UV-curable anti-corrosion and heat-resistant coatings, their preparation methods and applications

By introducing isocyanurate-based polyurethane acrylate oligomers and the triazine ring structure of tri(2-hydroxyethyl) isocyanurate triacrylate into UV-cured anti-corrosion and heat-resistant coatings, and combining them with hydrophobic fumed silica and corrosion inhibitors, a hierarchical initiation system was constructed. This solved the corrosion resistance and adhesion problems of traditional coatings in high-temperature and corrosive environments, and achieved uniform curing and good performance of brake discs.

CN123107530APending Publication Date: 2026-11-17HUNAN XIANGJIANG GUANXI COATINGS (CHANGSHA) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455472.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional UV-cured anti-corrosion and heat-resistant coatings are difficult to maintain excellent corrosion resistance after high-temperature impact, and cannot achieve uniform curing and good adhesion in the complex geometry of brake discs, thus failing to meet the application requirements of automotive brake discs in high-temperature and corrosive media environments.

Method used

A triazine ring structure is formed by isocyanurate-based polyurethane acrylate oligomer and tri(2-hydroxyethyl)isocyanurate triacrylate. Combined with hydrophobic fumed silica, anti-rust pigments and corrosion inhibitors, a hierarchical initiation system is constructed to enhance the heat resistance and corrosion resistance of the coating film. Furthermore, the adhesion to cast iron substrate is improved by using phosphate acrylate adhesion promoters.

Benefits of technology

It achieves improved coating integrity and corrosion resistance at high temperatures, adapts to the complex geometry of brake discs for uniform curing, and meets the application requirements of automotive brake discs under complex working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application provides a UV-curable anti-corrosion and heat-resistant coating, its preparation method, and its application. The UV-curable anti-corrosion and heat-resistant coating includes component A and component B. Based on the total mass of component A, component A includes 25wt~35wt% isocyanurate-based polyurethane acrylate oligomer, 10~15wt% tris(2-hydroxyethyl)isocyanurate triacrylate, 25~40wt% reactive diluent, 3~8wt% shallow photoinitiator, 1wt%~2wt% intermediate layer photoinitiator, 2~6wt% deep layer photoinitiator, 1~5wt% mercapto ester co-initiator, 0~3wt% carbon black paste, 1~5wt% hydrophobic fumed silica, 1~3wt% corrosion inhibitor, 2~5wt% anti-rust pigment, 5~10wt% filler, 0.1~0.5wt% leveling agent, and 0.1~0.3wt% defoamer; component B includes phosphate ester acrylate adhesion promoter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of coating technology, and in particular to UV-curable anti-corrosion and heat-resistant coatings, their preparation methods and applications. Background Technology

[0002] Automotive brake discs face the dual challenges of temperature and corrosion during service. During emergency braking or continuous downhill driving, the disc surface temperature can instantly rise to 400°C or even higher. In daily use, they are also continuously exposed to corrosive media such as rainwater, de-icing salt, road dust, and coastal salt spray. Industry standards typically use the heat resistance and corrosion resistance of automotive brake disc coatings as core evaluation indicators. However, in actual service, brake disc coatings are immediately exposed to corrosive media after experiencing high-temperature shocks; the two events usually occur sequentially rather than independently. Therefore, brake disc coatings must maintain excellent corrosion resistance even after experiencing high temperatures.

[0003] As a core component of the vehicle braking system that withstands high-frequency heat-force-humidity-salt coupling, brake discs have long faced three concurrent technical challenges in surface coating: First, the local temperature of brake discs can instantly rise to hundreds of degrees Celsius during braking, and the coating must maintain its structural integrity after such high-temperature impact; second, the service environment of brake discs is generally accompanied by rainwater, de-icing agents, road salt, and other media, and the coating must still have long-term salt spray corrosion resistance after high-temperature impact; third, brake discs are not simple planar or regular curved surface structures, but rather have ventilated disc pillars, ventilation holes, concave surfaces, etc. Complex geometric features such as chamfers and column root transition areas lead to significant differences in the actual light intensity and coating thickness that can be obtained in different areas during the UV curing process: areas with strong direct light exposure, such as the inner circle of the friction zone side and the cap plane, can obtain a higher light dose and form a relatively thick film (50μm~80μm), while areas such as the side wall of the ventilation disc column, column root, concave surface and ventilation holes have a significantly lower actual light dose due to light path obstruction, incident angle deflection and multiple reflections. At the same time, the coating thickness in these areas is relatively thinner (30μm~60μm) due to limitations in coating leveling and coating angle.

[0004] The cast iron material used to prepare brake discs has characteristics such as porous surface and uneven oxide film, which puts forward higher requirements for the barrier performance and interfacial bonding of coatings; however, traditional UV-cured anti-corrosion and heat-resistant coatings are difficult to achieve anti-corrosion performance of more than 240 hours after being subjected to high temperature.

[0005] Therefore, traditional UV-cured anti-corrosion and heat-resistant coatings still need further improvement. Summary of the Invention

[0006] Based on this, one or more embodiments of this application provide a UV-curable anti-corrosion and heat-resistant coating with excellent anti-sagging properties, adhesion properties, heat resistance properties and anti-corrosion properties, as well as its preparation method and application.

[0007] According to a first aspect of the embodiments of this application, a UV-curable anti-corrosion and heat-resistant coating is provided, comprising component A and component B;

[0008] Based on the total mass of component A, component A comprises 25wt%~35wt% isocyanurate-based polyurethane acrylate oligomer, 10wt%~15wt% tris(2-hydroxyethyl)isocyanurate triacrylate, 25wt%~40wt% reactive diluent, 3wt%~8wt% superficial photoinitiator, 1wt%~2wt% intermediate layer photoinitiator, 2wt%~6wt% deep layer photoinitiator, 1wt%~5wt% mercapto ester co-initiator, 0~3wt% carbon black paste, 1wt%~5wt% hydrophobic fumed silica, 1wt%~3wt% corrosion inhibitor, 2wt%~5wt% rust-preventive pigment, 5wt%~10wt% filler, 0.1wt%~0.5wt% leveling agent, and 0.1wt%~0.3wt% defoamer;

[0009] Component B includes a phosphate ester acrylate adhesion promoter; the sum of the mass of the triazine ring structure in the isocyanurate-based polyurethane acrylate oligomer and the tri(2-hydroxyethyl) isocyanurate triacrylate is 7.6% to 9.5% of the mass of the UV-curable anti-corrosion and heat-resistant coating after curing.

[0010] In some embodiments, the UV-curable anti-corrosion and heat-resistant coating satisfies at least one of the following characteristics:

[0011] (1) The active diluent includes at least three of the following: tripropylene glycol diacrylate, trimethylolpropane triacrylate, hydroxypropyl methacrylate, isobornyl acrylate and 2-phenoxyethyl acrylate;

[0012] (2) The shallow photoinitiator includes α-hydroxyketone photoinitiators;

[0013] (3) The deep photoinitiator includes acylphosphine oxide photoinitiators;

[0014] (4) The intermediate layer photoinitiator includes α-aminoketone photoinitiators;

[0015] (5) The thiol ester co-initiator includes one or more of the following: thiol ester modified acrylic compound, pentaerythritol tetramercaptopropionate, tris(3-mercaptopropionic acid) trimethylolpropane ester, tetra(3-mercaptobutyric acid) pentaerythritol ester and hexa(3-mercaptobutyric acid) dipentaerythritol ester;

[0016] (6) The hydrophobic fumed silica includes dimethyldichlorosilane surface-modified fumed silica;

[0017] (7) The specific surface area of ​​the hydrophobic fumed silica is 90 m².2 / g~130m 2 / g;

[0018] (8) The rust-preventive pigment includes one or more of aluminum tripolyphosphate-zinc oxide mixture and aluminum zinc phosphomolybdate;

[0019] (9) The filler includes one or more of barium sulfate, silica fume, talc, calcium carbonate and mica powder;

[0020] (10) The acid value of the phosphate ester acrylate adhesion promoter is 250 mg KOH / g to 310 mg KOH / g;

[0021] (11) The mass ratio of component A to component B is 100: (6~9).

[0022] In some embodiments, the corrosion inhibitor includes benzotriazole corrosion inhibitors and mercaptobenzothiazole corrosion inhibitors.

[0023] In some embodiments, the UV-curable anti-corrosion and heat-resistant coating satisfies at least one of the following characteristics:

[0024] (1) The benzotriazole corrosion inhibitors include one or more of benzotriazole and methylbenzotriazole;

[0025] (2) The mercaptobenzothiazole corrosion inhibitors include mercaptobenzothiazole.

[0026] According to a second aspect of the embodiments of this application, a method for preparing a UV-curable anti-corrosion and heat-resistant coating is provided, comprising the following steps:

[0027] The raw materials are provided according to the above-mentioned UV-cured anti-corrosion and heat-resistant coating;

[0028] The main resin premix was prepared by mixing isocyanurate-based polyurethane acrylate oligomer, tris(2-hydroxyethyl) isocyanurate triacrylate and a portion of reactive diluent.

[0029] The shallow photoinitiator, intermediate photoinitiator and deep photoinitiator are mixed with the remaining active diluent to prepare the initiator pre-dispersion;

[0030] The main resin premix is ​​mixed with hydrophobic fumed silica, corrosion inhibitor, rust-preventive pigment, filler, defoamer and leveling agent, and then ground to obtain a sand-grinding slurry;

[0031] The sand-milling slurry, the initiator pre-dispersion liquid, the carbon black slurry, and the mercapto ester co-initiator are mixed to obtain component A;

[0032] Phosphate acrylate adhesion promoters are used as component B.

[0033] In some embodiments, the method for preparing the isocyanurate-based polyurethane acrylate oligomer includes the following steps:

[0034] Hexamethylene diisocyanate trimer was mixed with acrylate monomers and then subjected to an addition reaction to obtain isocyanurate-based polyurethane acrylate oligomers.

[0035] The acrylate monomers contain hydroxyl groups.

[0036] In some embodiments, the acrylate monomers include one or more of hydroxypropyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

[0037] According to a third aspect of the embodiments of this application, a coating film is provided, which is formed using the above-described UV-curable anti-corrosion and heat-resistant coating.

[0038] According to a fourth aspect of the embodiments of this application, a cast iron article is provided, including the coating described above.

[0039] According to a fifth aspect of the embodiments of this application, a brake disc is provided, comprising the cast iron article described above.

[0040] Compared with traditional technologies, this application has the following advantages:

[0041] In component A of the UV-curable anti-corrosion and heat-resistant coating of this application, both isocyanurate-based polyurethane acrylate oligomer (IPUA) and tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA) contain a rigid isocyanurate ring skeleton. These two components synergistically provide high thermal stability and high crosslinking density, jointly forming a triazine ring heat-resistant skeleton. The hexamethylene long carbon chain in IPUA further introduces a flexible buffer segment, forming a rigid-flexible synergistic network with the rigid ring structure. During curing, this relaxes shrinkage stress, maintains dimensional stability, and prevents thick film cracking. Most of the Si-OH on the surface of the hydrophobic fumed silica particles is converted to Si-CH3, reducing the particles' hydrophilicity and giving them good dispersibility and compatibility in organic UV systems. The particles interact through residual Si-OH hydrogen bonds and van der Waals forces to form a reversible three-dimensional network, endowing the coating with excellent thixotropic properties. A hierarchical photoinitiator system is formed by the synergistic action of a superficial photoinitiator, an intermediate photoinitiator, a deep photoinitiator, and a mercapto ester co-initiator. The superficial and deep photoinitiators absorb UV photons and generate free radicals at the surface and depth of the coating, respectively. The intermediate photoinitiator bridges the initiation efficiency transition between the two, compensating for initiation gradient breaks caused by light obstruction in complex geometric areas such as brake disc ventilation disc pillars and concave surfaces. The mercapto ester co-initiator extends the limited free radical reaction chain through chain transfer, ensuring complete curing of the coating in both high-light thick film and low-light thin film regions. Rust-inhibiting pigments and corrosion inhibitors work synergistically to construct a multi-layered, hybrid anti-corrosion barrier on the cast iron surface. Phosphate ester and acrylate adhesion promoters can undergo a condensation reaction with the iron oxide layer on the cast iron surface, giving the coating excellent adhesion to the cast iron substrate. The combined and synergistic action of these raw materials results in a coating with excellent anti-sagging properties, low-light curing performance, adhesion, heat resistance, and corrosion resistance, meeting the application requirements of automotive brake discs under complex working conditions. Detailed Implementation

[0042] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, a detailed description of specific embodiments of this application is provided. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. Unless otherwise specifically stated, all raw materials, reagents, instruments, and equipment used in this application are commercially available or can be prepared by existing methods.

[0044] In this application, the terms "multiple", "various", "multiple times", "multi-dimensional", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0045] The terms “combinations of,” “any combination of,” and “any combination of” used in this article include all suitable combinations of any two or more of the listed items.

[0046] In this document, the term "suitable" as used in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.

[0047] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0048] In this application, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.

[0049] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0050] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to directly listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.

[0051] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.

[0052] In this application, "room temperature" or "normal temperature" generally refers to 4℃~35℃, for example, 20℃±5℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 10℃~30℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 20℃~30℃.

[0053] In this application, %(w / w) and wt% both represent weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass-volume percentage.

[0054] In traditional technologies, brake disc coating systems generally rely on solvent-based formulations or high-temperature sintering curing processes, resulting in high VOC emissions and low curing efficiency, which do not meet the requirements of green manufacturing. Furthermore, traditional UV-cured anti-corrosion and heat-resistant coatings have insufficient thick-film curing ability in black systems containing carbon black, making it impossible to guarantee reliable curing of the full film thickness in the complex curved areas of the brake disc. The coating system also has insufficient initial adhesion to the cast iron substrate, making it prone to interface failure under the sequential action of high-temperature impact and corrosive media.

[0055] Traditional UV-cured anti-corrosion coating technologies often rely on flat substrates and ample sunlight for validation. They fail to adequately consider the practical engineering challenges of coexisting "high-light thick film" and "low-light thin film" curing conditions in complex geometric components (especially brake discs), and the different requirements these conditions place on photoinitiator selection, dosage, and synergistic effects. Furthermore, they lack a systematic design for corrosion inhibitor selection and stability at microcracks in these components after high-temperature impact. Therefore, achieving a balanced curing degree between the high-light thick film and low-light thin film regions, while ensuring heat resistance, salt spray resistance, and initial adhesion, is a pressing technical problem that needs to be solved in this field, considering the actual light and film thickness distribution characteristics of complex brake disc geometries.

[0056] Based on this, some embodiments of this application provide a UV-curable anti-corrosion and heat-resistant coating, comprising component A and component B;

[0057] Based on the total mass of component A, component A includes 25wt%~35wt% isocyanurate-based polyurethane acrylate oligomer, 10wt%~15wt% tris(2-hydroxyethyl)isocyanurate triacrylate, 25wt%~40wt% reactive diluent, 3wt%~8wt% superficial photoinitiator, 1wt%~2wt% intermediate layer photoinitiator, 2wt%~6wt% deep layer photoinitiator, 1wt%~5wt% mercapto ester co-initiator, 0~3wt% carbon black paste, 1wt%~5wt% hydrophobic fumed silica, 1wt%~3wt% corrosion inhibitor, 2wt%~5wt% anti-rust pigment, 5wt%~10wt% filler, 0.1wt%~0.5wt% leveling agent, and 0.1wt%~0.3wt% defoamer;

[0058] Component B includes a phosphate ester acrylate adhesion promoter; isocyanurate-based polyurethane acrylate oligomer and the tri(2-hydroxyethyl) isocyanurate triacrylate, wherein the total mass of the triazine ring structure is 7.6% to 9.5% of the mass of the UV-curable anti-corrosion and heat-resistant coating after curing.

[0059] The complex geometry of brake discs means that coating curing and corrosion protection cannot adopt a unified, single strategy of photoinitiation and corrosion inhibition. Instead, a solution must be developed that combines graded initiation, synergistic corrosion inhibition, and heat-resistant residual film, taking into account the actual working conditions where both strong light thick film area and weak light thin film area coexist. Specifically, this application further enhances the coating integrity and corrosion resistance by adjusting the dosage range of IPUA and the dosage of trifunctional monomers (such as THEICTA and TMPTA), while maintaining the heat-resistant skeleton of the coating (the mass ratio of triazine ring structural units is 7.6wt%~9.5wt%). By increasing the dosage of shallow and deep photoinitiators and introducing intermediate photoinitiators, a graded relay initiation system is constructed for the low-light film area of ​​the brake disc, compensating for the gradient discontinuity of photoinitiation efficiency caused by geometric shading in this area. By increasing the dosage of mercapto co-initiator, the chain transfer and continuation ability of limited free radicals under low-light film conditions is enhanced. At the same time, the dosage of anti-rust pigments is strengthened to form a dual corrosion inhibition barrier that takes into account both the conventional service environment and the local defect area after high-temperature impact. By adjusting the mass ratio of components A and B, the above functional components maintain a stable ratio in the actual construction system. At the same time, it achieves both "salt spray corrosion resistance of conventional cast iron substrates" and "salt spray corrosion resistance after high temperature".

[0060] In component A of the UV-curable anti-corrosion and heat-resistant coating of this application, both the isocyanurate-based polyurethane acrylate oligomer and tris(2-hydroxyethyl)isocyanurate triacrylate contain a rigid isocyanurate ring skeleton. Their synergistic effect provides high thermal stability and high crosslinking density. The hexamethylene long carbon chain of the isocyanurate-based polyurethane acrylate oligomer introduces a flexible buffer segment, forming a rigid-flexible synergistic network with the rigid ring structure. This network relaxes shrinkage stress and maintains dimensional stability during curing, preventing thick film cracking. Most of the Si-OH on the surface of the hydrophobic fumed silica particles is converted to Si-CH3, reducing the particles' hydrophilicity and giving them good dispersibility and compatibility in the organic UV system. The particles interact through residual Si-OH hydrogen bonds and van der Waals forces, forming a reversible three-dimensional network structure in the system, endowing the coating with excellent thixotropic properties. The rust-inhibiting pigment and corrosion inhibitor work synergistically to construct a multi-layered, hybrid anti-corrosion barrier on the surface of cast iron materials. The synergistic effect of shallow photoinitiators, intermediate photoinitiators, deep photoinitiators, and mercapto ester co-initiators enables the absorption of UV photons and the generation of free radicals at both the surface and deep layers of the coating, achieving gradient initiation; simultaneously, it ensures complete curing of the resulting coating. Phosphate ester and acrylate adhesion promoters can undergo a condensation reaction with the iron oxide layer on the surface of cast iron materials, resulting in excellent adhesion of the coating to the cast iron substrate. The various raw materials in the above-mentioned UV-cured anti-corrosion and heat-resistant coating work together synergistically to form a coating film with excellent anti-sagging properties, adhesion properties, heat resistance, and anti-corrosion properties, meeting the application requirements of automotive brake discs under complex working conditions.

[0061] It should be noted that in this application, the "sum of the mass of the triazine ring structure" in the isocyanurate-based polyurethane acrylate oligomer and tris(2-hydroxyethyl)isocyanurate triacrylate refers to the "theoretical total mass of the triazine ring structural units." Specifically, the "theoretical total mass of the triazine ring structural units" refers to the sum of the theoretical mass of the triazine ring skeleton portion introduced by the triazine ring-containing components (IPUA and THEICTA) in the cured coating film, which can be calculated based on the feed mass, solid content, and theoretical mass percentage of the triazine ring structural units in the molecular structure of each triazine ring-containing component. Calculations show that the theoretical mass percentage of the triazine ring structural units in IPUA in this application is approximately 15.35 wt%, and the theoretical mass percentage of the triazine ring structural units in THEICTA is approximately 30.49 wt%.

[0062] In some embodiments, the mass ratio of component A to component B is 100:(6~9).

[0063] As an example, the mass ratio of component A to component B can be 100:6, 100:7, 100:8, 100:9, or any value within the range of any two of the above ratios.

[0064] As an example, the mass percentage of isocyanurate-based polyurethane acrylate oligomer in component A can be 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, or any value within the range of any two of the above points.

[0065] In some embodiments, the weight-average molecular weight of the isocyanurate-based polyurethane acrylate oligomer is 1500-3500.

[0066] As an example, the weight-average molecular weight of isocyanurate-based polyurethane acrylate oligomers can be 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, or any value within the range formed by any two of the above point values.

[0067] As an example, the mass percentage of tri(2-hydroxyethyl)isocyanurate triacrylate in component A can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, or any value within the range of any two of the above points.

[0068] Tri(2-hydroxyethyl)isocyanurate triacrylate theoretically contains 30.49 wt% of isocyanurate triazine ring structure (C3N3O3), which has extremely high thermal stability and a decomposition temperature much higher than that of ordinary acrylate systems. Isocyanurate-based polyurethane acrylate oligomers also theoretically contain 15.35 wt% isocyanurate backbone and have the flexibility of aliphatic segments. After the two are cross-linked together to form a film, a highly cross-linked network rich in isocyanurate triazine rings is formed, which enables the coating film to maintain a relatively uniform morphology and structure under high temperature of 400℃ for a long time without producing defects such as blistering and cracking, thereby maintaining good physical barrier integrity.

[0069] In some embodiments, the mass percentage of the isocyanurate triazine ring structure (C3N3O3) unit is 7.6wt% to 9.5wt% of the total mass of the UV-cured anti-corrosion and heat-resistant coating after curing.

[0070] As an example, the mass percentage of reactive diluent in component A can be 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, or any value within the range formed by any two of the above points.

[0071] In some embodiments, the reactive diluent includes at least three of tripropylene glycol diacrylate (TPGDA), trimethylolpropane triacrylate (TMPTA), hydroxypropyl methacrylate (HPMA), isobornyl acrylate (IBOA), and 2-phenoxyethyl acrylate (PHEA).

[0072] Understandably, TMPTA, being a trifunctional monomer, can further enhance crosslinking density within the system. TPGDA, IBOA, PHEA, and HPMA collectively play a role in balancing flexibility. TPGDA, a difunctional monomer with a longer chain segment, is the main driver of flexibility adjustment. The three monofunctional diluents (IBOA, PHEA, and HPMA) alleviate stress by reducing the effective crosslinking point density and introducing free volume at the chain ends. Using these specific types of reactive diluents in a compound formulation can effectively adjust the viscosity, crosslinking density of the cured network, and balanced flexibility of UV-cured anti-corrosion and heat-resistant coatings.

[0073] As an example, the mass percentage of the superficial photoinitiator in component A can be 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, or any value within the range formed by any two of the above points.

[0074] As an example, the mass percentage of deep photoinitiator in component A can be 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, or any value within the range of any two of the above points.

[0075] Shallow photoinitiators can efficiently initiate photoinitiation at the surface of the coating layer, which is 0-20 μm from the coating surface. Deep photoinitiators, with their long-wavelength absorption, can penetrate the strong absorption layer of carbon black pigment and effectively initiate photoinitiation at distances of 20-80 μm from the coating surface, thus ensuring uniform curing of the coating throughout its thickness. The shallow and deep photoinitiators constitute a basic dual-initiator system. Combined with a mercapto ester co-initiator, they synergistically enhance each other through a hydrogen atom transfer mechanism, achieving gradient initiation at different coating depths according to the Beer-Lambert law. This allows for effective curing even with carbon black and a film thickness of 80 μm.

[0076] In some embodiments, the superficial photoinitiator includes α-hydroxyketone photoinitiators.

[0077] Furthermore, α-hydroxy ketone photoinitiators include one or more of 1-hydroxycyclohexylphenyl ketone (184), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), and 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone (2959).

[0078] It is understandable that the absorption peak of α-hydroxy ketone photoinitiators is mainly in the range of 310 nm to 340 nm, which enables efficient initiation of coating surface layers (such as 0 to 20 μm).

[0079] In some embodiments, the deep photoinitiator includes acylphosphine oxide photoinitiators.

[0080] Furthermore, acylphosphine oxide photoinitiators include one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), ethyl 2,4,6-trimethylbenzoylphenylphosphine acid (TPO-L), and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (819).

[0081] As an example, the mass percentage of the intermediate layer photoinitiator can be 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, or any value within the range formed by any two of the above points.

[0082] In some embodiments, the intermediate layer photoinitiator includes α-aminoketone photoinitiators.

[0083] Furthermore, α-aminoketone photoinitiators include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone (369).

[0084] It is understandable that the absorption peak of acylphosphine oxide photoinitiators extends to 370nm~420nm. Through Norrish type I α-cleavage, acyl radicals and phosphonyl radicals are generated, which can penetrate the carbon black absorption layer and effectively initiate photoinitiation in the deep layers of the coating (such as 20μm~80μm).

[0085] In this application, a graded relay initiation system is formed by the synergistic action of a shallow photoinitiator, a 369-type intermediate layer photoinitiator, a deep layer photoinitiator, and a mercapto ester co-initiator: the shallow and deep initiators absorb UV photons and generate free radicals on the surface and deep layers of the coating, respectively; the 369-type initiator connects the transition range of initiation efficiency between the two, making up for the initiation gradient discontinuity caused by light shading in complex geometric areas such as brake disc ventilation disc pillars and concave surfaces; and the mercapto ester co-initiator continues the limited free radical reaction chain through chain transfer, so that the coating can achieve complete curing in both the strong light thick film region and the weak light thin film region.

[0086] It is understandable that, in the application scenario of brake discs, there is a problem of "coexistence of strong light thick film area and weak light thin film area". The introduction of α-amino ketone photoinitiators can connect the transition range of initiation efficiency between shallow photoinitiators and deep photoinitiators, compensate for the initiation efficiency gradient discontinuity caused by the decrease in light intensity in areas such as brake disc ventilation disc pillars and ventilation hole inner walls, and avoid the appearance of weak curing zones in the middle layer of the coating or in the partially obscured areas.

[0087] In some embodiments, the mass ratio of the superficial photoinitiator to the deep photoinitiator is (1~3):1.

[0088] As an example, the mass ratio of the superficial photoinitiator to the deep photoinitiator can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, or any value within the range of any two of the above ratios.

[0089] As an example, the mass percentage of the mercapto ester co-initiator in component A can be 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, or any value within the range formed by any two of the above points.

[0090] The thiol group (-SH) in the thiol ester co-initiator donates hydrogen to the carbon-center free radical, regenerating the sulfur-center free radical (RS·). RS· then further initiates the polymerization of acrylate double bonds, significantly improving free radical utilization efficiency in the depth of the coating where photons are limited, thereby increasing the C=C double bond conversion rate. Simultaneously, RS· reacts with dissolved oxygen in the system, reducing the quenching efficiency of free oxygen on the carbon-center free radical, and donates hydrogen to the peroxy radical (ROO·) generated by oxygen inhibition, restoring chain growth. This effectively inhibits surface oxygen inhibition and improves surface curing quality. The sulfur atom in the thiol ester possesses a lone pair of electrons, enabling it to form M←S coordination bonds with Lewis acid sites on the metal surface, serving as an auxiliary interfacial bonding layer for phosphate ester covalent bonding. Thus, the thiol ester co-initiator can achieve complete curing of dark-colored coatings containing carbon black paste with a thickness of 40μm~80μm, and exhibits excellent hardness properties.

[0091] In some embodiments, the thiol ester co-initiator includes one or more of the following: thiol ester modified acrylic compound, pentaerythritol tetramercaptopropionate (PETMP), tris(3-mercaptopropionic acid) trimethylolpropane ester (TMPMP), pentaerythritol tetrakis(3-mercaptobutyrate) ester (PE1), and dipentaerythritol hexa(3-mercaptobutyrate) ester (DiPE1).

[0092] In some embodiments, the thiol ester co-initiator is a polythiol compound or a thiol-functionalized acrylate oligomer. Further, the thiol-functionalized acrylate oligomer is an acrylate oligomer with thiol groups in its side chains and / or at its ends.

[0093] In some of these embodiments, the thiol ester modified acrylic compound includes EBECRIL 375 or EBECRIL LD01.

[0094] As an example, the mass percentage of carbon black paste in component A can be 0, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, or any value within the range of any two of the above points.

[0095] Furthermore, the mass percentage of carbon black paste in component A is 1wt%~3wt%.

[0096] As an example, the mass percentage of hydrophobic fumed silica in component A can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, or any value within the range formed by any two of the above points.

[0097] Furthermore, the mass percentage of hydrophobic fumed silica is 2wt%~3wt%.

[0098] Most of the Si-OH groups on the surface of hydrophobic fumed silica particles are converted to Si-CH3, reducing the particles' hydrophilicity and giving them good dispersibility and compatibility in organic UV systems. Through residual Si-OH hydrogen bonds and van der Waals forces, the particles interact to form a reversible three-dimensional network structure, endowing the coating with excellent thixotropic properties. Combined with the structural reinforcement effect of fillers, the coating achieves a dual rheological target: a viscosity of no less than 50 Pa·s under low shear conditions and a viscosity of no more than 0.04 Pa·s under high shear conditions. Specifically, the UV-curable anti-corrosion and heat-resistant coating of this application exhibits a complete three-dimensional network structure and high system viscosity at low shear rates, demonstrating excellent anti-sagging ability. At high temperatures and high shear rates, shear force disrupts the three-dimensional network, and the increased temperature further reduces the strength of intermolecular interactions, significantly lowering the system viscosity and achieving excellent atomization performance. After the shear force is removed and the temperature recovers, the three-dimensional network is rapidly rebuilt, and the viscosity quickly recovers, preventing the coating from sagging on vertical surfaces.

[0099] In some embodiments, the hydrophobic fumed silica includes dimethyldichlorosilane surface-modified fumed silica.

[0100] In some of these embodiments, the hydrophobic fumed silica is selected from Evonik AEROSIL R972.

[0101] In some embodiments, the specific surface area of ​​the hydrophobic fumed silica is 90 m². 2 / g~130m 2 / g.

[0102] As an example, the specific surface area of ​​hydrophobic fumed silica can be 90 m². 2 / g, 100m 2 / g、110m 2 / g、120m 2 / g、130m 2 / g, or any value within the range formed by any two of the above point values.

[0103] As an example, the mass percentage of corrosion inhibitor in component A can be 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt%, 3wt%, or any value within the range formed by any two of the above points.

[0104] In some embodiments, the corrosion inhibitors include benzotriazole corrosion inhibitors and mercaptobenzothiazole corrosion inhibitors.

[0105] In some embodiments, the benzotriazole corrosion inhibitor includes one or more of benzotriazole (BTA) and methylbenzotriazole (TTA).

[0106] In some of these embodiments, the mercaptobenzothiazole corrosion inhibitors include mercaptobenzothiazole (MBT).

[0107] In some of these embodiments, the corrosion inhibitors include benzotriazole (BTA) and mercaptobenzothiazole (MBT).

[0108] During short-duration high-temperature thermal shock, corrosion inhibitors should not be simply understood as remaining entirely in their original free state. They may primarily exist in the form of metal interface adsorption / complexation, free or semi-fixed states confined by coating networks, adsorption states on pigment and filler surfaces, and a small amount of residual thermal decay. Among these, BTA has relatively limited thermal stability and is more likely to volatilize, sublimate, or undergo further thermal oxidation / decomposition at 400℃. Its post-thermal residue mainly depends on metal interface adsorption, coating network confinement, or pigment and filler surface adsorption. MBT (mercaptobenzothiazole) at 400℃ should also not be considered as a simple complete molecule volatilization, but rather a process of simultaneous volatilization and thermal decomposition. Furthermore, the thiol groups and nitrogen and sulfur sites of the thiazole ring in MBT give it the potential for both interfacial adsorption corrosion inhibition and limited chain transfer. During the photocuring process, some MBT may be confined by the cross-linked network through chain transfer reactions or network association. Combined with its adsorption effect on the metal interface, after a short-term high-temperature thermal shock at 400°C, it may exhibit a lower tendency to migrate or volatilize compared to unconfined free MBT. This residual portion can synergistically work with the remaining BTA, rust-inhibiting pigments, and their passivation products to maintain the corrosion inhibition effect of the coating at the cast iron substrate interface to a certain extent.

[0109] As an example, the mass percentage of the rust-preventive pigment in component A can be 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, or any value within the range formed by any two of the above points.

[0110] In some embodiments, the rust-preventive pigment includes one or more of aluminum tripolyphosphate-zinc oxide mixture and aluminum zinc phosphomolybdate.

[0111] Furthermore, the rust-preventive pigments include aluminum tripolyphosphate and zinc oxide. Even further, a mixture of aluminum tripolyphosphate and zinc oxide can be selected from Guangxi Xinjing DY-222.

[0112] Understandably, the nitrogen- or sulfur-containing heterocyclic groups in the corrosion inhibitor can form a coordination adsorption film with the cast iron surface, inhibiting the anodic dissolution of iron; the rust-preventive pigment continuously releases passivating ions such as phosphate and molybdate to the metal surface, forming a dense passivation protective layer on the metal surface; the synergistic effect of the two gives the coating excellent anti-corrosion and salt spray resistance on the cast iron substrate.

[0113] As an example, the mass percentage of filler in component A can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, or any value within the range formed by any two of the above points.

[0114] Understandably, by adjusting the amount of filler, the viscosity, rheological properties, and other characteristics of UV-cured anti-corrosion and heat-resistant coatings can be kept stable and meet standards. Simultaneously, the filler can synergistically work with hydrophobic fumed silica to enhance low-shear viscosity.

[0115] In some embodiments, the filler includes one or more of barium sulfate, silica powder, talc, calcium carbonate, and mica powder.

[0116] Furthermore, the particle size of the filler is above 3000 mesh.

[0117] As an example, the mass percentage of leveling agent in component A can be 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, or any value within the range formed by any two of the above points.

[0118] In some of these embodiments, the leveling agent is selected from BYK-333.

[0119] As an example, the mass percentage of defoamer in component A can be 0.1wt%, 0.2wt%, 0.3wt%, or any value within the range formed by any two of the above points.

[0120] In some of these embodiments, the defoamer is selected from Defom 6800.

[0121] In some embodiments, the acid value of the phosphate acrylate adhesion promoter is 250 mg KOH / g to 310 mg KOH / g.

[0122] As an example, the acid value of the phosphate ester acrylate adhesion promoter can be 250 mg KOH / g, 260 mg KOH / g, 270 mg KOH / g, 280 mg KOH / g, 290 mg KOH / g, 300 mg KOH / g, 310 mg KOH / g, or any value within the range formed by any two of the above values.

[0123] In some of these embodiments, component B includes one or more of Changxing EM39, Nippon Kayaku PM-2, and Sartoma CD9051.

[0124] The coating described in this application has at least the following advantages: (1) It has an effective thixotropic and rheological control capability in a full-solid UV curing system, enabling the coating to have easy atomization and application properties that meet the requirements of automated brake disc spraying production lines. (2) Through a multi-initiation system, it achieves reliable curing of the entire film thickness range (40μm~80μm) in the complex curved areas and weak light irradiation areas of the brake disc. (3) Through the synergistic effect of functional components, it establishes a strong bond at the interface of the cast iron substrate, with an adhesion level of less than or equal to 1. (4) Through a composite anti-corrosion system of corrosion inhibitor and rust-preventive pigment, it achieves excellent abnormal temperature anti-corrosion performance on the cast iron substrate with a neutral salt spray resistance time of greater than or equal to 360h (rated as S0R0), which is about 50% higher than the industry standard for brake disc coating anti-corrosion requirements, providing a guarantee for the long-term protection of brake discs in harsh corrosive environments. (5) After heat treatment at 400℃ for 30 min, the coating film is free from cracking and blistering, and it is resistant to neutral salt spray for 240 h without rust (S0R0), which is significantly improved compared to the industry standard for heat-resistant salt spray.

[0125] Some embodiments of this application also provide a method for preparing a UV-curable anti-corrosion and heat-resistant coating, comprising the following steps:

[0126] S10. Provide raw materials according to the above-mentioned UV-curable anti-corrosion and heat-resistant coating;

[0127] S20. Mix isocyanurate-based polyurethane acrylate oligomer, tris(2-hydroxyethyl) isocyanurate triacrylate and a portion of reactive diluent to prepare the main resin premix.

[0128] S30. Mix the shallow photoinitiator, intermediate photoinitiator and deep photoinitiator with the remaining active diluent to prepare the initiator predispersant;

[0129] S40. The main resin premix is ​​mixed with hydrophobic fumed silica, corrosion inhibitor, rust-preventive pigment, filler, defoamer and leveling agent, and then ground to obtain a sand slurry.

[0130] S50. Mix the sand milling slurry, initiator predispersant, carbon black slurry and mercapto ester co-initiator to obtain component A;

[0131] S60, Phosphate ester acrylate adhesion promoter is used as component B.

[0132] It should be noted that components A and B should be stored separately. Before use, components A and B should be mixed evenly according to the mass ratio and used within 72 hours after mixing.

[0133] In some embodiments, the method for preparing isocyanurate-based polyurethane acrylate oligomers includes the following steps:

[0134] Hexamethylene diisocyanate trimer was mixed with acrylate monomers and then subjected to an addition reaction to obtain isocyanurate-based polyurethane acrylate oligomers.

[0135] Among them, acrylate monomers contain hydroxyl groups.

[0136] It is understandable that the -NCO in the hexamethylene diisocyanate trimer can undergo an addition reaction with the -OH in the acrylate monomer.

[0137] Furthermore, the temperature of the addition reaction is 65℃~75℃. As an example, the temperature of the addition reaction can be 65℃, 66℃, 67℃, 68℃, 69℃, 70℃, 71℃, 72℃, 73℃, 74℃, 75℃, or any value within the range formed by any two of the above points.

[0138] Furthermore, the addition reaction takes 4 to 5 hours.

[0139] Furthermore, the addition reaction is carried out in a protective atmosphere. Even further, the protective atmosphere includes a nitrogen atmosphere.

[0140] In some embodiments, the acrylate monomers include one or more of hydroxypropyl acrylate (HPA), hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).

[0141] In some embodiments, the preparation method of carbon black paste includes the following steps: mixing carbon black, reactive diluent, and dispersant, and grinding to a particle size ≤10μm to prepare carbon black paste. Further, the carbon black content of the carbon black paste is 10wt%.

[0142] In some embodiments, the particle size of the sand-milling slurry is ≤20μm.

[0143] Some embodiments of this application also provide a coating film formed using the above-described UV-curable anti-corrosion and heat-resistant coating.

[0144] In some embodiments, the method for preparing the coating film includes the following steps:

[0145] Mixing component A and component B in the above-mentioned UV-curable anti-corrosion and heat-resistant coating yields a mixed coating;

[0146] The mixed coating is heated to 50℃~70℃ and sprayed onto the substrate to form a wet film;

[0147] The wet film is cured to obtain the coated product.

[0148] As an example, the temperature at which the UV-cured anti-corrosion and heat-resistant coating is heated can be 50℃, 51℃, 52℃, 53℃, 54℃, 55℃, 56℃, 57℃, 58℃, 59℃, 60℃, 61℃, 62℃, 63℃, 64℃, 65℃, 66℃, 67℃, 68℃, 69℃, 70℃, or any value within the range formed by any two of the above points.

[0149] In some embodiments, the spraying is performed using a hot spray cold part process.

[0150] In some embodiments, the atomization pressure of the spray is 0.3 MPa to 0.5 MPa.

[0151] In some embodiments, the coating thickness is 40 μm to 80 μm.

[0152] In some embodiments, the curing process is a UV light curing process.

[0153] Furthermore, the UV curing treatment has a light intensity greater than or equal to 250 mW / cm². 2 .

[0154] Furthermore, the energy of the UV curing treatment is 800 mJ / cm². 2 ~1200mJ / cm 2 .

[0155] In some of these embodiments, the substrate comprises cast iron.

[0156] The coating of this application has a conventional neutral salt spray resistance time of 360 hours or more, with a rating of S0R0; after heat treatment at 400℃ for 30 minutes, the coating has no cracks or bubbles, and its neutral salt spray resistance time can reach 240 hours, with a rating of S0R0; and it has good anti-rheological properties.

[0157] Some embodiments of this application also provide a cast iron article including the above-described coating.

[0158] Some embodiments of this application also provide a brake disc, including the cast iron product described above.

[0159] Understandably, areas such as the concave arc surface of the brake disc cap's shoulder experience paint mist accumulation due to geometric shielding effects, resulting in a dry film thickness that is 10μm~20μm thicker than adjacent planar areas, reaching up to 70μm~80μm. If the coating does not possess reliable curing capabilities across a wide film thickness range, insufficient curing of the underlying layer will lead to decreased adhesion in these areas, resulting in localized failure under the sequential effects of high temperatures and corrosive media. Furthermore, automated brake disc spraying production lines place high demands on the ease of atomization and application of the coating.

[0160] It is understandable that areas such as the side ventilation columns and inner walls of ventilation holes on brake discs are affected by light shielding, incident angle deflection, and obstruction from adjacent structures, resulting in lower actual UV light intensity received compared to areas directly exposed to sunlight. Even with optimization of lamps, the light intensity in these locations is still only about 75% of the intensity of the front light. Furthermore, due to factors such as the spray gun's incident angle, paint mist accessibility, and airflow turbulence, the coating thickness in these areas is typically thinner than on the front planar area. If the coating lacks reliable curing capability under conditions of light intensity attenuation and film thickness fluctuations, these low-light film areas are prone to reduced adhesion and density due to insufficient free radical generation or incomplete cross-linking, leading to localized failure under high temperature, humidity, and salt spray conditions. Therefore, UV-curable protective coatings for brake discs must possess both deep curing capability in high-light, thick-film areas and low-light curing capability in low-light, thin-film areas.

[0161] The present application will be further described below with reference to specific embodiments and comparative examples, but these should not be construed as limiting the scope of protection of the present application. Unless otherwise specified, the raw materials involved in the following specific embodiments are all commercially available, the instruments used are all commercially available, and the processes involved are conventionally selected by those skilled in the art unless otherwise specified.

[0162] The preparation methods of some of the raw materials used in the embodiments and comparative examples of this application are as follows:

[0163] (1) Synthesis of isocyanurate-based polyurethane acrylate oligomer (IPUA): Hexamethylene diisocyanate (HDI) trimer (Desmodur® N3300, Covestro) and hydroxypropyl acrylate (HPA) were used as raw materials, and the feed was carried out at a molar ratio of -NCO to -OH of 1:1.05. Under nitrogen protection, the reaction was stirred at 70°C for 4 hours. 0.1 wt% dibutyltin dilaurate (DBTDL) was added as a catalyst, and 0.06 wt% 4-methoxyphenol (MEHQ) was added as a polymerization inhibitor. The reaction progress was monitored by infrared spectroscopy until the polymer reached 2270 cm⁻¹. -1 When the characteristic absorption peak of -NCO completely disappears, the isocyanurate-based polyurethane acrylate oligomer (IPUA) is obtained; the product is a colorless to slightly yellow transparent viscous liquid with a measured viscosity of 6800 mPa·s at 60℃.

[0164] The IPUA prepared above has the isocyanuric acid ring of HDI trimer as the core, and the three arm ends are connected to the acrylate groups of hydroxypropyl acrylate (HPA) through urethane bonds (-NH-COO-), forming a star oligomer containing three terminal acryloyl groups (CH2=CH-COO-).

[0165] FTIR analysis showed 3367.7 cm -1 2935.1 / 2859.9cm-1 The peak at 1718.2 cm⁻¹ corresponds to the stretching vibrations of NH / OH and -CH₂-. -1 1677.7cm -1 The strong absorption is attributed to the stretching vibrations of the ester carbonyl group and the C=O ring of the isocyanurate ester; 2270 cm⁻¹ -1 The characteristic peak of -NCO completely disappeared at 979.6 cm⁻¹. -1 808.0cm -1 The presence of the characteristic peak of acrylate =CH2 confirms that the -NCO of N3300 has completely reacted with HPA.

[0166] GPC analysis showed that the product was dominated by the main peak at Log M≈3.05~3.08, while the intensity of the secondary oligomer peaks decreased sharply and accounted for a very small proportion, indicating that the molecular weight distribution of the product was relatively concentrated, the target product was the main component and the structure was clear.

[0167] (2) Preparation of carbon black slurry: Carbon black, isobornyl acrylate (IBOA) and dispersant are mixed in a mass ratio of 1:8:1, pre-dispersed and then ground in a sand mill until the particle size is ≤10μm to obtain carbon black slurry with a carbon black content of 10wt%, which is then set aside.

[0168] (3) Tri(2-hydroxyethyl) isocyanurate triacrylate (THEICTA) is marketed under the brand name Changxing ETERMER. ® EM2308;

[0169] The product model for the carbon black is Orion FW200;

[0170] The product model of the talc is Liaoning Xinda SD-9286;

[0171] The product model of the silicon micro powder is Henan Nonferrous Metals Jinyuan JYER-12;

[0172] The commercial model for hydrophobic fumed silica is Evonik AEROSIL. ® R972;

[0173] The commercial model of benzotriazole (BTA) is Chengbei Chemical Industry BT-120;

[0174] Mercaptobenzothiazole (MBT) was purchased from Zibo Tailize Chemical Co., Ltd.

[0175] The commercial model for the mixture of aluminum tripolyphosphate and zinc oxide is Guangxi Xinjing DY-222;

[0176] Zinc aluminum phosphomolybdate was purchased from Guangxi Xinjing.

[0177] The product name of the dispersant is BYK-163 from BYK Chemicals.

[0178] The product name of the leveling agent is BYK-333 from BYK Chemicals.

[0179] The product model of the defoamer is Deqian Defom 6800.

[0180] Example 1

[0181] (1) Provide each raw material according to the mass fractions in Table 1; heat THEICTA to a temperature above 60°C until completely melted, add a portion of reactive diluent (60wt% of the total amount), stir and dilute at 60°C, and then mix it evenly with IPUA to obtain the main resin premix; dissolve the deep photoinitiator and the shallow photoinitiator with the remaining portion of reactive diluent at 60°C to obtain the initiator predispersant.

[0182] (2) While stirring, add corrosion inhibitor, rust-preventive pigment, filler, hydrophobic fumed silica, defoamer and leveling agent to the main resin premix, and continue stirring and mixing for 30 minutes until uniform to obtain the mixture.

[0183] (3) The above mixture is ground in a sand mill until the particle size is ≤20μm to obtain a sand mill slurry.

[0184] (4) Add the initiator pre-dispersion liquid, carbon black slurry and mercapto ester co-initiator to the sand mill slurry in sequence, and mix evenly to obtain component A.

[0185] (5) Mix component A and component B evenly according to the mass ratio before use to obtain UV-curable anti-corrosion and heat-resistant coating; use within 72 hours after mixing.

[0186] (6) The surface of the cast iron substrate HT-250 is sandblasted to remove rust (sandblasting Sa2.5 grade treatment) and remove oil and dust; the UV-cured anti-corrosion and heat-resistant coating is preheated to 60°C through a circulation system and then sprayed using a hot spray cold part process. The workpiece is kept at room temperature and no preheating is required. The atomization pressure is 0.4MPa; the dry film is controlled to reach a specific thickness. High-pressure mercury lamp UV light source is used for curing, with a light intensity of 250mW / cm² and a curing energy of 1000mJ / cm².

[0187] Examples 2-5 and Comparative Examples 1-6 are basically the same as Example 1, except that the raw materials used to prepare the UV-cured anti-corrosion and heat-resistant coating are different; Example 6 has a light intensity of 180 mW / cm². 2 Curing energy 800mJ / cm 2 This simulates scenarios with lower curing light intensity and lower curing energy. Specific details are shown in Tables 1 and 2, where the amounts of each raw material refer to parts by mass.

[0188] Table 1

[0189]

[0190] Table 2

[0191]

[0192] In Tables 1 and 2 above, " / " indicates that the component was not added or that the component is absent. BPUA refers to HDI biuret-type polyurethane acrylate, which has an open-chain biuret structure and does not contain isocyanurate triazine rings. It is prepared by reacting HDI dimer Desmodur N3200 with HPA. UPUA refers to polyurethane acrylate containing a urea diketone four-membered heterocyclic structure. It is prepared by reacting HDI dimer Desmodur N3400 with HPA. The synthesis of BPUA (Biuret Polyurethane Acrylate) and UPUA (Uretdione Polyurethane Acrylate) follows the same approach as IPUA, differing only in the starting materials and reaction temperature / duration: BPUA uses HDI biuret (Covestro Desmodur N3200) containing an open-chain biuret structure instead of HDI trimer (Covestro Desmodur N3300) containing a six-membered ring of isocyanurate. Given the higher reactivity of the biuret structure, the reaction conditions with HPA monomer are adjusted to 60°C for 2 hours. UPUA uses HDI dimer (Covestro Desmodur N3400) containing a four-membered ring of urea diketone instead of HDI trimer. Since the urea diketone ring requires a higher temperature for ring opening, the reaction conditions are correspondingly increased to 85°C for 6 hours. Both are prepared by reacting with HPA monomer at a molar ratio of -NCO:-OH = 1:1.05 and under the same other process conditions (catalyst, polymerization inhibitor, feeding method, etc.).

[0193] Performance testing

[0194] Initial adhesion: Tested according to GB / T 9286-2021 cross-cut adhesion test (film thickness ≤60μm, spacing 1mm; film thickness >60μm, spacing 2mm), ≤1 is qualified.

[0195] Heat resistance: The coated sample was placed in a muffle furnace and heat-treated at the set temperature (400℃) and time (30min). After cooling to room temperature, the appearance of the coating was visually evaluated (whether it cracks, bubbles, or peels off), and evaluated according to GB / T 1735.

[0196] Neutral salt spray after heat resistance: The coated samples, after being cooled to room temperature after heat resistance treatment, are subjected to a neutral salt spray test according to GB / T 10125-2021. The salt concentration is 5%, the temperature is 35℃, and the spraying is continuous. The samples are taken out and rated according to the specified time. The S0R0 (no rust, no blistering) is the pass criterion.

[0197] Direct neutral salt spray (without heat resistance treatment): After UV curing, the coated sample is placed at room temperature for 24 hours and then subjected to a neutral salt spray test according to GB / T10125-2021. The S0R0 (no rust, no blistering) is the pass criterion.

[0198] STVR testing: A rotational rheometer was used to measure the coating at 23℃ and 0.01s. -1 Low shear viscosity η1 under the conditions of 60℃ and 1000s -1 Under the condition of high shear viscosity η2, calculate STVR=η1 / η2.

[0199] Coating appearance: visually evaluate and record whether any abnormal phenomena such as cracking, blistering, or peeling occur after the heat treatment and cooling and after the salt spray test.

[0200] Film thickness: The dry film thickness was determined according to GB / T 13452.2.

[0201] Anti-flow coating thickness: The anti-flow coating thickness was measured 5cm above the hole at a position where the flow mark along the lower edge of the hole reaches 5mm. The coating was sprayed with a gradient paint film at 60℃ on a vertical φ6mm hole flow plate, leveled for 2 minutes, and then UV cured.

[0202] It should be noted that the shear-temperature viscosity ratio (STVR) in this application is defined as: STVR = η(23℃, 0.01s) -1 ) / η(60℃, 1000s) -1 );

[0203] Where η(23℃, 0.01s) -1 The coating was tested at 23°C and a shear rate of 0.01 s⁻¹. -1 Viscosity at 60℃, 1000s -1 The coating was subjected to a shear rate of 1000 s at 60°C. -1 The viscosity at that point.

[0204] The performance test results of the above embodiments and comparative examples are shown in Tables 3 and 4.

[0205] Table 3

[0206]

[0207] Table 4

[0208]

[0209] As shown in the table above, Example 1 had an initial adhesion rating of 0, an STVR of 2432, and an anti-sagging film thickness of 62 μm. After heat treatment at 400℃ for 30 min, the coating showed no cracking or blistering and was rated S0R0 after 240 h. The direct salt spray test was conducted for 360 h and the rating remained S0R0. Overall, the sample was deemed qualified.

[0210] In Example 2, after reducing the fumed silica content, the STVR of the sample decreased to 1536, and the anti-sagging film thickness narrowed to 40 μm, still meeting the construction requirements; the heat resistance and salt spray performance were consistent with those of Example 1, and the overall assessment was qualified.

[0211] In Example 3, after increasing the content of fumed silica, the STVR of the sample increased to 2672, the anti-sagging film thickness increased to 81 μm, and the thixotropic properties were further enhanced; the content of triazine ring unit structure was 9.49 wt%, and the heat resistance and salt spray performance were consistent with those of Example 1, and the overall assessment was qualified.

[0212] In Example 4, the mass ratio of component B was reduced, and the initial adhesion of the sample was grade 1. The heat resistance and salt spray performance at a film thickness of 80 μm were consistent with those in Example 1, and the overall assessment was qualified.

[0213] In Example 5, the mass ratio of component B was increased, and the initial adhesion of the sample was grade 0. The performance of the sample with a film thickness of 80 μm was consistent with that of Example 1, and the sample was deemed qualified.

[0214] Example 6 simulated low-light film curing conditions, and the initial adhesion of the sample was grade 1; the content of triazine ring unit structure was 7.65wt%, and the heat resistance and salt spray performance under the extreme low film thickness of 40μm still met the standard requirements, and the overall judgment was qualified.

[0215] In Comparative Example 1, no hydrophobic fumed silica was added, and the STVR of the sample plummeted to 750, the anti-sagging film thickness was only 23 μm, and the low shear viscosity decreased from 68.1 Pa·s to 21 Pa·s; the sample was deemed unqualified overall.

[0216] In Comparative Example 2, no corrosion inhibitors or rust-preventing pigments were added. The sample showed blistering (S2R2) in direct salt spray performance after 72 hours, and obvious rust appeared in salt spray performance after another 24 hours after heat resistance. It was judged to be unqualified overall.

[0217] In Comparative Example 3, no component B was added. The initial adhesion of the sample was grade 5, and the adhesion to the cast iron substrate was completely failed. The heat resistance and salt spray tests were not applicable. The overall judgment was that it was unqualified.

[0218] In Comparative Example 4, no mercapto ester co-initiator or intermediate layer initiator was added. The initial adhesion of the sample was grade 4, which failed the adhesion test. The heat resistance and salt spray tests were also not applicable. Overall, the sample was deemed unqualified.

[0219] In Comparative Example 5, BPUA was used instead of IPUA. Due to the fact that the thermal stability of the biuret structure is not as good as that of the triazine ring, the coating film cracked at a high temperature of 400℃, and the heat resistance was not up to standard. In addition, the coating film density was not as good as that of IPUA, and the salt spray test could not exceed 240h. Therefore, it was judged to be unqualified.

[0220] In Comparative Example 6, UPUA was used instead of IPUA. The urea diketone structure also showed significant differences in thermal stability and final coating density, and both heat resistance and initial salt spray resistance tests were unqualified; therefore, it was deemed unqualified overall.

[0221] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0222] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this application should be determined by the appended claims.

Claims

1. A UV-curable anti-corrosion and heat-resistant coating, characterized in that, Includes component A and component B; Based on the total mass of component A, component A comprises 25wt%~35wt% isocyanurate-based polyurethane acrylate oligomer, 10wt%~15wt% tris(2-hydroxyethyl)isocyanurate triacrylate, 25wt%~40wt% reactive diluent, 3wt%~8wt% superficial photoinitiator, 1wt%~2wt% intermediate layer photoinitiator, 2wt%~6wt% deep layer photoinitiator, 1wt%~5wt% mercapto ester co-initiator, 0~3wt% carbon black paste, 1wt%~5wt% hydrophobic fumed silica, 1wt%~3wt% corrosion inhibitor, 2wt%~5wt% rust-preventive pigment, 5wt%~10wt% filler, 0.1wt%~0.5wt% leveling agent, and 0.1wt%~0.3wt% defoamer; Component B includes a phosphate ester acrylate adhesion promoter; the sum of the mass of the triazine ring structure in the isocyanurate-based polyurethane acrylate oligomer and the tri(2-hydroxyethyl) isocyanurate triacrylate is 7.6% to 9.5% of the mass of the UV-curable anti-corrosion and heat-resistant coating after curing.

2. The UV-curable anti-corrosion and heat-resistant coating according to claim 1, characterized in that, The UV-cured anti-corrosion and heat-resistant coating satisfies at least one of the following characteristics: (1) The active diluent includes at least three of the following: tripropylene glycol diacrylate, trimethylolpropane triacrylate, hydroxypropyl methacrylate, isobornyl acrylate and 2-phenoxyethyl acrylate; (2) The shallow photoinitiator includes α-hydroxyketone photoinitiators; (3) The deep photoinitiator includes acylphosphine oxide photoinitiators; (4) The intermediate layer photoinitiator includes α-aminoketone photoinitiators; (5) The thiol ester co-initiator includes one or more of the following: thiol ester modified acrylic compound, pentaerythritol tetramercaptopropionate, tris(3-mercaptopropionic acid) trimethylolpropane ester, tetra(3-mercaptobutyric acid) pentaerythritol ester and hexa(3-mercaptobutyric acid) dipentaerythritol ester; (6) The hydrophobic fumed silica includes dimethyldichlorosilane surface-modified fumed silica; (7) The specific surface area of ​​the hydrophobic fumed silica is 90 m². 2 / g~130m 2 / g; (8) The rust-preventive pigment includes one or more of aluminum tripolyphosphate-zinc oxide mixture and aluminum zinc phosphomolybdate; (9) The filler includes one or more of barium sulfate, silica fume, talc, calcium carbonate and mica powder; (10) The acid value of the phosphate ester acrylate adhesion promoter is 250 mg KOH / g to 310 mg KOH / g; (11) The mass ratio of component A to component B is 100: (6~9).

3. The UV-curable anti-corrosion and heat-resistant coating according to any one of claims 1 to 2, characterized in that, The corrosion inhibitors include benzotriazole corrosion inhibitors and mercaptobenzothiazole corrosion inhibitors.

4. The UV-curable anti-corrosion and heat-resistant coating according to claim 3, characterized in that, The UV-cured anti-corrosion and heat-resistant coating satisfies at least one of the following characteristics: (1) The benzotriazole corrosion inhibitors include one or more of benzotriazole and methylbenzotriazole; (2) The mercaptobenzothiazole corrosion inhibitors include mercaptobenzothiazole.

5. A method for preparing a UV-curable anti-corrosion and heat-resistant coating, characterized in that, Includes the following steps: The raw materials are provided for the UV-curable anti-corrosion and heat-resistant coating according to any one of claims 1 to 4; The main resin premix was prepared by mixing isocyanurate-based polyurethane acrylate oligomer, tris(2-hydroxyethyl) isocyanurate triacrylate and a portion of reactive diluent. The shallow photoinitiator, intermediate photoinitiator and deep photoinitiator are mixed with the remaining active diluent to prepare the initiator pre-dispersion; The main resin premix is ​​mixed with hydrophobic fumed silica, corrosion inhibitor, rust-preventive pigment, filler, defoamer and leveling agent, and then ground to obtain a sand-grinding slurry; The sand-milling slurry, the initiator pre-dispersion liquid, the carbon black slurry, and the mercapto ester co-initiator are mixed to obtain component A; Phosphate acrylate adhesion promoters are used as component B.

6. The method for preparing the UV-curable anti-corrosion and heat-resistant coating according to claim 5, characterized in that, The preparation method of the isocyanurate-based polyurethane acrylate oligomer includes the following steps: Hexamethylene diisocyanate trimer was mixed with acrylate monomers and then subjected to an addition reaction to obtain isocyanurate-based polyurethane acrylate oligomers. The acrylate monomers contain hydroxyl groups.

7. The method for preparing the UV-curable anti-corrosion and heat-resistant coating according to claim 6, characterized in that, The acrylate monomers include one or more of hydroxypropyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

8. A coating film, characterized in that, The coating is formed using any one of claims 1 to 4, which is a UV-cured anti-corrosion and heat-resistant coating.

9. A cast iron product, characterized in that, Includes the coating as described in claim 8.

10. A brake disc, characterized in that, Including the cast iron articles as described in claim 9.