A wear-resistant silver plating protective agent and its preparation method

By synergistically designing nano-silica and oleoyl sarcosine and employing a temperature-controlled mixing process, the wear resistance and corrosion resistance of the silver plating layer are improved. This solves the problem of the difficulty in achieving both wear resistance and corrosion resistance in existing technologies, enabling the preparation of a highly efficient and environmentally friendly protective layer that meets the requirements for use over a wide temperature range.

CN123107512APending Publication Date: 2026-11-17深圳市安美科化学技术有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202511907826.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silver plating protective agents are difficult to balance wear resistance and corrosion resistance, have low preparation efficiency, poor environmental adaptability, and the protective layer is prone to peeling off under high-frequency friction scenarios. Furthermore, the film-forming agent and functional additives have poor compatibility.

Method used

A synergistic system of nano-silica and oleoyl sarcosine, combined with a compound emulsifier of OP-10 and isomeric tridecyl alcohol polyoxyethylene ether, is used to optimize the molecular weight of polyethylene glycol through a three-stage temperature-controlled mixing process, ensuring the dispersion of nanoparticles and the integrity of the film layer.

Benefits of technology

It achieves a more than 20% increase in the wear resistance of the silver plating, a 10%-20% extension in the 5% potassium sulfide test time, a 6%-12% extension in the neutral salt spray test time, maintains good performance in the range of -20℃ to 80℃, has excellent protective layer integrity, and good environmental performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a wear-resistant silver plating protective agent and its preparation method, relating to the field of materials chemistry. Each liter of the protective agent of this invention comprises the following components: 45-55g of n-octadecyl mercaptan, 6-9g of nano-silica, 3-6g of oleylsarcosine, 3-5g of octylphosphonic acid, 2-4g of benzotriazole, 30-45g of OP-10 and isomeric tridecyl alcohol polyoxyethylene ether emulsifier, 8-12g of polyethylene glycol, 4-6g of ethylene glycol phenyl ether, and the balance being deionized water. This invention pioneers a wear-resistant and dense synergistic system of "nano-silica (20-40nm) + oleoyl sarcosine" to solve the problem of wear / corrosion imbalance of single components; it designs a specific compounding ratio (1:(1-1.2)) of OP-10 and isomeric tridecyl alcohol polyoxyethylene ether to improve the dispersibility of nanoparticles and reduce the difficulty of cleaning; it develops a three-stage temperature-controlled mixing process to balance production efficiency and film integrity; this invention achieves synergistic improvement in wear resistance and corrosion resistance, with significantly optimized preparation process, strong environmental adaptability, excellent protective layer integrity, and good environmental performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials chemistry, specifically to a wear-resistant silver plating protective agent and its preparation method. Background Technology

[0002] Silver plating is widely used in electronics, communications, precision instruments, jewelry, and other fields due to its excellent electrical conductivity, thermal conductivity, and aesthetic appeal. However, silver plating faces two major technical challenges during use: First, silver readily reacts with corrosive gases such as sulfides and halides in the air, forming black or grayish-white compounds such as silver sulfide and silver chloride, leading to discoloration and decreased conductivity of the plating. Second, under mechanical friction, especially in high-frequency plugging and unplugging scenarios such as electronic connectors, the protective layer is prone to peeling off, further accelerating the corrosion and failure of the silver plating. The existing technology has the following drawbacks: (1) Poor synergy between wear resistance and corrosion resistance Existing technologies generally suffer from the problem of not being able to simultaneously achieve both wear resistance and corrosion resistance. For example, the existing invention patent with publication number CN108193209A introduces reduced graphene oxide, which can withstand a 5% potassium sulfide test for 12 minutes, but no quantitative test of wear resistance has been conducted; the existing invention patent with publication number CN110055523B has a wear resistance of about 1500 cycles (estimated based on its 352-day protection period), but the longest time to withstand a 5% potassium sulfide test is only 50 minutes; the existing invention patent with publication number CN116516331A adds oleylsarcosine to improve the density of the protective film, and the potassium sulfide resistance can reach 27 minutes, but it is easy to soften at high temperatures (>60℃), resulting in a significant decrease in wear resistance.

[0003] (2) Low process efficiency Existing technologies generally suffer from high energy consumption and long production cycles. Existing invention patent CN108193209A requires ultrasonic dispersion at 30kHz for 6 hours, and existing invention patent CN110055523B requires high-speed stirring at 800-1000r / min. These process conditions not only consume more than 30% more energy than this invention, but also extend the production cycle by two times, severely impacting industrial production efficiency.

[0004] (3) Poor environmental adaptability Existing protective agents have a narrow operating temperature range, making it difficult to adapt to temperature changes in different application scenarios. Existing invention patent CN110230061A uses film-forming agents such as paraffin wax and polyethylene wax, which exhibit brittleness at -10℃ and begin to soften above 60℃. Existing invention patent CN116516331A also uses paraffin wax as a film-forming agent, which lacks sufficient high-temperature stability. Furthermore, the operating environment of electronic devices typically requires temperatures ranging from -20℃ to 80℃, a requirement that existing technologies cannot meet.

[0005] (4) Poor integrity of the protective layer In high-frequency friction scenarios, the protective layer formed by existing protective agents is prone to peeling off. The existing invention patent with publication number CN115700296A uses OP / NP series emulsifiers, which are easy to clean and have minimal impact on the conductivity of the silver layer, but do not contain hard reinforcing particles, resulting in weak wear resistance and making them only suitable for low-friction scenarios. The existing invention patent with publication number CN108070863A uses octadecyl mercaptosulfonate + mercaptotetrazole components, with a maximum K2S resistance test time of 20 minutes, but does not contain wear-resistant reinforcing components, and the protective layer only focuses on preventing discoloration and cannot resist mechanical friction.

[0006] In summary, the core technical root cause of the aforementioned defects in existing protective agents lies in: Lack of synergistic design of "hard particle filling + dense organic film": For example, the invention patent with publication number CN108070863A relies solely on thiol compounds to form a film, which has a certain anti-discoloration effect but lacks mechanical strength support; the existing invention patent with publication number CN115700296A does not add hard reinforcing particles, and cannot form an effective wear-resistant structure.

[0007] The nanoparticle dispersion process is unreasonable: Although the existing invention patent with announcement number CN110055523B adds nano-silica, it uses high-speed stirring at 800-1000r / min, which easily leads to local agglomeration of nanoparticles and forms weak areas in wear resistance; the existing invention patent with publication number CN108193209A has an excessively long ultrasonic dispersion time (6 hours), which is not only inefficient, but may also cause excessive breakage of nanoparticles, affecting the wear resistance effect.

[0008] Poor compatibility between film-forming agents and functional additives: The paraffin film-forming agents used in the existing invention patents published in CN110230061A and CN116516331A have poor compatibility with functional additives, and phase separation easily occurs when the temperature changes, resulting in unstable film performance.

[0009] The information disclosed in the background section is only intended to enhance the understanding of the background of this disclosure, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention

[0010] The purpose of this invention is to provide a wear-resistant silver plating protective agent and its preparation method to solve the problems mentioned in the background art.

[0011] To achieve the above objectives, the present invention provides the following technical solution: A wear-resistant silver plating protectant, each liter of the protectant comprising the following components: 45-55g of n-octadecyl mercaptan Nano silica: 6-9g Oleylsarcosine: 3-6g Octylphosphonic acid: 3-5g Benzotriazole: 2-4g OP-10 and isotridecyl alcohol polyoxyethylene ether compound emulsifier: 30-45g Polyethylene glycol: 8-12g Ethylene glycol phenyl ether: 4-6g The remainder is deionized water.

[0012] Preferably, the mass ratio of OP-10 to isotridecyl alcohol polyoxyethylene ether in the compound emulsifier is 1:(1-1.2).

[0013] Preferably, the particle size of the nano-silica is 20-40 nm.

[0014] Preferably, the molecular weight of the polyethylene glycol is 6000-8000.

[0015] A method for preparing a wear-resistant silver plating protective agent includes the following steps: Step 1: Preparation of component A: Add n-octadecyl mercaptan and benzotriazole to deionized water and stir for 30-40 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 2: Preparation of Component B: Add nano-silica and octylphosphonic acid to deionized water, ultrasonically disperse for 20-30 minutes, and then continue stirring for 20 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 3: Preparation of component C: Add OP-10 and isomeric tridecyl alcohol polyoxyethylene ether compound emulsifier, polyethylene glycol, and ethylene glycol phenyl ether to deionized water, and stir for 25-35 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 4: Preparation of component D: Dissolve oleoylsarcosine in a small amount of deionized water; Step 5, Mixing Process: First stage: Under the condition of stirring speed of 400-500r / min, add component B dropwise to component A. After the addition is complete, keep it at 50℃ for 40-50 minutes, and then cool it down to 25℃. Second stage: Under the condition of stirring speed of 400-500r / min, component C is added dropwise to the intermediate liquid. After the addition is completed, the temperature is raised to 55℃ and kept at 15-20 minutes, and then cooled to 25℃. Third stage: Add component D and stir for 15-20 minutes at a stirring speed of 300-400 r / min to obtain the wear-resistant silver plating protectant.

[0016] Preferably, the ultrasonic dispersion power in step two is 20 kHz.

[0017] Preferably, the dissolution temperature of oleoylsarcosine in step four is 40-45℃.

[0018] Preferably, the cooling rate in the first stage of step five is 8-10℃ / min, and the dropping rate of component B in the first stage is 1-2mL / min.

[0019] Preferably, the cooling rate in the second stage of step five is 1.5-2℃ / min, and the heating rate in the second stage is 3-5℃ / min.

[0020] Preferably, in the second stage of step five, the dropping rate of component C is 1-2 mL / min.

[0021] Compared with the prior art, the beneficial effects of the present invention are: 1. The first-ever wear-resistant and dense synergistic system of "nano silica (20-40nm) + oleoyl sarcosine" solves the problem of wear resistance / corrosion resistance imbalance of single components; 2. A specific compounding ratio (1:(1-1.2)) of OP-10 and isomeric tridecyl alcohol polyoxyethylene ether was designed to improve the dispersibility of nanoparticles and reduce the difficulty of cleaning. 3. A three-stage temperature-controlled mixing process was developed, balancing production efficiency and film integrity, reducing energy consumption by 30% compared to existing technologies; 4. Optimize the molecular weight (6000-8000) and addition amount (8-12g / L) of polyethylene glycol to ensure wide temperature adaptability from -20℃ to 80℃.

[0022] In summary, the wear-resistant silver plating protective agent provided by this invention synergistically improves wear resistance and corrosion resistance, has significantly optimized preparation process, strong environmental adaptability, excellent protective layer integrity, and good environmental performance. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0024] It should be noted that, unless otherwise defined, the technical or scientific terms used in this invention should have the ordinary meaning understood by one of ordinary skill in the art to which this invention pertains. The terms "first," "second," and similar terms used in this invention do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed following the word and their equivalents, without excluding other elements or objects. Terms such as "connected" or "linked" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. Terms such as "upper," "lower," "left," and "right" are used only to indicate relative positional relationships; when the absolute position of the described object changes, the relative positional relationship may also change accordingly. Example

[0025] This invention provides a technical solution: a wear-resistant silver plating protective agent and its preparation method, with the following formulation (per liter of protective agent): 45g of n-octadecyl mercaptan Nano silica (30nm particle size): 6g Oleylsarcosine: 3g Octylphosphonic acid: 3g Benzotriazole: 2g OP-10 emulsifier: 15g Isomeric tridecyl alcohol polyoxyethylene ether: 15g Polyethylene glycol (molecular weight 6000): 8g Ethylene glycol phenyl ether: 4g Deionized water: Add to 1L.

[0026] Preparation method: The preparation steps of the above technical solution are carried out, wherein the ultrasonic dispersion time is 20 minutes, the stirring speed is 500 r / min, the dropping acceleration rate is 1 mL / min, and the heating rate is 3℃ / min.

[0027] Performance test results: Wear resistance: 1800 cycles (according to GB / T1768-2006 standard, CS-10 grinding wheel, load 500g, speed 75r / min).

[0028] The test time for tolerance to 5% potassium sulfide is 55 minutes (at a constant temperature of 25°C and a stirring rate of 100 r / min).

[0029] Neutral salt spray resistance test time: 85 hours (according to GB / T10125-2021 standard, 5% sodium chloride solution, pH 6.5-7.2, temperature 35℃).

[0030] High and low temperature cycling performance: After 10 cycles at -20℃ / 80℃, the protective layer did not peel off.

[0031] Contact resistance change: The change in contact resistance before and after treatment is <5mΩ. Example

[0032] Formula composition (per liter of preservative): 50g of n-octadecyl mercaptan Nano-silica (particle size 25nm): 7.5g Oleylsarcosine: 4.5g Octylphosphonic acid: 4g Benzotriazole: 3g OP-10 emulsifier: 20g Isomerized tridecyl alcohol polyoxyethylene ether: 20g Polyethylene glycol (molecular weight 7000): 10g Ethylene glycol phenyl ether: 5g Deionized water: Add to 1L.

[0033] Preparation method: The preparation steps were carried out according to the above technical solution, wherein the ultrasonic dispersion time was 25 minutes, the stirring speed was 550 r / min, the dropping acceleration rate was 1.5 mL / min, and the heating rate was 4 °C / min.

[0034] Performance test results: Wear resistance: 2000 cycles (according to GB / T1768-2006 standard, CS-10 grinding wheel, load 500g, speed 75r / min).

[0035] The test time for tolerance to 5% potassium sulfide is 58 minutes (at a constant temperature of 25°C and a stirring rate of 100 r / min).

[0036] Neutral salt spray resistance test time: 88 hours (according to GB / T10125-2021 standard, 5% sodium chloride solution, pH 6.5-7.2, temperature 35℃).

[0037] High and low temperature cycling performance: After 10 cycles at -20℃ / 80℃, the protective layer showed no abnormalities.

[0038] Contact resistance change: The change in contact resistance before and after treatment is <3mΩ. Example

[0039] Formula composition (per liter of preservative): 55g of n-octadecyl mercaptan Nano silica (particle size 40nm): 9g Oleylsarcosine: 6g Octylphosphonic acid: 5g Benzotriazole: 4g OP-10 emulsifier: 25g Isomerized tridecyl alcohol polyoxyethylene ether: 20g Polyethylene glycol (molecular weight 8000): 12g Ethylene glycol phenyl ether: 6g Deionized water: Add to 1L.

[0040] Preparation method: The preparation steps of the above technical solution are carried out, wherein the ultrasonic dispersion time is 30 minutes, the stirring speed is 600 r / min, the dropping acceleration rate is 2 mL / min, and the heating rate is 5℃ / min.

[0041] Performance test results: Wear resistance: 2200 cycles (according to GB / T1768-2006 standard, CS-10 grinding wheel, load 500g, speed 75r / min).

[0042] The test time for tolerance to 5% potassium sulfide is 60 minutes (at a constant temperature of 25℃ and a stirring rate of 100r / min).

[0043] Neutral salt spray resistance test time: 90 hours (according to GB / T10125-2021 standard, 5% sodium chloride solution, pH 6.5-7.2, temperature 35℃).

[0044] High and low temperature cycling performance: After 10 cycles at -20℃ / 80℃, the protective layer showed no abnormalities.

[0045] Contact resistance change: The change in contact resistance before and after treatment is <4mΩ.

[0046] Comparative Example 1 (refer to CN110055523B): Formula composition: 50g / L octadecyl mercaptan, 6g / L trimethyl mercaptophosphate, 30g / L OP-10 emulsifier, 3g / L KH-560 coupling agent, 8g / L nano silica (10-50nm), 12g / L isopropanol, and 5g / L polyoxymethylene dimethyl ether.

[0047] Preparation process: stirring at 800 r / min, without ultrasonic dispersion.

[0048] Test results: After 1500 abrasion cycles, 48 ​​minutes of 5% potassium sulfide resistance, 78 hours of salt spray resistance, and 5 cycles at -20℃, the film layer became brittle.

[0049] Compared with Example 2: the wear resistance is improved by 25%, the potassium sulfide resistance is improved by 20.8%, the salt spray resistance is improved by 12.8%, and the high and low temperature adaptability is significantly better than the comparative example.

[0050] Comparative Example 2 (refer to CN108193209A): Formula composition: 2g / L reduced graphene oxide, 30g / L dodecyl mercaptan, 50g / L ethanol, and the balance of deionized water.

[0051] Preparation process: ultrasonic dispersion at 30KHz for 6 hours.

[0052] Test results: withstood 5% potassium sulfide for 12 minutes, no abrasion resistance test was conducted, and the process time was 6 hours.

[0053] Compared with Example 2: the potassium sulfide resistance was improved by 383% and the processing time was shortened by 95.8%.

[0054] Comparative Example 3 (refer to CN110230061A): Formula composition: paraffin wax 15g / L, polyethylene wax 10g / L, benzotriazole 5g / L, OP-7 emulsifier 8g / L.

[0055] Preparation process: Melt mixing at 60℃.

[0056] Test results: brittle at -10℃, softens above 60℃, withstands 800 abrasion cycles, and withstands 80 hours of salt spray.

[0057] Compared with Example 2: Temperature adaptability is significantly improved and wear resistance is improved by 150%.

[0058] The test results are shown in the table below:

[0059] Specifically, the mass ratio of OP-10 to isomeric tridecyl alcohol polyoxyethylene ether in the compound emulsifier is 1:(1-1.2). The technical logic for component selection is as follows: (1) Step 5: n-Octadecanthiol (45-55 g / L) Referring to the 40-60 g / L range in step five of CN 110055523, step five B, this invention limits the concentration to 45-55 g / L: Below 45 g, insufficient thiol complexation on the silver surface results in an anti-tarnishing time of <50 minutes; above 55 g, excessive film thickness leads to an increase in the contact resistance of the silver plating layer >10 mΩ (not meeting the requirements of electronic connectors). Therefore, the optimal middle range is chosen. Compared to step five of CN 108070863, step five A, the concentration control of this invention is more precise, ensuring a balance between anti-tarnishing performance and conductivity.

[0060] (2) Step 5: Nano-sized silica (particle size 20-40nm, 6-9g / L) Compared to the 10-50 nm particle size range in step five of CN 110055523, this invention limits the particle size to 20-40 nm: when the particle size is less than 20 nm, the nanoparticles are prone to agglomeration and have poor dispersibility; when the particle size is greater than 40 nm, they cannot effectively fill the micropores on the surface of the silver plating layer. A concentration range of 6-9 g / L ensures sufficient wear resistance enhancement while avoiding increased film brittleness due to excessive concentration.

[0061] (3) Step 5: Compound emulsifier (OP-10: isomeric tridecyl alcohol polyoxyethylene ether = 1:(1-1.2)) Existing technologies often use a single emulsifier (such as step five A of CN 115700296, which only uses OP-10). After compounding in this invention: OP-10 ensures hydrophilicity, and isomeric tridecyl alcohol polyoxyethylene ether improves the dispersibility of nano silica. At a ratio of 1:(1-1.2), the agglomeration rate of nanoparticles is <5% (far lower than the 15% agglomeration rate of OP-10 alone), and the protective agent is easy to clean (residue can be removed by washing once with water).

[0062] (4) Step 5 Polyethylene glycol (molecular weight 6000-8000, 8-12 g / L) Select a molecular weight range of 6000-8000: below 6000, low-temperature toughness is insufficient; above 8000, high-temperature stability decreases. An addition amount of 8-12 g / L ensures good performance within a temperature range of -20℃ to 80℃, solving the temperature sensitivity issues of Step 5A in CN5110230061 and Step 5A in CN5116516331.

[0063] Preparation method The preparation method of the above-mentioned wear-resistant silver plating protective agent includes the following steps: Step 1: Preparation of Component A Add n-octadecyl mercaptan and benzotriazole to deionized water and stir for 30-40 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min to obtain component A.

[0064] Step 2: Preparation of Component B Nano-silica and octylphosphonic acid were added to deionized water and ultrasonically dispersed for 20-30 minutes at a power of 20 kHz. Then, stirring was continued for 20 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min to obtain component B.

[0065] Step 3: Preparation of Component C Add OP-10, isomeric tridecyl alcohol polyoxyethylene ether emulsifier, polyethylene glycol, and ethylene glycol phenyl ether to deionized water, and stir for 25-35 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min to obtain component C.

[0066] Step 4: Preparation of Component D Oleylsarcosine was dissolved in a small amount of deionized water and stirred at 40-45℃ until completely dissolved to obtain component D.

[0067] Step 5: Mixing Process First stage: Under the condition of stirring speed of 400-500 r / min, component B is slowly added dropwise to component A at a rate of 1-2 mL / min. After the addition is completed, the temperature is kept at 50℃ for 40-50 minutes, and then the temperature is lowered to 25℃ at a cooling rate of 8-10℃ / min to obtain the intermediate solution. Second stage: Under the condition of stirring speed of 400-500r / min, component C is slowly added dropwise to the intermediate liquid at a rate of 1-2mL / min. After the addition is completed, the temperature is raised to 55℃ at a heating rate of 3-5℃ / min and kept at 55℃ for 15-20 minutes. Then the temperature is lowered to 25℃ at a cooling rate of 1.5-2℃ / min. Third stage: Add component D and stir for 15-20 minutes at a stirring speed of 300-400 r / min to obtain the wear-resistant silver plating protectant.

[0068] The necessity of process parameters: (1) Step 5 Ultrasonic dispersion parameters (20KHz, 20-30 minutes) Choosing 20kHz instead of 30kHz (CN step 5 108193209 step 5A): Because 30kHz will cause the nano silica particles to break down (<10nm), which will reduce the wear resistance; at 20kHz, the particle size is stable at 20-40nm, and 98% dispersion can be achieved in 20-30 minutes (shorter than 6 hours in CN step 5 108193209 step 5A, with a 12-fold increase in efficiency).

[0069] (2) Step 5: Control the stirring speed (300-600 r / min) Compared to step five of CN 110055523, which uses 800-1000 r / min, the rotational speed of this invention is reduced by 30%-40%, resulting in a significant reduction in energy consumption. Furthermore, the rotational speed is controlled in stages: 400-500 r / min during the mixing stage ensures sufficient dispersion, while 300-400 r / min in the final stage avoids performance degradation caused by excessive shearing.

[0070] (3) Step 5 Temperature Control Strategy The preparation stage uses 50-55℃ to ensure that all components are fully dissolved and reacted; the mixing stage uses gradient cooling (8-10℃ / min → 1.5-2℃ / min): rapid cooling forms the initial structure, and slow cooling eliminates internal stress and avoids the film cracking problem in step 5A of CN step 5 110230061.

[0071] (4) Step 5: Acceleration rate control (1-2 mL / min) Slow dropwise addition avoids agglomeration caused by excessively high local concentrations, ensuring uniform dispersion of nanoparticles and solving the problem of uneven dispersion caused by rapid mixing in step five of CN (110055523, step five B).

[0072] Specifically, the technical solution of this invention achieves a synergistic improvement in wear resistance and corrosion resistance. Through the synergistic effect of nano-silica filling the micropores of the coating and the dense protective film of oleoyl sarcosine, the silver coating achieves a wear resistance of 1800-2200 cycles, which is more than 20% higher than the 1500 cycles of step 5B in CN step 5 110055523; the resistance time to 5% potassium sulfide test reaches 55-60 minutes, which is 10%-20% higher than the 50 minutes of step 5B in CN step 5 110055523; and the resistance to neutral salt spray test reaches 85-90 hours, which is 6%-12% higher than the 80 hours of step 5A in CN step 5 110230061.

[0073] Significant process optimization The ultrasonic dispersion time is shortened to less than 30 minutes, which is 91.7% shorter than the 6 hours in step 5A of CN 108193209; the stirring speed is reduced to less than 600 r / min, which is 30%-40% lower than the 800-1000 r / min in step 5B of CN 110055523; the overall process energy consumption is reduced by more than 30%, and the production efficiency is significantly improved, which is conducive to large-scale industrial production.

[0074] Strong environmental adaptability Through the synergistic effect of polyethylene glycol and compound emulsifiers, the protective layer maintains good flexibility and wear resistance within a temperature range of -20℃ to 80℃, without embrittlement or softening. Compared with the -10℃ embrittlement observed in Step 5A of CN 110230061 and the 60℃ softening observed in Step 5A of CN 116516331, the temperature adaptability is significantly improved, enabling it to meet the temperature variation requirements of different application scenarios.

[0075] Excellent protective layer integrity In high-frequency friction scenarios, the protective layer is not easily detached and can maintain its protective effect for a long time, significantly extending the service life of the silver plating. Compared with the low wear resistance of steps 5A in CN 115700296 and steps 5A in CN 108070863, the protective layer of this invention still maintains its integrity after 1800-2200 friction cycles.

[0076] Good environmental performance All raw materials used are environmentally friendly and free of heavy metals such as hexavalent chromium, lead, and mercury (compliant with RoHS Step 5 2.0 standard), with heavy metal content <10ppm; volatile organic compound (VOC) content <5g / L (compliant with GB Step 5 38508-2020 "Limits of Volatile Organic Compounds in Cleaning Agents"); waste liquid can be directly biochemically treated, with COD value <300mg / L (lower than the 1000mg / L of existing solvent-based protective agents), reducing treatment costs by 60%.

[0077] The protection mechanism of this invention is as follows: (1) Step 5 Film Formation Stage The thiol group (-SH) of octadecyl mercaptan forms an Ag-S covalent bond with the Ag+ on the silver surface, constructing a basic anti-tarnishing film. This process is carried out at 50-55℃, and temperature control ensures that the thiol group reacts fully with the silver surface while avoiding the volatilization of thiol caused by excessive temperature.

[0078] (2) Step 5: Wear-resistant reinforcement Nano-silica (20-40nm) fills the micropores of the base film through the coupling effect of octylphosphonic acid (phosphine group combines with nano-silica hydroxyl group), forming a "hard particle framework". The particle size selection of 20-40nm ensures that it can effectively fill the micropores while avoiding unevenness of the film layer caused by excessive particle size.

[0079] (3) Step 5 densification process The amino group (-NH2) of oleoylsarcosine forms hydrogen bonds with the hydroxyl group (-OH) of nano-silica, and the carboxyl group (-COOH) complexes with the Ag⁺ residue on the silver surface, further reducing the porosity of the membrane (to <2%, far lower than the 5% of the prior art). This multi-action mechanism ensures the compactness and integrity of the membrane.

[0080] (4) Step 5 Environmental adaptation mechanism The long-chain structure of polyethylene glycol is interwoven within the film layer, preventing the film from becoming brittle at low temperatures (-20°C) and maintaining its elasticity at high temperatures (80°C). The molecular weight range of 6000-8000 ensures good performance over a wide temperature range, solving the temperature sensitivity problem of existing technologies.

[0081] (5) Step 5 Dispersion stabilization mechanism The compound system of OP-10 and isomeric tridecyl alcohol polyoxyethylene ether ensures the uniform dispersion of nano-silica through steric hindrance and electrostatic stabilization. The 1:(1-1.2) ratio optimizes the balance between hydrophilicity and dispersibility, keeping the nanoparticle aggregation rate below 5%.

[0082] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A wear-resistant silver plating protective agent, characterized in that, Each liter of the protective agent comprises the following components: 45-55g of n-octadecyl mercaptan Nano silica: 6-9g Oleylsarcosine: 3-6g Octylphosphonic acid: 3-5g Benzotriazole: 2-4g OP-10 and isotridecyl alcohol polyoxyethylene ether compound emulsifier: 30-45g Polyethylene glycol: 8-12g Ethylene glycol phenyl ether: 4-6g The remainder is deionized water.

2. The wear-resistant silver plating protective agent according to claim 1, characterized in that: The mass ratio of OP-10 to isotridecyl alcohol polyoxyethylene ether in the compound emulsifier is 1:(1-1.2).

3. The wear-resistant silver plating protective agent according to claim 1, characterized in that: The particle size of the nano-silica is 20-40 nm.

4. The wear-resistant silver plating protective agent according to claim 1, characterized in that: The molecular weight of the polyethylene glycol is 6000-8000.

5. A method for preparing a wear-resistant silver plating protective agent as described in any one of claims 1-4, characterized in that, Includes the following steps: Step 1: Preparation of component A: Add n-octadecyl mercaptan and benzotriazole to deionized water and stir for 30-40 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 2: Preparation of Component B: Add nano-silica and octylphosphonic acid to deionized water, ultrasonically disperse for 20-30 minutes, and then continue stirring for 20 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 3: Preparation of component C: Add OP-10 and isomeric tridecyl alcohol polyoxyethylene ether compound emulsifier, polyethylene glycol, and ethylene glycol phenyl ether to deionized water, and stir for 25-35 minutes at a temperature of 50-55℃ and a stirring speed of 500-600 r / min. Step 4: Preparation of component D: Dissolve oleoylsarcosine in a small amount of deionized water; Step 5, Mixing Process: First stage: Under the condition of stirring speed of 400-500r / min, add component B dropwise to component A. After the addition is complete, keep it at 50℃ for 40-50 minutes, and then cool it down to 25℃. Second stage: Under the condition of stirring speed of 400-500r / min, component C is added dropwise to the intermediate liquid. After the addition is completed, the temperature is raised to 55℃ and kept at 15-20 minutes, and then cooled to 25℃. Third stage: Add component D and stir for 15-20 minutes at a stirring speed of 300-400 r / min to obtain the wear-resistant silver plating protectant.

6. The method for preparing the wear-resistant silver plating protective agent according to claim 5, characterized in that: In step two, the ultrasonic dispersion power is 20 kHz.

7. The method for preparing the wear-resistant silver plating protective agent according to claim 5, characterized in that: In step four, the dissolution temperature of oleoylsarcosine is 40-45℃.

8. The method for preparing the wear-resistant silver plating protective agent according to claim 5, characterized in that: The cooling rate in the first stage of step five is 8-10℃ / min, and the dropping rate of component B in the first stage is 1-2mL / min.

9. The method for preparing the wear-resistant silver plating protective agent according to claim 5, characterized in that: The cooling rate in the second stage of step five is 1.5-2℃ / min, and the heating rate in the second stage is 3-5℃ / min.

10. The method for preparing the wear-resistant silver plating protective agent according to claim 5, characterized in that: In the second stage of step five, the dropping rate of component C is 1-2 mL / min.

Citation Information

Patent Citations

  • Surface protective agent for silver plating layer

    CN108070863A

  • High-stability water-base silver-plating protective agent and preparation method thereof

    CN108193209A

  • Water-based silver protective agent and its preparation method

    CN110055523B

  • Gold and silver surface anti-oxidation and anti-color-change protecting agent and preparation method and application thereof

    CN110230061A

  • Water-soluble silver protective agent and preparation and use method thereof

    CN115700296A