A thermally conductive and insulating silicon-based composite material for semiconductor chip packaging and its preparation method
By designing a multi-layer structure for the modified filler, the compatibility and dispersibility issues between hexagonal boron nitride and the silica gel matrix were resolved, improving the thermal conductivity and insulation strength of the thermally conductive and insulating material and ensuring long-term stability.
Patent Information
- Application Number
- CN202611240110.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
In existing thermally conductive and insulating silicon-based composite materials for semiconductor packaging, the hexagonal boron nitride filler has insufficient compatibility with the silicon gel matrix, the filler is prone to agglomeration and has poor dispersion uniformity, resulting in high interfacial thermal resistance, which limits the improvement of thermal conductivity and leads to a decline in insulation performance after long-term thermal-oxidative aging.
Modified fillers are used, with hexagonal boron nitride micron and nano powders treated by heat annealing as the core, oxygen-containing functional groups are introduced by surface acid oxidation etching, and silane transition layer and phosphorus nitrogen silicon ternary coating layer are grafted to form a multilayer structure, which improves the interfacial bonding state and is fixed in the cross-linked network by chemical bonds during the curing process.
It improves the uniformity of filler dispersion in the matrix, reduces interfacial thermal resistance, enhances thermal conductivity and insulation strength, delays performance degradation after long-term thermal-oxidative aging, and meets the long-term reliability requirements of semiconductor packaging.
Smart Images

Figure CN123107367A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor packaging materials technology, specifically to a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging and its preparation method. Background Technology
[0002] As semiconductor chips continue to evolve towards higher integration and higher power density, the heat generated during chip operation is increasing dramatically. If this heat cannot be dissipated in a timely manner, it will significantly affect the chip's performance and lifespan. Therefore, packaging materials not only need to provide reliable electrical insulation protection, but also must have excellent thermal conductivity to efficiently transfer the heat generated by the chip to an external heat dissipation structure.
[0003] Silicone gel is a widely used insulating potting material in semiconductor packaging, but its intrinsic thermal conductivity is low. To improve thermal conductivity, high thermal conductivity fillers are usually added to the silicone gel matrix. Hexagonal boron nitride (BN) has good thermal conductivity, excellent electrical insulation, and high chemical stability, making it a relatively ideal choice for thermally conductive fillers. However, there is a significant difference in interfacial compatibility between hexagonal boron nitride and the silicone gel matrix, making it easy for the filler to agglomerate in the matrix and difficult to disperse uniformly. There is also a high interfacial thermal resistance between the filler and the matrix, which seriously affects the phonon transmission efficiency at the interface. Furthermore, under long-term thermo-oxidative aging and high-low temperature cycling, the molecular chains of silicone gel are prone to breakage, and the cross-linked structure gradually degrades, leading to a decrease in the material's breakdown strength. These factors collectively restrict further improvement in the thermal conductivity and insulation reliability of the composite material. How to effectively improve the interfacial bonding state between the boron nitride filler and the silicone gel matrix, reduce the interfacial thermal resistance, and improve the long-term stability of the composite system has become a technical problem that needs to be solved in the research and development of thermally conductive and insulating materials for semiconductor packaging. Summary of the Invention
[0004] The purpose of this invention is to address the problems in existing thermally conductive and insulating silicon-based composite materials for semiconductor packaging, such as insufficient compatibility between hexagonal boron nitride filler and silicone oil matrix, easy agglomeration and poor dispersion uniformity of filler, high interfacial thermal resistance between filler and matrix leading to limited improvement in thermal conductivity, and significant decline in insulation performance of composite materials after long-term thermo-oxidative aging and temperature cycling shock. This invention provides a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging, characterized by uniform filler dispersion, good interfacial bonding, high thermal conductivity, high insulation strength, and long-term reliability, as well as its preparation method.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is: a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging, comprising the following components in parts by weight: 60-80 parts of vinyl-terminated silicone oil, 20-35 parts of modified filler, 5-15 parts of hydrogen-containing silicone oil, 0.1-0.5 parts of platinum-based catalyst, and 0.05-0.2 parts of alkynyl alcohol inhibitor; The modified filler uses a mixed powder of hexagonal boron nitride micron powder and hexagonal boron nitride nano powder treated by heat annealing as the core. The surface of the core is etched by acid oxidation to introduce oxygen-containing functional groups, and then grafted with a silane graft transition layer formed by γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane. The outer layer is coated with a phosphorus-nitrogen-silicon ternary coating modification layer formed by the co-condensation of aminotrimethylphosphonic acid and melamine.
[0006] Furthermore, the modified filler is prepared from the following raw materials in parts by weight: 10-20 parts of hexagonal boron nitride micron powder, 5-10 parts of hexagonal boron nitride nano powder, 1-3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 0.5-1.5 parts of diphenyldimethoxysilane, 2-4 parts of aminotrimethylphosphonic acid, 0.5-1.5 parts of melamine, 25-35 parts of 98% concentrated sulfuric acid, 15-25 parts of 68% concentrated nitric acid, and 5-10 parts of glacial acetic acid.
[0007] Furthermore, the preparation method of the modified filler includes the following steps: S1. Place the hexagonal boron nitride micron powder and hexagonal boron nitride nano powder in a tube furnace, heat to 800-950℃ in air atmosphere and calcine for 2-4 hours. After cooling in the furnace, remove the powder to obtain heat-annealed mixed boron nitride powder.
[0008] S2. The heat-annealed mixed boron nitride powder is placed in a reaction vessel, and concentrated sulfuric acid, concentrated nitric acid and glacial acetic acid are added. The mixture is stirred at 300-500 r / min for 4-8 hours under a water bath at 60-80℃. After the reaction, the mixture is washed with deionized water until the pH of the filtrate is ≥5. The filtrate is then vacuum dried at 80-100℃ for 6-12 hours to obtain acid-oxidized etched boron nitride powder.
[0009] S3. Disperse the acid-oxidized boron nitride powder in a mixed solvent of 30-50 parts anhydrous ethanol and 50-100 parts deionized water, ultrasonically disperse for 30-60 minutes, adjust the pH of the system to 3.5-5.0 with glacial acetic acid, add the γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane under a water bath at 40-60℃, stir at 400-600 r / min for 4-8 hours, centrifuge after the reaction, wash with anhydrous ethanol 3-5 times, and vacuum dry at 60-80℃ for 6-12 hours to obtain silane-grafted modified boron nitride powder.
[0010] S4. The silane-grafted modified boron nitride powder is redispersed in 60-100 parts of anhydrous ethanol and ultrasonically dispersed for 20-40 minutes. The aminotrimethylphosphonic acid and melamine are added, and the mixture is refluxed and stirred at 300-500 r / min in a water bath at 50-70℃ for 2-4 hours. After the reaction is completed, the mixture is centrifuged and washed 3-5 times with anhydrous ethanol to obtain a wet hybrid coating product.
[0011] S5. The wet hybrid coating product is vacuum dried at 50-70℃ for 12-24 hours. The dried powder is then passed through a 200-400 mesh standard sieve for particle size classification. The powder that passes through the sieve is collected and is the modified filler.
[0012] The modified filler uses a hybrid powder of micron- and nano-hexagonal boron nitride treated with heat annealing as its core. The heat annealing process eliminates surface defects and improves the integrity of its crystal structure. Acid oxidation etching introduces oxygen-containing functional groups to the core surface, increasing surface active sites. A silane transition layer formed by grafting γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane to this core has one end chemically bonded to the functional groups on the boron nitride surface, while the epoxy groups at the other end are reactive with the vinyl groups in the silicone oil matrix. An outer layer, a ternary phosphorus-nitrogen-silicon coating formed by the co-condensation of aminotrimethylphosphonic acid and melamine, further enhances the organic nature of the filler surface. This multi-layered structure design allows the filler surface to gradually transition from inorganic to organic properties, reducing the interfacial polarity difference between boron nitride and the silicone oil matrix. The dispersion of the filler in the matrix is improved, reducing localized stress concentration and electric field distortion caused by agglomeration. Meanwhile, the silane graft layer and the silicone oil matrix undergo chemical cross-linking during the curing process, anchoring the filler in the cross-linked network through chemical bonds and shortening the path for phonons to travel from the filler to the matrix. The phosphorus, nitrogen, and silicon elements coated on the outer layer can delay the breaking process of the silicone oil molecular chains under thermo-oxidative conditions, maintaining the integrity of the cross-linked structure and enabling the composite material to maintain high breakdown strength during long-term use.
[0013] Furthermore, the platinum-based catalyst is 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0).
[0014] Furthermore, the vinyl-terminated silicone oil is vinyl-terminated dimethyl polysiloxane with an average molecular weight of 2000.
[0015] Furthermore, the alkynol inhibitor is selected from at least one of 1-ethynyl-1-cyclohexanol and 2-methyl-3-butyn-2-ol.
[0016] Furthermore, the hydrogen-containing silicone oil is polymethylhydrosiloxane, with a viscosity of 15-40 mPa·s at 20°C.
[0017] Furthermore, the particle size of the hexagonal boron nitride micron powder is 5-10 μm.
[0018] Furthermore, the particle size of the hexagonal boron nitride nanoparticles is 400-700 nm.
[0019] Furthermore, in step S3, the γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane are premixed evenly before addition and added dropwise over 30-60 minutes.
[0020] Furthermore, in step S5, the vacuum degree of the vacuum drying is -0.08 to -0.1 MPa.
[0021] A method for preparing a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging includes the following steps: P1. According to the mass ratio, the terminal vinyl silicone oil, modified filler, and alkynyl alcohol inhibitor are added to a planetary mixer and stirred and mixed at a speed of 800-1200 r / min for 30-60 minutes under vacuum to obtain component A.
[0022] P2. According to the mass ratio, the hydrogen-containing silicone oil and the platinum-based catalyst are mixed and stirred at a speed of 200-400 r / min for 10-20 minutes to obtain component B.
[0023] P3. Before use, mix component A and component B at a mass ratio of 100:5 to 100:15, stir at 500-800 r / min for 5-10 minutes at 20-30℃, and then degas under a vacuum of -0.095 MPa or higher for 10-20 minutes to obtain the thermally conductive and insulating silicon-based composite material.
[0024] Furthermore, in step P1, the vacuum degree of the vacuum condition is -0.08 to -0.1 MPa.
[0025] Furthermore, in step P3, during the degassing process, the material undergoes a combined motion of revolution and rotation within the rotating container.
[0026] The composite material of this invention uses vinyl-terminated silicone oil as the matrix. Hydrogen-containing silicone oil forms a cross-linked structure through hydrosilylation reaction under the action of a platinum-based catalyst. Alkyne alcohol inhibitors are used to regulate the curing rate. The key to improving thermal conductivity and insulation performance lies in the design of the modified filler. The filler first undergoes thermal annealing of micron- and nano-sized hexagonal boron nitride to make the powder surface structure more regular and reduce the influence of original defects on phonon scattering. Subsequently, oxygen-containing functional groups are introduced onto the boron nitride surface through mixed acid oxidation etching, providing reaction sites for subsequent grafting. The silane grafting transition layer is composed of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane. One end of the silane is bonded to the functional groups on the boron nitride surface, while the other end carries organic groups that have good affinity with the silicone oil matrix, thus building a transition bridge between the inorganic filler and the organic matrix. The co-condensation product of aminotrimethylphosphonic acid and melamine in the outer coating further increases the organic component on the filler surface, making the overall filler surface closer to the silicone oil matrix, reducing the tendency of filler agglomeration, and enabling more uniform dispersion in the matrix. The mixed combination of micron and nanoparticles allows small-diameter particles to fill the gaps between large-diameter particles, increasing the packing efficiency per unit volume and facilitating more direct heat transfer between fillers. The silane layer on the filler surface can participate in the cross-linking reaction of silicone oil during curing, fixing the filler in the cross-linking system through chemical bonds. This reduces the interfacial resistance encountered by phonons when they travel from the matrix to the filler, resulting in a smoother heat transfer path. The phosphorus, nitrogen, and silicon elements contained in the outer coating can delay the breaking reaction of silicone oil molecular chains under thermo-oxidative aging conditions and inhibit excessive degradation of the cross-linked structure, thus allowing the material to maintain a high breakdown field strength during long-term use and temperature cycling, and its insulation performance will not significantly decrease over time.
[0027] Compared with the prior art, the beneficial effects of the present invention are: 1. In this invention, after the surface of the modified filler is modified by silane grafting transition layer and outer coating, the difference between the surface properties of the filler and the silicone oil matrix is reduced, the uniformity of the filler dispersion in the matrix is improved, the interfacial bonding state is improved, and the cross-linking structure integrity is better after the material is cured.
[0028] 2. This invention uses a hybrid filler of micron- and nano-hexagonal boron nitride, with small-diameter particles filling the gaps between large-diameter particles, resulting in high filler packing efficiency. Combined with the reduced interfacial thermal resistance from the organic transition layer on the filler surface, the heat transfer path in the filler network is smoother.
[0029] 3. In this invention, the phosphorus-nitrogen-silicon ternary coating layer covering the filler can delay the breakage of silicone oil molecular chains under hot and oxygen conditions, inhibit the degradation of cross-linked structures, and the material can still maintain high breakdown strength after long-term aging, thus meeting the requirements of semiconductor packaging for long-term reliability. Attached Figure Description
[0030] Figure 1 The infrared spectrum of the modified filler prepared in Preparation Example 1 of the present invention is shown. Detailed Implementation
[0031] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0032] Preparation Example 1: Preparation of modified fillers: 1. Raw material composition: Hexagonal boron nitride micron powder: 15 parts; hexagonal boron nitride nano powder: 8 parts; γ-(2,3-epoxypropoxy)propyltrimethoxysilane: 2 parts; diphenyldimethoxysilane: 1 part; aminotrimethylphosphonic acid: 3 parts; melamine: 1 part; concentrated sulfuric acid, 98% by mass: 30 parts; concentrated nitric acid, 68% by mass: 20 parts; glacial acetic acid: 8 parts.
[0033] The hexagonal boron nitride micron powder was purchased from Shanghai McLean Biochemical Technology Co., Ltd., item number: B874955, with a particle size of 7μm.
[0034] The hexagonal boron nitride nanoparticles were purchased from Shanghai McLean Biochemical Technology Co., Ltd., item number: B909466, with a particle size of 500nm.
[0035] 2. Preparation method: S1. Place hexagonal boron nitride micron powder and hexagonal boron nitride nano powder in a tube furnace, heat to 900°C at a heating rate of 5°C / min in air atmosphere, hold for calcination for 3 hours, and remove after cooling to room temperature in the furnace to obtain heat-annealed mixed boron nitride powder.
[0036] S2. The heat-annealed mixed boron nitride powder obtained in step S1 was placed in a reaction vessel, and 98% concentrated sulfuric acid, 68% concentrated nitric acid, and glacial acetic acid were added. The mixture was stirred at 400 r / min for 6 hours in a water bath at 70°C. After the reaction was completed, the mixture was repeatedly washed with deionized water until the pH of the filtrate was ≥5. The filtrate was then vacuum dried at 90°C (vacuum degree -0.09 MPa) for 9 hours to obtain acid-oxidized etched boron nitride powder.
[0037] S3. The acid-oxidized boron nitride powder obtained in step S2 was dispersed in a mixed solvent of 40 parts by mass of anhydrous ethanol and 80 parts by mass of deionized water, and ultrasonically dispersed (ultrasonic power 300W, frequency 40kHz) for 45 minutes. The pH of the system was adjusted to 4.0 with glacial acetic acid. Under a water bath at 50℃, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 1 part by mass of diphenyldimethoxysilane were pre-mixed evenly and then added to the reaction system dropwise at a constant rate over 45 minutes. After the addition was complete, the mixture was stirred at 500 r / min for 6 hours. After the reaction was completed, the mixture was centrifuged at 8000 r / min for 15 minutes, the supernatant was discarded, and the precipitate was washed 4 times with anhydrous ethanol (50 parts by mass each time). After washing, the precipitate was vacuum dried at 70℃ (vacuum degree -0.09MPa) for 9 hours to obtain silane-grafted modified boron nitride powder.
[0038] S4. The silane-grafted modified boron nitride powder obtained in step S3 was redispersed in 80 parts by mass of anhydrous ethanol and ultrasonically dispersed (ultrasonic power 300W, frequency 40kHz) for 30 minutes. Aminotrimethylphosphonic acid and melamine were added, and the mixture was refluxed and stirred at 400 r / min for 3 hours in a 60℃ water bath. After the reaction was completed, the mixture was centrifuged at 8000 r / min for 15 minutes, the supernatant was discarded, and the precipitate was washed four times with anhydrous ethanol (50 parts by mass each time) to obtain a wet hybrid coating product.
[0039] S5. The wet hybrid coating product obtained in step S4 is vacuum dried at 60°C (vacuum degree -0.09MPa) for 18 hours. The dried powder is then passed through a 300-mesh standard sieve for particle size classification, and the powder passing through the sieve is collected as the modified filler.
[0040] like Figure 1 As shown in the figure, irregularly layered and stacked hexagonal boron nitride particles are visible in the SEM area. The main particles have a micron-scale sheet-like structure with many fine particles and rough protrusions attached to the surface and edges. B and N elements are continuously and relatively uniformly distributed in the particle area, indicating that the main body is still a boron nitride framework. O elements are mainly weakly distributed along the particle edges and surface, which can correspond to the hydroxyl / oxygen-containing active sites introduced by acid oxidation. Si elements are weakly but continuously distributed on the surface, which is consistent with the characteristics of silane layers after grafting γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane. P elements are distributed in dots or bands at the edges of the sheets and on the local surface, which can correspond to the phosphorus-containing hybrid coating layer formed by aminotrimethylphosphonic acid.
[0041] Preparation Example 2: The modified filler was prepared according to the preparation method in Preparation Example 1, except that the 7 μm hexagonal boron nitride micron powder was replaced by an equal mass of 5 μm hexagonal boron nitride micron powder, and everything else remained the same as in Preparation Example 1.
[0042] Preparation Example 3: The modified filler was prepared according to the preparation method in Preparation Example 1, except that the 500 nm hexagonal boron nitride nanoparticles were replaced by hexagonal boron nitride nanoparticles with a particle size of 700 nm, and the rest remained the same as in Preparation Example 1.
[0043] Preparation Example 4: The modified filler was prepared by referring to the preparation method in Preparation Example 1, except that the hot annealing and calcination temperature was replaced with 800°C, and everything else remained the same as in Preparation Example 1.
[0044] Comparative preparation example 1: The modified filler was prepared according to the preparation method in Preparation Example 1, except that the hot annealing and calcination temperature was replaced with 600°C instead of 900°C, and everything else remained the same as in Preparation Example 1.
[0045] Comparative preparation example 2: The modified filler was prepared by referring to the preparation method in Preparation Example 1, except that the γ-(2,3-epoxypropoxy)propyltrimethoxysilane in the silane grafting modification step was replaced by γ-aminopropyltriethoxysilane by mass, and the rest remained the same as in Preparation Example 1.
[0046] Comparative preparation example 3: The modified filler was prepared by referring to the preparation method in Preparation Example 1, except that the diphenyldimethoxysilane in the silane grafting modification step was replaced with dimethyldimethoxysilane by mass, and everything else remained the same as in Preparation Example 1.
[0047] Comparative preparation example 4: The modified filler was prepared by referring to the preparation method in Preparation Example 1, except that the aminotrimethylphosphonic acid in the outer coating step was replaced with aminotrimethylenephosphonic acid, and everything else remained the same as in Preparation Example 1.
[0048] Comparative preparation example 5: The modified filler was prepared by referring to the preparation method in Preparation Example 1, except that the melamine in the outer coating step was replaced with urea, and everything else remained the same as in Preparation Example 1.
[0049] Comparative preparation example 6: The modified filler was prepared according to the preparation method in Preparation Example 1, except that the mixed system of hexagonal boron nitride micron powder and hexagonal boron nitride nano powder was replaced with a single hexagonal boron nitride micron powder in equal mass, and everything else remained the same as in Preparation Example 1.
[0050] Comparative preparation example 7: The modified filler was prepared according to the preparation method in Preparation Example 1, except that the mixed system of hexagonal boron nitride micron powder and hexagonal boron nitride nano powder was replaced with a single hexagonal boron nitride nano powder in equal mass, and everything else remained the same as in Preparation Example 1.
[0051] Example 1: Preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging: 1. Raw material composition: Vinyl-terminated silicone oil: 70 parts, which is vinyl-terminated dimethyl polysiloxane.
[0052] Modified filler: 28 parts. Prepared according to the method of Preparation Example 1.
[0053] Hydrogen-containing silicone oil: 10 parts, which is polymethylhydrosiloxane.
[0054] Platinum-based catalyst: 0.3 parts, which is 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0).
[0055] Alkyne inhibitor: 0.12 parts, 1-ethynyl-1-cyclohexanol.
[0056] The vinyl-terminated dimethyl polysiloxane was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with product number V304361.
[0057] The polymethylhydrosiloxane was purchased from Shanghai McLean Biochemical Technology Co., Ltd., item number: P832168, with a viscosity of 28 mPa·s.
[0058] The 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) was purchased from Shanghai Jizhi Biochemical Technology Co., Ltd., item number: K71950.
[0059] 2. Preparation method: P1. By mass, vinyl-terminated dimethyl polysiloxane, modified filler, and 1-ethynyl-1-cyclohexanol were added to a planetary mixer and stirred at 1000 r / min for 45 minutes under a vacuum of -0.09 MPa to obtain component A.
[0060] P2. By mass, polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxaneplatinum (0) were mixed and stirred at 300 r / min for 15 minutes to obtain component B.
[0061] P3. Before use, mix component A and component B at a mass ratio of 100:10, stir at 25°C and 650 r / min for 8 minutes, and then degas under vacuum conditions of -0.098 MPa for 15 minutes. During the degassing process, the material undergoes a combined motion of revolution and rotation in the rotating container to obtain the thermally conductive and insulating silicon-based composite material.
[0062] Examples 2-4: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out by referring to the preparation method of Example 1, except that the modified filler is replaced with the modified filler in Preparation Examples 2-4 in sequence, and the rest is the same as in Example 1.
[0063] Example 5: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out by referring to the preparation method in Example 1, except that the polymethylhydrosiloxane is replaced with an equal mass of polymethylhydrosiloxane with a viscosity of 15 mPa·s, and the rest is the same as in Example 1.
[0064] Example 6: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out according to the preparation method in Example 1, except that the alkynyl alcohol inhibitor 1-ethynyl-1-cyclohexanol is replaced with an equal mass of 2-methyl-3-butyn-2-ol, and the rest is the same as in Example 1.
[0065] Comparative Examples 1-7: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out by referring to the preparation method in Example 1, except that the modified filler is replaced sequentially with the modified filler prepared in Comparative Preparation Examples 1-7, and the rest is the same as in Example 1.
[0066] Comparative Example 8: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out by referring to the preparation method in Example 1, except that 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) is replaced with chloroplatinic acid hexahydrate with an equimolar platinum content, and the rest is the same as in Example 1.
[0067] Comparative Example 9: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out by referring to the preparation method in Example 1, except that 1-ethynyl-1-cyclohexanol is replaced with an equal mass of triphenylphosphine, and the rest is the same as in Example 1.
[0068] Comparative Example 10: The preparation of a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging is carried out according to the preparation method in Example 1, except that the vinyl-terminated dimethyl polysiloxane with an average molecular weight of 2000 is replaced with an equal mass of vinyl-terminated dimethyl polysiloxane with an average molecular weight of 9400, and the rest remains the same as in Example 1.
[0069] Performance testing: 1. Thermal conductivity: Tested according to GB / T19466.8-2025. After the composite material was cured at 25℃ for 24 hours, a circular sample with a diameter of 10 mm and a thickness of 1 mm was prepared. The thermal conductivity was determined by differential scanning calorimetry at 25℃. The data are shown in Table 1.
[0070] 2. Breakdown strength: Tested according to GB / T1408.1-2016. After curing the composite material at 25℃ for 24 hours, a sheet sample with a thickness of 1 mm was prepared. A spherical electrode with a diameter of 25 mm was used, and a voltage was applied in transformer oil in a continuous and uniform voltage increase manner at a voltage increase rate of 500 V / s. The voltage value at which the sample broke down was recorded. The data are shown in Table 1.
[0071] 3. Volume resistivity: Tested according to GB / T31838.2-2019. After curing the composite material at 25℃ for 24 hours, a circular sample with a diameter of 50 mm and a thickness of 1 mm was prepared. A DC voltage of 500 V was applied for 60 s, and the volume resistivity was measured. The data are shown in Table 1.
[0072] 4. Shore Hardness: Tested according to GB / T39693.4-2025. After curing the composite material at 25℃ for 24 hours, sheet samples with a thickness of not less than 6 mm were prepared and measured using a Shore A hardness tester. The data are shown in Table 1.
[0073] 5. Breakdown strength retention rate after thermo-oxidative aging: Referring to the aging procedure in GB / T11026.1-2016, the composite material samples were placed in a constant temperature thermo-aging chamber at 150℃ for 1000 hours. After removal, they were equilibrated at 25℃ for 24 hours. The breakdown strength after aging was tested according to GB / T1408.1-2016, and the breakdown strength retention rate was calculated as (breakdown strength after aging / breakdown strength before aging × 100%). The data are shown in Table 1.
[0074] Table 1. Test data for examples and comparative examples The thermal conductivity, breakdown strength, volume resistivity, hardness, and breakdown strength retention rate after aging of the embodiments are all superior to those of the comparative examples. The heat annealing temperature directly affects the degree of elimination of surface defects in the filler. When the temperature is insufficient, the integrity of the crystal structure is poor, phonon scattering is enhanced, thermal conductivity decreases, and the insufficient number of active sites on the filler surface also restricts the full progress of the subsequent grafting reaction. The composition of the silane graft layer plays a decisive role in interfacial compatibility. The composite use of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane can form a suitable organic transition layer on the filler surface. After replacing it with a single silane or changing the silane molecular structure, the polarity difference between the filler and the matrix increases, the interfacial bonding state changes, the phonon transmission efficiency decreases, and the uniformity of the filler dispersion in the matrix deteriorates. The electric field distortion caused by local agglomeration leads to a decrease in breakdown strength. Changes in the composition of the outer coating layer also have a significant impact. The coating layer formed by the co-condensation product of aminotrimethylphosphonic acid and melamine on the filler surface has a high degree of organicification. After replacing it with other phosphonic acids or amine compounds, the compatibility between the chemical structure of the coating layer and the filler surface changes, and the interfacial transition effect between the filler and the matrix weakens. The size combination of the filler is also an important factor affecting performance. Single micron-sized fillers have insufficient packing density per unit volume due to large interparticle voids, while single nano-sized fillers are prone to agglomeration due to excessive specific surface area and high surface energy. After mixing the two sizes, the small-diameter particles can fill the voids between the large-diameter particles, forming a more compact packing structure, which is conducive to efficient heat conduction in the filler network. When the molecular weight of the matrix increases, the dispersion resistance of the filler increases, the uniformity decreases, and various properties show varying degrees of reduction. The phosphorus, nitrogen, and silicon elements present in the outer coating layer can inhibit the breaking reaction of silicone oil molecular chains under thermo-oxidative conditions, maintain the integrity of the cross-linked structure, and enable the composite material to maintain high insulation performance after long-term aging.
[0075] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A thermally conductive and insulating silicon-based composite material for semiconductor chip packaging, characterized in that, It is composed of the following components in parts by weight: 60-80 parts of vinyl-terminated silicone oil, 20-35 parts of modified filler, 5-15 parts of hydrogen-containing silicone oil, 0.1-0.5 parts of platinum-based catalyst, and 0.05-0.2 parts of alkynol inhibitor; The modified filler uses a mixed powder of hexagonal boron nitride micron powder and hexagonal boron nitride nano powder treated by heat annealing as the core. The surface of the core is etched by acid oxidation to introduce oxygen-containing functional groups, and then grafted with a silane graft transition layer formed by γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane. The outer layer is coated with a phosphorus-nitrogen-silicon ternary coating modification layer formed by the co-condensation of aminotrimethylphosphonic acid and melamine.
2. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 1, characterized in that, The modified filler is composed of the following raw materials in parts by weight: 10-20 parts of hexagonal boron nitride micron powder, 5-10 parts of hexagonal boron nitride nano powder, 1-3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 0.5-1.5 parts of diphenyldimethoxysilane, 2-4 parts of aminotrimethylphosphonic acid, 0.5-1.5 parts of melamine, 25-35 parts of 98% concentrated sulfuric acid, 15-25 parts of 68% concentrated nitric acid, and 5-10 parts of glacial acetic acid.
3. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 2, characterized in that, The method for preparing the modified filler includes the following steps: S1. Place the hexagonal boron nitride micron powder and hexagonal boron nitride nano powder in a tube furnace, heat to 800-950℃ in air atmosphere and calcine for 2-4 hours. After cooling in the furnace, take it out to obtain heat-annealed mixed boron nitride powder. S2. The heat-annealed mixed boron nitride powder is placed in a reaction vessel, and concentrated sulfuric acid, concentrated nitric acid and glacial acetic acid are added. The mixture is stirred at 300-500 r / min for 4-8 hours under a water bath at 60-80℃. After the reaction, the mixture is washed with deionized water until the pH of the filtrate is ≥5. The mixture is then vacuum dried at 80-100℃ for 6-12 hours to obtain acid-oxidized etched boron nitride powder. S3. Disperse the acid-oxidized etched boron nitride powder in a mixed solvent of 30-50 parts anhydrous ethanol and 50-100 parts deionized water, ultrasonically disperse for 30-60 minutes, adjust the pH of the system to 3.5-5.0 with glacial acetic acid, add the γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane under a water bath at 40-60℃, stir at 400-600 r / min for 4-8 hours, centrifuge after the reaction, wash with anhydrous ethanol 3-5 times, and vacuum dry at 60-80℃ for 6-12 hours to obtain silane-grafted modified boron nitride powder; S4. The silane-grafted modified boron nitride powder is redispersed in 60-100 parts of anhydrous ethanol and ultrasonically dispersed for 20-40 minutes. The aminotrimethylphosphonic acid and melamine are added, and the mixture is refluxed and stirred at 300-500 r / min in a water bath at 50-70℃ for 2-4 hours. After the reaction is completed, the mixture is centrifuged and washed 3-5 times with anhydrous ethanol to obtain a wet hybrid coating product. S5. The wet hybrid coating product is vacuum dried at 50-70℃ for 12-24 hours. The dried powder is then passed through a 200-400 mesh standard sieve for particle size classification. The powder that passes through the sieve is collected and is the modified filler.
4. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 1, characterized in that, The platinum-based catalyst is 1,3-divinyl-1,1,3,3-tetramethyldisiloxaneplatinum(0); The vinyl-terminated silicone oil is a vinyl-terminated dimethyl polysiloxane with an average molecular weight of 2000.
5. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 1, characterized in that, The alkynol inhibitor is selected from at least one of 1-ethynyl-1-cyclohexanol and 2-methyl-3-butyn-2-ol; The hydrogen-containing silicone oil is polymethylhydrosiloxane, with a viscosity of 15-40 mPa·s at 20°C.
6. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 2, characterized in that, The particle size of the hexagonal boron nitride micron powder is 5-10 μm; The particle size of the hexagonal boron nitride nanoparticles is 400-700 nm.
7. The thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 3, characterized in that, In step S3, the γ-(2,3-epoxypropoxy)propyltrimethoxysilane and diphenyldimethoxysilane are premixed evenly before addition and added dropwise over 30-60 minutes.
8. A method for preparing a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging as described in any one of claims 1-7, characterized in that, Includes the following steps: P1. According to the mass ratio, the terminal vinyl silicone oil, modified filler, and alkynyl alcohol inhibitor are added to a planetary mixer and stirred and mixed at a speed of 800-1200 r / min for 30-60 minutes under vacuum to obtain component A; P2. According to the mass ratio, the hydrogen-containing silicone oil and the platinum-based catalyst are mixed and stirred at a speed of 200-400 r / min for 10-20 minutes to obtain component B; P3. Before use, mix component A and component B at a mass ratio of 100:5 to 100:15, stir at 500-800 r / min for 5-10 minutes at 20-30℃, and then degas under a vacuum of -0.095 MPa or higher for 10-20 minutes to obtain the thermally conductive and insulating silicon-based composite material.
9. The method for preparing a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 8, characterized in that, In step P1, the vacuum level of the vacuum condition is -0.08 to -0.1 MPa.
10. The method for preparing a thermally conductive and insulating silicon-based composite material for semiconductor chip packaging according to claim 8, characterized in that, In step P3, during the degassing process, the material undergoes a combined motion of revolution and rotation within the rotating container.