A high-performance elastomer coating and its preparation method and application process

By using a high-performance elastomer coating of components A and B with a specific formula and a high-temperature and high-pressure impact spraying technology, the problems of insufficient coating adhesion and long construction cycle on bamboo composite pipes have been solved. This has achieved high compatibility between the coating and the bamboo substrate and rapid curing, thereby improving corrosion resistance and construction efficiency.

CN123107523APending Publication Date: 2026-11-17ANHUI ZITING HENGHUI NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611316138.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing anti-corrosion materials for pipes have insufficient adhesion to bamboo composite pipes, are prone to cracking, and have long construction cycles, making it difficult to meet the needs of integrated protection of the inner and outer walls of large-diameter bamboo pipes and rapid deployment.

Method used

A high-performance elastomer coating with A and B components using a specific formulation is applied using a high-temperature and high-pressure impact mixing spraying technology, combined with nanofiller modification and coupling agents, to construct a triple interface enhancement system of physical roughening, chemical primer transition, and polyurea coating, achieving high compatibility between the coating and bamboo substrate and rapid curing.

Benefits of technology

It significantly improves the adhesion and resistance to media penetration of the coating, shortens the construction cycle, and is suitable for the internal and external corrosion protection and trenchless repair of large-diameter bamboo-wound pipes, with both economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107523A_ABST
    Figure CN123107523A_ABST
Patent Text Reader

Abstract

This invention relates to the field of pipeline corrosion protection materials, and provides a high-performance elastomer coating comprising: a mixture of component A and component B in a 1:1 volume ratio, cured together; component A consists of a polyurethane prepolymer, a first isocyanate, and a second isocyanate; component B consists of an amino-terminated polyether, an amine curing agent, an alcohol curing agent, a coupling agent, a colorant, a dispersant and catalyst, talc, and surface-modified nanofillers. This invention, through precise control of the component ratio and modification with nanofillers, achieves a coating stiffness and toughness that matches the modulus of the bamboo substrate. Combined with a specialized construction process, it achieves high adhesion and rapid curing, making it suitable for corrosion protection of the inner and outer walls of bamboo-wound pipelines and trenchless repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of pipeline anti-corrosion materials technology, specifically a high-performance elastomer coating and its preparation method and construction process. Background Technology

[0002] Pipelines are core components for the long-distance transport of liquids, gases, and slurries, and are widely used in municipal water supply and drainage, water conservancy, petrochemicals, and farmland irrigation. Traditional pipelines are mainly made of steel, plastic, and concrete. Bamboo-wound or bamboo fiber composite pipelines, as new types of biomass green pipes, use bamboo as the base material and resin as the adhesive, and are formed through a winding process. They have advantages such as being renewable, lightweight and high-strength, corrosion-resistant, heat-insulating and sound-insulating, low-carbon and energy-saving, and having a long service life, and are being rapidly promoted in municipal, water conservancy, and energy fields.

[0003] Although bamboo-wound / bamboo fiber composite pipes possess natural corrosion resistance, they still suffer from problems such as insufficient chemical corrosion resistance of the inner lining, weak aging resistance, impact resistance, and cathodic disbondment resistance of the outer protection, inconsistent inner and outer wall protection systems, long construction cycles, poor environmental performance, and inability to be quickly put into use after repair under working conditions such as sewage, acid and alkali media, high-salt soil, low-temperature environment, and trenchless repair.

[0004] Existing pipe corrosion protection materials (such as epoxy coal tar, polyurethane, or ordinary polyurea) are mainly designed for metal pipes, and their direct application to bamboo composite pipes presents significant technical drawbacks. Firstly, the elastic modulus of bamboo substrates differs considerably from conventional anti-corrosion coatings, making the coating prone to cracking and delamination when the pipe deforms or temperature changes. Secondly, the complex surface characteristics of bamboo make it difficult for conventional coatings to form effective chemical bonds and physical anchoring, resulting in insufficient adhesion. Furthermore, existing solvent-based coatings have high volatile organic compound emissions and long construction cycles, making it difficult to meet the engineering requirements of integrated internal and external wall protection and rapid deployment for large-diameter bamboo pipes.

[0005] Therefore, the present invention provides a high-performance elastomer coating and its preparation method and application process. Summary of the Invention

[0006] In order to overcome the shortcomings of the prior art, at least one technical problem raised in the background art is solved.

[0007] The technical solution adopted by this invention to solve its technical problem is as follows: A high-performance elastomer coating of this invention is formed by mixing and curing component A and component B in a volume ratio of 1:1; component A is composed of the following raw materials in parts by mass: 45-55 parts of polyurethane prepolymer; 15-25 parts of first isocyanate; 28-38 parts of second isocyanate; component B is composed of the following raw materials in parts by mass: 30-45 parts of amino-terminated polyether; 15-25 parts of amine curing agent; 40-60 parts of alcohol curing agent; 0.5-3 parts of coupling agent; 1-5 parts of color paste; 0.5-2 parts of dispersant and catalyst; 0-10 parts of talc; and 3-13 parts of surface-modified nanofiller.

[0008] Preferably, the surface-modified nanofiller includes nano-silica and mica powder.

[0009] Preferably, component A satisfies at least one of the following physicochemical properties: viscosity of 1200-1700 mPa·s at 23±1℃; specific gravity of 1.05-1.15 g / cm³; non-volatile content of not less than 96%; and NCO content of 15.5%-16.8%.

[0010] Preferably, component B satisfies at least one of the following physicochemical properties: viscosity at 23±1℃ is 800~1300 mPa·s; nonvolatile matter content is not less than 92%; moisture content is not greater than 500 ppm; amine value is 3.9~4.5 meq / g.

[0011] This invention also provides a method for preparing a high-performance elastomer coating. This method, used to prepare the high-performance elastomer coating as described above, includes the following steps: Preparing component A: mixing polyurethane prepolymer, first isocyanate, and second isocyanate in parts by mass, and reacting at a reaction temperature of 75±5℃ and a vacuum degree of -0.04~-0.1MPa for 2 hours; Preparing component B: mixing amino-terminated polyether, amine curing agent, alcohol curing agent, coupling agent, color paste, dispersant, catalyst, talc powder, and surface-modified nanofiller in parts by mass, and dispersing at high speed in stages until the moisture content is no more than 500ppm.

[0012] Preferably, in the preparation step of component B, the graded high-speed dispersion includes a first dispersion stage and a second dispersion stage, and the rotation speed of the first dispersion stage is higher than that of the second dispersion stage.

[0013] This invention also provides a construction process for a high-performance elastomer coating. This process is used to form a high-performance elastomer coating as described above on the surface of a pipe substrate, comprising the following steps: S1, Surface treatment: The surface of the pipe substrate is polished and dusted, and then the polished surface is cleaned with a solvent; S2, Primer coating: A primer is applied to the treated substrate surface, the dry film thickness of which is not less than 50 μm, to form an interface transition layer; S3, Polyurea spraying: Component A and Component B are heated to 65-75°C using a high-temperature and high-pressure spraying device, mixed under high pressure at a volume ratio of 1:1, and sprayed onto the interface transition layer to form a polyurea elastomer coating; S4, Curing: The polyurea elastomer coating is cured at room temperature for 24-72 hours.

[0014] Preferably, in step S1, the surface roughness of the treated pipe substrate is 40–100 μm.

[0015] Preferably, in step S3, the spraying dynamic pressure of the spraying equipment is 2000-2500 psi.

[0016] Preferably, in step S3, the ambient temperature during construction is 0–45°C and the ambient humidity is no more than 70%.

[0017] The beneficial effects of this invention are as follows: The high-performance elastomer coating, its preparation method, and construction process provided by this invention achieve precise control of the coating's stiffness and toughness through specific A and B component formulation design, ensuring a high degree of matching between its elastic modulus and the bamboo substrate, fundamentally solving the problem of easy cracking and delamination in traditional coatings. Through the synergistic effect of nanofiller modification and coupling agents, combined with specialized surface treatment and primer transition processes, a triple interface reinforcement system of physical roughening, chemical primer transition, and polyurea coating is constructed, significantly improving the coating's adhesion and resistance to media penetration on bamboo substrates. The use of solvent-free two-component high-pressure impact spraying technology not only achieves zero volatile organic compound emissions but also features rapid curing and one-time thick film formation, greatly shortening the construction cycle. It is suitable for various working conditions such as internal and external wall corrosion protection, joint repair, and trenchless repair of large-diameter bamboo-wound pipes, demonstrating significant economic and environmental benefits. Attached Figure Description

[0018] The invention will now be further described with reference to the accompanying drawings.

[0019] Figure 1 This is a flowchart of the preparation method of the high-performance elastomer coating in this invention; Figure 2 This is a flowchart of the construction process for the high-performance elastomer coating in this invention. Detailed Implementation

[0020] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.

[0021] Example 1 This embodiment provides a high-performance elastomer coating formed by mixing and curing components A and B in a 1:1 volume ratio. This two-component system design aims to achieve millisecond-level rapid curing through high-temperature, high-pressure impact mixing, thereby meeting the continuous construction requirements for large-diameter, long-length bamboo-based composite pipes.

[0022] Component A consists of the following parts by weight of raw materials: 45-55 parts of polyurethane prepolymer; 15-25 parts of first isocyanate; and 28-38 parts of second isocyanate.

[0023] Among them, polyurethane prepolymer, as the soft segment base of the coating, endows the cured product with excellent flexibility and resilience due to its molecular chain structure. It is a key component in solving the problem of cracking caused by modulus mismatch in traditional anti-corrosion coatings on bamboo substrates. For example, the polyurethane prepolymer can be an NCO-terminated prepolymer obtained by reacting polyether polyol or polyester polyol with excess diisocyanate. Polyether-type prepolymers are preferred to obtain better hydrolysis resistance.

[0024] The first and second isocyanates together constitute the hard segment source of the coating and provide the active NCO groups required for the crosslinking reaction. In this embodiment, two different isocyanates are introduced to synergistically regulate the reaction rate and balance the mechanical properties of the final coating. For example, the first isocyanate can be a highly reactive aromatic isocyanate (such as diphenylmethane diisocyanate MDI and its liquefied modified form) to ensure rapid molding; the second isocyanate can be an isocyanate with lower functionality or greater steric hindrance (such as carbodiimide-modified MDI or isophorone diisocyanate IPDI) to improve leveling and reduce internal stress. By adjusting the ratio of these two types of isocyanates, the modulus of the cured polyurea elastomer can be made between that of rigid resin and high-elasticity rubber, thereby achieving a gradient match with the modulus of the bamboo-wound pipe substrate and effectively alleviating interfacial stress concentration.

[0025] Component B consists of the following raw materials in parts by weight: 30-45 parts of amino-terminated polyether; 15-25 parts of amine curing agent; 40-60 parts of alcohol curing agent; 0.5-3 parts of coupling agent; 1-5 parts of color paste; 0.5-2 parts of dispersant and catalyst; 0-10 parts of talc; and 3-13 parts of surface-modified nanofiller.

[0026] Amino-terminated polyethers form the main backbone of the polyurea molecular chain, determining the basic physical and mechanical properties and media resistance of the coating. For example, polyoxypropylene diamine or polytetrahydrofuran diamine with a molecular weight between 1000 and 4000 can be selected.

[0027] Amine curing agents are mainly used as chain extenders, utilizing their extremely fast reaction rate with isocyanates to achieve instantaneous gelation of the coating. For example, liquid aromatic diamines such as diethyltoluene diamine (DETDA) or dimethylthiotoluene diamine (DMTDA) can be selected.

[0028] Alcohol-based curing agents serve a dual purpose: regulating the reaction rate and improving the coating's toughness. Since the reaction rate of hydroxyl groups with NCO is significantly lower than that of amino groups, their addition can delay the local exothermic peak, reducing microbubble defects caused by excessively rapid reactions. Simultaneously, the introduced urethane bonds increase the hydrogen bond density between molecular chains, enhancing the coating's tear resistance. Alcohol-based curing agents can be selected from one or a combination of two of polypropylene glycol (PPG-2000) or 1,4-butanediol.

[0029] Specifically, the coupling agents and surface-modified nanofillers in component B are core elements for constructing a high-performance interface. Coupling agents (such as silane coupling agents and titanate coupling agents) can establish chemical bridges between inorganic fillers and the organic resin matrix, and also participate in the chemical bonding reaction between the coating and the bamboo substrate surface. Surface-modified nanofillers refer to nanoscale inorganic particles treated with surfactants, coupling agents, or polymer grafting. For example, the filler can be nano-silica and mica powder treated with silane coupling agents. Compared to unmodified ordinary fillers, surface-modified nanofillers not only avoid stress weaknesses caused by agglomeration, but also hinder crack propagation and extend the penetration path of corrosive media through nano-effects. With the addition of appropriate amounts of talc as a extender filler to adjust viscosity and cost, and the assistance of dispersants, catalysts, and colorants, component B, after mixing with component A, can form a dense, tough, and highly compatible anti-corrosion protective layer with the bamboo substrate.

[0030] To ensure the metering accuracy and complete reaction of the two components during high-pressure impact mixing, component A must meet at least one of the following physicochemical properties: viscosity of 1200–1700 mPa·s at 23±1℃; specific gravity of 1.05–1.15 g / cm³; non-volatile content of not less than 96%; and NCO content of 15.5%–16.8%. When the NCO content is below 15.5%, the isocyanate groups are insufficient to completely react with the active hydrogen in component B, resulting in insufficient cross-linking density of the coating, manifesting as a sticky surface, low hardness, and poor resistance to media. Conversely, when the NCO content is above 16.8%, excessive isocyanate leads to excessively high cross-linking density, a sharp increase in coating brittleness, and a significant decrease in elongation at break, failing to match the flexible deformation of the bamboo substrate and making it highly susceptible to cracking during pipe bending or settling. Therefore, strictly limiting the NCO content to the range of 15.5%–16.8% is a necessary condition for achieving a balance between rigidity and toughness while ensuring rapid curing. The viscosity and specific gravity limits are designed to match the pumping characteristics and mixing chamber pressure requirements of existing mainstream high-temperature and high-pressure spraying equipment, ensuring that the two components achieve molecular-level uniform mixing at a 1:1 volume ratio.

[0031] Accordingly, component B must meet at least one of the following physicochemical properties: viscosity of 800–1300 mPa·s at 23±1℃; non-volatile content of not less than 92%; moisture content of not more than 500 ppm; and amine value of 3.9–4.5 meq / g. Isocyanates in polyurea systems are extremely sensitive to water. If the moisture content of component B exceeds the standard, it will react with NCO groups to generate carbon dioxide gas, forming microbubbles or pinholes inside the coating, severely damaging the coating's density and adhesion, and even leading to corrosion failure. An amine value range of 3.9–4.5 meq / g matches the NCO content of component A, ensuring the accuracy of the stoichiometry and placing the gel time and surface drying time within the optimal application window.

[0032] Specifically, the detailed core performance indicators of this high-performance elastomer coating applied to bamboo pipes are shown in the table below: Serial Number Testing items Technical requirements Testing standards 1 Solid content ≥98% GB / T 1725-2007 2 gel time 30–120 s (adjustable) GB / T 1728-1979 3 Surface drying time 3–15 min (adjustable) GB / T 1728-1979 4 Tensile strength ≥16MPa GB / T 528-2009 5 Elongation at break ≥300 GB / T 528-2009 6 Tear strength ≥70kN / m GB / T 529-2008 7 Shore hardness ≥A85 GB / T531.1-2008 8 Adhesion (pull-off test, dry state) ≥2MPa (cohesive failure) GB / T 5210-2006 9 Adhesion (pull-out test, after immersion in 60°C water for 30 days) Cohesion destruction GB / T 5210-2006 10 Impact resistance ≥2kg·m GB / T 1732-1993 11 Abrasion resistance (750g / 500r) ≤15mg GB / T 1768-2006 12 Salt spray resistance ≥4000 h, no rust, no blistering, no peeling GB / T 1771-2007 13 Water resistance (40℃, 30 days) No rust, no blistering, no peeling GB / T30648.2-2015 14 Resistant to liquid media (30% H2SO4, 3000h) No rust, no blistering, no peeling GB / T 30648.1-2014 15 Resistant to liquid media (30% NaOH, 3000h) No rust, no blistering, no peeling GB / T 30648.1-2014 16 Resistant to liquid media (5% NaCl, 4000h) No rust, no blistering, no peeling GB / T 30648.1-2014 17 Resistant to liquid media (30% HCl, 3000h) No rust, no blistering, no peeling GB / T 30648.1-2014 18 Artificial climate aging (xenon lamp, 1000h) No bubbling, no cracking, no powdering, color difference ΔE≤6 GB / T 14522-2008 19 UV aging (QUV, 1000 h) No bubbling, no cracking, no powdering GB / T 23987-2009 20 Low-temperature bending performance (-40℃) No cracks GB / T 16777-2008 21 High temperature stability (80℃, 7 days) Tensile strength retention ≥ 85% GB / T 528-2009 22 Humid heat cycle (-40℃~60℃, 20 cycles) No significant decrease in adhesion GB / T 5210-2006 23 VOC content 0 GB 18581-2020 Example 2 like Figure 1 As shown, this embodiment provides a method for preparing a high-performance elastomer coating. This method is used to prepare the above-mentioned high-performance elastomer coating. The preparation method mainly includes two independent but related processes: the preparation of component A and the preparation of component B.

[0033] Specifically, in preparing component A, the polyurethane prepolymer, the first isocyanate, and the second isocyanate are mixed in proportion to their mass and reacted at a temperature of 75±5℃ and a vacuum of -0.04 to -0.1 MPa for 2 hours. The reaction temperature of 75±5℃ ensures that the reaction rate between the isocyanate and the polyol is within a suitable range, and effectively avoids side reactions such as isocyanate self-polymerization or oxidative discoloration caused by excessively high temperatures. The vacuum environment of -0.04 to -0.1 MPa is not only used to remove trace amounts of moisture introduced from the raw materials to prevent the generation of carbon dioxide bubbles during subsequent spraying, but also to promptly remove any small molecule volatiles that may remain in the reaction system. This ensures that the NCO content of component A can be accurately and stably maintained within the critical range of 15.5% to 16.8%, providing a reliable stoichiometric basis for the cross-linked network structure after the two components are mixed.

[0034] In preparing component B, terminal amino polyether, amine curing agent, alcohol curing agent, coupling agent, color paste, dispersant, catalyst, talc powder, and surface-modified nanofiller are mixed in parts by mass and then dispersed at high speed in a stepwise manner until the moisture content is no more than 500 ppm. The stepwise high-speed dispersion includes a first dispersion stage and a second dispersion stage, with the rotational speed of the first dispersion stage being higher than that of the second dispersion stage.

[0035] The first dispersion stage, as a high-shear disagglomeration stage, typically has a rotation speed controlled at 1000–1500 rpm and a duration of approximately 15–30 minutes. The main objective of this stage is to utilize high-intensity fluid shear force to completely break down the hard agglomerates formed during storage or transportation of the surface-modified nanofillers, allowing them to be uniformly suspended in the resin matrix as primary particles or soft agglomerates, thereby fully leveraging the reinforcing and barrier effects of the nanofillers.

[0036] The second dispersion stage, serving as a low-speed homogenization and degassing stage, typically involves reducing the rotation speed to 400–600 rpm for approximately 20–40 minutes. This stage serves multiple functions: firstly, the lower rotation speed is sufficient to maintain the macroscopic homogeneity of the system, promoting adequate wetting and compatibility between the liquid phase components and preventing stratification due to density differences; secondly, reducing the rotation speed significantly reduces mechanical shear heat generation, preventing component B from absorbing moisture from the environment due to temperature rise or causing oxidative discoloration of the amine curing agent, which is crucial for strictly controlling the moisture content to no more than 500 ppm; furthermore, low-speed stirring helps the microbubbles entrained in the first stage to slowly rise and escape under viscosity-allowed conditions, further improving the compactness of the slurry.

[0037] Example 3 like Figure 2As shown, this embodiment provides a construction process for a high-performance elastomer coating, specifically designed to form an anti-corrosion protective layer on the surface of bamboo-based composite pipes. Unlike traditional metal pipe anti-corrosion processes, bamboo-based composite pipes exhibit anisotropy, low surface energy, and a significantly different elastic modulus compared to conventional anti-corrosion materials. Therefore, this invention constructs a four-step construction system comprising surface treatment, primer coating, polyurea spraying, and curing. This system aims to solve the cracking and delamination problem caused by the modulus mismatch between the coating and the bamboo substrate, and to meet the construction needs of complex conditions such as integrated protection of the inner and outer walls of large-diameter, long-length pipes and trenchless repair.

[0038] Specifically, the construction process includes the following steps: Step S1, Surface Treatment: The surface of the pipe substrate is sanded and dusted, then cleaned with solvent. During the winding process of bamboo-based composite pipes, the surface often retains release agents, wax, or oxide layers, and the surface resin has a high degree of curing, making it easy to form a weak boundary layer when directly coated. Sanding effectively removes these contaminants and weak bonding layers, exposing fresh resin matrix and some bamboo fibers, thus increasing surface energy. Furthermore, the microscopic roughness created by sanding provides mechanical anchoring points for subsequent coatings, significantly enhancing physical adhesion. The subsequent solvent cleaning not only removes dust and grease generated during sanding but, more importantly, utilizes the slight swelling effect of the solvent on the resin layer of the bamboo surface to further activate surface functional groups, creating conditions for chemical bonding. For example, sandpaper, grinding wheels, or wire brushes can be used for sanding, and acetone, ethanol, or special cleaning agents can be used as solvents. The specific choice should be determined based on the surface condition of the bamboo pipe and the construction environment; this invention does not impose any limitations on this.

[0039] Step S2, Primer Coating: Apply a primer to the treated substrate surface. The dry film thickness of the primer should be no less than 50 μm to form an interface transition layer. Since the elastic modulus of bamboo substrate is much lower than that of polyurea elastomer, if polyurea is directly sprayed, the strain difference generated by temperature changes or pipe deformation will accumulate huge stress at the interface, leading to coating peeling. The primer acts as a chemical bridge and stress buffer. Its molecular structure contains both active groups that can react with the hydroxyl and carboxyl groups on the bamboo surface, and compatible segments that can react with the NCO groups or amino groups of polyurea, thus establishing a stable chemical bond between the inorganic / organic interface. Simultaneously, the primer's modulus is between that of bamboo and polyurea, allowing for a gradient transition of stress concentration and effectively inhibiting crack initiation. A dry film thickness of no less than 50 μm ensures that the primer completely covers the micropores, textures, and sanding marks on the bamboo surface, forming a continuous and dense transition film, avoiding adhesion failure or corrosive media penetration due to localized exposure of the substrate. The primer can be applied by brushing, rolling, or low-pressure spraying to suit different pipe diameters and construction spaces.

[0040] Step S3, Polyurea Spraying: Using high-temperature, high-pressure spraying equipment, components A and B are heated to 65–75°C and mixed under high pressure in a 1:1 volume ratio. The mixture is then sprayed onto the interface transition layer to form a polyurea elastomer coating. The high-pressure impact mixing allows components A and B to achieve uniform mixing at the molecular level within the impact chamber with extremely high kinetic energy, triggering an instantaneous gel reaction. This prevents the coating from sagging even when applied to vertical walls or the top of large-diameter pipes, and allows it to reach walking strength within seconds, significantly shortening the construction cycle. More importantly, the high-pressure impact mixing ensures the uniformity of the coating's internal structure, avoiding localized performance deficiencies caused by uneven mixing. This allows the cured polyurea elastomer to fully utilize its balanced rigidity and toughness, working synergistically with the interface transition layer formed in step S2 to achieve long-term protection for bamboo-based composite pipes.

[0041] Step S4, Curing: Cur the polyurea elastomer coating at room temperature for 24–72 hours. Although the surface drying time of the polyurea coating is extremely short, the completion of its internal cross-linking network and the release of residual stress still require a certain amount of time. During this window period, the coating can complete deep cross-linking under natural environmental conditions without additional heating or baking, which not only saves energy costs but also avoids heat damage to the bamboo substrate or excessive internal stress in the coating caused by forced heating. During the curing period, avoid rain, heavy impacts, and chemical contact to ensure the integrity and reliability of the final anti-corrosion system.

[0042] Example 4 Based on Example 4, this example further limits the key parameters in the construction process to construct the optimal construction conditions suitable for bamboo-based composite pipes.

[0043] Specifically, in step S1, the surface roughness of the treated pipe substrate is 40–100 μm. When the surface roughness is below 40 μm, the microstructure of the substrate surface is too smooth, failing to provide sufficient mechanical anchoring points for the polyurea coating, resulting in insufficient physical adhesion. The coating is prone to interfacial slippage or even peeling when subjected to pipe deformation or thermal stress. Conversely, when the surface roughness exceeds 100 μm, although the anchoring area increases, excessively deep troughs can trap air during spraying, forming microbubble defects. Simultaneously, the coating thickness at sharp peaks is often insufficient, becoming a preferred channel for corrosive media penetration, thus reducing the overall density and durability of the anti-corrosion system. Therefore, strictly controlling the roughness within the range of 40–100 μm ensures sufficient mechanical anchoring while guaranteeing complete wetting and coverage of the substrate surface, achieving the optimal balance between adhesion and density.

[0044] In step S3, the dynamic spraying pressure of the spraying equipment is 2000–2500 psi. In the solvent-free high-viscosity system used in this invention, only when the dynamic pressure reaches above 2000 psi can component A and component B obtain sufficient kinetic energy to achieve uniform mixing and full atomization at the molecular level within milliseconds, thereby triggering a rapid and complete cross-linking reaction. If the pressure is below 2000 psi, the mixing energy of the two components is insufficient, which can easily lead to local stoichiometric imbalance, resulting in quality problems such as stickiness, low strength, or poor resistance to media after curing.

[0045] In step S3, the ambient temperature during construction is 0–45℃, and the ambient humidity is no more than 70%. As a biomass composite material, the resin layer on the surface of bamboo-based composite pipes is highly sensitive to ambient temperature and humidity, and bamboo itself has a certain degree of hygroscopicity. Within the temperature range of 0–45℃, the reaction rate and leveling performance of the polyurea coating are optimally matched: too low a temperature leads to a slow reaction, poor leveling, and orange peel or ripples on the coating surface; too high a temperature results in a short gel time, causing the coating to solidify before fully wetting the substrate, affecting adhesion. The restriction of ambient humidity not exceeding 70% is to prevent the isocyanate component from reacting with moisture in the air to generate carbon dioxide bubbles. Especially when bamboo has many micropores on its surface and easily absorbs moisture, strictly controlling the upper limit of humidity is crucial to avoiding appearance and performance defects such as pinholes and blistering in the coating.

[0046] To further verify the practical application effect of the anti-corrosion bamboo-based composite pipe provided by this invention under different working conditions, three typical engineering cases are described below. These cases are for illustrative purposes only and are not intended to limit the scope of protection of this invention.

[0047] In the first application case, the external corrosion protection requirements of large-diameter municipal sewage pipes were addressed, specifically DN1200 bamboo-wound sewage pipes, each 12 meters long, laid in a high-salt-alkali soil environment. This placed extremely high demands on the coating's salt spray corrosion resistance and adhesion. During construction, the processes described in Examples 3 and 4 were strictly followed: First, the outer wall of the bamboo-based composite pipe was mechanically ground to control the surface roughness within the range of 40–100 μm, followed by solvent cleaning and activation. Then, a special primer was applied to form an interface transition layer, with a dry film thickness controlled above 50 μm. Finally, high-temperature, high-pressure spraying equipment was used to spray a 1:1 volume ratio mixture of components A and B under dynamic pressure of 2000–2500 psi and raw material heating temperature of 65–75°C, forming a polyurea elastomer anti-corrosion coating approximately 2 mm thick, which was then cured at room temperature for 72 hours. Acceptance test results showed that the adhesion pull-out strength between the coating and the bamboo substrate was greater than 2MPa, and the failure mode was the failure of the bamboo substrate itself, indicating that the interface bonding strength had exceeded the strength of the substrate itself; the salt spray test for more than 4,000 hours did not show any blistering, rusting or peeling; and no leaks were found by spark leak detection.

[0048] In the second application case, the internal wall protection requirements of drinking water pipelines, specifically DN800 bamboo water pipes, were addressed. These pipes come into direct contact with drinking water, requiring a coating that is non-toxic, harmless, and resistant to long-term water corrosion. The construction employed the same surface treatment and primer coating process as in Case 1, but a food-grade raw material system meeting drinking water hygiene standards was selected for the polyurea spraying stage, with the coating thickness controlled at 1.5mm. Because component B strictly controlled its moisture content to no more than 500ppm and contained no volatile organic solvents, the cured coating was dense and free of microbubbles, effectively preventing the release of harmful substances and the risk of microbial growth. Testing showed that all hygiene indicators of the coating immersion solution met the national safety evaluation standards for drinking water transmission and distribution equipment and protective materials. After 30 days of continuous immersion in room temperature tap water, the coating surface remained smooth and even, without whitening, swelling, or peeling, and the adhesion retention rate exceeded 95%.

[0049] In the third application case, the repair of a leaking bamboo pipe beneath a main urban road was addressed. Specifically, a DN1000 bamboo pipe was leaking due to localized corrosion and perforation, and excavation for replacement was impossible due to traffic restrictions. The repair work employed a robotic platform to enter the pipe and perform automated operations: first, the robot, equipped with a grinding device, performed in-situ surface treatment of the inner wall to achieve a cleanliness level of Sa2.5 and the specified roughness; then, a special primer and a polyurea elastomer coating were sprayed. Thanks to the excellent fast-curing and leveling properties of the coating composition of this invention, the coating gelled and dried within seconds of spraying, exhibiting no sagging even when applied to vertical walls or ceilings; under ambient temperature conditions of 15℃ and humidity of 60%, the coating reached full curing after 24 hours of room temperature curing, passed the water tightness test, and the pipe quickly resumed water flow. Compared to the curing cycle of traditional epoxy or polyurethane repair materials, which often takes several days, the technical solution of this invention significantly shortens the construction period and minimizes the impact on urban traffic and residents' lives. At the same time, the good adhesion between the coating and the old pipe substrate ensures the overall structural strength and sealing performance after repair.

[0050] In summary, the three application cases described above verify, from different perspectives, the comprehensive advantages of the anti-corrosion bamboo-based composite pipe provided by this invention in terms of mechanical performance matching, corrosion resistance, hygiene and safety, and construction efficiency. It should be understood that the specific pipe specifications, coating thickness, curing time, and test data in the above cases are merely illustrative examples. In practical applications, those skilled in the art can adaptively adjust the parameters within the scope of the technical solution disclosed in this invention according to specific engineering needs. As long as these adjustments do not depart from the core inventive concept of this invention, they should be considered to fall within the protection scope of this invention.

[0051] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that the high-performance elastomer coating formulations, preparation process parameters, and construction methods described in the above embodiments are preferred examples listed to fully disclose the technical solution of the present invention, and are not exhaustive limitations on the scope of protection of the present invention. Any equivalent substitution of raw materials, adaptive adjustment of process parameters, or reasonable expansion of application scenarios that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention, based on the core technical concept of the present invention, should be included within the scope of protection of the present invention.

Claims

1. A high-performance elastomer coating, characterized in that: It is formed by mixing and curing components A and B in a volume ratio of 1:1; Component A is composed of the following raw materials in parts by mass: 45-55 parts of polyurethane prepolymer; 15-25 parts of the first isocyanate; 28–38 parts of the second isocyanate; Component B is composed of the following raw materials in parts by mass: 30-45 parts of amino-terminated polyether; 15-25 parts of amine curing agent; 40-60 parts of alcohol-based curing agent; 0.5 to 3 parts of coupling agent; 1-5 parts of colorant; Dispersant and catalyst 0.5-2 parts; 0-10 parts of talc powder; 3 to 13 parts of surface-modified nanofiller.

2. The high-performance elastomer coating according to claim 1, characterized in that: The surface-modified nanofiller includes nano-silica and mica powder.

3. The high-performance elastomer coating according to claim 1, characterized in that: Component A satisfies at least one of the following physicochemical properties: The viscosity at 23±1℃ is 1200~1700 mPa·s; the specific gravity is 1.05~1.15 g / cm³; the nonvolatile content is not less than 96%; and the NCO content is 15.5%~16.8%.

4. The high-performance elastomer coating according to claim 1, characterized in that: Component B satisfies at least one of the following physicochemical properties: The viscosity at 23±1℃ is 800~1300 mPa·s; the nonvolatile content is not less than 92%; the moisture content is not greater than 500 ppm; and the amine value is 3.9~4.5 meq / g.

5. A method for preparing a high-performance elastomer coating, the method being used to prepare the high-performance elastomer coating according to any one of claims 1-4, characterized in that: Includes the following steps: Preparation of component A: The polyurethane prepolymer, the first isocyanate and the second isocyanate are mixed in the indicated mass fractions and reacted at a reaction temperature of 75±5℃ and a vacuum degree of -0.04 to -0.1MPa for 2 hours. Preparation of Component B: The terminal amino polyether, amine curing agent, alcohol curing agent, coupling agent, color paste, dispersant, catalyst, talc powder and surface modified nanofiller are mixed in parts by mass and dispersed at high speed in stages until the moisture content is no more than 500 ppm.

6. The method for preparing a high-performance elastomer coating according to claim 5, characterized in that: In the preparation step of component B, the graded high-speed dispersion includes a first dispersion stage and a second dispersion stage, and the rotation speed of the first dispersion stage is higher than that of the second dispersion stage.

7. A process for applying a high-performance elastomer coating, wherein the process is used to form the high-performance elastomer coating of any one of claims 1-4 on the surface of a pipe substrate, characterized in that: Includes the following steps: S1. Surface treatment: The surface of the pipe substrate is polished and dust is removed, and then the polished surface is cleaned with solvent; S2. Primer Coating: Apply primer to the treated substrate surface. The dry film thickness of the primer shall not be less than 50 μm to form an interface transition layer. S3. Polyurea spraying: Using high-temperature and high-pressure spraying equipment, components A and B are heated to 65-75°C, mixed under high pressure at a volume ratio of 1:1, and sprayed onto the interface transition layer to form a polyurea elastomer coating. S4. Curing: Cur the polyurea elastomer coating at room temperature for 24 to 72 hours.

8. The construction process of a high-performance elastomer coating according to claim 7, characterized in that: In step S1, the surface roughness of the treated pipe substrate is 40–100 μm.

9. The construction process of a high-performance elastomer coating according to claim 7, characterized in that: In step S3, the dynamic spraying pressure of the spraying equipment is 2000-2500 psi.

10. The construction process of a high-performance elastomer coating according to claim 7, characterized in that: In step S3, the ambient temperature during construction is 0–45℃ and the ambient humidity is no more than 70%.