A low-temperature ultra-tough modified polyamide composite material and its preparation method
By using a partitioned side-feed reactive extrusion technique with self-made interface agent and modified masterbatch, a low-temperature ultra-tough modified polyamide composite material was prepared, which solved the problems of brittleness and water absorption of polyamide at low temperatures and achieved the effect of high toughness and low water absorption.
Patent Information
- Application Number
- CN202611335104.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyamide materials become more brittle and less impact-resistant at low temperatures, and have high water absorption, resulting in a shortened service life. Existing modified systems have weak interfacial bonding, making it difficult to improve both low-temperature toughness and water absorption at the same time.
Using self-made interface agents and modified masterbatches, low-temperature ultra-tough modified polyamide composites were prepared by using partitioned side-feed reactive extrusion technology combined with low-temperature catalytic hydrothermal treatment. Aromatic disulfide bonds and microgel networks were used to improve the interfacial bonding strength and hydrophobicity, and to inhibit water molecule penetration.
Maintaining high toughness and reducing water absorption at low temperatures, the material achieves low-temperature ultra-toughness and low water absorption by breaking interfacial aromatic disulfide bonds and forming a microgel network, thus extending its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, specifically to a low-temperature ultra-tough modified polyamide composite material and its preparation method. Background Technology
[0002] Polyamides possess excellent mechanical strength, wear resistance, and chemical stability, making them widely used in automotive parts, construction machinery, and cryogenic pipes. However, pure polyamides have significant drawbacks. At low temperatures, the molecular chain mobility weakens, leading to a significant increase in brittleness and a substantial decrease in impact toughness, making them unsuitable for low-temperature operating conditions in cold regions. Furthermore, polyamide molecules contain numerous polar amide groups, resulting in high water absorption. Water molecules easily penetrate the matrix and diffuse along the two-phase interface, causing dimensional deformation and mechanical property degradation, severely limiting service life. Currently, the industry often uses elastomer blending for toughening modification. However, conventional modification systems exhibit weak interfacial bonding, easily leading to interfacial debonding failure at low temperatures, and cannot effectively improve the material's water absorption defects. Therefore, it is difficult to simultaneously achieve both low-temperature ultra-toughness and low water absorption. Thus, novel modification solutions are urgently needed to address the technical challenges of low-temperature brittleness and high water absorption in polyamides. Summary of the Invention
[0003] The purpose of this invention is to provide a low-temperature ultra-tough modified polyamide composite material and its preparation method, so as to solve the problems existing in the prior art.
[0004] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing a low-temperature ultra-tough modified polyamide composite material, comprising the following steps: (1) 4,4'-dithiodibenzoic acid, thionyl chloride, organic solvent and anhydrous DMF are mixed in a mass ratio of 2~4:3~6:15:0.01, stirred and refluxed at 40~45℃ for 6h, and distilled under reduced pressure to obtain an intermediate. The intermediate is mixed with an organic solvent in a mass ratio of 3.3~3.5:15 and the mixture is placed in an ice bath to obtain a reaction solution. 1.2~1.4 times the mass of the intermediate polyetheramine is mixed with an organic solvent and triethylamine in a mass ratio of 1:3:0.25 and placed in an ice bath to obtain a polyetheramine solution. The solution is added dropwise to the reaction solution, stirred at room temperature for 12h, and then post-treated and dried under vacuum at 60℃ for 24h to obtain a self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and initiator A are mixed in a mass ratio of 1~2:0.2~0.4:0.02 and stirred at 65~70℃ for 1~2h to obtain oligomeric silane; 90~110 parts by weight of elastomer, 1~3 parts by weight of oligomeric silane, 0.05 parts by weight of initiator B, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of auxiliary antioxidant are premixed, melt grafted, water cooled, air dried and granulated to obtain self-made modified masterbatch; 90~110 parts by weight of polyamide, 1~3 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 are premixed, melt extruded and granulated to obtain mixed masterbatch; (3) 650-700 parts by weight of polyamide, 0.5-1.5 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of auxiliary antioxidant and 0.3 parts by weight of release agent are added through the main feed. 10-20 parts by weight of self-made modified masterbatch, 3-5 parts by weight of self-made interface agent and 0.2 parts by weight of triphenyl phosphite are added to the side feed of different zones respectively. The modified polyamide composite material is obtained by melt extrusion, water cooling and shaping at 20-40℃, pelleting and drying.
[0005] Furthermore, the organic solvent in step (1) is anhydrous dichloromethane.
[0006] Furthermore, the polyetheramine mentioned in step (1) is polyetheramine ED900.
[0007] Furthermore, the initiator A in step (2) is azobisisobutyronitrile.
[0008] Furthermore, the elastomer in step (2) is an ethylene-octene copolymer elastomer of model Engage8150.
[0009] Furthermore, the initiator B mentioned in step (2) is dicumyl peroxide.
[0010] Furthermore, the auxiliary antioxidant in step (2) is dilauryl thiodipropionate.
[0011] Furthermore, the polyamide mentioned in step (2) is: polyamide with the model number Baling Petrochemical YH800.
[0012] Furthermore, the release agent in step (3) is ethylene bis-stearamide.
[0013] Furthermore, in the application of a low-temperature ultra-tough modified polyamide composite material, the low-temperature ultra-tough modified polyamide composite material is dried at 80℃ for 4 hours by forced air, and then injection molded. The sample is prepared under the following conditions: nozzle temperature 240℃, mold temperature 85℃, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample is first cooled at room temperature for 30 minutes, and then placed in an 80℃ deionized water bath for 45 minutes. After treatment, the sample is removed, the surface moisture is wiped off, and then dried at 80℃ for 4 hours to obtain the low-temperature ultra-tough modified polyamide composite material specimen.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are: This invention achieves excellent low-temperature toughness and water resistance by using a self-made interface agent, a self-made modified masterbatch, polyamide and additives through a partitioned side-feed reaction extrusion and a low-temperature catalytic hydrothermal post-treatment.
[0015] This invention first prepares a self-made interface agent by condensing diacyl chloride with polyetheramine. Then, 3-mercaptopropyltrimethoxysilane and trimethylolpropane triacrylate are pre-reacted and melt-grafted onto ethylene-octene copolymer elastomer to obtain a self-made modified masterbatch. This masterbatch, along with mixed masterbatch, polyamide, triphenyl phosphite, and composite antioxidant, is then subjected to a side-feed reaction extrusion process to obtain a low-temperature ultra-tough modified polyamide composite material. At low temperatures, the ethylene-octene copolymer elastomer maintains high elasticity. Upon impact, cavitation occurs within the particles, absorbing energy, and the interfacial aromatic disulfide bonds break as sacrificial bonds, dissipating stress at the crack tip and preventing interfacial delamination. The siloxane microgel inside the elastomer stabilizes the particle morphology, preventing excessive fragmentation, promoting stress transfer to the matrix, and inducing large-area shear yielding. These three factors work together to achieve low-temperature ultra-toughness. The microgel cross-linking network inside the elastomer particles reduces the free volume of the elastomer phase, inhibits water molecule penetration, and the interfacial disulfide bond layer enhances the bonding between the elastomer and the polyamide matrix, eliminating interfacial voids and defects, cutting off the rapid diffusion path of water molecules along the interfacial capillary channels. At the same time, the hydrophobic elastomer particles are uniformly dispersed to form a barrier phase, extending the water molecule diffusion path, thereby significantly reducing the overall water absorption rate of the composite material. Detailed Implementation
[0016] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0017] To more clearly illustrate the method provided by the present invention, the following examples are provided. The test methods for various properties of the modified polyamide composite materials prepared in the following examples are as follows: Low-temperature super-toughness test: The test was conducted in accordance with GB / T1043.1-2021 "Determination of impact properties of simply supported beams of plastics - Part 1: Non-instrumental impact test". The specimens prepared in Examples 1-5 and Comparative Examples 1-6 were made into standard strips of 80mm×10mm×4mm with a type A notch and a residual thickness of 8.0mm. Before the test, the strips were placed in a low-temperature test chamber and kept at a constant temperature of -40℃ for no less than 30 minutes to ensure that the core temperature of the strips reached the test temperature. The simply supported beam notched impact test was completed within 10 seconds after the strips were removed. There were no less than 5 specimens in each group. Abnormal discrete data were discarded and the arithmetic mean was taken as the notched impact strength of the simply supported beam at -40℃.
[0018] Water absorption rate test: Performed according to GB / T1034-2008 "Determination of water absorption of plastics". The specimens prepared in Examples 1-5 and Comparative Examples 1-6 were made into φ50mm×4mm round samples. The samples were first dried in a 50℃ forced-air drying oven to constant weight, cooled to room temperature and weighed to obtain the dry mass m0. Then the samples were completely immersed in 23℃ deionized water for 24h. After taking them out, the free water on the surface of the samples was quickly wiped off with dust-free filter paper and the mass after water absorption was immediately weighed to obtain the mass m1. Water absorption rate calculation formula: Water absorption rate (%) = [(m1-m0) / m0]×100%; There were no less than 3 parallel samples in each group, and the arithmetic mean was taken. Example 1
[0019] (1) 4,4'-dithiodibenzoic acid, thionyl chloride, anhydrous dichloromethane, and anhydrous N,N-dimethylformamide were mixed in a mass ratio of 2:3:15:0.01 and stirred under reflux at 40°C and 300 rpm for 6 h. After the reaction was completed, excess thionyl chloride and solvent were removed by vacuum distillation at -0.08 MPa and 50°C to obtain a diacyl chloride intermediate. The diacyl chloride intermediate was mixed with anhydrous dichloromethane in a mass ratio of 3.3:15 and cooled in an ice bath at 0°C and 200 rpm to obtain a reaction solution. 1.2 times the mass of the diacyl chloride intermediate, polyetheramine ED900, was mixed with anhydrous dichloromethane and triethylamine in a mass ratio of 1:3:15:0.01. The mixture was prepared by mixing 3:0.25 and cooling in an ice bath at 0°C and 200 rpm for 10 min to obtain a polyetheramine solution. The polyetheramine solution was slowly added dropwise to the reaction solution with stirring in an ice bath over 1 h. After the addition was complete, the ice bath was removed and stirring was continued at room temperature for 12 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration. The filtrate was concentrated to four-fifths of its original volume by rotary evaporation. It was then slowly poured into five times the volume of deionized water and stirred for 2 h to completely hydrolyze the terminal acyl chloride to a carboxyl group. The precipitate was collected by filtration, washed three times with deionized water, and then washed with a small amount of diethyl ether. The precipitate was dried at 60°C and vacuum -0.09 MPa for 24 h to obtain the self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and azobisisobutyronitrile were mixed in a mass ratio of 1:0.2:0.02 and stirred at 200 rpm for 1 h at 65 °C to obtain oligomeric silane; 90-110 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 1-3 parts by weight of oligomeric silane, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate were added. Premixed at 500 rpm for 5 min, the mixture was melt-grafted using a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, and the sixth zone was subjected to vacuum devolatilization at -0.08 MPa with a residence time of 60 s under nitrogen protection throughout the process. The extruded strips were water-cooled, air-dried, pelletized, and immediately vacuum-sealed and stored in a low-temperature, light-protected place to obtain the self-made modified masterbatch. (3) 90 parts by weight of polyamide of Baling Petrochemical YH800, 1 part by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 were premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch; (4) 650 parts by weight of polyamide, 0.5 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, and 0.3 parts by weight of ethylene bis-stearamide were fed into a twin-screw extruder via the main feed; 10 parts by weight of self-made modified masterbatch were fed into the fifth zone side feed; 3 parts by weight of a premix of self-made interface agent and 0.2 parts by weight of triphenyl phosphite were fed into the seventh zone side feed; the extruder length-to-diameter ratio was 40:1, and the temperatures of each section were set as follows: Zone 1: 230℃, Zone 2: 235℃, Zone 3: 240℃, Zone 4: 240℃, and Zone 5: 230℃. Zone 5: 245℃, Zone 6: 245℃, Zone 7: 240℃, Zone 8: 240℃, Die head: 235℃, Screw speed: 250rpm, Feed rate: 8kg / h, Vacuum devolatilization in Zones 6 and 8: -0.09MPa, Residence time: 90s, Nitrogen protection throughout; During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent undergo an amidation reaction promoted by triphenyl phosphite, which enables the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortens the thermal history of the self-made interface agent and reduces the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibit the premature hydrolysis of silane during the extrusion stage. (5) The melt is extruded from the die head in strip form, and immediately cooled and shaped by passing through a 20°C circulating water bath. After the surface moisture is dried by an air dryer, it is cut into cylindrical particles with a diameter of 3 mm and a length of 3 mm by a pelletizer. Then, it is screened by a vibrating screen to remove excessively fine powder and adhering particles. The resulting composite material particles are dried at 80°C for 4 hours until the moisture content is below 0.1%. Finally, they are sealed and packaged and stored in a desiccator to obtain a low-temperature ultra-tough modified polyamide composite material. (6) After drying the low-temperature super-tough modified polyamide composite material at 80°C for 4 hours, a sample was prepared using an injection molding machine under the following conditions: nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was cooled at room temperature for 30 minutes and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate was used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel was formed in situ inside the elastomer particles. After the treatment, the sample was taken out, the surface moisture was wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen. Example 2
[0020] (1) 4,4'-dithiodibenzoic acid, thionyl chloride, anhydrous dichloromethane and anhydrous N,N-dimethylformamide were mixed in a mass ratio of 2.5:3.5:15:0.01 and stirred under reflux at 41°C and 300 rpm for 6 h. After the reaction was completed, excess thionyl chloride and solvent were removed by vacuum distillation at -0.08 MPa and 50°C to obtain a diacyl chloride intermediate. The diacyl chloride intermediate was mixed with anhydrous dichloromethane in a mass ratio of 3.35:15 and cooled in an ice bath at 0°C and 200 rpm to obtain a reaction solution. 1.25 times the mass of the diacyl chloride intermediate was mixed with anhydrous dichloromethane and triethylamine in a mass ratio of 1.25:15:0.01. The mixture was prepared by mixing in a ratio of 1:3:0.25 and cooling in an ice bath at 0°C and 200 rpm for 10 min to obtain a polyetheramine solution. The polyetheramine solution was slowly added dropwise to the reaction solution with stirring in an ice bath over a period of 1 h. After the addition was complete, the ice bath was removed and stirring was continued at room temperature for 12 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration. The filtrate was concentrated to four-fifths of its original volume by rotary evaporation and slowly poured into five times the volume of deionized water. The mixture was stirred for 2 h to completely hydrolyze the terminal acyl chloride to a carboxyl group. The precipitate was collected by filtration, washed three times with deionized water, and then washed with a small amount of diethyl ether. The precipitate was dried at 60°C and vacuum -0.09 MPa for 24 h to obtain the self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and azobisisobutyronitrile were mixed in a mass ratio of 1.2:0.25:0.02 and stirred at 66°C and 200 rpm for 1.2 h to obtain oligomeric silane; 95 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 1.5 parts by weight of oligomeric silane, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate were mixed. The ester was premixed at 500 rpm for 5 min, then melt-grafted using a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, the sixth zone was vacuum devolatilization at -0.08 MPa, the residence time was 60 s, and nitrogen protection was maintained throughout the process. The extruded strips were water-cooled, air-dried, pelletized, and immediately vacuum-sealed and stored in a low-temperature, light-protected place to obtain the self-made modified masterbatch. (3) 95 parts by weight of polyamide of Baling Petrochemical YH800, 1.5 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 were premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch; (4) 660 parts by weight of polyamide, 0.8 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, and 0.3 parts by weight of ethylene bis-stearamide were fed into a twin-screw extruder via the main feed; 12 parts by weight of self-made modified masterbatch were fed into the fifth zone side feed; and 3.5 parts by weight of a premix of self-made interface agent and 0.2 parts by weight of triphenyl phosphite were fed into the seventh zone side feed; the length-to-diameter ratio of the extruder was 40:1, and the temperatures of each section were set as follows: Zone 1: 230℃, Zone 2: 235℃, Zone 3: 240℃, Zone 4: 240℃. The temperature was set at 245℃ in zone 5, 245℃ in zone 6, 240℃ in zone 7, 240℃ in zone 8, and 235℃ at the die head. The screw speed was 250 rpm, and the feed rate was 8 kg / h. Vacuum devolatilization was performed in zones 6 and 8 at -0.09 MPa, with a residence time of 98 s. Nitrogen protection was maintained throughout the process. During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent underwent an amidation reaction promoted by triphenyl phosphite. This allowed the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortened the thermal history of the self-made interface agent and reduced the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibited the premature hydrolysis of silanes during the extrusion stage. (5) The melt is extruded from the die head in strip form, and immediately cooled and shaped by a 25°C circulating water bath. After the surface moisture is dried by an air dryer, it is cut into cylindrical particles with a diameter of 3 mm and a length of 3.2 mm by a pelletizer. Then, the excessively fine powder and adhering particles are removed by a vibrating screen. The resulting composite material particles are dried at 80°C for 4 hours until the moisture content is below 0.1%. Finally, they are sealed and packaged and stored in a desiccator to obtain a low-temperature super-tough modified polyamide composite material. (6) After drying the low-temperature super-tough modified polyamide composite material at 80°C for 4 hours, a sample was prepared using an injection molding machine under the following conditions: nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was cooled at room temperature for 30 minutes and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate was used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel was formed in situ inside the elastomer particles. After the treatment, the sample was taken out, the surface moisture was wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen. Example 3
[0021] (1) 4,4'-dithiodibenzoic acid, thionyl chloride, anhydrous dichloromethane and anhydrous N,N-dimethylformamide were mixed in a mass ratio of 3:4.5:15:0.01 and stirred under reflux at 42°C and 300 rpm for 6 h. After the reaction was completed, excess thionyl chloride and solvent were removed by vacuum distillation at -0.08 MPa and 50°C to obtain a diacyl chloride intermediate. The diacyl chloride intermediate was mixed with anhydrous dichloromethane in a mass ratio of 3.4:15 and cooled in an ice bath at 0°C and 200 rpm to obtain a reaction solution. 1.3 times the mass of the diacyl chloride intermediate was mixed with anhydrous dichloromethane and triethylamine in a mass ratio of 3:4.5:15 to obtain a reaction solution. The mixture was prepared by mixing in a 1:3:0.25 ratio and cooling in an ice bath at 0°C and 200 rpm for 10 min to obtain a polyetheramine solution. The polyetheramine solution was slowly added dropwise to the reaction solution with stirring in an ice bath over 1 h. After the addition was complete, the ice bath was removed and stirring was continued at room temperature for 12 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration. The filtrate was concentrated to four-fifths of its original volume by rotary evaporation and slowly poured into five times the volume of deionized water. The mixture was stirred for 2 h to completely hydrolyze the terminal acyl chloride to a carboxyl group. The precipitate was collected by filtration, washed three times with deionized water, and then washed with a small amount of diethyl ether. The precipitate was dried at 60°C and vacuum -0.09 MPa for 24 h to obtain the self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and azobisisobutyronitrile were mixed in a mass ratio of 1.5:0.3:0.02 and stirred at 200 rpm for 1.5 h at 67 °C to obtain oligomeric silane; 100 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 2 parts by weight of oligomeric silane, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate were mixed. Premixed at 500 rpm for 5 min, the mixture was melt-grafted using a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, and the sixth zone was subjected to vacuum devolatilization at -0.08 MPa with a residence time of 60 s under nitrogen protection throughout the process. The extruded strips were water-cooled, air-dried, pelletized, and immediately vacuum-sealed and stored in a low-temperature, light-protected place to obtain the self-made modified masterbatch. (3) 100 parts by weight of polyamide of Baling Petrochemical YH800, 2 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 were premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch; (4) 675 parts by weight of polyamide, 1 part by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, and 0.3 parts by weight of ethylene bis-stearamide were fed into a twin-screw extruder via the main feed; 15 parts by weight of self-made modified masterbatch were fed into the 5th zone side feed; 4 parts by weight of a premix of self-made interface agent and 0.2 parts by weight of triphenyl phosphite were fed into the 7th zone side feed; the length-to-diameter ratio of the extruder was 40:1, and the temperature of each section was set as follows: 230℃ in zone 1, 235℃ in zone 2, 240℃ in zone 3, 240℃ in zone 4, and 235℃ in zone 5. 245℃, Zone 6 245℃, Zone 7 240℃, Zone 8 240℃, Die head 235℃, Screw speed 250rpm, Feed rate 8kg / h, Vacuum devolatilization in Zones 6 and 8 at -0.09MPa, Residence time 105s, Nitrogen protection throughout; During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent undergo an amidation reaction promoted by triphenyl phosphite, which enables the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortens the thermal history of the self-made interface agent and reduces the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibit the premature hydrolysis of silane during the extrusion stage. (5) The melt is extruded from the die head in strip form and immediately cooled and shaped by a 30°C circulating water bath. After the surface moisture is dried by an air dryer, it is cut into cylindrical particles with a diameter of 3 mm and a length of 3.5 mm by a pelletizer. Then, the excessively fine powder and adhering particles are removed by a vibrating screen. The resulting composite material particles are dried at 80°C for 4 hours until the moisture content is below 0.1%. Finally, they are sealed and packaged and stored in a desiccator to obtain a low-temperature super-tough modified polyamide composite material. (6) After drying the low-temperature super-tough modified polyamide composite material at 80°C for 4 hours, a sample was prepared using an injection molding machine under the following conditions: nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was cooled at room temperature for 30 minutes and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate was used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel was formed in situ inside the elastomer particles. After the treatment, the sample was taken out, the surface moisture was wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen. Example 4
[0022] (1) 4,4'-dithiodibenzoic acid, thionyl chloride, anhydrous dichloromethane and anhydrous N,N-dimethylformamide were mixed in a mass ratio of 3.5:5:15:0.01 and stirred under reflux at 44°C and 300 rpm for 6 h. After the reaction was completed, excess thionyl chloride and solvent were removed by vacuum distillation at -0.08 MPa and 50°C to obtain a diacyl chloride intermediate. The diacyl chloride intermediate was mixed with anhydrous dichloromethane in a mass ratio of 3.45:15 and cooled in an ice bath at 0°C and 200 rpm to obtain a reaction solution. 1.35 times the mass of the diacyl chloride intermediate was mixed with anhydrous dichloromethane and triethylamine in a mass ratio of 3.5:5:15:0.01. A polyetheramine solution was obtained by mixing a mixture in a ratio of 1:3:0.25 and cooling it in an ice bath at 0°C and 200 rpm for 10 min. The polyetheramine solution was then slowly added dropwise to the reaction solution with stirring in an ice bath over a period of 1 h. After the addition was complete, the ice bath was removed and stirring was continued at room temperature for 12 h. After the reaction was complete, the triethylamine hydrochloride was removed by filtration. The filtrate was concentrated to four-fifths of its original volume by rotary evaporation and then slowly poured into five times the volume of deionized water. The mixture was stirred for 2 h to completely hydrolyze the terminal acyl chloride to a carboxyl group. The precipitate was collected by filtration, washed three times with deionized water, and then washed with a small amount of diethyl ether. The precipitate was dried at 60°C and a vacuum of -0.09 MPa for 24 h to obtain the self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and azobisisobutyronitrile were mixed in a mass ratio of 1.8:0.35:0.02 and stirred at 200 rpm for 1.8 h at 69 °C to obtain oligomeric silane; 105 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 2.5 parts by weight of oligomeric silane, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate were mixed. The ester was premixed at 500 rpm for 5 min, then melt-grafted using a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, the sixth zone was vacuum devolatilization at -0.08 MPa, the residence time was 60 s, and nitrogen protection was maintained throughout the process. The extruded strips were water-cooled, air-dried, pelletized, and immediately vacuum-sealed and stored in a low-temperature, light-protected place to obtain the self-made modified masterbatch. (3) 105 parts by weight of polyamide of Baling Petrochemical YH800, 2.5 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 were premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch; (4) 690 parts by weight of polyamide, 1.2 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, and 0.3 parts by weight of ethylene bis-stearamide were fed into a twin-screw extruder via the main feed; 18 parts by weight of self-made modified masterbatch were fed into the fifth zone side feed; 4.5 parts by weight of a premix of self-made interface agent and 0.2 parts by weight of triphenyl phosphite were fed into the seventh zone side feed; the extruder length-to-diameter ratio was 40:1, and the temperatures of each section were set as follows: Zone 1: 230℃, Zone 2: 235℃, Zone 3: 240℃, Zone 4: 240℃, and Zone 5: 230℃. Zone 5: 245℃, Zone 6: 245℃, Zone 7: 240℃, Zone 8: 240℃, Die head: 235℃, Screw speed: 250rpm, Feed rate: 8kg / h, Vacuum devolatilization in Zones 6 and 8: -0.09MPa, Residence time: 115s, Nitrogen protection throughout; During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent undergo an amidation reaction promoted by triphenyl phosphite, which enables the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortens the thermal history of the self-made interface agent and reduces the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibit the premature hydrolysis of silane during the extrusion stage. (5) The melt is extruded from the die head in strip form and immediately cooled and shaped by a 35°C circulating water bath. After the surface moisture is dried by an air dryer, it is cut into cylindrical particles with a diameter of 3 mm and a length of 3.8 mm by a pelletizer. Then, the excessively fine powder and adhering particles are removed by a vibrating screen. The resulting composite material particles are dried at 80°C for 4 hours until the moisture content is below 0.1%. Finally, they are sealed and packaged and stored in a desiccator to obtain a low-temperature super-tough modified polyamide composite material. (6) After drying the low-temperature super-tough modified polyamide composite material at 80°C for 4 hours, a sample was prepared using an injection molding machine under the following conditions: nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was cooled at room temperature for 30 minutes and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate was used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel was formed in situ inside the elastomer particles. After the treatment, the sample was taken out, the surface moisture was wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen. Example 5
[0023] (1) 4,4'-dithiodibenzoic acid, thionyl chloride, anhydrous dichloromethane, and anhydrous N,N-dimethylformamide were mixed in a mass ratio of 4:6:15:0.01 and stirred under reflux at 45°C and 300 rpm for 6 h. After the reaction was completed, excess thionyl chloride and solvent were removed by vacuum distillation at -0.08 MPa and 50°C to obtain a diacyl chloride intermediate. The diacyl chloride intermediate was mixed with anhydrous dichloromethane in a mass ratio of 3.5:15 and cooled in an ice bath at 0°C and 200 rpm to obtain a reaction solution. Polyetheramine ED900, at a mass ratio of 1.4 times that of the diacyl chloride intermediate, was mixed with anhydrous dichloromethane and triethylamine in a mass ratio of 1:6:15:0.01. The mixture was prepared by mixing 3:0.25 and cooling in an ice bath at 0°C and 200 rpm for 10 min to obtain a polyetheramine solution. The polyetheramine solution was slowly added dropwise to the reaction solution with stirring in an ice bath over 1 h. After the addition was complete, the ice bath was removed and stirring was continued at room temperature for 12 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration. The filtrate was concentrated to four-fifths of its original volume by rotary evaporation. It was then slowly poured into five times the volume of deionized water and stirred for 2 h to completely hydrolyze the terminal acyl chloride to a carboxyl group. The precipitate was collected by filtration, washed three times with deionized water, and then washed with a small amount of diethyl ether. The precipitate was dried at 60°C and vacuum -0.09 MPa for 24 h to obtain the self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and azobisisobutyronitrile were mixed in a mass ratio of 2:0.4:0.02 and stirred at 200 rpm for 2 h at 65~70℃ to obtain oligomeric silane; 110 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 3 parts by weight of oligomeric silane, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate were mixed in a nitrogen atmosphere. Premixed at 500 rpm for 5 min, the material was melt-grafted using a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, and the sixth zone was subjected to vacuum devolatilization at -0.08 MPa with a residence time of 60 s under nitrogen protection throughout the process. The extruded strips were water-cooled, air-dried, pelletized, and immediately vacuum-sealed and stored in a low-temperature, light-protected place to obtain the self-made modified masterbatch. (3) 110 parts by weight of polyamide of Baling Petrochemical YH800, 3 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 were premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch; (4) 700 parts by weight of polyamide, 1.5 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, and 0.3 parts by weight of ethylene bis-stearamide were fed into a twin-screw extruder via the main feed; 20 parts by weight of self-made modified masterbatch were fed into the fifth zone side feed; 5 parts by weight of a premix of self-made interface agent and 0.2 parts by weight of triphenyl phosphite were fed into the seventh zone side feed; the extruder length-to-diameter ratio was 40:1, and the temperatures of each section were set as follows: Zone 1: 230℃, Zone 2: 235℃, Zone 3: 240℃, Zone 4: 240℃, Zone 5: 235℃, Zone 6: 230℃, Zone 7: 230℃, Zone 8: 235℃, Zone 9: 230℃, Zone 1: 235℃, Zone 1: 230℃, Zone 2: 235℃, Zone 3: 230℃, Zone 4: 230℃, Zone 5 ...6: 230℃, Zone 7: 230℃, Zone 8: 235℃, Zone 9: 230℃, Zone 1: 230℃, Zone 1: 235℃, Zone 1: 230℃, Zone 1: 235℃, Zone 2: 235℃, Zone 1: 230℃, Zone 2: 235℃, Zone 245℃, Zone 6 245℃, Zone 7 240℃, Zone 8 240℃, Die head 235℃, Screw speed 250rpm, Feed rate 8kg / h, Vacuum devolatilization in Zones 6 and 8 at -0.09MPa, Residence time 120s, Nitrogen protection throughout; During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent undergo an amidation reaction promoted by triphenyl phosphite, which enables the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortens the thermal history of the self-made interface agent and reduces the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibit the premature hydrolysis of silane during the extrusion stage; (5) The melt is extruded from the die head in strip form and immediately cooled and shaped by a 40°C circulating water bath. After the surface moisture is dried by an air dryer, it is cut into cylindrical particles with a diameter of 3 mm and a length of 4 mm by a pelletizer. Then, it is removed by a vibrating screen to remove excessively fine powder and adhering particles. The resulting composite material particles are dried at 80°C for 4 hours until the moisture content is below 0.1%. Finally, they are sealed and packaged and stored in a desiccator to obtain a low-temperature super-tough modified polyamide composite material. (6) After drying the low-temperature super-tough modified polyamide composite material at 80°C for 4 hours, a sample was prepared using an injection molding machine under the following conditions: nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was cooled at room temperature for 30 minutes and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate was used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel was formed in situ inside the elastomer particles. After the treatment, the sample was taken out, the surface moisture was wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen.
[0024] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that step (1) is omitted and no self-made interface agent is added during the experiment; the remaining steps are the same as in Example 3.
[0025] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that step (1) is omitted, and the same amount of double-terminated carboxyl polyethylene glycol is used instead of the self-made interface agent for the experiment. The remaining steps are the same as in Example 3.
[0026] Comparative Example 3 The difference between Comparative Example 3 and Example 3 lies in step (2). Step (2) is changed to: 100 parts by weight of Engage8150 ethylene-octene copolymer elastomer, 0.05 parts by weight of dicumyl peroxide, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of dilauryl thiodipropionate are premixed at 500 rpm for 5 min, and then melt-grafted through a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1. The temperatures of each section were 150℃, 155℃, 160℃, 160℃, 165℃, 165℃, 160℃, and 155℃ at the die head. The screw speed was 180 rpm, the feed rate was 5 kg / h, the vacuum devolatilization in zone 6 was -0.08 MPa, the residence time was 60 s, and nitrogen protection was maintained throughout the process. After the extruded strip was water-cooled, air-dried, and pelletized, it was immediately vacuum-sealed and stored in a low-temperature, light-proof place to obtain the self-made modified masterbatch. The remaining steps were the same as in Example 3.
[0027] Comparative Example 4 The difference between Comparative Example 4 and Example 3 lies in step (3). Step (3) is changed to: 100 parts by weight of polyamide of Baling Petrochemical YH800 and 0.2 parts by weight of antioxidant 1098 are premixed at 500 rpm for 5 min, and then melt-extruded and granulated using a co-rotating twin-screw extruder at 230°C, screw speed of 200 rpm and residence time of 90 s to obtain mixed masterbatch. The remaining steps are the same as in Example 3.
[0028] Comparative Example 5 The difference between Comparative Example 5 and Example 3 lies in step (4). Step (4) is changed to: 675 parts by weight of polyamide, 1 part by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of dilauryl thiodipropionate, 0.3 parts by weight of ethylene bis-stearamide, 15 parts by weight of self-made modified masterbatch, 4 parts by weight of self-made interface agent, and 0.2 parts by weight of triphenyl phosphite are fed into a twin-screw extruder via the main feeder. The length-to-diameter ratio of the extruder is 40:1, and the temperatures of each section are set as follows: Zone 1: 230°C, Zone 2: 235°C, Zone 3: 240°C, Zone 4: 240°C, Zone 5: 230°C, Zone 6: 235°C, Zone 7: 230°C, Zone 8: 235°C, Zone 9: 230°C, Zone 10: 235 ... The temperature was set at 245℃ in zone 6, 245℃ in zone 7, 240℃ in zone 8, and 235℃ at the die head. The screw speed was 250 rpm, and the feed rate was 8 kg / h. Vacuum devolatilization was performed in zones 6 and 8 at -0.09 MPa, with a residence time of 105 s. Nitrogen protection was maintained throughout the process. During the melting process, the amino groups at the ends of the polyamide and the carboxyl groups at both ends of the self-made interface agent underwent an amidation reaction promoted by triphenyl phosphite. This allowed the elastomer particles to be covalently connected to the matrix through an interface layer containing aromatic disulfide bonds. The stepwise addition of side feed shortened the thermal history of the self-made interface agent and reduced the thermal decomposition of disulfide bonds. Vacuum devolatilization and nitrogen protection inhibited the premature hydrolysis of silane during the extrusion stage. The remaining steps were the same as in Example 3.
[0029] Comparative Example 6 The difference between Comparative Example 6 and Example 3 lies in step (6). Step (6) is changed to: after drying the low-temperature ultra-tough modified polyamide composite material at 80°C for 4 hours, a sample is prepared using an injection molding machine under the conditions of nozzle temperature 240°C, mold temperature 85°C, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample is cooled at room temperature for 30 minutes, and then placed in an 80°C deionized water bath for 45 minutes. The catalyst dibutyltin dilaurate is used to accelerate the hydrolysis and condensation of silane, and a uniform siloxane microgel is formed in situ inside the elastomer particles. After the treatment, the sample is taken out, the surface moisture is wiped off, and then dried at 80°C for 4 hours to obtain the low-temperature ultra-tough modified polyamide composite material specimen. The remaining steps are the same as in Example 3.
[0030] Example of effect Table 1 below shows the performance analysis results of the modified polyamide composite materials of Examples 1 to 5 and Comparative Examples 1 to 6 of the present invention.
[0031] Table 1
[0032] A comparison of the experimental data on the notched impact strength of a simply supported beam at -40℃ in the examples and comparative examples reveals that the present invention first prepares a self-made interface agent by condensing diacyl chloride with polyetheramine. Then, after pre-reaction of 3-mercaptopropyltrimethoxysilane with trimethylolpropane triacrylate, it is melt-grafted with ethylene-octene copolymer elastomer to obtain a self-made modified masterbatch. This masterbatch, along with the mixed masterbatch, polyamide, triphenyl phosphite, and composite antioxidant, is extruded via a zoned side-feed reaction to obtain a low-temperature ultra-tough modified polyamide composite material. At low temperatures, the ethylene-octene copolymer elastomer maintains high elasticity. Upon impact, cavitation occurs within the particles, absorbing energy, and the interfacial aromatic disulfide bonds break as sacrificial bonds, dissipating stress at the crack tip and preventing cracking. The interface debonding, combined with the siloxane microgel inside the elastomer stabilizing the particle morphology and preventing excessive fragmentation, promotes stress transfer to the matrix and induces large-area shear yielding, the three work synergistically to achieve low-temperature super-toughness. A comparison of the water absorption data from the examples and comparative examples reveals that the microgel crosslinking network inside the elastomer particles in this invention reduces the free volume of the elastomer phase, inhibits water molecule penetration, and the interfacial disulfide bond layer enhances the bonding between the elastomer and the polyamide matrix, eliminating interfacial voids and defects, cutting off the rapid diffusion path of water molecules along the interfacial capillary channels. Simultaneously, the hydrophobic elastomer particles are uniformly dispersed to form a barrier phase, extending the water molecule diffusion path, thereby significantly reducing the overall water absorption rate of the composite material.
[0033] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.
Claims
1. A method for preparing a low-temperature ultra-tough modified polyamide composite material, characterized in that, Includes the following steps: (1) 4,4'-dithiodibenzoic acid, thionyl chloride, organic solvent and anhydrous DMF are mixed in a mass ratio of 2~4:3~6:15:0.01, stirred and refluxed at 40~45℃ for 6h, and distilled under reduced pressure to obtain an intermediate. The intermediate is mixed with an organic solvent in a mass ratio of 3.3~3.5:15 and the mixture is placed in an ice bath to obtain a reaction solution. 1.2~1.4 times the mass of the intermediate polyetheramine is mixed with an organic solvent and triethylamine in a mass ratio of 1:3:0.25 and placed in an ice bath to obtain a polyetheramine solution. The solution is added dropwise to the reaction solution, stirred at room temperature for 12h, and then post-treated and dried under vacuum at 60℃ for 24h to obtain a self-made interface agent. (2) Under a nitrogen atmosphere, 3-mercaptopropyltrimethoxysilane, trimethylolpropane triacrylate and initiator A are mixed in a mass ratio of 1~2:0.2~0.4:0.02 and stirred at 65~70℃ for 1~2h to obtain oligomeric silane; 90~110 parts by weight of elastomer, 1~3 parts by weight of oligomeric silane, 0.05 parts by weight of initiator B, 0.1 parts by weight of antioxidant 1010 and 0.1 parts by weight of auxiliary antioxidant are premixed, melt grafted, water cooled, air dried and granulated to obtain self-made modified masterbatch; 90~110 parts by weight of polyamide, 1~3 parts by weight of dibutyltin dilaurate and 0.2 parts by weight of antioxidant 1098 are premixed, melt extruded and granulated to obtain mixed masterbatch; (3) 650-700 parts by weight of polyamide, 0.5-1.5 parts by weight of mixed masterbatch, 0.2 parts by weight of antioxidant 1098, 0.2 parts by weight of antioxidant 168, 0.1 parts by weight of auxiliary antioxidant and 0.3 parts by weight of release agent are added through the main feed. 10-20 parts by weight of self-made modified masterbatch, 3-5 parts by weight of self-made interface agent and 0.2 parts by weight of triphenyl phosphite are added to the side feed of different zones respectively. The modified polyamide composite material is obtained by melt extrusion, water cooling and shaping at 20-40℃, pelleting and drying.
2. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The organic solvent in step (1) is anhydrous dichloromethane.
3. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The polyetheramine mentioned in step (1) is polyetheramine ED900.
4. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, Initiator A in step (2) is azobisisobutyronitrile (AIBN).
5. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The elastomer in step (2) is an ethylene-octene copolymer elastomer of model Engage8150.
6. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The initiator B mentioned in step (2) is dicumyl peroxide.
7. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The auxiliary antioxidant mentioned in step (2) is dilaurate thiodipropionate.
8. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The polyamide mentioned in step (2) is: polyamide with model number Baling Petrochemical YH800.
9. The low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, The release agent in step (3) is ethylene bis-stearamide.
10. The application of the low-temperature ultra-tough modified polyamide composite material according to claim 1, characterized in that, After drying the low-temperature super-tough modified polyamide composite material at 80℃ for 4 hours, it was injection molded under the following conditions: nozzle temperature 240℃, mold temperature 85℃, injection pressure 85MPa, holding pressure 55MPa, holding time 10s, and cooling time 30s. After demolding, the sample was first cooled at room temperature for 30 minutes, and then placed in an 80℃ deionized water bath for 45 minutes. After treatment, the sample was removed, the surface moisture was wiped off, and then dried at 80℃ for 4 hours to obtain the low-temperature super-tough modified polyamide composite material specimen.