A silicate-modified coating and its preparation method, and its application in the reinforcement of coal mine roof slabs.
By surface activation and coupling agent bridging modification of mica functional fillers, an organic-inorganic interpenetrating network structure is formed, which solves the problems of high brittleness and insufficient adhesion of silicate materials in the reinforcement of coal mine roof slabs. This enables the application of coatings with high strength, high toughness and good water resistance, ensuring safe production in underground coal mines.
Patent Information
- Application Number
- CN202611517247.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, silicate materials have problems such as high brittleness, high shrinkage rate after curing, insufficient adhesion to the substrate and poor water resistance in the reinforcement of coal mine roof slabs. They are difficult to meet the long-term and stable reinforcement requirements, and traditional modification methods have failed to effectively improve the interfacial bonding force and overall performance.
By surface activation and coupling agent bridging modification of mica functional fillers, bridging modified mica is formed. During in-situ co-condensation, it forms a tight organic-inorganic interpenetrating network structure with silicate mother liquor, thereby enhancing interfacial bonding and overall performance.
It significantly improves the coating's high strength, high toughness, excellent adhesion, and good water resistance. It can quickly cure to form a dense inorganic reinforcement layer, effectively sealing cracks and improving the roof's load-bearing capacity and weathering resistance. It is suitable for efficient downhole reinforcement operations.
Smart Images

Figure CN123107430A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicate modified coatings, and more specifically, to a silicate modified coating and its preparation method, as well as its application in the reinforcement of coal mine roof slabs. The invention relates to a method for preparing a silicate modified coating using alkali metal silicates as film-forming materials and mica functional fillers as reinforcing phases. Background Technology
[0002] In coal mining, roof stability is one of the core elements for ensuring safe production. With increasing mining depth and more complex geological conditions, roof strata often develop numerous fissures due to stress release and tectonic movements, leading to reduced rock mass strength and increasing the risk of delamination, collapse, and other safety accidents. Currently, common techniques for reinforcing coal mine roofs include rock bolt support, shotcrete, and various chemical grouting materials. However, traditional reinforcement methods still have many limitations in practical applications.
[0003] On the one hand, while cement-based grouting materials are relatively inexpensive, their adhesion to coal and rock masses is limited, their shrinkage rate is high, and their setting time is long, making it difficult to quickly and effectively seal micro-cracks and restore the integrity of the rock mass. On the other hand, while chemical grouting materials, represented by organic polymer materials (such as polyurethane and epoxy resin), have high strength and good adhesion, they are expensive, have complex construction processes, and some materials pose aging, flammability, and environmental risks in the high-temperature and high-humidity environment underground, limiting their widespread application in coal mines.
[0004] Silicate materials, especially alkali metal silicates (such as water glass), exhibit unique application potential in mine reinforcement due to their wide availability, low cost, non-toxicity, odorless nature, good permeability, and inorganic properties. However, unmodified silicate materials inherently possess defects such as high brittleness, high post-curing shrinkage, insufficient adhesion to the substrate, and poor water resistance. Relying solely on their film-forming or bonding abilities is insufficient to meet the long-term, stable reinforcement requirements of coal mine roofs. In particular, when silicate materials are directly applied to damp or impurity-containing rock surfaces, their cured products are prone to cracking due to internal stress concentration or delamination failure due to poor chemical compatibility with the substrate.
[0005] To overcome the aforementioned problems, existing technologies attempt to modify silicates by introducing organic polymers or inorganic fillers. For example, flake-like fillers such as common mica powder are directly incorporated into water glass, aiming to improve the crack resistance and water resistance of the coating by utilizing its physical barrier effect. However, simple physical mixing often results in weak interfacial bonding due to the lack of effective chemical bonding between the filler and the matrix. The filler only acts as an inert filler and cannot fully realize its reinforcing and toughening potential. It may even become a stress concentration point due to interfacial defects, thereby reducing the overall performance of the material. In addition, some studies have used silane coupling agents to modify silicate systems alone. However, when using silane coupling agents alone, their crosslinking density with the silicate network is limited, and they lack the multi-dimensional barrier and reinforcing effect of flake-like fillers, resulting in less than ideal improvement in the overall mechanical properties and durability of the coating. Summary of the Invention
[0006] The purpose of this invention is to develop a silicate-modified coating that can fully utilize the low-cost and environmentally friendly advantages of silicate materials, and significantly improve their interfacial bonding with functional fillers through reasonable chemical modification methods, thereby constructing a tight organic-inorganic interpenetrating network structure. This would result in a silicate-modified coating with high strength, high toughness, excellent adhesion, and good water resistance, which can then be effectively applied to the specific condition of coal mine roof reinforcement. This is a technical problem that urgently needs to be solved.
[0007] To achieve the above-mentioned objectives and improve the aforementioned problems, this invention provides a silicate-modified coating comprising sodium silicate, potassium silicate, bridging modified mica, sulfuric acid solution, sodium hexametaphosphate, sodium carboxymethyl cellulose, silicone defoamer, and deionized water. By weight, it comprises 54.60 parts sodium silicate, 23.40 parts potassium silicate, 3.60-4.45 parts bridging modified mica, 8.25-9.90 parts sulfuric acid solution, 0.40 parts sodium hexametaphosphate, 0.15 parts sodium carboxymethyl cellulose, 0.08 parts silicone defoamer, and 7.47-9.52 parts deionized water.
[0008] A method for preparing a silicate-modified coating, using the silicate-modified coating as described in claim 1, includes the following preparation steps:
[0009] S1: Surface activation of mica functional filler: Disperse mica functional filler in deionized water, add citric acid at a dosage of 5%-8% of mica mass, and acid etch activation at 60℃-70℃ for 1.5h-2h. Wash until the conductivity of the washing solution is not higher than 50μS / cm, and dry to obtain activated mica powder with a total reactive hydroxyl density of not less than 1.2mmol / g.
[0010] S2: Coupling agent bridging modification: The activated mica powder is dispersed in a mixed solvent of ethanol and deionized water in a volume ratio of 4:1. The pH is adjusted to 4.0-5.0 with glacial acetic acid. γ-glycidyl oxypropyltrimethoxysilane is added dropwise at 60°C in an amount of 1.5%-2.5% of the mica mass. The mixture is refluxed for 3 hours. After washing and drying, bridging modified mica is obtained with one end anchored to the mica surface by Si-O-Si bonds and the other end retaining ring-opening epoxy groups.
[0011] S3: Oligopolymerization prepolymerization of silicate mother liquor. Sodium silicate and potassium silicate are mixed at a solids mass ratio of 7:3 to form a silicate mother liquor. While stirring, a pre-diluted sulfuric acid solution is added dropwise online until the pH reaches 10.5-11.0. Polymerization is carried out at 40℃ for 1 hour, controlling the apparent degree of polymerization (DP). * The ratio is 5-8, yielding oligomer mother liquor;
[0012] S4: In-situ copolymerization and compounding: Under stirring at 50℃-55℃ and 600r / min-800r / min, the bridged modified mica is added to the oligomer mother liquor in three batches at 12%-15% of the solid mass of the oligomer mother liquor, with an interval of 10min between each batch. The reaction is kept at the temperature for 2h-3h, so that the residual silanol groups and siloxane oligomer segments on the surface of the bridged modified mica dehydrate and condense with the silanol groups at the end of the oligomer to form Si-O-Si bonds, and the epoxy groups open the ring to participate in crosslinking.
[0013] S5: Additive compounding, cool the system obtained in S4 to 40°C, add sodium hexametaphosphate, sodium carboxymethyl cellulose and organosilicon defoamer that are pre-dissolved in deionized water for formulation, stir and compound to obtain compound coating liquid;
[0014] S6: Curing and packaging: The compound coating liquid is left to stand at 25℃±5℃ for 24 hours for curing. After curing, the viscosity of the Forecast-4 cup is retested. The slurry with D90 not greater than 45μm is filtered through a 200-mesh sieve, sealed and packaged to obtain the finished silicate modified coating.
[0015] As a preferred technical solution of this application, step S1 specifically includes:
[0016] S101: Raw material dispersion: Take mica functional filler and disperse it in deionized water at a solid-liquid mass ratio of 1:5. Stir at 300r / min-400r / min for 30min to obtain a uniform slurry.
[0017] S102: Acid etching activation, adding citric acid to the slurry, heating to 60℃-70℃, and stirring at a constant temperature for 1.5h-2h, so that citric acid complexes and dissolves Fe / Al and interlayer cations on the mica surface, increasing edge Al-OH and broken Si-OH;
[0018] S103: Washing, drying and activation determination: After centrifugation, wash with deionized water 3-5 times until the conductivity of the washing solution is not higher than 50 μS / cm; dry at 105℃ for 4 hours to obtain activated mica powder.
[0019] As a preferred technical solution of this application, step S2 specifically includes:
[0020] S201: Solvent dispersion, the activated mica powder is dispersed in a mixed solvent of ethanol and deionized water, and ultrasonically dispersed for 15 min;
[0021] S202: Grafting reaction, add γ-glycidoxypropyltrimethoxysilane dropwise, adjust the pH of the system to 4.0-5.0 with glacial acetic acid, heat to 60℃ and reflux for 3h;
[0022] S203: Post-treatment, followed by cooling and centrifugation, washing twice with anhydrous ethanol and twice with deionized water, and vacuum drying at 60℃ for 6 hours to obtain bridged modified mica.
[0023] As a preferred technical solution of this application, step S3 specifically includes:
[0024] S301: Mother liquor compounding: Sodium silicate and potassium silicate are compounded at a solid mass ratio of 7:3 and stirred until homogeneous to obtain silicate mother liquor;
[0025] S302: Oligopolymerization control and apparent degree of polymerization calibration: Slowly add sulfuric acid solution pre-diluted to 20% by mass while stirring to adjust the pH of the silicate mother liquor from 12.5 to 10.5-11.0.
[0026] As a preferred technical solution of this application, step S4 specifically includes:
[0027] S401: In-situ introduction, the oligomer mother liquor is heated to 50℃-55℃, and the bridging modified mica is added in three batches with an interval of 10min between each batch under stirring at 600r / min-800r / min;
[0028] S402: Copolymerization reaction, after feeding, keep the reaction at the temperature for 2-3 hours, during which two types of bonding occur;
[0029] S403: Endpoint determination: Take samples at 50℃-55℃ in a hot state, immediately measure the outflow time with a Tu-4 cup, control it to 30s-45s, and simultaneously monitor the pH to ensure it is stable at 10.0-10.8.
[0030] As a preferred technical solution of this application, the two types of bonding are:
[0031] The residual silanol groups and siloxane oligomers on the surface of the bridging modified mica undergo dehydration condensation with the terminal silanol groups of the oligomers to generate Si-O-Si covalent bonds, and the silane self-polymerization segments are grafted onto the silicate matrix network.
[0032] The epoxy groups retained in the bridging modified mica undergo ring-opening under alkaline conditions of pH 10.0-10.8 and 50℃-55℃, reacting with the terminal silanol groups of the oligomer and water.
[0033] As a preferred technical solution of this application, step S5 specifically includes:
[0034] S501: Dispersion stable. First, dissolve all of the sodium hexametaphosphate in the deionized water used in the formula to pre-complex the Ca / Mg impurity ions in the mother liquor with the sodium hexametaphosphate. After the S4 reaction is completed and the system is cooled to 40°C, add the solution along with the water and stir for 15 minutes.
[0035] S502: Construction adjustment: Add sodium carboxymethyl cellulose and organosilicon defoamer, stir for 10 minutes to obtain compound coating liquid.
[0036] As a preferred technical solution of this application, step S6 specifically includes:
[0037] S601: Curing, the compound coating liquid is allowed to stand at 25℃±5℃ for 24 hours to cure;
[0038] S602: Filter packaging. After measuring the slurry D90 with a laser particle size analyzer and confirming that it is no larger than 45μm, filter it with a 200-mesh sieve, seal and package it to obtain the finished silicate modified coating.
[0039] An application of a silicate-modified coating in the reinforcement of the roof slab of a coal mine involves applying the silicate-modified coating to the rock surface of the roof slab, allowing the silicate-modified coating to penetrate into the cracks of the roof rock layer and solidify, forming an inorganic reinforcement layer on the roof rock surface.
[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0041] In the scheme of this application:
[0042] 1. By subjecting mica functional fillers to two-step pretreatment—surface activation and coupling agent bridging modification—bridged modified mica with reactive hydroxyl groups and ring-opening epoxy groups on its surface was obtained. In the subsequent in-situ co-condensation step, the bridged modified mica was not simply physically dispersed in the silicate mother liquor. Instead, Si-O-Si covalent bonds were formed through the dehydration condensation of residual silanol groups and siloxane oligomer segments on its surface with the terminal silanol groups of the oligomers. Simultaneously, the retained epoxy groups participated in the cross-linking reaction under alkaline conditions. This process enabled the bridged modified mica to act as a chemical node, forming a strong covalent interpenetrating network structure with the silicate matrix, rather than a simple physical coating. This chemical bonding fundamentally solves the problem of weak interfacial bonding between fillers and the matrix in traditional physical blending, greatly enhancing the integrity and cohesiveness of the coating. Furthermore, the coating of this invention shows significant improvements in pull-out adhesion, crack-free dry film thickness, and resistance to neutral salt spray.
[0043] 2. By precisely controlling the oligomerization prepolymerization process of silicate mother liquor, the apparent degree of polymerization (DP) is reduced. * Maintaining a pH range of 5-8 provided suitable reactivity and molecular size for subsequent in-situ introduced bridging-modified mica. Simultaneously, by adding the bridging-modified mica in three batches, controlling the reaction temperature, stirring speed, and the endpoint determination (Tu-4 cup effluent time and pH value), the uniform and orderly progress of the co-condensation reaction was ensured, avoiding localized excessive cross-linking or incomplete reaction. Finally, after curing, filtration, and packaging, a finished coating with stable quality and excellent application performance was obtained.
[0044] 3. The coating is specifically optimized for use in coal mine roof reinforcement. As an inorganic system, it boasts excellent environmental safety and is suitable for underground operations. Its superior permeability allows it to penetrate deep into roof rock fissures and rapidly solidify through a chemical reaction, forming a tightly bonded inorganic reinforcement layer. This layer not only effectively seals fissures and prevents rock delamination but also significantly enhances the overall load-bearing capacity and weathering resistance of the roof. Combined with specific pneumatic spraying techniques and construction parameters, it enables efficient and reliable roof reinforcement operations in coal mines, providing strong support for safe mine production. Attached Figure Description
[0045] Figure 1 A flowchart illustrating the silicate-modified coating and its preparation method provided in this application, as well as its application in the reinforcement of coal mine roof slabs;
[0046] Figure 2 A schematic diagram of the mica-silicate covalent interpenetrating network structure in the silicate modified coating, preparation method, and application in the reinforcement of coal mine roof slabs provided in this application;
[0047] Figure 3The colorimetric calibration curve of molybdenum yellow in silicate modified coatings and preparation methods provided in this application, and their application in the reinforcement of coal mine roof slabs. Detailed Implementation
[0048] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0049] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings.
[0050] It should be noted that, unless otherwise specified, the embodiments and features and technical solutions in the present invention can be combined with each other.
[0051] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0052] Please refer to Figures 1-3 A silicate-modified coating comprises sodium silicate, potassium silicate, bridging modified mica, sulfuric acid solution, sodium hexametaphosphate, sodium carboxymethyl cellulose, silicone defoamer, and deionized water. By weight, it comprises 54.60 parts sodium silicate, 23.40 parts potassium silicate, 3.60-4.45 parts bridging modified mica, 8.25-9.90 parts sulfuric acid solution, 0.40 parts sodium hexametaphosphate, 0.15 parts sodium carboxymethyl cellulose, 0.08 parts silicone defoamer, and 7.47-9.52 parts deionized water.
[0053] A method for preparing a silicate-modified coating includes the following preparation steps:
[0054] S1: Surface activation of mica functional filler: Disperse mica functional filler in deionized water, add citric acid at a dosage of 5%-8% of mica mass, and acid etch activation at 60℃-70℃ for 1.5h-2h. Wash until the conductivity of the washing solution is not higher than 50μS / cm, and dry to obtain activated mica powder with a total reactive hydroxyl density of not less than 1.2mmol / g.
[0055] S2: Coupling agent bridging modification: Activated mica powder is dispersed in a mixed solvent of ethanol and deionized water in a volume ratio of 4:1. The pH is adjusted to 4.0-5.0 with glacial acetic acid. γ-glycidyl oxypropyltrimethoxysilane is added dropwise at 60℃ at an amount of 1.5%-2.5% of the mica mass. The mixture is refluxed for 3 hours. After washing and drying, bridging modified mica is obtained with one end anchored to the mica surface by Si-O-Si bonds and the other end retaining ring-opening epoxy groups.
[0056] S3: Oligopolymerization prepolymerization of silicate mother liquor. Sodium silicate and potassium silicate are mixed at a solids mass ratio of 7:3 to form a silicate mother liquor. While stirring, a pre-diluted sulfuric acid solution is added dropwise online until the pH reaches 10.5-11.0. Polymerization is carried out at 40℃ for 1 hour, controlling the apparent degree of polymerization (DP). * The ratio is 5-8, yielding oligomer mother liquor;
[0057] S4: In-situ copolymerization and compounding: Under stirring at 50℃-55℃ and 600r / min-800r / min, the bridged modified mica is added to the oligomer mother liquor in three batches at 12%-15% of the solid mass of the oligomer mother liquor, with an interval of 10min between each batch. The reaction is kept at the temperature for 2h-3h, so that the residual silanol groups and siloxane oligomer segments on the surface of the bridged modified mica dehydrate and condense with the silanol groups at the end of the oligomer to form Si-O-Si bonds, and the epoxy groups open the ring to participate in crosslinking. The endpoint is controlled by the flow time of the Forte-4 cup of 30s-45s (hot sampling at 50℃-55℃) and pH of 10.0-10.8.
[0058] S5: Additive compounding. Cool the system obtained in S4 to 40°C, add sodium hexametaphosphate, sodium carboxymethyl cellulose and organosilicon defoamer that have been dissolved in deionized water for formulation, with the amounts being 0.3%-0.5%, 0.1%-0.2% and 0.05%-0.1% of the total mass of the coating, respectively, and stir to obtain the compound coating liquid.
[0059] S6: Curing and Packaging. The compound coating liquid is left to stand at 25℃±5℃ for 24 hours to cure. After curing, the viscosity of the Forecast-4 cup is retested. The slurry with D90 not greater than 45μm is filtered through a 200-mesh sieve, sealed and packaged to obtain the finished silicate modified coating.
[0060] Furthermore, such as Figures 1-3 As shown, S1 specifically includes:
[0061] S101: Raw material dispersion: Take mica functional filler and disperse it in deionized water at a solid-liquid mass ratio of 1:5. Stir at 300r / min-400r / min for 30min to obtain a uniform slurry.
[0062] S102: Acid etching activation. Add citric acid to the slurry, heat to 60℃-70℃, and stir at a constant temperature for 1.5h-2h to allow citric acid to complex and dissolve with Fe / Al and interlayer cations on the mica surface, increase edge Al-OH and broken Si-OH, and improve the total reactive hydroxyl density on the surface.
[0063] S103: Washing, drying and activation determination: After centrifugation, wash with deionized water 3-5 times until the conductivity of the washing solution is not higher than 50 μS / cm; dry at 105℃ for 4 hours to obtain activated mica powder.
[0064] The activation degree was determined as follows: 1.000 g of activated mica powder was weighed and added to 25.00 mL of 0.100 mol / L NaOH standard solution. The mixture was shaken at 25 °C for 2 h to allow the total reactive hydroxyl groups on the surface to react with NaOH. The mixture was centrifuged, and the entire supernatant was potentiometrically titrated to pH 7.0 with 0.100 mol / L HCl standard solution. The volume of HCl consumed, V1, was recorded. An unactivated mica powder was used as a control in the same manner to obtain V2. A reagent blank without the sample was used to determine the volume of HCl consumed, V0. The results were calculated using the following formula:
[0065] ;
[0066] In the formula: The density of total reactive hydroxyl groups on the surface is expressed in mmol / g. This represents the volume of HCl consumed for the reagent blank, in mL. The volume of HCl consumed by the sample is expressed in mL. The concentration of the HCl standard solution is 0.100 mol / L. The sample mass is 1.000g.
[0067] Furthermore, such as Figures 1-3 As shown, S2 specifically includes:
[0068] S201: Solvent dispersion, the activated mica powder is dispersed in a mixed solvent of ethanol and deionized water in a volume ratio of 4:1 and a solid-liquid mass ratio of 1:4, and ultrasonically dispersed for 15 min.
[0069] S202: Grafting reaction. γ-glycidoxypropyltrimethoxysilane was added dropwise, and the pH of the system was adjusted to 4.0-5.0 with glacial acetic acid. The mixture was heated to 60°C and stirred under reflux for 3 hours. Under these conditions, the methoxy groups of the silane were fully hydrolyzed to silanol groups, which then reacted with the total reactive hydroxyl groups on the surface of the activated mica powder through dehydration and partial self-condensation, forming a siloxane graft layer on the mica surface. After 3 hours of reflux, the methoxy groups were basically consumed.
[0070] S203: Post-treatment, after cooling and centrifugation, wash twice with anhydrous ethanol and twice with deionized water, and vacuum dry at 60℃ for 6h to obtain bridged modified mica; one end of its surface silane layer is anchored to the mica surface by Si-O-Si bonds, and the other end retains ring-opening epoxy groups, while residual incompletely self-condensed silanol groups and siloxane oligomer segments are available for grafting with the parent network in step four.
[0071] Furthermore, such as Figures 1-3 As shown, S3 specifically includes:
[0072] S301: Mother liquor compounding: Sodium silicate and potassium silicate are compounded at a solid mass ratio of 7:3 and stirred until homogeneous to obtain silicate mother liquor;
[0073] S302: Oligopolymerization control and apparent degree of polymerization determination: Slowly add a sulfuric acid solution pre-diluted to 20% by mass under stirring to adjust the pH of the silicate mother liquor from 12.5 to 10.5-11.0. During the addition process, maintain a stirring speed of no less than 300 r / min, and the dropping rate should be such that no local turbidity appears in the system. When the pH drops to around 10.5, the water glass approaches the accelerated gelation boundary. If local turbidity occurs, immediately cool down to 30℃ and add a small amount of silicate mother liquor. After the addition is completed, keep warm at 40℃ for 1 hour to allow the silicate ions to polymerize appropriately into oligomers.
[0074] Apparent degree of polymerization was determined using the molybdenum method: total silicon was determined by the silicomolybdenum blue colorimetric method (the sample was depolymerized and then ammonium molybdate and a reducing agent were added, and the colorimetric value was measured at 660 nm); molybdenum-active monosilicon was determined by the silicomolybdenum yellow colorimetric method (ammonium molybdate was added under acidic conditions, and the colorimetric value was measured at 410 nm). Silicomolybdenum yellow reacts with monosilicic acid and some oligomeric silicons under acidic conditions, therefore the calculated value is the apparent degree of polymerization, denoted as DP. * :
[0075] ;
[0076] In the formula: The total silicon concentration in the mother liquor (silicon molybdenum blue method). This refers to the concentration of molybdenum active monosilicon in the mother liquor (silicomolybdenum yellow method). Both units are consistent. This ratio is used to control the degree of oligomerization and is not equivalent to a strict number-average degree of polymerization. If a strict number-average degree of polymerization is required, it can be expressed separately. 29 SiNMR according to Q 0 -Q 3 Peak area integral verification is not used as a control indicator for this process.
[0077] Furthermore, such as Figures 1-3 As shown, S4 specifically includes:
[0078] S401: In-situ introduction, heat the oligomer mother liquor to 50℃-55℃, and add the bridged modified mica in three batches with a 10min interval between each batch while stirring at 600r / min-800r / min;
[0079] S402: Copolymerization reaction, after feeding, keep the reaction at the temperature for 2-3 hours, during which two types of bonding occur;
[0080] S403: Endpoint determination: Take samples at 50℃-55℃ in a hot state, and immediately measure the outflow time using a Forte-4 cup (100mL, standard outflow well), controlling it to 30s-45s. Simultaneously monitor the pH to ensure it remains stable at 10.0-10.8. If the viscosity exceeds the upper limit, add deionized water to adjust it. During the reaction, the hydroxyl groups on the mica surface consume OH groups. - The pH dropped from 10.80 before addition to 10.45 after 2 hours of reaction, a drop of about 0.3-0.4 pH units.
[0081] Furthermore, such as Figures 1-3 As shown, the two types of bonds are:
[0082] The residual silanol groups and siloxane oligomers on the surface of the bridged modified mica undergo dehydration condensation with the terminal silanol groups of the oligomers to generate Si-O-Si covalent bonds, and the silane self-polymers are grafted onto the silicate matrix network.
[0083] The epoxy groups retained in the bridged-modified mica undergo ring-opening under alkaline conditions (pH 10.0–10.8, 50–55°C) and react with the terminal silanol groups of the oligomers and water. Under alkaline conditions (pH 10.0–10.8, 50–55°C), the epoxy groups retained in the bridged-modified mica mainly undergo ring-opening reactions. Due to the high water content in the water glass system, the epoxy groups preferentially undergo ring-opening with water to form vicinal diol structures. Simultaneously, the silanol groups (—SiOH) present in the system may also participate in ring-opening, but due to their weak nucleophilicity, the contribution of this pathway needs further investigation using 29SiNMR or model inversion. It should be verified that the vicinal diol can subsequently undergo dehydration condensation with silanols to form ether bonds (C—O—Si), or further crosslink with other active groups. The resulting flexible crosslinked segments coexist with the rigid Si—O—Si network, jointly constructing a mica-silicate interpenetrating structure. The rigid Si—O—Si bonds and the flexible crosslinked segments containing Si—OC work synergistically to make the mica sheets become chemical nodes within the network, forming a mica-silicate covalent interpenetrating structure. The essential difference between this step and physical blending is that the bridging modified mica participates in network construction during the oligomerization stage of the oligomerization mother liquor, rather than being mixed in after the finished product stage.
[0084] Furthermore, such as Figures 1-3 As shown, S5 specifically includes:
[0085] S501: Dispersion and stability. First, dissolve all of the sodium hexametaphosphate in the deionized water used in the formula to pre-complex the Ca / Mg impurity ions in the mother liquor, so as to avoid the formation of flocculation precipitates with silicate ions. After the S4 reaction is completed and the system is cooled to 40°C, add the solution along with the water and stir for 15 minutes.
[0086] S502: Construction adjustment: Add sodium carboxymethyl cellulose and organosilicon defoamer, stir for 10 minutes to obtain compound coating liquid.
[0087] It should be noted that adjusting the pH using sulfuric acid in step S3 introduces sulfate ions (SO4). 2- In the final coating, sulfate exists in the form of Na₂SO₄ / K₂SO₄. A suitable amount of sulfate helps adjust the rheological properties of the coating, but excessive amounts may cause the coating to crystallize and turn white or reduce its water resistance. In this formulation, the amount of sulfuric acid solution is controlled at 8.25–9.90 parts, and the calculated sulfate content in the finished product is approximately X%–Y% (which can be estimated based on the data from the examples). If higher water resistance is required, some sulfate can be removed by dialysis or ion exchange resin, or it can be replaced with volatile / degradable acids such as hydrochloric acid or phosphoric acid (the process parameters need to be adjusted accordingly). This scheme uses sulfuric acid as an example, but the feasibility of other acids is not excluded.
[0088] Furthermore, such as Figures 1-3 As shown, S6 specifically includes:
[0089] S601: Curing. The compound coating liquid was allowed to stand at 25℃±5℃ for 24 hours to allow the residual reaction to reach equilibrium and for bubbles to escape fully. Before and after curing, the flow time was measured again using a Forte-4 cup after being kept at 25℃±1℃ for 30 minutes: 30s-45s when hot at the time of discharge, and 36s-40s after curing at 25℃.
[0090] S602: Filter packaging. After measuring the slurry D90 with a laser particle size analyzer and confirming that it is not greater than 45μm (i.e., not exceeding the 200-mesh sieve aperture to prevent clogging), filter it with a 200-mesh sieve, seal and package it to obtain the finished silicate modified coating.
[0091] An application of a silicate-modified coating in the reinforcement of the roof slab of a coal mine involves applying the silicate-modified coating to the rock surface of the roof slab, allowing the silicate-modified coating to penetrate into the cracks of the roof rock layer and solidify, forming an inorganic reinforcement layer on the roof rock surface.
[0092] The application method is air pressure spraying, with a spraying air pressure of 0.3MPa-0.6MPa, a single spray thickness of 0.5mm-1.0mm, and 2 to 3 sprays, with a total thickness of 1.5mm-3.0mm.
[0093] Curing is carried out in an underground environment with a temperature of 10℃-30℃ and a relative humidity of no more than 90%, and the curing time is 4h-8h.
[0094] Before applying silicate-modified coating, the top rock surface is cleaned to remove loose rock and dust, exposing fresh bedrock with a moisture content of no more than 8%.
[0095] Before application, the silicate-modified coating is cured at 25℃±5℃ for 24 hours. The adhesion between the inorganic reinforcement layer and the top rock surface is not less than 6MPa, and the dry film thickness is 2mm without cracking.
[0096] Example 1:
[0097] Prepared according to the entire process from S1 to S6; bridging modified mica accounted for 13.5% of the solids in the oligomerizing mother liquor, and the DP of the oligomerizing mother liquor... * =5.9, S4 reacted at 55℃ for 3h, including 54.60 parts by mass of sodium silicate, 23.40 parts of potassium silicate, 4.0 parts of bridging modified mica, 8.25 parts of sulfuric acid solution, 0.40 parts of sodium hexametaphosphate, 0.15 parts of sodium carboxymethyl cellulose, 0.08 parts of organosilicon defoamer, and 9.12 parts of deionized water.
[0098] Example 2:
[0099] The bridging modified mica was adjusted to 3.60 parts (accounting for 12.1%), and the remaining processes were the same as in Example 1. By weight, it included 54.60 parts of sodium silicate, 23.40 parts of potassium silicate, 3.60 parts of bridging modified mica, 8.25 parts of sulfuric acid solution, 0.40 parts of sodium hexametaphosphate, 0.15 parts of sodium carboxymethyl cellulose, 0.08 parts of silicone defoamer, and 9.25 parts of deionized water.
[0100] Example 3:
[0101] The bridging modified mica was adjusted to 4.45 parts (accounting for 15.0%), and the remaining processes were the same as in Example 1. By weight, it included 54.60 parts of sodium silicate, 23.40 parts of potassium silicate, 4.45 parts of bridging modified mica, 8.25 parts of sulfuric acid solution, 0.40 parts of sodium hexametaphosphate, 0.15 parts of sodium carboxymethyl cellulose, 0.08 parts of silicone defoamer, and 8.67 parts of deionized water.
[0102] Example 4:
[0103] The sulfuric acid solution was increased to 9.90 parts, and the pH of the oligomer mother liquor was adjusted to 10.5-10.7, DP... *=5.1, 4.00 parts of bridging modified mica, the rest of the process is the same as in Example 1, including 54.60 parts of sodium silicate, 23.40 parts of potassium silicate, 4.0 parts of bridging modified mica, 9.90 parts of sulfuric acid solution, 0.40 parts of sodium hexametaphosphate, 0.15 parts of sodium carboxymethyl cellulose, 0.08 parts of organosilicon defoamer, and 7.47 parts of deionized water by weight.
[0104] Actual measurements based on S1 in Example 1: =25.00mL, activated mica =12.60mL, obtained =1.24mmol / g; Unactivated control =20.60mL, obtained =0.44mmol / g. FTIR also corroborated this: after activation, 3450cm⁻¹ -1 The relative absorbance of the broad peak of the Si-OH stretching vibration was increased by about 1.6 times. The activation level was controlled to be no less than 1.2 mmol / g; if it was lower than this value, S102 was repeated once.
[0105] Based on S3: the standardization curve of molybdenum silicoammonia is given in μg / mL system: A 410 =0.0214×C(μg / mL)+0.003, correlation coefficient r=0.999. Samples were uniformly diluted 100-fold before colorimetric analysis. The results were converted back to the original solution concentration based on 1 mg / mL = 1000 μg / mL. Example 1: Actual measurement: Diluent A 410 =0.069, C single, dilution = (0.069−0.003) / 0.0214 = 3.08μg / mL, refractory to original solution =0.31 mg / mL; Silicomolybdenum blue method: =1.82 mg / mL; DP * =1.82 / 0.31≈5.9, Example 4: Diluent A 410 =0.080, =0.36 mg / mL, DP * ≈5.1, both fall under DP * =5-8 interval;
[0106] The amount of sulfuric acid solution used is not limited by a fixed theoretical acid consumption, but is based on the endpoint of online pH titration; in Example 1, 8.25 parts of 20% sulfuric acid solution were actually consumed when titrating to pH 10.8, and in Example 4, 9.90 parts were actually consumed when titrating to pH 10.5.
[0107] Based on S4, the degree of epoxy ring opening was verified using FTIR: at 1270 cm⁻¹ -1 With siloxane absorption peak as reference, epoxy is at 910 cm⁻¹. -1The peak disappearance rate (loop opening rate) after processing was measured to be 65% in Example 1, and the calculation formula is: loop opening rate = [1−(A 910 / A 1270 After processing / (A) 910 0 / A 1270 [Before processing] × 100%.
[0108] Comparative Example 1: Steps S1 and S2 are omitted. 4.00 parts of ordinary sericite powder (unactivated, unbridged) are directly added to the sodium potassium silicate mother liquor at temperature S4. The amounts of other raw materials and process conditions are the same as in Example 1.
[0109] Comparative Example 2: Without adding mica, 0.50 parts of γ-glycidyl etheroxypropyltrimethoxysilane were directly added to the silicate mother liquor and stirred to react. The amounts of other raw materials and process conditions were the same as in Example 1.
[0110] Comparative Example 3: 4.00 parts of bridging modified mica were prepared according to S1 and S2, but this mica was not added in S4, but instead added simultaneously with sodium hexametaphosphate in S5; no mica was added during the heat preservation reaction stage in S4, and the remaining raw material amounts and process conditions were the same as in Example 1. Evidence that a covalent network was not formed: FTIR of the coating cross-section showed that the epoxy was 910 cm². -1 The peak disappearance rate was only about 20% (about 65% in Example 1); the weight loss rate of the coating after 24 hours of Soxhlet extraction with ethanol was 3.5% (about 0.8% in Example 1), indicating that the added mica did not form a covalent network with the parent material, but was only a physical coating.
[0111] Performance comparison:
[0112] Sample preparation: Sandblasted steel plates were treated to Sa2.5 grade according to GB / T8923.1-2011, with a surface roughness Rz of 40-75μm; three parallel samples were prepared for each sample, and three wet films were applied, with a 6-hour interval between each film; the dry film thickness was determined according to the magnetic thickness measurement method of GB / T13452.2; after 7 days of standard curing, the adhesion test was conducted according to GB / T5210-2006. The dry film thickness without cracks was observed and recorded at the time of the first appearance of cracks using a 10x magnifying glass. The time of the first blistering was recorded according to GB / T1771-2007 for neutral salt spray testing. The following is a comparison table:
[0113]
[0114] Results analysis:
[0115] Comparative Example 1 uses the same amount of mica as Example 1, with the only difference being the activation and bridging treatment: the adhesion increased from 4.5 MPa to 8.2 MPa, and the salt spray duration increased from 480 h to 1200 h. Based on this, the substantial contribution of surface activation and coupling bridging can be demonstrated.
[0116] Comparative Example 2 demonstrates that the sheet barrier is missing when mica is absent, and all three indicators are significantly lower than in the embodiments.
[0117] Comparative Example 3 and Example 1 mica were activated and bridged in the same way, only the timing of addition was different: the adhesion decreased from 8.2 MPa to 5.8 MPa, and the salt spray test time decreased from 1200 h to 650 h; combined with the evidence of FTIR ring-opening rate and ethanol extraction weight loss rate, it was proved that the in-situ introduction of the oligomerization stage is the key to the formation of covalent network.
[0118] The indicators in each embodiment change steadily within a defined range with varying mica dosage and apparent aggregation degree. Embodiments 2, 4, and 3 respectively support the range of mica dosage and DP. * The lower, middle, and upper ends of the interval.
[0119] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection, an electrical connection, or a connection that allows communication between them; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise explicitly limited. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0120] Obviously, the embodiments described above are merely some embodiments of the present invention, not all embodiments. The accompanying drawings show preferred embodiments of the present invention, but do not limit the patent scope of the present invention. The present invention can be implemented in many different forms; rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing specific embodiments, or make equivalent substitutions for some of the technical features. Any equivalent structures made using the content of this specification and drawings, directly or indirectly applied to other related technical fields, are similarly within the patent protection scope of this invention.
Claims
1. A silicate-modified coating, characterized in that, The product comprises sodium silicate, potassium silicate, bridging modified mica, sulfuric acid solution, sodium hexametaphosphate, sodium carboxymethyl cellulose, silicone defoamer, and deionized water. By weight, it includes 54.60 parts sodium silicate, 23.40 parts potassium silicate, 3.60-4.45 parts bridging modified mica, 8.25-9.90 parts sulfuric acid solution, 0.40 parts sodium hexametaphosphate, 0.15 parts sodium carboxymethyl cellulose, 0.08 parts silicone defoamer, and 7.47-9.52 parts deionized water.
2. A method for preparing a silicate-modified coating, using the silicate-modified coating as described in claim 1, characterized in that, The preparation steps include the following: S1: Surface activation of mica functional filler: Disperse mica functional filler in deionized water, add citric acid at a dosage of 5%-8% of mica mass, and acid etch activation at 60℃-70℃ for 1.5h-2h. Wash until the conductivity of the washing solution is not higher than 50μS / cm, and dry to obtain activated mica powder with a total reactive hydroxyl density of not less than 1.2mmol / g. S2: Coupling agent bridging modification: The activated mica powder is dispersed in a mixed solvent of ethanol and deionized water in a volume ratio of 4:
1. The pH is adjusted to 4.0-5.0 with glacial acetic acid. γ-glycidyl oxypropyltrimethoxysilane is added dropwise at 60°C in an amount of 1.5%-2.5% of the mica mass. The mixture is refluxed for 3 hours. After washing and drying, bridging modified mica is obtained with one end anchored to the mica surface by Si-O-Si bonds and the other end retaining ring-opening epoxy groups. S3: oligomerization of silicate solution, sodium water glass and potassium water glass were mixed as silicate solution with solid mass ratio 7:3, pre-diluted sulfuric acid solution was added on-line with stirring to pH 10.5-11.0, and the solution was incubated at 40°C for 1 h to control the apparent degree of polymerization DP * 5-8, to obtain an oligomerization solution; S4: In-situ copolymerization and compounding: Under stirring at 50℃-55℃ and 600r / min-800r / min, the bridged modified mica is added to the oligomer mother liquor in three batches at 12%-15% of the solid mass of the oligomer mother liquor, with an interval of 10min between each batch. The reaction is kept at the temperature for 2h-3h, so that the residual silanol groups and siloxane oligomer segments on the surface of the bridged modified mica dehydrate and condense with the silanol groups at the end of the oligomer to form Si-O-Si bonds, and the epoxy groups open the ring to participate in crosslinking. S5: Additive compounding, cool the system obtained in S4 to 40°C, add sodium hexametaphosphate, sodium carboxymethyl cellulose and organosilicon defoamer that are pre-dissolved in deionized water for formulation, stir and compound to obtain compound coating liquid; S6: Curing and packaging: The compound coating liquid is left to stand at 25℃±5℃ for 24 hours for curing. After curing, the viscosity of the Forecast-4 cup is retested. The slurry with D90 not greater than 45μm is filtered through a 200-mesh sieve, sealed and packaged to obtain the finished silicate modified coating.
3. The method for preparing a silicate-modified coating according to claim 2, characterized in that, Specifically, S1 includes: S101: Raw material dispersion: Take mica functional filler and disperse it in deionized water at a solid-liquid mass ratio of 1:
5. Stir at 300r / min-400r / min for 30min to obtain a uniform slurry. S102: Acid etching activation, adding citric acid to the slurry, heating to 60℃-70℃, and stirring at a constant temperature for 1.5h-2h, so that citric acid complexes and dissolves Fe / Al and interlayer cations on the mica surface, increasing edge Al-OH and broken Si-OH; S103: Washing, drying and activation determination: After centrifugation, wash with deionized water 3-5 times until the conductivity of the washing solution is not higher than 50 μS / cm; dry at 105℃ for 4 hours to obtain activated mica powder.
4. The method for preparing a silicate-modified coating according to claim 3, characterized in that, Specifically, S2 includes: S201: Solvent dispersion, the activated mica powder is dispersed in a mixed solvent of ethanol and deionized water, and ultrasonically dispersed for 15 min; S202: Grafting reaction, add γ-glycidoxypropyltrimethoxysilane dropwise, adjust the pH of the system to 4.0-5.0 with glacial acetic acid, heat to 60℃ and reflux for 3h; S203: Post-treatment, followed by cooling and centrifugation, washing twice with anhydrous ethanol and twice with deionized water, and vacuum drying at 60℃ for 6 hours to obtain bridged modified mica.
5. The method for preparing a silicate-modified coating according to claim 4, characterized in that, Specifically, S3 includes: S301: Mother liquor compounding: Sodium silicate and potassium silicate are compounded at a solid mass ratio of 7:3 and stirred until homogeneous to obtain silicate mother liquor; S302: Oligopolymerization control and apparent degree of polymerization calibration: Slowly add sulfuric acid solution pre-diluted to 20% by mass while stirring to adjust the pH of the silicate mother liquor from 12.5 to 10.5-11.
0.
6. The method for preparing a silicate-modified coating according to claim 5, characterized in that, Specifically, S4 includes: S401: In-situ introduction, the oligomer mother liquor is heated to 50℃-55℃, and the bridging modified mica is added in three batches with an interval of 10min between each batch under stirring at 600r / min-800r / min; S402: Copolymerization reaction, after feeding, keep the reaction at the temperature for 2-3 hours, during which two types of bonding occur; S403: Endpoint determination: Take samples at 50℃-55℃ in a hot state, immediately measure the outflow time with a Tu-4 cup, control it to 30s-45s, and simultaneously monitor the pH to ensure it is stable at 10.0-10.
8.
7. The method for preparing a silicate-modified coating according to claim 6, characterized in that, The two types of bonding are: The residual silanol groups and siloxane oligomers on the surface of the bridging modified mica undergo dehydration condensation with the terminal silanol groups of the oligomers to generate Si-O-Si covalent bonds, and the silane self-polymerization segments are grafted onto the silicate matrix network. The epoxy groups retained in the bridging modified mica undergo ring-opening under alkaline conditions of pH 10.0-10.8 and 50℃-55℃, reacting with the terminal silanol groups of the oligomer and water.
8. The method for preparing a silicate-modified coating according to claim 7, characterized in that, Specifically, S5 includes: S501: Dispersion stable. First, dissolve all of the sodium hexametaphosphate in the deionized water used in the formula to pre-complex the Ca / Mg impurity ions in the mother liquor with the sodium hexametaphosphate. After the S4 reaction is completed and the system is cooled to 40°C, add the solution along with the water and stir for 15 minutes. S502: Construction adjustment: Add sodium carboxymethyl cellulose and organosilicon defoamer, stir for 10 minutes to obtain compound coating liquid.
9. The method for preparing a silicate-modified coating according to claim 8, characterized in that, Specifically, S6 includes: S601: Curing, the compound coating liquid is allowed to stand at 25℃±5℃ for 24 hours to cure; S602: Filter packaging. After measuring the slurry D90 with a laser particle size analyzer and confirming that it is no larger than 45μm, filter it through a 200-mesh sieve, seal the packaging, and you will get the finished silicate modified coating.
10. An application of a silicate-modified coating in the reinforcement of the roof slab of a coal mine, comprising the preparation method of the silicate-modified coating as described in claim 9, characterized in that... The silicate-modified coating is applied to the roof slab surface of a coal mine, allowing the silicate-modified coating to penetrate into the cracks of the roof slab and solidify, forming an inorganic reinforcement layer on the roof slab surface.