A highly sealing and penetrating primer and its preparation method

By using an inorganic-organic interpenetrating network structure of low-modulus potassium silicate, compound emulsion, and pigments and fillers, the problems of shallow penetration, poor sealing, insufficient resistance to salt efflorescence, and failure to meet environmental protection standards in exterior wall penetrating primers are solved, achieving a comprehensive performance improvement of high-sealing penetrating primers and meeting relevant standards and environmental protection requirements.

CN123107464APending Publication Date: 2026-11-17NIPPON PAINT YASHILI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611536791.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing exterior wall penetrating primers are inadequate in terms of penetration performance, sealing properties, resistance to efflorescence and environmental friendliness, and cannot meet the requirements of JG/T 210-2018 and GB 30981.1-2025 standards. Furthermore, they have poor system stability and short shelf life.

Method used

An inorganic-organic interpenetrating network structure is formed by using low-modulus potassium silicate with low-Tg and high-Tg compound emulsions. Combined with pigments and fillers such as ultrafine heavy calcium carbonate, wollastonite powder, nano silica and nano zinc oxide, environmentally friendly additives are used, the modulus and pH value are controlled, and the preparation process is optimized to form a highly sealing and penetrating primer.

Benefits of technology

It achieves excellent penetration and reinforcement performance, outstanding sealing and alkali resistance, high environmental compliance, and good system stability, meeting the standards of JG/T 210-2018 and GB 30981.1-2025. It is suitable for the pretreatment of exterior wall substrates, with strong adhesion and long storage period.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107464A_ABST
    Figure CN123107464A_ABST
Patent Text Reader

Abstract

This invention discloses a highly sealing and penetrating primer and its preparation method. The primer comprises the following components by weight: 5.0–10.0 parts potassium silicate; 55.0–65.0 parts compound primer emulsion; 20.0–25.0 parts pigments and fillers; 4.0–8.0 parts environmentally friendly additives; and an appropriate amount of deionized water. The potassium silicate has a modulus of 2.0–2.4, a solid content of 28–32%, Na₂O ≤ 2%, and a pH of 12.5 ± 0.5. The compound primer emulsion is prepared by mixing a low-Tg styrene-acrylic emulsion and a high-Tg pure acrylic emulsion at a mass ratio of (7–9):1. This invention utilizes the inorganic penetrating and curing properties of potassium silicate and the organic film-forming and sealing properties of the emulsion to form an inorganic-organic interpenetrating network structure, solving the technical problems of shallow penetration, poor sealing, insufficient resistance to salt efflorescence, and failure to meet environmental protection standards in traditional primers. The product performance meets the requirements, is suitable for the pretreatment of exterior wall substrates, and has strong adhesion, good stability, and a long shelf life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of architectural coatings technology, specifically a highly sealing and penetrating primer and its preparation method, particularly a highly sealing and penetrating primer based on potassium silicate and emulsion and its preparation method, which is suitable for the pretreatment of exterior wall substrates and can effectively improve the durability, resistance to salt efflorescence and environmental performance of exterior wall coating systems. Background Technology

[0002] Exterior wall primer is a key base material in exterior wall coating systems. Its main function is to penetrate into the base layer, strengthen and seal it, and prevent moisture, salt, and alkaline substances in the base layer from migrating to the surface. This improves the adhesion, weather resistance, and decorative effect of the topcoat, and extends the service life of the exterior wall coating system.

[0003] Currently, exterior wall penetrating primers on the market are mainly divided into two categories: pure organic emulsion primers and single inorganic potassium silicate primers. However, both have obvious technical defects: pure organic emulsion primers have poor penetration performance, can only form a film on the surface of the substrate, and cannot penetrate into the substrate for reinforcement. They also have insufficient sealing properties and are easily affected by efflorescence and salt precipitation in the substrate, leading to peeling, flaking, and discoloration of the topcoat. Their resistance to efflorescence and salt precipitation is difficult to meet the 120h requirement of the JG / T 210-2018 standard for exterior wall type I film-forming type. Although single inorganic potassium silicate primers have better penetration performance and can react with calcium and magnesium ions in the substrate to form a gel and play a reinforcing role, they have poor film-forming properties, insufficient film toughness, are prone to cracking, have low adhesion, and limited sealing properties when used alone, and cannot meet the comprehensive performance requirements of exterior wall primers.

[0004] Meanwhile, with increasingly stringent environmental policies, GB 30981.1-2025 "Limits of Volatile Organic Compounds in Architectural Coatings and Adhesives Part 1: Architectural Coatings" will be mandatory on June 1, 2026. Many existing exterior wall primers exceed the limits for harmful substances such as VOCs, SVOCs, MIT, and APEO, failing to meet the environmental limits required by this standard. Furthermore, when potassium silicate is compounded with emulsions, it is prone to layering and gelation, resulting in poor system stability, short shelf life, and affecting application performance and product quality.

[0005] In view of the shortcomings of the existing technologies, there is an urgent need to develop an exterior wall penetrating primer that combines high penetration, strong sealing, excellent resistance to salt and alkali, environmental compliance, and system stability to meet the actual engineering needs and relevant national standards. Summary of the Invention

[0006] To address the aforementioned problems, the present invention aims to provide a highly sealing and penetrating primer and its preparation method. This invention utilizes the inorganic penetrating and curing properties of potassium silicate and the organic film-forming and sealing properties of emulsions to form an inorganic-organic interpenetrating network structure. This solves the technical problems of traditional primers, such as shallow penetration, poor sealing, insufficient resistance to salt efflorescence, and failure to meet environmental standards. The product performance meets the JG / T 210-2018 standard for Type I film-forming primers for exterior walls and satisfies the environmental protection limits of GB 30981.1-2025. It is suitable for the pretreatment of exterior wall substrates such as cement mortar and putty, exhibiting strong adhesion, good stability, and a long shelf life.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A highly sealing and penetrating primer comprising the following components in parts by weight: Potassium silicate 5.0–10.0 parts; 55.0–65.0 parts of compound primer emulsion; Pigments and fillers: 20.0–25.0 parts; Environmentally friendly additives: 4.0–8.0 parts; Appropriate amount of deionized water; The potassium silicate is a low-modulus stabilized potassium silicate with a modulus of 2.0 to 2.4, a solid content of 28% to 32%, Na₂O ≤ 2%, and pH 12.5 ± 0.5. The compound primer emulsion is prepared by compounding low Tg styrene-acrylic emulsion and high Tg pure acrylic emulsion at a mass ratio of (7-9):1.

[0008] This invention uses low-modulus potassium silicate, which has excellent permeability and can quickly penetrate into the micropores of the substrate, reacting with free Ca²⁺ in the substrate. + Mg² + The reaction produces calcium silicate and magnesium silicate gels, achieving chemical anchoring and reinforcement of the substrate. Simultaneously, low-modulus potassium silicate exhibits better stability; after stabilization treatment, gelation during compounding can be avoided, extending the product's shelf life. Excessively high modulus leads to slow potassium silicate penetration and easy stratification, while excessively low modulus results in poor system stability and easy whitening. Therefore, controlling the modulus within the range of 2.0–2.4 balances penetration performance and system stability.

[0009] Preferably, the low-Tg styrene-acrylic emulsion has a Tg of 0–10℃ and a particle size of 50–80 nm, exhibiting excellent penetration and wetting properties. It can work synergistically with potassium silicate to penetrate deep into the substrate and form a strong bond. The high-Tg pure acrylic emulsion has a Tg of 20–30℃ and a particle size of 120–150 nm, demonstrating good film-forming properties. It can form a dense, sealed film on the substrate surface, reducing the water permeability of the primer and improving water resistance and hardness. The combination of these two emulsions forms an organic film-forming system, which works synergistically with the inorganic penetration system of potassium silicate to construct an inorganic-organic interpenetrating network structure, achieving both penetration reinforcement and sealing protection. Furthermore, both emulsions are selected as APEO-free, VOC-≤50g / L water-based emulsions to ensure the product's environmental compliance.

[0010] Preferably, the pigment and filler are composed of ultrafine heavy calcium carbonate, wollastonite powder, nano silica, and nano zinc oxide in a mass ratio of 18:4:1.5:1.5.

[0011] Preferably, the ultrafine heavy calcium carbonate has a particle size of 1000 mesh, the wollastonite powder has a particle size of 800 mesh, the nano-silica has a particle size of 10-20 nm, and the nano-zinc oxide has a particle size of 30-80 nm.

[0012] Among them, ultrafine heavy calcium carbonate (1000 mesh) has good filling properties, which can fill the micropores of the base layer, build a dense shielding layer, and reduce the water permeability of the primer; wollastonite powder (800 mesh) has excellent alkali resistance and reinforcing properties, which can improve the primer's resistance to salt efflorescence and mechanical strength; nano silica (10-20 nm) has high specific surface area and high activity, which can fill the micropores after the emulsion film is formed, further improving the sealing and hardness; nano zinc oxide has alkali resistance, antibacterial and weather resistance properties, which can work synergistically with wollastonite powder to improve the primer's resistance to salt efflorescence, while preventing the primer from becoming moldy and deteriorating.

[0013] Preferably, the environmentally friendly additive comprises the following components in parts by weight: 1.5–2.5 parts of silane coupling agent; Film-forming aid 2.0–3.5 parts; 0.3–0.8 parts without APEO dispersant; 0.2–0.4 parts of organosilicon wetting agent; Defoamer 0.1-0.3 parts; pH adjuster 0.1–0.3 parts; 0.1 to 0.3 parts of BIT preservative.

[0014] The selected silane coupling agent, KH-560, enhances the interfacial bonding between potassium silicate, the emulsion, and the substrate, preventing film peeling and improving the compatibility between potassium silicate and the emulsion, thus preventing system delamination. The selected film-forming aid, alcohol ester-12, is a low-VOC film-forming aid that lowers the film-forming temperature of the emulsion, ensuring the primer forms a dense film even at low temperatures, while controlling SVOC content within limits. The selected dispersant, Sanopco 5027, ensures uniform dispersion of pigments and fillers in the system, preventing sedimentation, reducing primer viscosity, and improving application performance. The selected silicone wetting agent, GENAPOLPF20, improves the wetting performance of the primer on high-alkali substrates and aids in the penetration of potassium silicate and the emulsion. The selected defoamer, 5800D mineral oil-based defoamer, effectively inhibits and eliminates bubbles generated during primer preparation, preventing pinholes in the film and ensuring proper sealing. The pH adjuster selected is AMP-95, which can stabilize the system pH within the range of 8.0 to 9.0 and prevent potassium silicate gel and emulsion hydrolysis. The BIT preservative selected is Hanning 701, and the MIT content in the preservative is ≤300mg / kg, which can effectively prevent the primer from becoming moldy and deteriorating during storage and use, while meeting the limit requirements of GB 30981.1-2025.

[0015] The performance indicators of the primer of this invention meet the following requirements: (1) Meets the JG / T 210-2018 standard for film-forming type of exterior wall: water permeability ≤0.3mL, salt and alkali resistance ≥120h with no blistering, no efflorescence, no discoloration, reinforcement performance ≥0.2MPa, surface drying time ≤2h, actual drying time ≤24h, adhesion to cement board ≥1MPa, water resistance (96h) no abnormality, alkali resistance (48h, 0.5% NaOH solution) no abnormality; (2) Meets the limits of GB 30981.1-2025: VOC≤80g / L, SVOC≤150g / L, formaldehyde≤100mg / kg, lead≤90mg / kg, arsenic≤60mg / kg, APEO≤100mg / kg.

[0016] The present invention also provides a method for preparing the above-mentioned highly sealing and penetrating primer, comprising the following steps: (1) Pre-dispersion: Add deionized water, organosilicon wetting agent, APEO-free dispersant, defoamer and pH adjuster to the dispersion vessel, stir at a low speed of 280-320 r / min for 4-6 min, adjust the pH of the system to 8.0-9.0, mix evenly to obtain a pre-dispersion liquid; (2) Filler dispersion: Add pigments and fillers to the pre-dispersion liquid, heat to 38-42℃, disperse at a high speed of 1200-1500r / min for 20-30min until the fineness of the slurry is ≤30μm, and then cool down to ≤40℃; (3) Potassium silicate premix: Add potassium silicate and silane coupling agent to another stirred tank and stir at a low speed of 180-220 r / min for 8-12 min to obtain a uniform potassium silicate premix solution; (4) Emulsion compounding: Add compound primer emulsion to the slurry obtained in step (2) and stir at a medium speed of 580-620 r / min for 13-17 min. Then slowly add potassium silicate premix obtained in step (3) for ≥10 min. After the addition is complete, continue stirring for 8-12 min to form a uniform and stable system. (5) Viscosity adjustment and filtration: Add film-forming aid and BIT preservative to the system obtained in step (4), stir for 4 to 6 minutes, then add deionized water to adjust the viscosity of the primer to 35 ± 5 seconds, and after filtration, a high-sealing penetration primer is obtained.

[0017] Preferably, in step (1), the pH of the system is adjusted to 8.5 ± 0.5; in step (2), the dispersion speed is 1300 r / min and the dispersion time is 25 min; in step (4), the emulsion stirring speed is 600 r / min and the stirring time is 15 min, the potassium silicate premix is ​​added in drops over a time of 10–15 min, and stirring continues for 10 min after addition; in step (5), the stirring time is 5 min. These preferred process parameters can further improve the stability of the system and the performance of the product, ensuring that all indicators of the primer meet the standard requirements.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Excellent penetration and reinforcement performance: Low-modulus potassium silicate can quickly penetrate into the micropores of the substrate (penetration depth ≥ 1.5mm), and react with Ca²⁺ in the substrate. + Mg² + The reaction generates calcium silicate and magnesium silicate gels, achieving chemical anchoring of the substrate; the low Tg and small particle size emulsion synergistically penetrates, further improving the reinforcement effect, with a reinforcement strength ≥0.2MPa, effectively solving the problems of shallow penetration and poor reinforcement effect of traditional primers.

[0019] 2. Outstanding sealing and alkali resistance: The high Tg large particle size emulsion and ultrafine pigments and fillers work together to form a dense sealing film with a water permeability of ≤0.3mL; wollastonite powder and zinc oxide work together to enhance the resistance to salt efflorescence, with a resistance to salt efflorescence ≥120h. This effectively prevents the migration of moisture, salt, and alkaline substances in the substrate, avoiding peeling and discoloration of the topcoat, and meeting the requirements of JG / T 210-2018 exterior wall type I film-forming standard.

[0020] 3. High environmental compliance: Low VOC emulsion, no APEO additives, and low MIT preservatives are selected. The content of various harmful substances is strictly controlled. VOC≤80g / L, SVOC≤150g / L, formaldehyde≤100mg / kg, and heavy metals and APEO all meet the limits of GB 30981.1-2025, satisfying environmental protection policy requirements.

[0021] 4. Good system stability: By strictly controlling the potassium silicate modulus, system pH and preparation process, the layering and gelation phenomenon when potassium silicate is compounded with emulsion is avoided, and the product has a shelf life of ≥12 months; at the same time, the inorganic-organic interpenetrating network structure improves the toughness and adhesion of the coating film, with an adhesion to cement board of ≥1MPa and excellent construction performance.

[0022] 5. Simple and controllable preparation process: The preparation method of the present invention has clear steps, easy-to-control process parameters, no special equipment required, suitable for large-scale industrial production, moderate production cost, and good economic benefits and application prospects. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the penetration and curing mechanism of a highly sealing and penetrating primer according to the present invention; Figure 2 This is a process flow diagram for preparing a highly sealing and penetrating primer according to the present invention. Detailed Implementation

[0024] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents and instruments used in the embodiments are all commercially available conventional products. Unless otherwise specified, the experimental methods used in the embodiments are all conventional experimental methods or techniques in the art.

[0025] Embodiments of the present invention provide a highly sealing and penetrating primer, comprising the following components in parts by weight: Potassium silicate 5.0–10.0 parts; 55.0–65.0 parts of compound primer emulsion; Pigments and fillers: 20.0–25.0 parts; Environmentally friendly additives: 4.0–8.0 parts; Add an appropriate amount of deionized water.

[0026] Adjust the primer viscosity to 35±5s with deionized water (Ford Cup 4, 25°C).

[0027] The potassium silicate used is a low-modulus stabilized potassium silicate with a modulus of 2.0–2.4, a solid content of 28–32%, Na₂O ≤ 2%, and a pH of 12.5 ± 0.5. This invention selects low-modulus potassium silicate, which has excellent permeability and can quickly penetrate into the micropores of the substrate, reacting with free Ca²⁺ in the substrate. + Mg² + The reaction produces calcium silicate and magnesium silicate gels, achieving chemical anchoring and reinforcement of the substrate. Simultaneously, low-modulus potassium silicate exhibits better stability; after stabilization treatment, gelation during compounding can be avoided, extending the product's shelf life. Excessively high modulus leads to slow potassium silicate penetration and easy stratification, while excessively low modulus results in poor system stability and easy whitening. Therefore, controlling the modulus within the range of 2.0–2.4 balances penetration performance and system stability.

[0028] The compound primer emulsion is made by compounding low Tg styrene-acrylic emulsion and high Tg pure acrylic emulsion at a mass ratio of (7-9):1.

[0029] Figure 1 This is a schematic diagram illustrating the penetration and curing mechanism of a highly sealing and penetrating primer according to the present invention. Wherein, 1-substrate (cement mortar / putty); 2-potassium silicate penetrating layer; 3-inorganic-organic interpenetrating network layer; 4-sealing paint film layer; potassium silicate penetrates into the substrate and reacts with Ca²⁺ in the substrate. + Mg² + The reaction generates calcium silicate and magnesium silicate gels, forming a penetrating reinforcement layer. The emulsion forms a film on the surface of the base layer, forming an interpenetrating network with the potassium silicate penetrating layer to achieve closed protection.

[0030] The primer relies on its low viscosity and fluidity to quickly penetrate into the capillary pores of the substrate. As the solvent evaporates, it reacts with the active components and completes cross-linking and curing inside the pores. At the same time, it chemically combines with the alkaline substances in the substrate, forming a three-in-one structure of penetration reinforcement, micropore sealing and surface sealing from the inside out, achieving high-strength sealing, anti-efflorescence, and solid foundation and anti-detachment effects.

[0031] In some implementations, the low-Tg styrene-acrylic emulsion has a Tg of 0–10°C and a particle size of 50–80 nm, exhibiting excellent penetration and wetting properties. It can work synergistically with potassium silicate to penetrate deep into the substrate and form a strong bond. The high-Tg pure acrylic emulsion has a Tg of 20–30°C and a particle size of 120–150 nm, demonstrating good film-forming properties. It can form a dense, sealed film on the substrate surface, reducing the water permeability of the primer and improving water resistance and hardness. The combination of these two emulsions forms an organic film-forming system, which synergistically works with the inorganic penetration system of potassium silicate to construct an inorganic-organic interpenetrating network structure, achieving both penetration reinforcement and sealing protection. Furthermore, both emulsions are selected as APEO-free, VOC-≤50g / L water-based emulsions to ensure the product's environmental compliance.

[0032] In some embodiments, the pigments and fillers are composed of ultrafine heavy calcium carbonate, wollastonite powder, nano-silica, and nano-zinc oxide in a mass ratio of 18:4:1.5:1.5. The ultrafine heavy calcium carbonate has a particle size of 1000 mesh, the wollastonite powder has a particle size of 800 mesh, the nano-silica has a particle size of 10-20 nm, and the nano-zinc oxide has a particle size of 30-80 nm.

[0033] Among them, ultrafine heavy calcium carbonate (1000 mesh) has good filling properties, which can fill the micropores of the base layer, build a dense shielding layer, and reduce the water permeability of the primer; wollastonite powder (800 mesh) has excellent alkali resistance and reinforcing properties, which can improve the primer's resistance to salt efflorescence and mechanical strength; nano silica (10-20 nm) has high specific surface area and high activity, which can fill the micropores after the emulsion film is formed, further improving the sealing and hardness; nano zinc oxide has alkali resistance, antibacterial and weather resistance properties, which can work synergistically with wollastonite powder to improve the primer's resistance to salt efflorescence, while preventing the primer from becoming moldy and deteriorating.

[0034] In some embodiments, the environmentally friendly additive includes the following components in parts by weight: 1.5–2.5 parts of silane coupling agent; Film-forming aid 2.0–3.5 parts; 0.3–0.8 parts without APEO dispersant; 0.2–0.4 parts of organosilicon wetting agent; Defoamer 0.1-0.3 parts; pH adjuster 0.1–0.3 parts; 0.1 to 0.3 parts of BIT preservative.

[0035] The silane coupling agent selected is KH-560, which enhances the interfacial bonding between potassium silicate, emulsion, and substrate, preventing paint film peeling and improving the compatibility between potassium silicate and emulsion to avoid system stratification. The film-forming aid selected is alcohol ester-12, a low-VOC film-forming aid that lowers the film-forming temperature of the emulsion, ensuring the primer forms a dense film even at low temperatures, while controlling SVOC content within limits. The APEO-free dispersant selected is Sanopco 5027, which ensures uniform dispersion of pigments and fillers in the system, prevents sedimentation, reduces primer viscosity, and improves application performance. The silicone wetting agent selected is GENAPOL PF20, which improves the wetting performance of the primer on high-alkali substrates and assists in the penetration of potassium silicate and emulsion. The defoamer selected is 5800D mineral oil defoamer, which effectively inhibits and eliminates bubbles generated during primer preparation, preventing pinholes in the paint film and affecting sealing properties. The pH adjuster selected is AMP-95, which can stabilize the system pH within the range of 8.0 to 9.0 and prevent potassium silicate gel and emulsion hydrolysis. The BIT preservative selected is Hanning 701, and the MIT content in the preservative is ≤300mg / kg, which can effectively prevent the primer from becoming moldy and deteriorating during storage and use, while meeting the limit requirements of GB 30981.1-2025.

[0036] The performance indicators of the primer of this invention meet the following requirements: (1) Meets the JG / T 210-2018 standard for film-forming type of exterior wall: water permeability ≤0.3mL, salt and alkali resistance ≥120h with no blistering, no efflorescence, no discoloration, reinforcement performance ≥0.2MPa, surface drying time ≤2h, actual drying time ≤24h, adhesion to cement board ≥1MPa, water resistance (96h) no abnormality, alkali resistance (48h, 0.5% NaOH solution) no abnormality; (2) Meets the limits of GB 30981.1-2025: VOC≤80g / L, SVOC≤150g / L, formaldehyde≤100mg / kg, lead≤90mg / kg, arsenic≤60mg / kg, APEO≤100mg / kg.

[0037] The preparation method of the above-mentioned highly sealing and penetrating primer, such as Figure 2 As shown, it includes the following steps: (1) Pre-dispersion: Add deionized water, organosilicon wetting agent, APEO-free dispersant, defoamer, and pH adjuster to the dispersion vessel, and stir at a low speed of 280-320 r / min for 4-6 min to adjust the pH of the system to 8.0-9.0. Mix evenly to obtain a pre-dispersion. Low-speed stirring can avoid the generation of a large number of bubbles and ensure that the additives are evenly dispersed. Adjusting the pH to 8.0-9.0 can prevent gelation after the subsequent addition of potassium silicate and stabilize the emulsion system to avoid emulsion hydrolysis.

[0038] (2) Filler grinding: Add pigments and fillers to the pre-dispersion liquid, heat to 38-42℃, and disperse at a high speed of 1200-1500 r / min for 20-30 min until the fineness of the slurry is ≤30μm, and then cool down to ≤40℃. Heating can improve the dispersion efficiency of pigments and fillers, and high-speed dispersion can ensure that pigments and fillers are fully dispersed, ensuring that they can play a dense shielding role. Controlling the fineness to ≤30μm can avoid the paint film from having a grainy feel and affecting the sealing performance; cooling down to ≤40℃ can prevent the emulsion from breaking down due to high temperature when the emulsion is added later.

[0039] (3) Potassium silicate premixing: Add potassium silicate and silane coupling agent to another stirred tank, and stir at a low speed of 180-220 r / min for 8-12 min to obtain a uniform potassium silicate premixed solution. Premixing potassium silicate alone can avoid its direct contact with the emulsion, which would lead to excessively high local concentration and gelation. It also ensures that potassium silicate and the additives are fully combined, thereby improving the permeability and compatibility.

[0040] (4) Emulsion compounding: Add the compounded primer emulsion to the ground slurry obtained in step (2), and stir at a medium speed of 580-620 r / min for 13-17 min. Then, slowly add the potassium silicate premix obtained in step (3) dropwise for ≥10 min. After the addition is complete, continue stirring for 8-12 min to form a uniform and stable system. Medium-speed stirring ensures that the emulsion is uniformly dispersed in the slurry. Slowly adding the potassium silicate premix and extending the stirring time allows the potassium silicate to fully integrate with the emulsion, forming an inorganic-organic interpenetrating network structure and avoiding system stratification and gelation.

[0041] (5) Viscosity Adjustment and Filtration: Add film-forming aid and BIT preservative to the system obtained in step (4), stir for 4-6 minutes, then add deionized water to adjust the primer viscosity to 35±5s (Ford-4 cup, 25℃), filter with a 100-mesh filter, and package after filtration to obtain a high-sealing penetration primer. After adding the film-forming aid and preservative, stir thoroughly to ensure uniform dispersion; adjusting the viscosity to 35±5s can improve the primer's workability and facilitate application; filtration with a 100-mesh filter can remove impurities and unevenly dispersed particles from the system, ensuring uniform primer quality.

[0042] The present invention will be further described below through Examples 1-3 and Comparative Examples 1-15.

[0043] Example 1 A highly sealing and penetrating primer based on potassium silicate and emulsion, with the following raw material composition by weight: Potassium silicate (modulus 2.2, solid content 30%, Na2O ≤ 2%, pH 12.5): 8.0 parts; Compound primer emulsion (low Tg styrene-acrylic emulsion Tg 5℃, particle size 60nm, high Tg pure acrylic emulsion Tg 25℃, particle size 130nm, mass ratio 8:1, both without APEO, VOC ≤50g / L): 60.0 parts; Pigments and fillers (1000-mesh ultrafine heavy calcium carbonate, 800-mesh wollastonite powder, 15nm nano silica, 50nm nano zinc oxide, mass ratio 18:4:1.5:1.5): 25.0 parts; Environmentally friendly additives: 2 parts silane coupling agent KH-560, 3 parts alcohol ester-12, 0.8 parts APEO-free dispersant (Shengnuopco 5027 dispersant), 0.3 parts organosilicon wetting agent (wetting agent GENAPOL PF20), 0.3 parts mineral oil defoamer (5800D), 0.2 parts AMP-95, 0.2 parts BIT preservative (Hanning 701); Deionized water: appropriate amount.

[0044] The preparation method includes the following steps: (1) Pre-dispersion: Add deionized water, organosilicon wetting agent, APEO-free dispersant, mineral oil defoamer and AMP-95 to the dispersion vessel, stir at a low speed of 300r / min for 5min, adjust the pH of the system to 8.5, mix evenly to obtain a pre-dispersion liquid; (2) Filler dispersion: Add pigments and fillers to the pre-dispersion liquid, heat to 40℃, disperse at high speed of 1300r / min for 25min until the fineness of the slurry is ≤30μm, and then cool down to 38℃; (3) Potassium silicate premix: Add potassium silicate and KH-560 to another stirred tank and stir at a low speed of 200r / min for 10min to obtain potassium silicate premix solution; (4) Emulsion compounding: Add compound primer emulsion to the slurry obtained in step (2) and stir at a medium speed of 600 r / min for 15 min. Then slowly add potassium silicate premix obtained in step (3) for 12 min. After the addition is complete, continue stirring for 10 min to form a uniform and stable system. (5) Viscosity adjustment and filtration: Add alcohol ester-12 and BIT preservative to the system obtained in step (4), stir for 5 minutes, add deionized water to adjust the viscosity of the primer to 35s (Ford-4 cup, 25℃), filter with a 100-mesh filter, and package to obtain the finished product.

[0045] Performance testing: (1) JG / T 210-2018 Standard test for film-forming type of exterior wall: water permeability 0.22mL, no abnormality in salt efflorescence resistance for 120h, reinforcement strength 0.28MPa, surface drying time 1.2h, actual drying time 18h, adhesion to cement board 1.2MPa, water resistance (96h) no abnormality, alkali resistance (48h, 0.5% NaOH solution) no abnormality; (2) GB 30981.1-2025 standard test: VOC 42g / L, SVOC 85g / L, formaldehyde 28mg / kg, lead not detected, arsenic not detected, APEO not detected, MIT 120mg / kg, all of which meet the standard limits.

[0046] Example 2 A highly sealing and penetrating primer based on potassium silicate and emulsion, with the following raw material composition by weight: Potassium silicate (modulus 2.0, solid content 28%, Na2O ≤ 2%, pH 12.3): 5.0 parts; Compound primer emulsion (low Tg styrene-acrylic emulsion Tg0℃, particle size 50nm, high Tg pure acrylic emulsion Tg20℃, particle size 120nm, mass ratio 7:1, both without APEO, VOC ≤50g / L): 55.0 parts; Pigments and fillers (1000-mesh ultrafine heavy calcium carbonate, 800-mesh wollastonite powder, 10nm nano silica, 50nm nano zinc oxide, mass ratio 18:4:1.5:1.5): 20.0 parts; Environmentally friendly additives: 2.0 parts of silane coupling agent KH-560, 2.5 parts of alcohol ester-12, 0.5 parts of APEO-free dispersant (Shengnuopco 5027 dispersant), 0.2 parts of organosilicon wetting agent (wetting agent GENAPOL PF20), 0.2 parts of mineral oil defoamer (5800D), 0.1 parts of AMP-95, and 0.1 parts of BIT preservative (Hanning 701); Deionized water: appropriate amount.

[0047] The preparation method is the same as in Example 1, only the process parameters are adjusted: Step (1) Stirring speed 280 r / min, stirring time 4 min, pH adjusted to 8.0; Step (2) Dispersion speed 1200 r / min, dispersion time 20 min, cooling to 39℃; Step (3) Stirring speed 180 r / min, stirring time 8 min; Step (4) Emulsion stirring speed 580 r / min, stirring time 13 min, potassium silicate premixed solution drop time 10 min, continue stirring for 8 min after drop; Step (5) Stirring time 4 min, viscosity adjusted to 32 s.

[0048] Performance testing: (1) JG / T 210-2018 Standard test for film-forming type of exterior wall: water permeability 0.25mL, no abnormality in salt efflorescence resistance for 120h, reinforcement strength 0.25MPa, surface drying time 1.5h, actual drying time 20h, adhesion to cement board 1.1MPa, water resistance (96h) no abnormality, alkali resistance (48h, 0.5% NaOH solution) no abnormality; (2) GB 30981.1-2025 standard test: VOC 38g / L, SVOC 78g / L, formaldehyde 25mg / kg, lead not detected, arsenic not detected, APEO not detected, MIT 100mg / kg, all of which meet the standard limits.

[0049] Example 3 A highly sealing and penetrating primer based on potassium silicate and emulsion, with the following raw material composition by weight: Potassium silicate (modulus 2.4, solid content 32%, Na2O ≤ 2%, pH 12.7): 10.0 parts; Compound primer emulsion (low Tg styrene-acrylic emulsion Tg10℃, particle size 80nm, high Tg pure acrylic emulsion Tg30℃, particle size 150nm, mass ratio 9:1, both without APEO, VOC ≤50g / L): 65.0 parts; Pigments and fillers (1000-mesh ultrafine heavy calcium carbonate, 800-mesh wollastonite powder, 20nm nano silica, 50nm nano zinc oxide, mass ratio 18:4:1.5:1.5): 23.0 parts; Environmentally friendly additives: 2.5 parts of silane coupling agent KH-560, 3.2 parts of alcohol ester-12, 0.6 parts of APEO-free dispersant (Shengnuopco 5027 dispersant), 0.5 parts of organosilicon wetting agent (wetting agent GENAPOL PF20), 0.4 parts of mineral oil defoamer (5800D), 0.2 parts of AMP-95, and 0.2 parts of BIT preservative (Hanning 701); Deionized water: appropriate amount.

[0050] The preparation method is the same as in Example 1, except that the process parameters are adjusted: Step (1) Dispersion speed 320 r / min, stirring time 6 min, pH adjusted to 9.0; Step (2) Dispersion speed 1500 r / min, dispersion time 30 min, cooling to 40℃; Step (3) Stirring speed 220 r / min, stirring time 12 min; Step (4) Emulsion stirring speed 620 r / min, stirring time 17 min, potassium silicate premixed solution drop time 15 min, and stirring continued for 12 min after drop; Step (5) Stirring time 6 min, viscosity adjusted to 38 s.

[0051] Performance testing: (1) JG / T 210-2018 Standard test for film-forming type of exterior wall: water permeability 0.28mL, no abnormality in salt efflorescence resistance for 120h, reinforcement strength 0.23MPa, surface drying time 1.8h, actual drying time 22h, adhesion to cement board 1.0MPa, water resistance (96h) no abnormality, alkali resistance (48h, 0.5% NaOH solution) no abnormality; (2) GB 30981.1-2025 standard test: VOC 45g / L, SVOC 92g / L, formaldehyde 30mg / kg, lead not detected, arsenic not detected, APEO not detected, MIT 150mg / kg, all of which meet the standard limits.

[0052] Comparative Example 1 (Compound primer emulsion, without potassium silicate) A primer, the same as in Example 1, except that "potassium silicate is not added".

[0053] The preparation method is the same as in Example 1, except that: "Delete step (3);" Step (4) is as follows: Emulsion compounding: Add the compounded primer emulsion to the ground slurry obtained in step (2), stir at a medium speed of 600 r / min for 15 min, then slowly add KH-560 dropwise over a period of 12 min. After the addition is complete, continue stirring for 10 min to form a uniform and stable system. Performance testing: water permeability 0.45mL (standard <0.3), blistering resistance after 72h (standard no abnormality), reinforcement strength 0.12MPa (standard ≥0.2MPa), and other indicators meet the requirements of JG / T 210-2018 and GB 30981.1-2025 standards.

[0054] Comparative Example 2 (Single Low Tg Styrene-Acrylic Emulsion) A primer, the same as in Example 1, except that: the “compound primer emulsion” is replaced with “low Tg styrene-acrylic emulsion (low Tg styrene-acrylic emulsion Tg 5℃, particle size 60nm, no APEO, VOC ≤ 50g / L)”.

[0055] The preparation method is the same as in Example 1, except that: Step (4) is: emulsion compounding: add low Tg styrene-acrylic emulsion to the ground slurry obtained in step (2), stir at a medium speed of 600 r / min for 15 min, and then slowly add potassium silicate premixed solution obtained in step (3) for 12 min. After the addition is completed, continue stirring for 10 min to form a uniform and stable system.

[0056] Performance testing: water permeability 0.35mL (standard <0.3ml), reinforcement strength 0.2MPa (standard >0.2MPa), water resistance (96h) no abnormalities in the paint film, alkali resistance (96h) no abnormalities in alkali efflorescence, does not meet the requirements of JG / T 210-2018 Type I standard.

[0057] Comparative Example 3 (Single High Tg Styrene-Acrylic Emulsion) A primer, the same as in Example 1, except that: the "compound primer emulsion" is replaced with "high Tg pure acrylic emulsion (high Tg pure acrylic emulsion Tg25℃, particle size 130nm, no APEO, VOC≤50g / L)".

[0058] The preparation method is the same as in Example 1, except that: Step (4) is: emulsion compounding: add high Tg pure acrylic emulsion to the slurry obtained in step (2) and stir at a medium speed of 600 r / min for 15 min. Then slowly add the potassium silicate premix obtained in step (3) for 12 min. After the addition is complete, continue stirring for 10 min to form a uniform and stable system. Performance testing: water permeability 0.2mL (standard <0.3ml), reinforcement strength 0.15MPa (standard >0.2MPa), water resistance (96h) no abnormalities in the paint film, alkali resistance (96h) no abnormalities in alkali efflorescence, does not meet the requirements of JG / T 210-2018 Type I standard.

[0059] Potassium silicate parameter study Comparative Example 4 A primer, the same as in Example 1, except that: "potassium silicate (modulus 2.2, solid content 30%, Na2O ≤ 2%, pH 12.5)" is replaced with "potassium silicate (modulus 1.8, solid content 26%, Na2O 2.5%, pH 12.0)".

[0060] The preparation method is the same as in Example 1.

[0061] Performance testing: After 7 days of storage, the system showed slight whitening, water permeability of 0.34 mL (standard < 0.3 mL), reinforcement strength of 0.17 MPa (standard > 0.2 MPa), and alkali efflorescence resistance after 96 hours, failing to meet the JG / T 210-2018 External Wall Type I film-forming index; Comparative Example 4-B: During the preparation process, the system locally gelled, and after filtration, small particles were still present, with water permeability of 0.36 mL (standard < 0.3 mL) and reinforcement strength of 0.16 MPa (standard > 0.2 MPa).

[0062] Comparative Example 5 A primer, the same as in Example 1, except that: "potassium silicate (modulus 2.2, solid content 30%, Na2O ≤ 2%, pH 12.5)" is replaced with "potassium silicate (modulus 2.6, solid content 34%, Na2O 2.8%, pH 13.1)".

[0063] The preparation method is the same as in Example 1.

[0064] Performance testing: During the preparation process, the system exhibited localized gelation, and even after filtration, small particles remained. The water permeability was 0.36 mL (standard < 0.3 mL), the reinforcement strength was 0.16 MPa (standard > 0.2 MPa), and it foamed after 96 hours of efflorescence resistance and separated into layers after 30 days of storage, failing to meet the usage requirements. The results indicate that the system foamed after 96 hours of efflorescence resistance and separated into layers after 30 days of storage, failing to meet the usage requirements.

[0065] Compared with Example 1 and Comparative Examples 4-5, potassium silicate can only achieve a balance between permeation reinforcement, alkali resistance and storage stability when controlled within the parameter range of modulus 2.0-2.4, solid content 28-32%, Na2O≤2%, and pH 12.5±0.5.

[0066] Studies on different low-Tg styrene-acrylic emulsions and high-Tg pure acrylic emulsions Comparative Example 6 A primer, the same as in Example 1, except that: "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg25℃)" is replaced with "compound primer emulsion (low Tg styrene-acrylic emulsion Tg-5℃, high Tg pure acrylic emulsion Tg25℃)".

[0067] The preparation method is the same as in Example 1.

[0068] Performance testing: The paint film is relatively soft; the water resistance is whitish after 96 hours; the water permeability is 0.33 mL (standard < 0.3 mL); and there are no abnormalities in the salt and alkali resistance after 96 hours.

[0069] Comparative Example 7 A primer, the same as in Example 1, except that: "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg25℃)" is replaced with "compound primer emulsion (low Tg styrene-acrylic emulsion Tg15℃, high Tg pure acrylic emulsion Tg25℃)".

[0070] The preparation method is the same as in Example 1.

[0071] Performance testing: The Tg of the styrene-acrylic emulsion is too high, resulting in decreased permeability and a reinforcement strength of 0.16 MPa (standard > 0.2 MPa).

[0072] Comparative Example 8 A primer, the same as in Example 1, except that: "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg25℃)" is replaced with "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg15℃)".

[0073] The preparation method is the same as in Example 1.

[0074] Performance testing: The Tg of the pure acrylic emulsion is low, the surface film density is insufficient, and the water permeability is 0.37mL (standard <0.3ml).

[0075] Comparative Example 9 A primer, the same as in Example 1, except that: "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg25℃)" is replaced with "compound primer emulsion (low Tg styrene-acrylic emulsion Tg5℃, high Tg pure acrylic emulsion Tg35℃)".

[0076] The preparation method is the same as in Example 1.

[0077] Performance testing: If the Tg of pure acrylic emulsion is too high, the paint film is prone to micro-cracks, and the adhesion is 0.82MPa (≥1MPa).

[0078] Comparative Examples 6-9 do not fully meet all the indicators of JG / T 210-2018 External Wall Type I Film-Forming Emulsion. This indicates that only a combination of low-Tg styrene-acrylic emulsion with a Tg of 0-10℃ and high-Tg pure acrylic emulsion with a Tg of 20-30℃ can simultaneously achieve both penetration reinforcement and surface sealing effects.

[0079] Study on low-Tg styrene-acrylic emulsions and high-Tg pure acrylic emulsions with different mass ratios Comparative Example 10 A primer, the same as in Example 1, except that: "compound primer emulsion (mass ratio of low Tg styrene-acrylic emulsion Tg5℃ to high Tg pure acrylic emulsion Tg25℃ 8:1)" is replaced with "compound primer emulsion (mass ratio of low Tg styrene-acrylic emulsion Tg5℃ to high Tg pure acrylic emulsion Tg25℃ 5:1)".

[0080] The preparation method is the same as in Example 1.

[0081] Performance testing: The high proportion of high Tg pure acrylic emulsion resulted in decreased primer penetration and a reinforcement strength of 0.17 MPa (standard > 0.2 MPa).

[0082] Comparative Example 11 A primer, the same as in Example 1, except that: "compound primer emulsion (mass ratio of low Tg styrene-acrylic emulsion Tg5℃ to high Tg pure acrylic emulsion Tg25℃ 8:1)" is replaced with "compound primer emulsion (mass ratio of low Tg styrene-acrylic emulsion Tg5℃ to high Tg pure acrylic emulsion Tg25℃ 10:1)".

[0083] The preparation method is the same as in Example 1.

[0084] Performance testing: The proportion of low Tg styrene-acrylic emulsion is too high, the surface film density is insufficient, the water permeability is 0.34mL (standard <0.3ml), and the salt efflorescence resistance is 96h.

[0085] Comparing Example 1 and Comparative Examples 10-11, it is shown that the mass ratio of the emulsion compound must be controlled at (7-9):1 in order to balance the two major properties of penetration reinforcement and surface sealing.

[0086] Study on pigment and filler ratio Comparative Example 12 A primer, the same as in Example 1, except that: the "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm nano zinc oxide, mass ratio 18:4:1.5:1.5)" is replaced with "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm nano zinc oxide, mass ratio 20:2:1.5:1.5)" (reducing the proportion of wollastonite powder and increasing the proportion of heavy calcium carbonate).

[0087] The preparation method is the same as in Example 1.

[0088] Performance testing: Lacking wollastonite powder reinforcement, efflorescence occurred after 96 hours of salt efflorescence resistance, and water permeability was 0.33 mL (standard < 0.3 mL).

[0089] Comparative Example 13 A primer, the same as in Example 1, except that: the "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm nano zinc oxide, mass ratio 18:4:1.5:1.5)" is replaced with "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm zinc oxide, mass ratio 14:8:1.5:1.5)" (increasing the proportion of wollastonite powder and reducing heavy calcium carbonate).

[0090] The preparation method is the same as in Example 1.

[0091] Performance testing: Excessive wollastonite powder increases slurry viscosity, makes it difficult to meet fineness standards, results in noticeable granular texture in the paint film, and reduces adhesion to 0.86 MPa (≥1 MPa).

[0092] Comparative Example 14 A primer, the same as in Example 1, except that: "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm zinc oxide, mass ratio 18:4:1.5:1.5)" is replaced with "pigment and filler (1000 mesh ultrafine heavy calcium carbonate, 800 mesh wollastonite powder, 15 nm nano silica, 50 nm zinc oxide, mass ratio 18:4:0:3.0)" (nano silica is removed, and zinc oxide is increased).

[0093] The preparation method is the same as in Example 1.

[0094] Performance testing: The micropores are not filled with nano-silica, the paint film has many pores, water permeability is 0.38mL (standard <0.3ml), and the sealing effect is poor.

[0095] Therefore, it can be seen that under the specific pigment and filler ratio of the present invention, the fillers work together to fill, reinforce and resist alkali, so as to achieve high sealing and resistance to salt efflorescence.

[0096] Comparative Example 15 A primer, with the same formulation as in Example 1.

[0097] The preparation method is the same as in Example 1, except that: "Delete step (3) potassium silicate premixing; " Step (4) is as follows: Emulsion compounding: Add the compounded primer emulsion to the ground slurry obtained in step (2), stir at a medium speed of 600 r / min for 15 min, and directly and quickly add the unmixed potassium silicate and KH-560 to the slurry system at one time, stir for 10 min, and form a uniform and stable system. Performance and condition testing: Gel particles appeared locally during the preparation process, and a small amount of fine gel particles remained after filtration through a 100-mesh sieve; the finished product showed stratification after 60 days of storage; water permeability was 0.32 mL (standard < 0.3 mL), reinforcement strength was 0.18 MPa (standard > 0.2 MPa), and bubbling occurred after 96 hours of salt efflorescence resistance.

[0098] This indicates that potassium silicate and silane coupling agents must be premixed separately. If potassium silicate is directly added to the emulsion-slurry system, excessively high local concentrations can easily lead to gelation, which will compromise system stability and reduce the primer's strengthening and sealing properties. As can be seen from the comparison of Examples 1-3 and Comparative Examples 1-15, the present invention adopts a synergistic system of potassium silicate and compound emulsion, combined with optimized formulation and preparation process, which significantly improves the penetration, sealing, anti-efflorescence and environmental performance of the primer. All indicators meet the requirements of JG / T 210-2018 and GB 30981.1-2025 standards, and are superior to existing pure organic emulsion primers and single potassium silicate primers.

[0099] The technical solutions provided by the embodiments of the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the embodiments of the present invention. The descriptions of the embodiments above are only for helping to understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the embodiments of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.

Claims

1. A high block permeation primer, characterized by, Includes the following ingredients by weight: Potassium silicate 5.0–10.0 parts; 55.0–65.0 parts of compound primer emulsion; Pigments and fillers: 20.0–25.0 parts; Environmentally friendly additives: 4.0–8.0 parts; Appropriate amount of deionized water; The potassium silicate is a low-modulus stabilized potassium silicate with a modulus of 2.0 to 2.4, a solid content of 28% to 32%, Na₂O ≤ 2%, and pH 12.5 ± 0.

5. The compound primer emulsion is prepared by compounding low Tg styrene-acrylic emulsion and high Tg pure acrylic emulsion at a mass ratio of (7-9):

1.

2. The highly sealing and penetrating primer according to claim 1, characterized in that, The low-Tg styrene-acrylic emulsion has a Tg of 0–10 °C and a particle size of 50–80 nm.

3. The highly sealing and penetrating primer according to claim 1, characterized in that, The high-Tg pure acrylic emulsion has a Tg of 20–30 °C and a particle size of 120–150 nm.

4. The highly sealing and penetrating primer according to claim 1, characterized in that, The pigments and fillers are composed of ultrafine heavy calcium carbonate, wollastonite powder, nano silica, and nano zinc oxide in a mass ratio of 18:4:1.5:1.

5.

5. The highly sealing and penetrating primer according to claim 4, characterized in that, The ultrafine heavy calcium carbonate has a particle size of 1000 mesh, the wollastonite powder has a particle size of 800 mesh, the nano-silica has a particle size of 10-20 nm, and the nano-zinc oxide has a particle size of 30-80 nm.

6. The highly sealing and penetrating primer according to claim 1, characterized in that, The environmentally friendly additives comprise the following components by weight: 1.5 to 2.5 parts of silane coupling agent; Film-forming aid 2.0–3.5 parts; 0.3–0.8 parts without APEO dispersant; 0.2–0.4 parts of organosilicon wetting agent; Defoamer 0.1-0.3 parts; pH adjuster 0.1–0.3 parts; 0.1 to 0.3 parts of BIT preservative.

7. The highly sealing and penetrating primer according to claim 6, characterized in that, The silane coupling agent is KH-560; the film-forming aid is alcohol ester-12; the APEO-free dispersant is Sanopco 5027 dispersant; the organosilicon wetting agent is GENAPOL PF20; the defoamer is 5800D mineral oil defoamer; the pH adjuster is AMP-95; and the BIT preservative is Hanning 701 with an MIT content ≤300mg / kg.

8. The highly sealing and penetrating primer according to claim 1, characterized in that, The primer conforms to the JG / T210-2018 standard for exterior wall type I film-forming coating: water permeability ≤0.3mL, salt and alkali resistance ≥120h with no bubbling, no efflorescence, no discoloration, reinforcement performance ≥0.2MPa, surface drying time ≤2h, complete drying time ≤24h, adhesion to cement board ≥1MPa, water resistance (96h) without abnormalities, alkali resistance (48h, 0.5% NaOH solution) without abnormalities; and meets the limits of GB 30981.1-2025 standard: VOC≤80g / L, SVOC≤150g / L, formaldehyde≤100mg / kg, lead≤90mg / kg, arsenic≤60mg / kg, APEO≤100mg / kg.

9. A method for preparing a highly sealing and penetrating primer as described in any one of claims 1 to 8, characterized in that, Includes the following steps: (1) Pre-dispersion: Add deionized water, organosilicon wetting agent, APEO-free dispersant, defoamer and pH adjuster to the dispersion vessel, stir at a low speed of 280-320 r / min for 4-6 min, adjust the pH of the system to 8.0-9.0, mix evenly to obtain a pre-dispersion liquid; (2) Filler grinding: Add pigments and fillers to the pre-dispersion liquid, heat to 38-42℃, disperse at high speed of 1200-1500r / min for 20-30min until the fineness of the slurry is ≤30μm, and then cool down to ≤40℃; (3) Potassium silicate premix: Add potassium silicate and silane coupling agent to another stirred tank and stir at a low speed of 180-220 r / min for 8-12 min to obtain a uniform potassium silicate premix solution; (4) Emulsion compounding: Add compound primer emulsion to the dispersed slurry obtained in step (2), stir at a medium speed of 580-620 r / min for 13-17 min, then slowly add potassium silicate premix obtained in step (3) for ≥10 min, and continue stirring for 8-12 min after the addition is complete to form a uniform and stable system. (5) Viscosity adjustment and filtration: Add film-forming aid and BIT preservative to the system obtained in step (4), stir for 4 to 6 minutes, then add deionized water to adjust the viscosity of the primer to 35 ± 5 seconds, and after filtration, a high-sealing penetration primer is obtained.

10. The method for preparing a highly sealing and penetrating primer according to claim 9, characterized in that, In step (1), the pH of the system is adjusted to 8.5±0.5; in step (2), the dispersion speed is 1300r / min and the dispersion time is 25min; in step (4), the emulsion stirring speed is 600r / min and the stirring time is 15min, the potassium silicate premix is ​​added dropwise for 10-15min, and stirring is continued for 10min after addition; in step (5), the stirring time is 5min.