A high weather-resistant and high-flowability titanium dioxide and its preparation method
By coating the surface of titanium dioxide with strontium titanate, silica alumina and magnesium lithium silicate films, and then modifying it with betaine containing hydroxyl and sulfonyl groups, the problems of insufficient flowability and weather resistance of titanium dioxide were solved, achieving a balance between high flowability and weather resistance.
Patent Information
- Application Number
- CN202611214256.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
The poor flowability of existing titanium dioxide leads to difficulties in conveying and feeding, easy clogging, poor dispersibility, and insufficient weather resistance, which affects production efficiency and product quality.
A strontium titanate film, a silica-alumina composite film, and a magnesium-lithium silicate film are sequentially coated onto the surface of titanium dioxide, and then organically modified with betaine containing hydroxyl and sulfonyl groups to form a composite coating layer.
It significantly improves the flowability and weather resistance of titanium dioxide, solves the problem of conveying blockage, enhances dispersibility and production efficiency, and meets the high-standard requirements of industries such as coatings.
Smart Images

Figure CN123107419A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of titanium dioxide preparation technology, specifically relating to a high weather-resistant and high-flowability titanium dioxide and its preparation method. Background Technology
[0002] Titanium dioxide (TiO2), an important inorganic white pigment, is widely used in coatings, plastics, rubber, inks, and papermaking. During the production, storage, transportation, and use by downstream customers, flowability is a key performance indicator that directly affects production efficiency and product quality.
[0003] Currently, titanium dioxide produced using existing technologies generally suffers from poor flowability, the most obvious impact being difficulties in conveying and feeding. In pneumatic or pipeline conveying, the poorly flowing titanium dioxide easily forms bridging or rat holes in hoppers and bins, leading to poor discharge or even blockages, requiring manual intervention. This severely impacts production continuity and automation, and cleaning the discharge port after blockages easily introduces impurities. Furthermore, poor dispersibility means that agglomerated titanium dioxide particles are difficult to break up in solvents or resin matrices, requiring higher shear forces and longer grinding times to achieve ideal dispersion. This increases energy consumption and time costs, reducing production efficiency. Incomplete dispersion directly affects all subsequent properties.
[0004] Existing technologies generally use the addition of organic additives to improve flowability. However, organic substances are mainly bonded to the surface of titanium dioxide inorganic particles through physical adsorption or weak chemical bonds, and are easily detached during subsequent high-speed stirring, grinding, or use, leading to a decrease in the flowability improvement effect. In addition, weather resistance is also an important quality indicator for titanium dioxide, especially in the coatings industry. As the most commonly used white inorganic pigment, the weather resistance of titanium dioxide directly affects the performance and service life of outdoor coatings.
[0005] Therefore, it is necessary to develop a preparation method for titanium dioxide that maintains high fluidity over a long period of time, to solve the problems of poor material flow and blockage in the production and application stages, to meet the needs of industrial production, and at the same time to maintain the excellent weather resistance of titanium dioxide to meet the needs of industries such as coatings and plastics. Summary of the Invention
[0006] The purpose of this invention is to provide a high-weather-resistant and high-flowability titanium dioxide and its preparation method to overcome the shortcomings of the prior art.
[0007] The objective of this invention is achieved through the following technical solution: The first aspect of this application provides a high weather-resistant and high-flowability titanium dioxide, which, from the inside out, comprises a titanium dioxide substrate, an inorganic coating layer, and an organic coating layer. The inorganic coating layer, from the inside out, includes a strontium titanate film layer, a silicon oxide-alumina composite film layer, and a lithium magnesium silicate film layer. The organic coating layer is a membrane obtained by organic modification treatment using betaine containing hydroxyl and sulfonyl groups.
[0008] Preferably, the betaine containing hydroxyl and sulfonyl groups is at least one selected from lauryl hydroxysulfonyl betaine, cocamidopropyl hydroxysulfonyl betaine, lauramide propyl hydroxysulfonyl betaine, or octadecyl dimethyl hydroxypropyl sulfonyl betaine.
[0009] Preferably, the strontium titanate film is formed by the following steps: Strontium source and carbonic acid source are added to titanium dioxide-based material slurry, and the pH is adjusted to 8.0~8.5 to generate strontium carbonate precursor. Then, the mixture is reacted at 160~200℃ for 2~24h to generate strontium titanate precipitate in situ.
[0010] Preferably, the lithium magnesium silicate film is formed by the following steps: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
[0011] Preferably, the coating amount of the strontium titanate film, calculated as strontium titanate, is 0.5% to 2% of the mass of the titanium dioxide substrate; In the aforementioned silicon oxide-alumina composite film, the amount of silicon oxide coating is 2-4% of the mass of the titanium dioxide substrate; the amount of alumina coating is 1-3% of the mass of the titanium dioxide substrate. The coating amount of the lithium magnesium silicate film, calculated based on lithium magnesium silicate, is 1-3% of the mass of the titanium dioxide substrate. The amount of betaine containing hydroxyl and sulfonyl groups in the coating is 0.2 to 0.6% of the mass of the titanium dioxide substrate.
[0012] The second aspect of this application provides a method for preparing high weather-resistant and high-flowability titanium dioxide as described above, comprising the following steps: S1. Preparation of titanium dioxide-based material slurry; S2. Perform strontium titanate coating; S3. Perform a composite coating of silica and alumina; S4. Perform lithium magnesium silicate coating; S5. Perform betaine organic coating containing hydroxyl and sulfonyl groups.
[0013] Preferably, step S2 further includes: A strontium source is added to the titanium dioxide-based material slurry, followed by a certain amount of carbonic acid source, and the pH is adjusted to 8.0-8.5 to generate a strontium carbonate precursor. The slurry is then reacted at 160-200°C for 2-24 hours. The amount of the soluble strontium source added, based on strontium oxide, is 0.5-2% of the mass of the titanium dioxide substrate; The amount of the added carbonic acid source, calculated as carbonic acid, is 0.3 to 1% of the mass of the titanium dioxide substrate.
[0014] Preferably, step S3 further includes: A soluble silica source is added to the slurry coated with a strontium titanate film. After aging, an acidic aluminum source is added, and the pH is controlled at 6-8 to allow silica and alumina to co-deposit.
[0015] Preferably, step S4 further includes: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
[0016] Preferably, the lithium magnesium silicate sol is prepared by the following steps: Lithium magnesium silicate is added to hot water and stirred continuously until it swells fully to form a hydrogel. The solid content is controlled at 4-5%, and then allowed to stand and mature to obtain the lithium magnesium silicate sol.
[0017] This application significantly improves the weather resistance of titanium dioxide by coating it with a composite film of strontium titanate, silica, and alumina, and significantly improves its flowability by coating it with lithium magnesium silicate and betaine containing hydroxyl and sulfonyl groups, thus obtaining a titanium dioxide that has both high weather resistance and high flowability. Attached Figure Description
[0018] Figure 1 The graph shows the test results of the samples obtained in Examples 1-4 and Comparative Examples 1-3 in the xenon lamp rapid aging test, showing the change of 60° light retention rate (%) over time. Detailed Implementation
[0019] This application provides a high weather-resistant and high-flowability titanium dioxide, which, from the inside out, comprises a titanium dioxide substrate, an inorganic coating layer, and an organic coating layer.
[0020] The inorganic coating layer, from the inside out, includes a strontium titanate film layer, a silicon oxide-alumina composite film layer, and a lithium magnesium silicate film layer. The organic coating layer is obtained by organic modification of betaine containing hydroxyl and sulfonyl groups.
[0021] This invention involves sequentially coating the surface of titanium dioxide with a strontium titanate film (SrTiO3), a silicon oxide / alumina composite film, a lithium magnesium silicate film, and a hydroxysulfonate betaine film, thereby obtaining a titanium dioxide that combines weather resistance and flowability, and has the following beneficial effects: (1) In the strontium titanate film layer, SrTiO3 is coated on the surface of titanium dioxide in a uniform and dense film form. The lattice constant of SrTiO3 has a certain matching with rutile TiO2. It can suppress the crystal transformation of TiO2 through the interfacial lattice anchoring effect. SrTiO3 can absorb some ultraviolet light or shield ultraviolet light, reduce the damage to the structure of TiO2 caused by photogenerated carriers generated by ultraviolet light irradiation, and suppress the generation and migration of electron-hole pairs on the surface of TiO2. This greatly reduces the photocatalytic activity of titanium dioxide, prevents the degradation of surrounding organic media, and extends the service life of the material in the outdoor environment.
[0022] (2) The second layer of the silicon dioxide and aluminum oxide composite film is uniform and dense, which can effectively block ultraviolet rays, moisture and oxygen from contacting the surface of titanium dioxide particles, fundamentally inhibiting the photocatalytic activity of titanium dioxide and further improving the weather resistance of titanium dioxide. Compared to sequentially coated silicon oxide and aluminum oxide films, the simultaneous silicon-aluminum composite film can form a large number of Si-O-Al covalent cross-linked structures between the silicon-oxygen and aluminum-oxygen frameworks, with no obvious interlayer interface defects. The overall film density is higher, which can more effectively block ultraviolet rays, moisture and oxygen, fundamentally inhibiting the photocatalytic activity of titanium dioxide. At the same time, the composite film combines the excellent ultraviolet blocking ability of silicon oxide with the good dispersibility of aluminum oxide, avoiding the film cracking and local leakage problems caused by the difference in the thermal expansion coefficients of the two layers in the stepwise double-layer film. The finished titanium dioxide has a lower oil absorption value, and the gloss and long-term weather resistance of the paint film are improved simultaneously. In addition, co-precipitation coating can simplify the production process and shorten the reaction cycle.
[0023] (3) The third layer is a lithium magnesium silicate film. Lithium magnesium silicate has a nano-two-dimensional sheet structure, which can be uniformly coated on the surface of powder particles to play a role in physical isolation and filling micro-roughness, greatly reducing the friction and van der Waals adsorption between particles. At the same time, it relies on its unique end face and one-sided anisotropic charge characteristics to neutralize the static electricity of powder friction and eliminate static agglomeration. In addition, it has excellent hydrophilic and water-binding ability, which can form a stable hydration and lubrication film on the particle surface. It can not only greatly improve the looseness and self-flowability of dry powder, but also reduce the viscosity of water-based slurry system, reduce particle flocculation and accumulation, and significantly improve powder flow.
[0024] (4) Finally, a betaine organic coating layer containing hydroxyl and sulfonyl groups is coated on the outside of the titanium dioxide. Betaine containing hydroxyl and sulfonyl groups is an amphoteric compound. Its structure includes hydroxyl, sulfonic acid and amino groups. The coating on the outside of the titanium dioxide can further improve the dispersibility through electrostatic repulsion, steric hindrance and enhanced medium compatibility. The positive and negative charges on its surface can form "ion conduction channels", which can quickly release the static charge on the surface of the titanium dioxide particles, improve the antistatic properties and further improve the flowability.
[0025] Therefore, this application significantly improves the weather resistance of titanium dioxide by coating it with a composite film of strontium titanate, silica, and alumina, and significantly improves its flowability by coating it with lithium magnesium silicate and betaine containing hydroxyl and sulfonyl groups, thus obtaining a titanium dioxide that has both high weather resistance and high flowability.
[0026] Furthermore, by combining inorganic and organic coatings, complementary structures and performance can be achieved. Firstly, the inorganic film ensures weather resistance and provides adsorption sites for organic modification. The organic film layer addresses the shortcomings of inorganic coated powders, such as easy agglomeration and processing difficulties. Simultaneously, the uniformly dispersed powder allows for full utilization of weather resistance. This breaks the traditional limitation of titanium dioxide where "high weather resistance often sacrifices flowability, and vice versa," allowing the product to simultaneously meet the dual high standards of weather resistance and processability.
[0027] As mentioned above, since strontium titanate and rutile titanium dioxide have good compatibility, rutile titanium dioxide is preferred in this application.
[0028] Preferably, the betaine containing hydroxyl and sulfonyl groups is at least one selected from lauryl hydroxysulfonyl betaine, cocamidopropyl hydroxysulfonyl betaine, lauramide propyl hydroxysulfonyl betaine, or octadecyl dimethyl hydroxypropyl sulfonyl betaine.
[0029] Preferably, the inorganic coating layers of this application are all completed by wet coating. Compared with other coating methods such as dry coating, wet coating is easier to control in terms of coating process and film structure.
[0030] Preferably, the strontium titanate film is formed by the following steps: A soluble strontium source is added to a titanium dioxide-based material slurry, followed by a certain amount of carbonate source, and the pH is adjusted to 8.0-8.5 to generate a strontium carbonate precursor. The mixture is then reacted in a sealed environment at 160-200℃ for 2-24 hours, resulting in the in-situ formation of strontium titanate precipitate. Under high temperature and pressure, dehydration condensation occurs between the titanium hydroxyl groups and the strontium hydroxyl groups, gradually forming Ti-O-Sr chemical bonds. The carbonate source decomposes slowly upon heating, stabilizing the microenvironment of the system and generating an in-situ strontium titanate SrTiO3 crystalline coating layer. This layer grows uniformly on the surface of the titanium dioxide particles, forming a dense and well-crystallized strontium titanate film.
[0031] In existing technologies, titanate films such as zinc titanate and magnesium titanate generally require the addition of titanium sources such as titanium oxychloride and titanium oxysulfate to react with zinc and magnesium salts. However, this application does not require the addition of titanium sources. It utilizes a high-temperature hydrothermal reaction to allow strontium salts to react with titanium dioxide itself in situ to generate strontium titanate, which can improve the adhesion of the film and the performance of titanium dioxide, while also simplifying the process.
[0032] More preferably, the soluble strontium source is added over 10-30 minutes, followed by homogenization for 10-30 minutes, and then a certain amount of buffer carbonate source is added. The pH of the slurry is then fine-tuned to 8.0-9.5 using a pH adjuster such as ammonia. The mixture is then reacted in a sealed environment at 160-200°C for 2-24 hours. Soluble strontium sources can include strontium nitrate, strontium chloride, strontium hydroxide, etc. Carbonate sources can include ammonium bicarbonate, urea, ammonium carbonate, etc.
[0033] More preferably, the amount of soluble strontium source added, based on strontium oxide, is 0.5 to 2% of the mass of the titanium dioxide substrate; and the amount of carbonic acid source added, based on carbonic acid, is 0.3 to 1% of the mass of the titanium dioxide substrate.
[0034] Preferably, the silica-alumina composite film is formed through the following steps: A soluble silica source is added to the slurry coated with a strontium titanate film. After aging, an acidic aluminum source is added, and the pH is controlled at 6-8 to allow silica and alumina to co-deposit.
[0035] As is generally known to those skilled in the art, conventional soluble silica sources such as sodium silicate and potassium silicate are alkaline, and the pH of their aqueous solutions is generally above 11. It is necessary to use acid to adjust the pH of the slurry to allow Si(OH)4 to deposit. In this application, acidic aluminum sources such as aluminum sulfate and aluminum chloride are used instead of pH adjusters, and the pH is controlled at 6 to 8, so that Si(OH)4 is deposited and aluminum oxide is deposited simultaneously, thereby forming a silicon oxide and aluminum oxide composite film.
[0036] Preferably, the lithium magnesium silicate film is formed by the following steps: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
[0037] More preferably, the lithium magnesium silicate sol is prepared by the following steps: Lithium magnesium silicate is added to hot water and stirred continuously until it swells fully to form a hydrogel. The solid content is controlled at 4-5%, and then allowed to stand and mature to obtain lithium magnesium silicate sol.
[0038] More preferably, the hot water temperature is 70~90℃, the stirring time is 90~150min, and the maturation time is 20~50min.
[0039] Commonly used organic coating methods in the prior art include dry coating and wet coating. Dry coating generally involves adding an organic modifier during the gas powder process. Gas powder is a routine step in preparing the finished product after coating. Adding an organic modifier to the gas powder allows the organic modifier to fully react and combine with the titanium dioxide using the high temperature of the gas powder.
[0040] Dry coating is simpler to operate than wet coating. This application preferably uses dry coating, in which betaine organic modifier containing hydroxyl and sulfonyl groups is added during the gas powder process. As mentioned above, the high temperature of the gas powder can fully combine the hydroxyl and sulfonyl groups in the organic modifier with the hydroxyl groups on the surface of the titanium dioxide, preventing them from falling off, so as to give full play to the role of the organic modifier.
[0041] As those skilled in the art will understand, when the coating amount is too small, the coating is easily incomplete and fails to achieve the desired coating effect. Conversely, when the coating amount is too large, it not only wastes resources but may also affect the original properties of the titanium dioxide. Therefore, preferably, the coating amount of the strontium titanate film, calculated based on strontium titanate, is 0.5% to 2% of the mass of the titanium dioxide substrate. In the silica-alumina composite film, the amount of silica coating is 2-4% of the mass of the titanium dioxide substrate; the amount of alumina coating is 1-3% of the mass of the titanium dioxide substrate. The coating amount of the lithium magnesium silicate film, based on lithium magnesium silicate, is 1-3% of the mass of the titanium dioxide substrate; The amount of betaine containing hydroxyl and sulfonyl groups in the coating is 0.2 to 0.6% of the mass of the titanium dioxide substrate.
[0042] This application also provides a method for preparing the high weather-resistant and high-flowability titanium dioxide as described above, comprising the following steps: S1. Preparation of titanium dioxide-based material slurry; S2. Perform strontium titanate coating; S3. Perform a composite coating of silica and alumina; S4. Perform lithium magnesium silicate coating; S5. Perform betaine organic coating containing hydroxyl and sulfonyl groups.
[0043] As those skilled in the art will understand, in the production of titanium dioxide, after inorganic coating, the inorganic salts introduced during the inorganic coating process are generally removed by pressure filtration and water washing, then dried to remove excess moisture from the filter cake, and then organic coating is performed.
[0044] Titanium dioxide-based material slurry can be prepared using conventional methods, with a preferred concentration of 250-500 g / L to facilitate coating. Simultaneously, to further promote coating, the inorganic coating temperature is preferably 50-80℃.
[0045] Preferably, step S2 further includes: Strontium source is added to titanium dioxide-based material slurry, followed by a certain amount of carbonic acid source, and the pH is adjusted to 8.0~8.5 to generate strontium carbonate precursor. Then, the mixture is reacted at 160~200℃ for 2~24h to generate strontium titanate precipitate in situ.
[0046] Soluble strontium sources can include strontium nitrate, strontium chloride, strontium hydroxide, etc. Carbonic acid sources can include ammonium bicarbonate, urea, ammonium carbonate, etc.
[0047] The amount of soluble strontium source added, based on strontium oxide, is 0.5-2% of the mass of the titanium dioxide substrate; the amount of carbonic acid source added, based on carbonic acid, is 0.3-1% of the mass of the titanium dioxide substrate.
[0048] To ensure a uniform reaction, the soluble strontium source is preferably added at a rate of 1-3 mL / min, with continuous stirring during the addition process and for 20-40 min after addition.
[0049] Preferably, step S3 further includes: A soluble silica source is added to the slurry coated with a strontium titanate film. After aging, an acidic aluminum source is added, and the pH is controlled at 6-8 to allow silica and alumina to co-deposit.
[0050] Preferably, the soluble silica source is selected from at least one of sodium silicate, potassium silicate, etc., and the acidic aluminum source is selected from at least one of aluminum sulfate, aluminum chloride, etc.
[0051] Preferably, the soluble silica source is added at a time of 20-40 minutes, followed by a 20-40 minute curing period; the acidic aluminum source is added at a time of 2-4 hours, followed by a 0.5-1.5 hour curing period.
[0052] The amount of soluble silica source added, calculated as silicon dioxide, is 2-4% of the mass of the titanium dioxide substrate; The amount of acidic aluminum source added, calculated as alumina, is 1 to 3% of the mass of the titanium dioxide substrate.
[0053] Preferably, step S4 further includes: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
[0054] Preferably, magnesium silicate sol is prepared by the following steps: Add lithium magnesium silicate powder to hot water and stir continuously until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 4-5% and then let it stand to mature, to obtain lithium magnesium silicate sol without particles or precipitates.
[0055] More preferably, the hot water temperature is 70~90℃, the stirring time is 90~150min, and the maturation time is 20~50min.
[0056] To ensure the pH stability of the slurry after the addition of lithium magnesium silicate sol, it is preferable to adjust the pH of the slurry to 8.0~10.5 before adding the lithium magnesium silicate sol. The lithium magnesium silicate sol is added over 1~3 hours, and then allowed to mature for 1~5 hours to stabilize the lithium magnesium silicate film.
[0057] The amount of magnesium lithium silicate sol added, calculated as magnesium lithium silicate, is 1 to 3% of the mass of the titanium dioxide substrate.
[0058] The pH adjuster in this application can be an inorganic acid or base such as sulfuric acid, hydrochloric acid, sodium hydroxide, potassium hydroxide, or ammonia.
[0059] Preferably, after inorganic coating, the pH of the slurry can be adjusted to 5-7 to meet the needs of downstream products.
[0060] Preferably, after drying, the product is steamed, and during the steaming process, a betaine organic modifier containing hydroxyl and sulfonyl groups is added to perform organic coating modification.
[0061] Preferably, the amount of betaine organic modifier containing hydroxyl and sulfonyl groups added is 0.2 to 0.6% of the mass of the titanium dioxide substrate.
[0062] Example 1 Preparation of lithium magnesium silicate sol: Add lithium magnesium silicate dry powder to hot water at 80℃ and stir continuously for 120 minutes until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 5%, and then let it stand for 30 minutes to obtain lithium magnesium silicate sol without particles or precipitates.
[0063] Take titanium dioxide sand grinding slurry, raise its temperature to 60℃, and adjust the slurry concentration to 300g / L; add strontium chloride solution (100g / L concentration) accounting for 1% of titanium dioxide mass fraction to the slurry, add ammonium bicarbonate solution (100g / L concentration) accounting for 0.5% of titanium dioxide mass fraction, and adjust the pH value to 8.0 with ammonia water, and mature at 180℃ for 6 hours.
[0064] A sodium silicate solution with a mass fraction of 2.5% of titanium dioxide was slowly added to the slurry over a period of 30 minutes, followed by aging for 30 minutes. An aluminum sulfate solution with a mass fraction of 3% of titanium dioxide was then slowly added to the slurry, with the pH controlled at 6. The addition was completed over 3 hours, followed by homogenization for 1 hour.
[0065] The solution pH was adjusted to 10.0, and magnesium lithium silicate sol and pH adjuster, accounting for 1% of the mass fraction of titanium dioxide, were added in parallel flow. The pH was maintained at 10.0 in parallel flow for 2 hours, and then the solution was allowed to mature for 2 hours.
[0066] To meet the needs of downstream products, the final pH was adjusted to 6.0.
[0067] The titanium dioxide product is obtained by pressure filtration, washing, drying, steaming, and adding lauryl hydroxysulfonate betaine at a mass fraction of 0.2% of titanium dioxide to the steamed powder.
[0068] Example 2 Preparation of lithium magnesium silicate sol: Add lithium magnesium silicate dry powder to hot water at 70℃ and stir continuously for 150 min until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 5%, and then let it stand for 50 min to obtain lithium magnesium silicate sol without particles or precipitates.
[0069] Take titanium dioxide sand grinding slurry, raise its temperature to 70℃, and adjust the slurry concentration to 300g / L; add 100g / L strontium chloride solution (0.5% by mass of titanium dioxide) and 100g / L ammonium bicarbonate solution (0.3% by mass) to the slurry, and adjust the pH value to 8.5 with ammonia water, and mature at 180℃ for 6 hours.
[0070] A sodium silicate solution with a mass fraction of 4% of titanium dioxide was slowly added to the slurry over a period of 30 minutes, followed by homogenization for 30 minutes. An aluminum sulfate solution with a mass fraction of 1% of titanium dioxide was then slowly added to the slurry, with the pH controlled at 7. The addition was completed over 3 hours, followed by homogenization for 1 hour.
[0071] Adjust the pH of the solution to 9.0, add 2% (by mass) lithium magnesium silicate and a pH adjuster in parallel flow, maintain the pH at 9.0 in parallel flow, add in parallel flow for 2 hours, and then let it mature for 2 hours.
[0072] The final pH was adjusted to 6.0.
[0073] The titanium dioxide product is obtained by pressure filtration, washing, drying, steaming, and adding cocamidopropyl hydroxysulfonate at a mass fraction of 0.4% of titanium dioxide to the steamed powder.
[0074] Example 3 Preparation of lithium magnesium silicate sol: Add lithium magnesium silicate dry powder to hot water at 90℃ and stir continuously for 90 minutes until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 4%, and then let it stand for 30 minutes to obtain lithium magnesium silicate sol without particles or precipitates.
[0075] Take titanium dioxide sand grinding slurry, raise its temperature to 80℃, and adjust the slurry concentration to 300g / L; add 100g / L strontium nitrate solution (0.5% by mass of titanium dioxide) and 100g / L ammonium bicarbonate solution (0.3% by mass) to the slurry, and adjust the pH value to 8.0 with ammonia water, and mature at 180℃ for 10h.
[0076] A sodium silicate solution with a mass fraction of 3% of titanium dioxide was slowly added to the slurry over 30 minutes, followed by homogenization for 30 minutes. An aluminum sulfate solution with a mass fraction of 2% of titanium dioxide was slowly added to the slurry, with the pH controlled at 7, over 3 hours, followed by homogenization for 1 hour.
[0077] The solution pH was adjusted to 10.5, and magnesium lithium silicate and pH adjuster were added in parallel flow at a mass fraction of 3% of titanium dioxide. The pH was maintained at 10.5 in parallel flow for 3 hours, followed by aging for 3 hours.
[0078] The final pH was adjusted to 6.0.
[0079] The titanium dioxide product is obtained by pressure filtration, washing, drying, steaming, and adding lauramidopropyl hydroxysulfonate at a mass fraction of 0.6% of titanium dioxide to the steamed powder.
[0080] Example 4 Preparation of lithium magnesium silicate sol: Add lithium magnesium silicate dry powder to hot water at 80℃ and stir continuously for 120 minutes until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 4%, and then let it stand for 30 minutes to obtain lithium magnesium silicate sol without particles or precipitates.
[0081] Take titanium dioxide sand grinding slurry, raise its temperature to 80℃, and adjust the slurry concentration to 300g / L; add 100g / L strontium nitrate solution (2% by mass of titanium dioxide) and 100g / L ammonium bicarbonate solution (0.5% by mass) to the slurry, and adjust the pH value to 8.5 with ammonia water, and mature at 200℃ for 10h.
[0082] A sodium silicate solution with a mass fraction of 2% of titanium dioxide was slowly added to the slurry for 20 minutes, followed by homogenization for 30 minutes. An aluminum sulfate solution with a mass fraction of 2% of titanium dioxide was slowly added to the slurry, with the pH controlled at 7. The addition was completed in 3 hours, followed by homogenization for 1 hour.
[0083] The solution pH was adjusted to 10.5, and magnesium lithium silicate and pH additives were added in parallel flow at a mass fraction of 3% of titanium dioxide. The pH was maintained at 10.5 in parallel flow for 2 hours, followed by aging for 3 hours.
[0084] The final pH was adjusted to 6.0.
[0085] The process involves pressure filtration, washing, drying, steaming, and adding lauramidopropyl hydroxysulfonate betaine at a mass fraction of 0.4% of titanium dioxide to the steamed powder to obtain the finished titanium dioxide product.
[0086] Comparative Example 1 (without a strontium titanate film compared to Example 4) Preparation of lithium magnesium silicate sol: Add lithium magnesium silicate dry powder to hot water at 80℃ and stir continuously for 120 minutes until it swells fully to form a transparent and slippery hydrogel. Control the solid content to 4%, and then let it stand for 30 minutes to obtain lithium magnesium silicate sol without particles or precipitates.
[0087] Take titanium dioxide sand grinding slurry, raise its temperature to 80℃, and adjust the slurry concentration to 300g / L; slowly add sodium silicate solution with a titanium dioxide mass fraction of 2% to the slurry for 20 minutes, and then homogenize for 30 minutes; slowly add aluminum sulfate solution with a titanium dioxide mass fraction of 2% to the slurry, control the pH to 7, complete the addition in 3 hours, and then homogenize for 1 hour.
[0088] The solution pH was adjusted to 10.5, and magnesium lithium silicate and pH additives were added in parallel flow at a mass fraction of 3% of titanium dioxide. The pH was maintained at 10.5 in parallel flow for 2 hours, followed by aging for 3 hours.
[0089] The final pH was adjusted to 6.0.
[0090] The process involves pressure filtration, washing, drying, steaming, and adding lauramidopropyl hydroxysulfonate betaine at a mass fraction of 0.4% of titanium dioxide to the steamed powder to obtain the finished titanium dioxide product.
[0091] Comparative Example 2 (compared to Example 4, without a lithium magnesium silicate film coating, and TMP was used instead of lauramidopropyl hydroxysulfonate betaine) Take titanium dioxide sand grinding slurry, raise its temperature to 80℃, and adjust the slurry concentration to 300g / L; add 100g / L strontium nitrate solution (2% by mass of titanium dioxide) and 100g / L ammonium bicarbonate solution (0.5% by mass) to the slurry, and adjust the pH value to 8.5 with ammonia water, and mature at 200℃ for 10h.
[0092] A sodium silicate solution with a mass fraction of 2% of titanium dioxide was slowly added to the slurry for 20 minutes, followed by homogenization for 30 minutes. An aluminum sulfate solution with a mass fraction of 2% of titanium dioxide was slowly added to the slurry, with the pH controlled at 7. The addition was completed in 3 hours, followed by homogenization for 1 hour.
[0093] The final pH was adjusted to 6.0.
[0094] The process involves pressure filtration, washing, drying, steaming, and adding TMP at a mass fraction of 0.6% of titanium dioxide to the steamed powder to obtain the finished titanium dioxide product.
[0095] Comparative Example 3 (Conventional Silicon-Aluminum Coating) Take titanium dioxide sand mill slurry, raise its temperature to 80℃, adjust the slurry concentration to 300g / L, and adjust the pH to 10.0; slowly add sodium silicate solution with a titanium dioxide mass fraction of 2.5% to the slurry, and homogenize for 30min; adjust the slurry pH to 6.0 with dilute sulfuric acid, complete the addition over 3h, and homogenize for 1h; then adjust the slurry pH to 8.0±0.2 with dilute alkali, and add aluminum aluminate solution with a titanium dioxide mass fraction of 1.5% and dilute sulfuric acid in parallel flow, maintaining the pH at 8.0 in parallel flow, complete the addition over 2h, and homogenize for 30min; filter, wash, flash dry, and add 0.6% TMP to obtain the finished titanium dioxide product.
[0096] Experimental results The application performance of the samples obtained in Examples 1-3 and the comparative examples was evaluated (dispersion test refers to GB / T6753.1-2007, and angle of repose test refers to GB / T 16913-2008), and the results are shown in Table 1.
[0097] Table 1
[0098] Based on the data from Examples 1-4 and Comparative Examples 2-3, the samples in Examples 1-4 coated with lithium magnesium silicate and hydroxysulfobetaine showed better flowability and dispersibility than the uncoated comparative samples. Furthermore, the more the amount of coating was added, the better the flowability and dispersibility, which is beneficial for improving the hiding power.
[0099] The samples obtained in Examples 1-4 and Comparative Examples 1-3 were subjected to a rapid xenon lamp aging test (the test method was as follows: titanium dioxide was prepared into a coating and applied to an aluminum plate, which was then placed in a xenon lamp aging chamber for accelerated aging. The aging conditions were light irradiation + hydrogen peroxide spraying, with a radiation intensity of 0.51 W / m²). 2 The blackboard temperature was 50℃, the chamber temperature was 30℃, and the time was 50 minutes. The cycle was 50 minutes of light / spray exposure followed by 60 minutes of darkness. The test was conducted to determine the change in 60° light retention rate (%) over time. The test results are as follows: Figure 1 As shown.
[0100] Based on the data from Examples 1-4 and Comparative Examples 1 and 3, the weather resistance of the samples coated with strontium titanate in Examples 1-3 was better than that of the uncoated samples in the comparative examples, and the greater the amount of strontium titanate coating in Example 4, the better the weather resistance.
[0101] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention. Clearly, those skilled in the art can make various alterations and modifications to the invention without departing from its spirit and scope. Thus, if these modifications and modifications of the invention fall within the scope of the claims and their equivalents, the invention is also intended to include these modifications and modifications.
Claims
1. A high weather resistance high fluidity titanium white pigment, characterized by, From the inside out, it consists of a titanium dioxide substrate, an inorganic coating layer, and an organic coating layer. The inorganic coating layer, from the inside out, includes a strontium titanate film layer, a silicon oxide-alumina composite film layer, and a lithium magnesium silicate film layer. The organic coating layer is a membrane obtained by organic modification treatment using betaine containing hydroxyl and sulfonyl groups.
2. The high weather-resistant and high-flowability titanium dioxide as described in claim 1, characterized in that, The betaine containing hydroxyl and sulfonyl groups is selected from at least one of lauryl hydroxysulfonyl betaine, cocamidopropyl hydroxysulfonyl betaine, lauramide propyl hydroxysulfonyl betaine, or octadecyl dimethyl hydroxypropyl sulfonyl betaine.
3. The high weather-resistant and high-flowability titanium dioxide as described in claim 1, characterized in that, The strontium titanate film layer is formed through the following steps: Strontium source and carbonic acid source are added to titanium dioxide-based material slurry, and the pH is adjusted to 8.0~8.5 to generate strontium carbonate precursor. Then, the mixture is reacted at 160~200℃ for 2~24h to generate strontium titanate precipitate in situ.
4. The high weather-resistant and high-flowability titanium dioxide as described in claim 1, characterized in that, The lithium magnesium silicate film is formed through the following steps: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
5. The high weather-resistant and high-flowability titanium dioxide as described in claim 1, characterized in that, The coating amount of the strontium titanate film, calculated as strontium titanate, is 0.5% to 2% of the mass of the titanium dioxide substrate. In the silicon oxide-alumina composite film, the amount of silicon oxide coating is 2-4% of the mass of the titanium dioxide substrate; The amount of alumina coating is 1-3% of the mass of the titanium dioxide substrate; The coating amount of the lithium magnesium silicate film, calculated based on lithium magnesium silicate, is 1-3% of the mass of the titanium dioxide substrate. The amount of betaine containing hydroxyl and sulfonyl groups in the coating is 0.2 to 0.6% of the mass of the titanium dioxide substrate.
6. A method for producing the high-weatherability high-fluidity titanium white pigment according to any one of claims 1 to 5, characterized by, Includes the following steps: S1. Preparation of titanium dioxide-based material slurry; S2. Perform strontium titanate coating; S3. Perform a composite coating of silica and alumina; S4. Perform lithium magnesium silicate coating; S5. Perform betaine organic coating containing hydroxyl and sulfonyl groups.
7. The method for preparing high weather-resistant and high-flowability titanium dioxide as described in claim 6, characterized in that, Step S2 further includes: A strontium source is added to the titanium dioxide-based material slurry, followed by a certain amount of carbonic acid source, and the pH is adjusted to 8.0-8.5 to generate a strontium carbonate precursor. The slurry is then reacted at 160-200°C for 2-24 hours. The amount of the soluble strontium source added, based on strontium oxide, is 0.5-2% of the mass of the titanium dioxide substrate; The amount of the added carbonic acid source, calculated as carbonic acid, is 0.3 to 1% of the mass of the titanium dioxide substrate.
8. The method for preparing high weather-resistant and high-flowability titanium dioxide as described in claim 6, characterized in that, Step S3 further includes: A soluble silica source is added to the slurry coated with a strontium titanate film. After aging, an acidic aluminum source is added, and the pH is controlled at 6-8 to allow silica and alumina to co-deposit.
9. The method for preparing high weather-resistant and high-flowability titanium dioxide as described in claim 6, characterized in that, Step S4 further includes: Magnesium silicate lithium sol and pH adjuster are added concurrently to the slurry coated with strontium titanate film and silica-alumina composite film to maintain the concurrent pH at 8.0~10.5, so as to allow magnesium silicate lithium to deposit.
10. The method for preparing high weather-resistant and high-flowability titanium dioxide as described in claim 9, characterized in that, The lithium magnesium silicate sol was prepared through the following steps: Lithium magnesium silicate is added to hot water and stirred continuously until it swells fully to form a hydrogel. The solid content is controlled at 4-5%, and then allowed to stand and mature to obtain the lithium magnesium silicate sol.