printing. Modification with a single filler cannot simultaneously meet the multiple requirements of thermal conductivity, dispersion, strength, and flowability.
PLA modified materials were prepared by blending pyrrolidone-coated boron nitride and micron-sized silica with PLA and PBAT resins and then using a twin-screw extruder to construct a continuous thermally conductive pathway, thereby improving the melting rate and bonding strength.
It achieves high-speed printing (≥500mm/min), high layer bonding strength (>30MPa), and high tensile strength (≥4 days) of PLA materials, solving the problems of poor melt flow and weak interlayer fusion of traditional PLA materials in high-speed printing.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the fields of 3D printing consumable modification technology and polymer composite material technology, specifically to a high-speed printing, high-strength PLA modified material adapted to FDM fused deposition modeling process, its preparation method and application. Background Technology
[0002] Polylactic acid (PLA) is currently the most widely used environmentally friendly consumable in FDM 3D printing, boasting advantages such as ease of printing, low shrinkage, odorless, biodegradable, and low cost. However, pure PLA itself has inherent defects: extremely low thermal conductivity, with conventional pure PLA exhibiting a thermal conductivity of only about 0.2 W / (m·K), resulting in slow heat transfer. During FDM printing, normal extrusion is possible at a conventional printing speed of 200 mm / s. However, when the printing speed is increased to above 300 mm / s, the nozzle cannot fully melt the consumable in a short time, easily leading to defects such as extrusion interruption, poor melt flow, and weak interlayer fusion. Simply increasing the nozzle temperature to compensate for melting efficiency will significantly increase PLA thermal degradation and material stringing.
[0003] In existing modification schemes, the industry mostly uses methods such as toughening resin blending, nano-inorganic filler doping, and plasticizer addition to optimize PLA printing performance. Among them, boron nitride thermal conductivity modification often uses nano-scale ultrafine powder, which has problems such as easy agglomeration, high addition amount, high cost, and weak mechanical reinforcement effect; ordinary micron filler modification only focuses on reinforcement or wear resistance, without specifically addressing the technical pain point of insufficient melting rate in high-speed printing; at the same time, single filler modification cannot simultaneously meet the multiple requirements of thermal conductivity, dispersion, strength, and flowability. Patent CN108285623A provides a method for preparing impact-resistant and aging-resistant PLA composite material for 3D printing, which uses PLA compounded with boron nitride, but does not specifically optimize the printing speed and lamination strength of PLA material. Patent CN119570219A provides a high lamination strength PLA solution, but does not significantly improve the printing speed.
[0004] Therefore, it is essential to optimize PLA materials and develop a high-strength FDM high-speed printing PLA composite material. Summary of the Invention
[0005] To address the aforementioned problems in existing technologies, this invention provides a modified PLA material, its preparation method, and its application. This modified PLA material is compatible with FDM (Fused Deposition Modeling) processes, enabling high-speed printing and high strength. The material has a printing speed ≥500mm / min, a lamination strength >30MPa, and a tensile strength ≥4 days, exhibiting significant performance advantages compared to conventional PLA printing filaments.
[0006] To achieve the above technical effects, the technical solution adopted by the present invention is as follows:
[0007] In a first aspect, a PLA-modified material comprises the following raw materials in parts by weight:
[0008] 65-85 parts of PLA resin, preferably 70-81 parts;
[0009] 3 to 10 parts of PBAT resin, preferably 5 to 8 parts;
[0010] 5-20 parts of boron nitride coated with pyrrolidone, preferably 8-15 parts;
[0011] 1-10 parts of silicon dioxide, preferably 3-6 parts;
[0012] Lubricant: 0.1 to 0.5 parts, preferably 0.2 to 0.4 parts.
[0013] Preferably, the PLA resin has a weight-average molecular weight of 150,000 to 250,000 and an acid value of 10 to 40 mol / t; more preferably, it has a weight-average molecular weight of 180,000 to 210,000 and an acid value of 20 to 30 mol / t.
[0014] Preferably, the PBAT resin has a weight-average molecular weight of 100,000 to 150,000 and an acid value of 10 to 40 mol / t; more preferably, it has a weight-average molecular weight of 120,000 to 130,000 and an acid value of 10 to 20 mol / t.
[0015] Preferably, the silica is precipitated silica with a D50 particle size of 2-10 μm and a porosity of 0.4-1.5 cm⁻¹. 3 / g, preferably silica D50 with a particle size of 3~4µm and a porosity of 0.8~1.0cm³. 3 / g.
[0016] Preferably, the lubricant includes amide lubricants, and more preferably one or more of erucamide, oleamide, and behenamide.
[0017] Preferably, the pyrrolidone-coated boron nitride is obtained by melt blending carboxypyrrolidone with grafted boron nitride.
[0018] Preferably, the boron nitride is hexagonal boron nitride, and the boron nitride D50 particle size is 10~70 μm with an aspect ratio of 20~80. More preferably, the D50 particle size is 30~40 μm with an aspect ratio of 30~55.
[0019] The carboxypyrrolidone includes at least one of 4-carboxy-2-pyrrolidone (also known as 5-oxopyrrolidone-3-carboxylic acid, CAS No.: 7268-43-1) and 5-carboxy-2-pyrrolidone (also known as pyroglutamic acid, CAS No. includes 149-87-1, 98-79-3, 149-87-1 depending on chirality), preferably 4-carboxy-2-pyrrolidone.
[0020] The pyrrolidone-coated boron nitride described in this invention is prepared by melt blending and grafting. The specific preparation method includes the following steps:
[0021] Carboxypyrrolidone, catalyst and boron nitride are mixed and stirred at 800-1200 rpm for 3-5 min at room temperature. Then the mixture is heated to 140-150℃ in a high-speed mixer and stirred at 800-1200 rpm for 10-15 min. After drying, pyrrolidone-coated boron nitride is obtained.
[0022] Preferably, the catalyst can be an organotin catalyst, specifically including at least one of stannous octoate, dibutyltin dilaurate, tin lactate, and stannous isooctanoate, with stannous octoate being the most preferred.
[0023] Preferably, the mass ratio of boron nitride, carboxypyrrolidone, and catalyst is 5-10:0.1-5:0.001-0.05, and more preferably, the mass ratio is 8-10:0.2-0.5:0.005-0.01.
[0024] Preferably, the drying temperature is 80-120℃ and the drying time is 1-3 hours to remove adsorbed water.
[0025] Secondly, a method for preparing a PLA-modified material is provided, the method comprising the following steps:
[0026] Pyrrolidone-coated boron nitride, silica, and lubricant are mixed (e.g., using a mixer, preferably a low-temperature mixer) and fed into a twin-screw extruder through a side feed port. PLA resin and PBAT resin are mixed and fed into the twin-screw extruder through a main feed port. After extrusion, the mixture is water-cooled and granulated to obtain PLA modified material.
[0027] Preferably, the twin-screw extruder temperature is 180-200℃ and the screw speed is 300-500rpm.
[0028] Thirdly, a PLA filament is provided, which is prepared from a PLA modified material including the PLA modified material described in the first aspect or the PLA modified material prepared by the preparation method described in the second aspect. The PLA filament is a PLA filament for FDM printing, preferably a PLA filament for high-speed FDM printing.
[0029] Fourthly, a method for preparing PLA wire is provided, specifically including: feeding the aforementioned modified PLA material into a single-screw extruder, traction extrusion, and water cooling to obtain PLA wire.
[0030] Preferably, the screw temperature of the single-screw extruder is 180-200℃. The cooling water temperature after single-screw extrusion is preferably 40-70℃.
[0031] When the PLA filament described in this invention is used for high-speed FDM printing, the printing speed is ≥500mm / min, the bonding strength is >30MPa, and the tensile strength is ≥4 days.
[0032] Compared with the prior art, the beneficial effects of the technical solution of the present invention are as follows:
[0033] By grafting boron nitride with pyrrolidone, its dispersibility in the system is improved, the material polarity is increased, and the impact of boron nitride on the printing layer strength is reduced. At the same time, it does not affect the ultra-high thermal conductivity of hexagonal boron nitride, which can build a continuous thermal conduction path within the PLA system, significantly improving the heat dissipation speed and heat transfer efficiency of the consumables, enabling the printing speed to reach 500 mm / min, and preventing stringing during printing. Micron-sized silica can optimize the dispersibility of fillers and fill the voids in the system, synergistically achieving high strength and high fluidity of the material. Detailed Implementation
[0034] The present invention will be further illustrated below with specific embodiments. These embodiments are merely illustrative and do not limit the scope of the invention.
[0035] I. The main raw material sources in the embodiments and comparative examples of this invention are as follows:
[0036] PBAT resin: Wanhua Chemical;
[0037] PLA resin: Zhejiang Hisun;
[0038] Boron nitride: Shandong Jinyao Advanced Materials Co., Ltd.;
[0039] Silica: Shandong Xinhua Silica Co., Ltd.;
[0040] Erucamide: Paswell Biotechnology (Shanghai) Co., Ltd.;
[0041] Octopic sulfide: Beijing Innocare;
[0042] All other raw materials are commercially available products.
[0043] II. The main testing methods used in the embodiments and comparative examples of this invention are as follows:
[0044] Interlayer bonding strength: The interlayer bonding strength of the printed specimen is tested using a universal material testing machine Instron 5966 in accordance with the national standard GB / T 1040.3-2006, with a gauge length of 100 mm, a tensile speed of 50 mm / min, a sample thickness of 4 mm, a width of 15 mm, a length of 150 mm, a test temperature of 23°C, and a humidity of 50%.
[0045] Notched Izod impact strength: The notched impact strength of the printed specimen is tested using a ZwickRoell HIT impact tester in accordance with the national standard GB / T 1843-2008, with a sample thickness of 4 mm, a width of 10 mm, a length of 80 mm, a test temperature of 23°C, and a humidity of 50%.
[0046] Printing speed: The printing temperature is 220°C, the build plate temperature is 60°C, the printing speed increases in gradients of 50 mm / min, such as 200 / 250 / 300 / 350 mm / min, evaluated using a grid disk model, with an ambient temperature of 23°C and a humidity of 50%. A complete printed grid disk is judged as qualified, and the printing speed is continuously increased until the grid disk cannot be printed completely at that speed, and the previous speed is defined as the maximum printing speed.
[0047] Anti-stringing performance: The printing temperature is 220°C, the build plate temperature is 60°C, the printing speed is 200 mm / min, evaluated using an antenna model, with an ambient temperature of 23°C and a humidity of 50%. The evaluation criteria are: the filament is placed for different days, and printing is carried out every day. If filaments appear between the antennas of the printed antenna model, it is judged as stringing; if there is no any stray filament between the antennas, it is judged as qualified, and the number of days of printing without stringing is counted as the anti-stringing time.
[0048] III. Information on the main equipment used in the examples and comparative examples of the present invention is as follows:
[0049] Twin-screw extruder: screw diameter 32 mm, length-to-diameter ratio 52, Coperion, ZSK MvPLUS;
[0050] Single-screw extruder: length-to-diameter ratio 30, Fude, FLD-35A;
[0051] High-speed mixer: Suzhou Kennith, HT-10L;
[0052] Low-speed mixer: Qingdao Chaojie, SHL-200A;
[0053] 3D printer: Bambu Lab A1.
[0054] Example 1
[0055] Weigh 97.9 kg of boron nitride (D50 particle size of 30 μm and aspect ratio of 40), 2 kg of 4-carboxy-2-pyrrolidone, and 0.1 kg of stannous octoate. Stir the mixture at 800 rpm for 5 min at room temperature using a high-speed mixer. Then heat the mixture to 150 °C and stir at 1200 rpm for 15 min. Dry the mixture at 100 °C for 2 h to obtain pyrrolidone-coated boron nitride powder A.
[0056] Weigh out 10 kg of pyrrolidone-coated boron nitride powder A and 5 kg of silica (D50 particle size 3 μm, porosity 0.9 cm). 3 0.3 kg of erucamide and 76.7 kg of PLA resin (weight-average molecular weight 200,000, acid value 25 mol / t) and 8 kg of PBAT resin (weight-average molecular weight 120,000, acid value 15 mol / t) were weighed and mixed using a low-frequency mixer at 20 rpm. The mixture was then fed into the main feed port of the twin-screw extruder. The twin-screw extruder has 14 heating zones. Zones 1-6 are set to temperatures of 180℃, 180℃, 180℃, 190℃, 190℃, 190℃; zones 7-10 are set to temperatures of 200℃, 200℃, 200℃, 200℃; and zones 11-14 are set to temperatures of 190℃, 190℃, 190℃, 190℃. The side feed port is located in zone 6, and the screw speed is set to 500 rpm. After extrusion by a twin-screw extruder, the material is cooled by water and granulated to obtain modified PLA material.
[0057] The aforementioned modified PLA material was extruded using a single-screw extruder to produce high-speed FDM printed PLA filaments. Specifically, the single-screw extruder has 5 zones with temperature settings of 180℃, 200℃, 200℃, 200℃, and 190℃, and a capacity setting of 20kg / h; the cooling water temperature is set to 65℃.
[0058] Example 2
[0059] Weigh 98.95 kg of boron nitride (D50 particle size of 40 μm and aspect ratio of 55), 1 kg of 4-carboxy-2-pyrrolidone, and 0.05 kg of stannous octoate. Stir the mixture at 1200 rpm for 3 min at room temperature using a high-speed mixer. Then heat the mixture to 140 °C and stir at 1000 rpm for 10 min. Dry the mixture at 100 °C for 2 h to obtain pyrrolidone-coated boron nitride powder B.
[0060] Weigh out 20 kg of the above-mentioned pyrrolidone-coated boron nitride powder B and 1 kg of silica (D50 particle size 4 μm, porosity 1.0 cm). 30.5 kg of erucamide (weight average molecular weight 150,000, acid value 10 mol / t) and 3 kg of PBAT resin (weight average molecular weight 150,000, acid value 30 mol / t) were weighed and mixed using a low-frequency mixer at a speed of 20 rpm. This mixture was then fed into the main feeder of the twin-screw extruder. The twin-screw extruder has 14 heating zones. Zones 1-6 are set to temperatures of 180℃, 180℃, 180℃, 190℃, 190℃, 190℃; zones 7-10 are set to temperatures of 200℃, 200℃, 200℃, 200℃; and zones 11-14 are set to temperatures of 190℃, 190℃, 190℃, 190℃. The side feeder is located in zone 6, and the screw speed is set to 500 rpm. After extrusion by a twin-screw extruder, the material is cooled by water and granulated to obtain modified PLA material.
[0061] The aforementioned modified PLA material was extruded using a single-screw extruder to produce high-speed FDM printed PLA filaments. Specifically, the single-screw extruder has 5 zones with temperature settings of 180℃, 200℃, 200℃, 200℃, and 190℃, and a capacity setting of 20kg / h; the cooling water temperature is set to 65℃.
[0062] Example 3
[0063] Weigh 94.995 kg of boron nitride (D50 particle size of 30 μm and aspect ratio of 30), 5 kg of 4-carboxy-2-pyrrolidone, and 0.05 kg of stannous octoate. Stir the mixture at 800 rpm for 4 min at room temperature using a high-speed mixer. Then heat the mixture to 140 °C and stir at 800 rpm for 13 min. Dry the mixture at 100 °C for 2 h to obtain pyrrolidone-coated boron nitride powder C.
[0064] Weigh out 8 kg of the above-mentioned pyrrolidone-coated boron nitride powder C and 5 kg of silica (D50 particle size 3 μm, porosity 0.9 cm). 30.4 kg of erucamide (weight average molecular weight 250,000, acid value 30 mol / t) and 3 kg of PBAT resin (weight average molecular weight 150,000, acid value 15 mol / t) were weighed and mixed using a low-frequency mixer at a speed of 20 rpm. These were then fed into the main feeder of the twin-screw extruder. The twin-screw extruder has 14 heating zones. Zones 1-6 are set to temperatures of 180℃, 180℃, 180℃, 190℃, 190℃, 190℃; zones 7-10 are set to temperatures of 200℃, 200℃, 200℃, 200℃; and zones 11-14 are set to temperatures of 190℃, 190℃, 190℃, 190℃. The side feeder is located in zone 6, and the screw speed is set to 500 rpm. After extrusion by a twin-screw extruder, the material is cooled by water and granulated to obtain modified PLA material.
[0065] The aforementioned modified PLA material was produced by single-screw extrusion molding to obtain high-speed FDM printed PLA filaments. Specifically, the single-screw extruder has 5 zones with temperature settings of 180℃, 200℃, 200℃, 200℃, and 190℃, and a capacity setting of 20kg / h; the cooling water temperature is set to 65℃.
[0066] Comparative Example 1
[0067] Referring to the method in Example 1, the difference is that the added boron nitride is replaced with ordinary boron nitride (without pyrrolidone coating) to obtain PLA modified material, which is then extruded into PLA wire.
[0068] Comparative Example 2
[0069] Referring to the method in Example 1, the difference is that the added pyrrolidone-coated boron nitride powder A is replaced with alkylated hexagonal boron nitride powder to obtain PLA modified material, which is then extruded into PLA wire.
[0070] The alkylated hexagonal boron nitride powder was prepared according to CN109608771A, and the specific steps are as follows:
[0071] Weigh 50 kg of hydrogen peroxide and 50 kg of concentrated sulfuric acid and mix them for later use. Weigh 9 kg of boron nitride (D50 particle size of 40 μm and aspect ratio of 55) and stir it with 91 kg of the above mixed solution for 1 h. Wash and filter the treated hexagonal boron nitride and dry it at 80 °C for 2 h. Weigh 5 kg of the dried hexagonal boron nitride and ultrasonically disperse it in 100 kg of N,N-dimethylformamide solvent. Stir it at 60 °C for 3 min under nitrogen atmosphere. Weigh 0.5 kg of aluminate coupling agent and add it to the solvent. Continue stirring for 24 h, filter, wash and dry to prepare alkylated hexagonal boron nitride powder.
[0072] Comparative Example 3
[0073] Referring to the method in Example 1, the difference is that boron nitride is replaced with talc, that is, talc coated with pyrrolidone. The original talc powder has a D50 particle size of 30 mm and an aspect ratio of 30. Other operations and conditions remain unchanged to obtain PLA modified material, which is then extruded into PLA wire.
[0074] The performance test results of the materials obtained in each embodiment and comparative example are shown in Table 1.
[0075] Table 1. Test results of material printing performance in each embodiment and comparative example.
[0076]
[0077] PLA filaments typically have a printing speed of only 200 mm / min, and the maximum fiber tearing time is around 2-3 days. Example 1 uses boron carbide with appropriate particle size and aspect ratio to construct an efficient thermally conductive network, rapidly improving the heat transfer and melting efficiency of the PLA melt, thus increasing printing speed and fiber tearing resistance. The use of silica with appropriate particle size improves filler dispersion and significantly optimizes lamination strength. Comparative Example 1 replaces uncoated boron nitride. Due to the high internal friction of the virgin boron nitride powder directly dispersed in the melt, the melt is unstable during high-speed extrusion, easily resulting in output fluctuations. Therefore, it has the worst printing fiber tearing performance, insufficient resin compatibility, numerous melt defects, significantly reduced printing lamination strength, and thermal conductivity is also affected by defects, resulting in insufficient printing speed. Comparative Example 2 uses alkylated coated boron carbide. Due to insufficient dispersion, severe agglomeration occurs in the system, failing to establish an efficient thermally conductive network and significantly reducing lamination strength. Comparative Example 3 uses talc as a substitute, significantly reducing thermal conductivity, failing to improve lamination strength, and losing high-speed printing characteristics.
[0078] In summary, this solution effectively addresses the problems of severe agglomeration, poor compatibility, high cost, and numerous molding defects inherent in existing single-filler modification and nanofiller modification technologies. The formulation of this invention is rationally designed, and the preparation process is simple and controllable. It can be directly adapted to existing FDM consumable production lines for mass production, exhibits strong compatibility with mainstream FDM printing equipment, and can meet the ultra-high-speed 3D printing needs of different scenarios in consumer and industrial applications. It has a wide range of applications and significant economic benefits and industrialization potential.
Claims
1. A PLA-modified material, characterized in that, Raw materials comprising the following parts by weight: 65-85 parts of PLA resin, preferably 70-81 parts; 3 to 10 parts of PBAT resin, preferably 5 to 8 parts; 5-20 parts of boron nitride coated with pyrrolidone, preferably 8-15 parts; 1-10 parts of silicon dioxide, preferably 3-6 parts; Lubricant: 0.1 to 0.5 parts, preferably 0.2 to 0.4 parts.
2. The modified material according to claim 1, characterized in that, The PLA resin has a weight-average molecular weight of 150,000 to 250,000 and an acid value of 10 to 40 mol / t; preferably, the molecular weight is 180,000 to 210,000 and the acid value is 20 to 30 mol / t. And / or, the weight-average molecular weight of the PBAT resin is 100,000 to 150,000, and the acid value is 10 to 40 mol / t, preferably 120,000 to 130,000, and the acid value is 10 to 20 mol / t.
3. The modified material according to claim 1 or 2, characterized in that, The pyrrolidone-coated boron nitride is obtained by melt blending carboxypyrrolidone with grafted boron nitride. Preferably, the boron nitride is hexagonal boron nitride with a D50 particle size of 10~70 μm and an aspect ratio of 20~80, and more preferably a D50 particle size of 30~40 μm and an aspect ratio of 30~55; Preferably, the carboxypyrrolidone includes at least one of 4-carboxy-2-pyrrolidone and 5-carboxy-2-pyrrolidone.
4. The modified material according to claim 3, characterized in that, The method for preparing the pyrrolidone-coated boron nitride includes the following steps: Carboxypyrrolidone, catalyst and boron nitride are mixed at room temperature, heated to 140-150°C, stirred at 800-1200 rpm for 10-15 min, and dried to obtain pyrrolidone-coated boron nitride; Preferably, the catalyst comprises at least one of stannous octoate, dibutyltin dilaurate, tin lactate, and stannous isooctanoate; Preferably, the mass ratio of boron nitride, carboxypyrrolidone, and catalyst is 5-10:0.1-5:0.001-0.05, and more preferably, the mass ratio is 8-10:0.2-0.5:0.005-0.
01.
5. The modified material according to claim 1 or 2, characterized in that, The silica is precipitated silica with a D50 particle size of 2-10 μm and a porosity of 0.4-1.5 cm⁻¹. 3 / g; preferably, the D50 particle size is 3~4µm, and the porosity is 0.8~1.0cm³. 3 / g.
6. The modified material according to claim 1 or 2, characterized in that, The lubricant is an amide lubricant, preferably including one or more of erucamide, oleamide, and behenamide.
7. A method for preparing the PLA modified material according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: After mixing pyrrolidone-coated boron nitride, silica, and lubricant, the mixture is fed into a twin-screw extruder through a side feed port. After mixing PLA resin and PBAT resin, the mixture is fed into a twin-screw extruder through a main feed port. After extrusion, the mixture is water-cooled and granulated to obtain PLA modified material.
8. The method for preparing PLA modified material according to claim 7, characterized in that, The temperature of the twin-screw extruder is 180-200℃, and the screw speed is 300-500rpm.
9. An FDM-printed PLA filament, characterized in that, The FDM-printed PLA filament is prepared from the PLA modified material according to any one of claims 1-6 or the PLA modified material prepared by the preparation method according to claim 7 or 8; preferably, the PLA modified material is fed into a single screw extruder, traction extruded, and water-cooled to form the PLA filament.
10. The FDM printing PLA filament according to claim 9, wherein the FDM printing PLA filament has a printing speed ≥ 500 mm / min, a bonding strength > 30 MPa, and a tensile strength ≥ 4 days.
Citation Information
Patent Citations
Impact-resistant and anti-ageing PLA composite material for 3D printing and preparation method thereof
CN108285623A
Polypropylene modified material with flame retardancy, thermal conductivity and high dielectric constant and preparation method thereof
CN109608771A
Modified PLA material for 3D printing and preparation method thereof
CN119570219A