A method for purifying high-structure carbon black

By employing a liquid-phase oxidation and gas-phase media mixing process, the problems of deep impurity removal and structural protection of high-structure carbon black have been solved, achieving an efficient and environmentally friendly purification method suitable for industrial production.

CN123107420APending Publication Date: 2026-11-17HUNAN CHENYU FUJI NEW ENERGY TECHNOLOGY CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611197368.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for purifying high-structure carbon black suffer from problems such as incomplete deep impurity removal, inability to balance purification and structure protection, cumbersome procedures, and numerous byproducts.

Method used

Liquid-phase moderate oxidation is used to open the gaps in carbon black aggregates. Combined with a gaseous medium of hydrogen chloride gas and water vapor, deep purification and structural regulation are carried out under moderate etching conditions, including liquid-phase oxidation reaction and gas thermal reaction.

Benefits of technology

It achieves deep impurity removal and complete removal of metallic impurities, retains the original properties of high-structure carbon black, shortens the production cycle, reduces wastewater discharge, and lowers chlorine residue, making it suitable for continuous industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for purifying high-structure carbon black, comprising the following steps: mixing high-structure carbon black with an oxidizing liquid for liquid-phase oxidation to obtain oxidized carbon black; placing the oxidized carbon black in a reactor, introducing a mixed gas for gas-thermal reaction and post-treatment to obtain high-purity high-structure carbon black, wherein the mixed gas includes nitrogen, hydrogen chloride gas, and water vapor. The high-structure carbon black purification method provided by this invention first opens the gaps in the carbon black aggregates and exposes the internally encapsulated metallic impurities through moderate liquid-phase oxidation, and then simultaneously completes deep purification and structure regulation under moderate etching conditions using a mixed gaseous medium of hydrogen chloride gas and water vapor. The process is simplified, impurity removal is thorough, and the original high structure of the carbon black can be preserved to the greatest extent, with low chlorine residue, making it suitable for continuous industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon material processing technology, and in particular to a method for purifying high-structure carbon black. Background Technology

[0002] High-structure carbon black, due to its well-developed chain-like and dendritic aggregate structure, possesses excellent oil absorption, electrical conductivity, and reinforcing properties, making it a core raw material for high-end rubber, conductive agents for lithium-ion batteries, and functional coatings. During the production process of industrial virgin high-structure carbon black, the internal components and intercrystalline gaps are affected by raw oil, the reactor body, and production aids, resulting in the inclusion of a large number of metallic impurities such as iron, copper, calcium, magnesium, and aluminum. These metallic impurities severely degrade the conductive stability, electrochemical cycle life, and aging resistance of the carbon black products.

[0003] Currently, the mainstream impurity removal processes in the industry fall into two categories. Liquid-phase strong acid immersion / reflux pickling can only remove surface and shallow impurities from carbon black, making it difficult to remove metals deeply embedded in the carbon matrix. Furthermore, prolonged liquid-phase pickling weakens the neck points of carbon black aggregates, causing a slight decrease in structure and resulting in high wastewater treatment pressure. Single high-temperature steam etching or single gas-phase chlorination purification can only etch amorphous carbon and expand pores, with weak impurity removal capabilities. Single high-temperature hydrogen chloride gas is highly corrosive and easily over-etches the weak neck points of high-structure carbon black, leading to aggregate breakage, structural collapse, loss of high-structure core performance, and the generation of large amounts of residual chlorine. Therefore, existing technologies generally suffer from incomplete deep impurity removal, an inability to balance purification and structural protection, cumbersome processes, and numerous byproducts.

[0004] Therefore, there is an urgent need to develop a new integrated process that can simultaneously achieve deep impurity removal, medium etching, and maximum preservation of the original high structure. Summary of the Invention

[0005] In view of the above-mentioned shortcomings in the current high-structure carbon black purification methods, the present invention provides a high-structure carbon black purification method. First, the gaps in the carbon black aggregates are opened by liquid-phase moderate oxidation to expose the internal encapsulated metallic impurities. Then, deep purification and structure regulation are simultaneously completed under moderate etching conditions using a mixed gaseous medium of hydrogen chloride gas and water vapor. The process is simplified, impurities are thoroughly removed, the original high structure of carbon black is preserved to the greatest extent, chlorine residue is low, and it is suitable for continuous industrial production.

[0006] To achieve the above objectives, the embodiments of the present invention adopt the following technical solutions:

[0007] A method for purifying high-structure carbon black includes the following steps:

[0008] High-structure carbon black is mixed with an oxidizing liquid and subjected to a liquid-phase oxidation reaction to obtain oxidized modified carbon black.

[0009] Oxidized modified carbon black is placed in a reactor, and a mixed gas is introduced for gas-thermal reaction and post-treatment to obtain high-purity, high-structure carbon black. The mixed gas includes nitrogen, hydrogen chloride gas, and water vapor.

[0010] According to one aspect of the invention, the oxidizing solution is an aqueous nitric acid solution with a molar concentration of 3 to 4 mol / L. Preferably, the molar concentration of the aqueous nitric acid solution is 3 mol / L.

[0011] According to one aspect of the invention, the mass ratio of the oxidizing liquid to the high-structure carbon black is (7-9):1.

[0012] According to one aspect of the present invention, the reaction temperature of the liquid-phase oxidation reaction is 120–125°C, and the reaction time is 1.8–2.2 h. Preferably, the reaction temperature is 125°C.

[0013] According to one aspect of the present invention, the liquid-phase oxidation reaction further includes natural cooling, solid-liquid separation to obtain filter cake and filtrate, washing the filter cake with deionized water until the pH of the washing liquid is 6-7, and placing the filter cake in an oven to dry at 120°C to constant weight.

[0014] According to one aspect of the present invention, the oxygen content in the oxidized modified carbon black is 5-7 wt%, the weight loss rate is 10-15%, and the DBP oil absorption value decreases by ≤10%.

[0015] According to one aspect of the invention, the volume concentration of hydrogen chloride in the mixed gas is 5-10%, and the volume concentration of water vapor is 20-30%.

[0016] According to one aspect of the present invention, the gas-thermal reaction temperature is 750–850°C, and the reaction time is 60–90 min. The nitrogen gas has a purity of ≥99.9%.

[0017] According to one aspect of the present invention, the volume concentration of hydrogen chloride in the gas-thermal reaction is 8%, the volume concentration of water vapor is 25%, the reaction temperature is 800°C, and the reaction is carried out at a constant temperature for 75 min.

[0018] According to one aspect of the present invention, the post-processing includes: after the gas-thermal reaction is completed, stopping the flow of hydrogen chloride and water vapor, and only maintaining the continuous flow of high-purity nitrogen; purging with nitrogen for 28-32 minutes to remove free chlorine and acidic gaseous residues adsorbed on the surface of carbon black; and naturally cooling to room temperature under a nitrogen protective atmosphere to obtain the finished high-purity, high-structure carbon black.

[0019] A high-structure carbon black is obtained by purification using the high-structure carbon black purification method. The high-structure carbon black has a metal impurity content of less than 50 ppm, a structure retention rate of greater than or equal to 85%, and a chlorine residue of less than 35 ppm.

[0020] Advantages of implementing this invention:

[0021] 1. High impurity removal depth, thorough removal of impurities.

[0022] First, the closed pores inside the carbon black are opened by moderate oxidation, so that the metal impurities that were originally wrapped by the carbon layer are fully exposed. Then, the metal oxides are converted into volatile chlorides and carried out by a high-temperature hydrogen chloride gas phase system. The total metal impurity content can be reduced to below 50 ppm, achieving deep metal impurity removal, which is far superior to the traditional liquid phase acid washing process.

[0023] 2. Balancing moderate etching with high structure preservation

[0024] A gas-phase system combining hydrogen chloride and water vapor is employed. The water vapor buffers the strong corrosive effect of hydrogen chloride, preventing excessive etching and breakage of the fine aggregate necks of high-structure carbon black. The finished carbon black's DBP oil absorption value can be maintained at over 85%–90% of the original raw material, without overall structural collapse, fully preserving the chain-like and dendritic morphology of the high-structure carbon black. Simultaneously, the water vapor selectively etches amorphous carbon on the carbon black surface, repairs carbon defects caused by oxidation, and moderately enlarges pores, while buffering the strong corrosive effect of hydrogen chloride on the carbon black aggregate necks, protecting the high-structure carbon black.

[0025] 3. Integrated processes and streamlined workflow

[0026] The traditional two separate processes of acid pickling and water vapor etching are combined into a single gas phase reaction, shortening the production cycle. The entire process is based on gas phase reaction, which greatly reduces the discharge of acidic wastewater, making it more environmentally friendly and suitable for industrial continuous production.

[0027] 4. Low chlorine residue, wide product applicability

[0028] After the reaction, a long-term purging with high-purity nitrogen can effectively remove the adsorbed chlorine from the surface, resulting in a low chlorine residue in the finished product. This will not have a negative impact on conductivity, energy storage, or rubber products, and will broaden the application scenarios.

[0029] 5. Strong process controllability

[0030] The oxidation concentration, gas phase component ratio, reaction temperature, and time are all controllable parameters within a narrow range, resulting in good process stability and uniform performance of batch products. Detailed Implementation

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] A method for purifying high-structure carbon black includes the following steps:

[0033] High-structure carbon black is mixed with an oxidizing liquid and subjected to a liquid-phase oxidation reaction to obtain oxidized modified carbon black.

[0034] Oxidized modified carbon black is placed in a reactor, and a mixed gas is introduced for gas-thermal reaction and post-treatment to obtain high-purity, high-structure carbon black. The mixed gas includes nitrogen, hydrogen chloride gas and water vapor, with nitrogen serving as the carrier gas.

[0035] In practical applications, the oxidizing solution is an aqueous nitric acid solution with a molar concentration of 3–4 mol / L. Preferably, the molar concentration of the aqueous nitric acid solution is 3 mol / L. Using a dilute nitric acid system for oxidation allows for control of the oxidation intensity, etching only the edges of carbon black microcrystals and the gaps between aggregates without damaging the main framework.

[0036] In practical applications, the mass ratio of the oxidizing liquid to the high-structure carbon black is (7-9):1. Preferably, the mass ratio of the oxidizing liquid to the high-structure carbon black is 8:1.

[0037] In practical applications, the high-structure carbon black is pretreated before being mixed with the oxidizing liquid. Specifically, the pretreatment includes passing the high-structure carbon black through an 80-120 mesh sieve to remove large agglomerated particles.

[0038] In practical applications, the reflux ratio in the liquid-phase oxidation reaction is controlled at (1.0-1.5):1, the reaction temperature is 120-125℃, and the reaction time is 1.8-2.2 h. Preferably, the reaction temperature is 125℃ and the reaction time is 2 h.

[0039] In practical applications, the liquid-phase oxidation reaction is followed by natural cooling and separation of the reaction solution to obtain a filter cake and a filtrate. The filter cake is washed with deionized water until the pH of the washing solution is 6-7, and then dried in an oven at 120°C to a constant weight.

[0040] In practical applications, the oxygen content in the oxidized modified carbon black is 5-7 wt%, the weight loss rate is 10-15%, and the DBP oil absorption value decreases by ≤10%.

[0041] In practical applications, the volume concentration of hydrogen chloride in the mixed gas is 5-10%, the volume concentration of water vapor is 20-30%, and the remainder is nitrogen, wherein the purity of the nitrogen is ≥99.9%.

[0042] In practical applications, the reaction temperature in the gas-thermal reaction is 750–850℃, and the reaction time is 60–90 min. Through gas-thermal reaction treatment, deep removal of metal impurities and moderate etching of carbon black can be achieved, along with structural strengthening.

[0043] Preferably, the volume concentration of hydrogen chloride in the gas-thermal reaction is 8%, the volume concentration of water vapor is 25%, the reaction temperature is 800℃, and the reaction is carried out at a constant temperature for 75 minutes.

[0044] In practical applications, the post-processing includes: after the gas-thermal reaction is completed, stopping the flow of hydrogen chloride and water vapor, and only maintaining the continuous flow of high-purity nitrogen; purging with nitrogen for 28-32 minutes to remove free chlorine and acidic gaseous residues adsorbed on the carbon black surface; and naturally and slowly cooling to room temperature under a nitrogen protective atmosphere to obtain the finished high-purity, high-structure carbon black.

[0045] In practical applications, the reactor is a high-temperature corrosion-resistant tubular reactor, and the material of the high-temperature corrosion-resistant tubular reactor is quartz or corundum.

[0046] A high-structure carbon black is obtained by purification using the high-structure carbon black purification method. The high-structure carbon black has a metal impurity content of less than 50 ppm, a structure retention rate of greater than or equal to 85%, and a chlorine residue of less than 35 ppm.

[0047] Example 1

[0048] A method for purifying high-structure carbon black includes the following steps:

[0049] S1: Raw material pretreatment

[0050] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 100-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0051] S2: Liquid phase oxidation treatment

[0052] 100g of pretreated high-structure carbon black was mixed with 800g of 3mol / L nitric acid solution and refluxed at 125℃ for 2 h for liquid-phase oxidation. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black. The oxidized modified carbon black had an oxygen content of 6.2 wt%, a weight loss of 12.3%, and a DBP of 118 mL / 100g.

[0053] S3: Gas-thermal reaction treatment

[0054] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen gas with a purity of 99.9% was used as the carrier gas. A mixed gaseous medium of hydrogen chloride gas with a volume concentration of 8% and water vapor with a volume concentration of 25% was introduced. The temperature was increased to 800℃ at a heating rate of 5℃ / min and the reaction was carried out at a constant temperature for 75min.

[0055] S4: Post-processing

[0056] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0057] Test results of finished high-purity, high-structure carbon black:

[0058] The total metal impurities were 32 ppm, the DBP oil absorption value was 114 mL / 100g, and the chlorine residue was 28 ppm. The high-purity, high-structure carbon black had a complete structure and no aggregate breakage or collapse.

[0059] Example 2

[0060] A method for purifying high-structure carbon black includes the following steps:

[0061] S1: Raw material pretreatment

[0062] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through an 80-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0063] S2: Liquid phase oxidation treatment

[0064] 100g of pretreated high-structure carbon black was mixed with 800g of 4mol / L nitric acid solution and refluxed at 120℃ for 2 h for liquid-phase oxidation reaction. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black.

[0065] S3: Gas-thermal reaction treatment

[0066] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen gas with a purity of 99.9% was used as the carrier gas. A mixed gaseous medium of hydrogen chloride gas with a volume concentration of 10% and water vapor with a volume concentration of 30% was introduced. The temperature was raised to 850℃ at a heating rate of 5℃ / min and the reaction was carried out at a constant temperature for 60min.

[0067] S4: Post-processing

[0068] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0069] Finished product test results:

[0070] The total metal impurities were 41 ppm, the DBP oil absorption value was 109 mL / 100g, and the chlorine residue was 35 ppm. The high-purity, high-structure carbon black had a complete structure and no aggregate breakage or collapse.

[0071] Example 3

[0072] A method for purifying high-structure carbon black includes the following steps:

[0073] S1: Raw material pretreatment

[0074] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 120-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0075] S2: Liquid phase oxidation treatment

[0076] 100g of pretreated high-structure carbon black was mixed with 800g of 4mol / L nitric acid solution and refluxed at 125℃ for 2.2 h for liquid-phase oxidation reaction. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black.

[0077] S3: Gas-thermal reaction treatment

[0078] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen with a purity of 99.9% was used as the carrier gas, and a mixed gaseous medium of hydrogen chloride gas with a volume concentration of 5% and water vapor with a volume concentration of 20% was introduced. The temperature was increased to 750℃ at a heating rate of 5℃ / min, and the reaction was carried out at a constant temperature for 90min.

[0079] S4: Post-processing

[0080] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0081] Finished product test results: total metal impurities xx ppm, DBP oil absorption value xx mL / 100g, chlorine residue xx ppm.

[0082] Comparative Example 1

[0083] A method for purifying high-structure carbon black includes the following steps:

[0084] S1: Raw material pretreatment

[0085] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 100-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0086] S2: Liquid phase oxidation treatment

[0087] 100g of pretreated high-structure carbon black was mixed with 800g of 3mol / L nitric acid solution and refluxed at 125℃ for 2 h for liquid-phase oxidation. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain high-structure carbon black.

[0088] Test results:

[0089] The high-structure carbon black was tested and found to have a total metal impurity content of 216 ppm and a DBP oil absorption value of 82 mL / 100g, indicating that the removal of deep impurities did not meet the standards.

[0090] Comparative Example 2

[0091] A method for purifying high-structure carbon black includes the following steps:

[0092] S1: Raw material pretreatment

[0093] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 100-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0094] S2: Liquid phase oxidation treatment

[0095] 100g of pretreated high-structure carbon black was mixed with 800g of 3mol / L nitric acid solution and refluxed at 125℃ for 2 h for liquid-phase oxidation reaction. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black.

[0096] S3: Gas-thermal reaction treatment

[0097] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen gas with a purity of 99.9% was used as the carrier gas, and hydrogen chloride gas with a volume concentration of 33% was introduced. The temperature was raised to 800℃ at a heating rate of 5℃ / min and kept at a constant temperature for 75min to achieve deep removal of metal impurities and moderate etching and structural strengthening of carbon black.

[0098] S4: Post-processing

[0099] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0100] Test results: Total metal impurities 29 ppm, but DBP oil absorption value dropped to 82 mL / 100g, indicating severe structural collapse.

[0101] Comparative Example 3

[0102] A method for purifying high-structure carbon black includes the following steps:

[0103] S1: Raw material pretreatment

[0104] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 100-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0105] S2: Liquid phase oxidation treatment

[0106] 100g of pretreated high-structure carbon black was mixed with 800g of 3mol / L nitric acid solution and refluxed at 125℃ for 2 h for liquid-phase oxidation reaction. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black.

[0107] S3: Gas-thermal reaction treatment

[0108] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen with a purity of 99.9% was used as the carrier gas, and water vapor with a volume concentration of 33% was introduced. The temperature was raised to 800℃ at a rate of 5℃ / min and kept at a constant temperature for 75min to achieve deep removal of metal impurities and moderate etching and structural strengthening of carbon black.

[0109] S4: Post-processing

[0110] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0111] Test results: Total metal impurities 209ppm, DBP oil absorption value 63mL / 100g, structure not repaired, deep impurity removal not up to standard.

[0112] Comparative Example 4

[0113] A method for purifying high-structure carbon black includes the following steps:

[0114] S1: Raw material pretreatment

[0115] The virgin high-structure carbon black with a DBP oil absorption value of 126 mL / 100 g and a total metal impurity content of 860 ppm was passed through a 100-mesh sieve to remove large agglomerated particles, thus obtaining pretreated high-structure carbon black.

[0116] S2: Liquid phase oxidation treatment

[0117] 100g of pretreated high-structure carbon black was mixed with 800g of 5mol / L nitric acid solution and refluxed at 120℃ for 2 h for liquid-phase oxidation reaction. After the oxidation reaction was completed, the mixture was allowed to cool naturally and the carbon black filter cake was repeatedly washed with deionized water until the pH of the washing solution was 7. The filter cake was then placed in an oven and dried at 120℃ to constant weight to obtain oxidized modified carbon black.

[0118] S3: Gas-thermal reaction treatment

[0119] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen gas with a purity of 99.9% was used as the carrier gas. A mixed gaseous medium of hydrogen chloride gas with a volume concentration of 10% and water vapor with a volume concentration of 30% was introduced. The temperature was raised to 850℃ at a heating rate of 5℃ / min and the reaction was carried out at a constant temperature for 60min.

[0120] S4: Post-processing

[0121] After the isothermal reaction is completed, the flow of hydrogen chloride and water vapor is stopped, and only high-purity nitrogen is continuously introduced. The nitrogen purging time is 30 minutes. Under the nitrogen protective atmosphere, the mixture is naturally cooled to room temperature and discharged to obtain the finished high-purity, high-structure carbon black.

[0122] Finished product test results: total metal impurities 38 ppm, DBP oil absorption value 89 mL / 100g, chlorine residue 31 ppm.

[0123] Comparative Example 5

[0124] The only difference between Comparative Example 5 and Example 1 is that the gas-phase reaction treatment in Comparative Example 5 is different in S3; all other aspects are the same. Specifically, the gas-phase reaction treatment in Comparative Example 5 in S3 is as follows:

[0125] S3: Gas-thermal reaction treatment

[0126] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen with a purity of 99.9% was used as the carrier gas, and a mixed gaseous medium of hydrogen chloride gas with a volume concentration of 15% and water vapor with a volume concentration of 25% was introduced. The temperature was increased to 800℃ at a heating rate of 5℃ / min and the reaction was maintained at a constant temperature for 75min to achieve deep removal of metal impurities and moderate etching and structural strengthening of carbon black.

[0127] Finished product test results:

[0128] Total metal impurities: 15 ppm; DBP oil absorption value: 95 mL / 100g; chlorine residue: 60 ppm.

[0129] Comparative Example 6

[0130] The only difference between Comparative Example 6 and Example 1 is that the gas-phase reaction treatment in Comparative Example 6 is different in S3; all other aspects are the same. Specifically, the gas-phase reaction treatment in Comparative Example 6 in S3 is as follows:

[0131] S3: Gas-thermal reaction treatment

[0132] The dried oxidized carbon black was placed in a high-temperature and corrosion-resistant tubular reactor. Nitrogen gas with a purity of 99.9% was used as the carrier gas. A mixed gaseous medium of hydrogen chloride gas with a volume concentration of 8% and water vapor with a volume concentration of 35% was introduced. The temperature was increased to 800℃ at a heating rate of 5℃ / min and the reaction was carried out at a constant temperature for 75min.

[0133] Finished product test results: total metal impurities 32 ppm, DBP oil absorption value 98 mL / 100g, chlorine residue 40 ppm, significant material loss, yield 63%.

[0134] Comparative Example 7

[0135] The only difference between Comparative Example 7 and Example 1 is that the reaction temperature in S3: gas phase reaction treatment in Comparative Example 7 is 1000°C, and all other conditions are the same.

[0136] Finished product test results: total metal impurities 20ppm, DBP oil absorption value 62mL / 100g, chlorine residue 32ppm, significant material loss, yield only 43%.

[0137] Advantages of implementing this invention:

[0138] 1. High impurity removal depth, thorough removal of impurities.

[0139] First, moderate oxidation is used to open up the closed pores inside the carbon black, so that the metal impurities that were originally wrapped by the carbon layer are fully exposed. Then, a high-temperature hydrogen chloride gas phase system is used to convert the metal oxides into volatile chlorides and carry them out. The total metal impurity content can be reduced to below 50 ppm, achieving deep metal impurity removal, which is far superior to the traditional liquid phase acid washing process.

[0140] 2. Balancing moderate etching with high structure preservation

[0141] A gas-phase system combining hydrogen chloride and water vapor is employed. The water vapor buffers the strong corrosive effect of hydrogen chloride, preventing excessive etching and breakage of the fine aggregate necks of high-structure carbon black. The finished carbon black's DBP oil absorption value can be maintained at over 85%–90% of the original raw material, without overall structural collapse, fully preserving the chain-like and dendritic morphology of the high-structure carbon black. Simultaneously, the water vapor selectively etches amorphous carbon on the carbon black surface, repairs carbon defects caused by oxidation, and moderately enlarges pores, while buffering the strong corrosive effect of hydrogen chloride on the carbon black aggregate necks, protecting the high-structure carbon black.

[0142] 3. Integrated processes and streamlined workflow

[0143] The traditional two separate processes of acid pickling and water vapor etching are combined into a single gas phase reaction, shortening the production cycle. The entire process is based on gas phase reaction, which greatly reduces the discharge of acidic wastewater, making it more environmentally friendly and suitable for industrial continuous production.

[0144] 4. Low chlorine residue, wide product applicability

[0145] After the reaction, a long-term purging with high-purity nitrogen can effectively remove the adsorbed chlorine from the surface, resulting in a low chlorine residue in the finished product. This will not have a negative impact on conductivity, energy storage, or rubber products, and will broaden the application scenarios.

[0146] 5. Strong process controllability

[0147] The oxidation concentration, gas phase component ratio, reaction temperature, and time are all controllable parameters within a narrow range, resulting in good process stability and uniform performance of batch products.

[0148] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for purifying high-structure carbon black, characterized in that, Includes the following steps: High-structure carbon black is mixed with an oxidizing liquid and subjected to a liquid-phase oxidation reaction to obtain oxidized modified carbon black. Oxidized modified carbon black is placed in a reactor, and a mixed gas is introduced for gas-thermal reaction and post-treatment to obtain high-purity, high-structure carbon black. The mixed gas includes nitrogen, hydrogen chloride gas, and water vapor.

2. The method for purifying high-structure carbon black according to claim 1, characterized in that, The oxidizing solution is an aqueous nitric acid solution with a molar concentration of 3–4 mol / L.

3. The method for purifying high-structure carbon black according to claim 1, characterized in that, The mass ratio of the oxidizing liquid to the high-structure carbon black is (7-9):

1.

4. The method for purifying high-structure carbon black according to claim 1, characterized in that, The reaction temperature of the liquid-phase oxidation reaction is 120–125°C, and the reaction time is 1.8–2.2 h.

5. The method for purifying high-structure carbon black according to claim 1, characterized in that, The oxidized modified carbon black has an oxygen content of 5-7 wt%, a weight loss rate of 10-15%, and a DBP oil absorption value decrease of ≤10%.

6. The method for purifying high-structure carbon black according to claim 1, characterized in that, The volume concentration of hydrogen chloride in the mixed gas is 5-10%, and the volume concentration of water vapor is 20-30%.

7. The method for purifying high-structure carbon black according to claim 1, characterized in that, The volume concentration of hydrogen chloride is 8%, and the volume concentration of water vapor is 25%.

8. The method for purifying high-structure carbon black according to claim 1, characterized in that, The gas-thermal reaction is carried out at a temperature of 750–850°C for 60–90 minutes.

9. The method for purifying high-structure carbon black according to claim 1, characterized in that, The gas-thermal reaction was carried out at a temperature of 800°C for 75 minutes.

10. The method for purifying high-structure carbon black according to claim 1, characterized in that, The post-treatment includes purging with nitrogen for 28–32 minutes.