A hydrophobic and dust-proof coating for photovoltaic modules and its preparation method
By combining nano-silica and methyl MQ silicone resin, and combining polysilane stepwise pre-hydrolysis and MQ resin cross-linking to form a film, a hydrophobic and dustproof coating with a dense three-dimensional network structure was prepared, which solved the problems of poor dustproof effect and low light transmittance of photovoltaic modules, and achieved efficient self-cleaning and weather resistance.
Patent Information
- Application Number
- CN202611554885.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing protective coatings for photovoltaic modules have poor dustproof performance, low light transmittance, and are prone to failure. Furthermore, their manufacturing processes are complex and costly, making them unsuitable for large-scale applications of photovoltaic modules.
A combination of nano-silica, methyl MQ silicone resin, crosslinking agent, silane modifier and composite organic solvent is used to form a dense three-dimensional network structure through the principle of multisilane step pre-hydrolysis and MQ resin crosslinking. Combined with staged curing process, a hydrophobic and dustproof coating is prepared.
It achieves hydrophobic self-cleaning, strong adhesion, and aging resistance on the surface of photovoltaic modules, with a light transmittance of ≥92%, and can withstand the erosion of sand and sand in desert environments, resulting in a long service life.
Smart Images

Figure CN123107539A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic module protective coating technology, specifically relating to a hydrophobic and dustproof coating for photovoltaic modules and its preparation method. Background Technology
[0002] Photovoltaic modules are exposed to complex outdoor environments for extended periods, and their surfaces are prone to accumulating dust, rainwater, and smog pollutants. Dust accumulation significantly reduces the light transmittance of photovoltaic glass, hindering sunlight from entering and causing a continuous decline in the photoelectric conversion efficiency of photovoltaic modules. At the same time, rainwater adhesion and alternating wet and dry conditions can cause scale buildup, corrosion, and aging on the glass surface, further shortening the lifespan of photovoltaic modules.
[0003] Currently, most conventional photovoltaic protective coatings on the market are ordinary hydrophilic or weakly hydrophobic coatings, which have poor dustproof and self-cleaning effects, insufficient adhesion, and are prone to peeling, failure, and decreased light transmittance after long-term outdoor use. Existing hydrophobic coatings mostly use a single silane modified system, which has defects such as uneven micro-nano structure, weak bonding of hydrophobic groups, and poor film formation. In addition, the preparation process is complex and the raw material cost is high, making it difficult to adapt to the large-scale application scenarios of photovoltaic modules. Summary of the Invention
[0004] To address the problems of poor dustproof performance, low light transmittance, and easy failure of existing photovoltaic coatings, this invention develops a hydrophobic dustproof coating adapted to photovoltaic modules based on the principle of hydrophobic modification of nano-silica and cross-linking of polysilanes. By optimizing the raw material ratio and preparation process, it takes into account hydrophobic self-cleaning, high light transmittance, strong adhesion, and aging resistance, while simplifying the production process and reducing costs, thus meeting the long-term outdoor protection needs of photovoltaic modules.
[0005] The purpose of this invention is to provide a hydrophobic and dustproof coating for photovoltaic modules, which can effectively block dust adhesion, achieve self-cleaning by rainwater, and at the same time not affect the light transmittance of photovoltaic glass. It also features strong adhesion and a long service life.
[0006] To achieve the above objectives, the technical solution adopted is as follows:
[0007] A hydrophobic and dust-proof coating for photovoltaic modules is formed by applying a coating liquid to the surface of photovoltaic glass and then curing it.
[0008] The coating liquid comprises: nano-silica, methyl MQ silicone resin, crosslinking agent, silane modifier, composite organic solvent, acidic catalyst, and deionized water;
[0009] The crosslinking agent is methyltrimethoxysilane;
[0010] The silane modifier includes: hexadecyltrimethoxysilane, tetraethyl orthosilicate, and tetramethoxysilane;
[0011] The composite organic solvent includes: n-heptane, n-butyl acetate, and anhydrous ethanol.
[0012] Furthermore, the coating liquid, by weight, comprises: 0.1-0.2 parts of nano-silica, 25-35 parts of n-heptane, 15-25 parts of n-butyl acetate, 10-15 parts of anhydrous ethanol, 0.5-0.7 parts of hexadecyltrimethoxysilane, 0.2-0.4 parts of tetraethyl orthosilicate, 0.08-0.15 parts of tetramethoxysilane, 0.15-0.25 parts of crosslinking agent, 1.0-1.5 parts of methyl MQ silicone resin, 0.2-0.3 parts of deionized water, and 0.05-0.1 parts of acidic catalyst.
[0013] Furthermore, the nano-silica has a particle size of 15-20 nm and a purity of ≥99.5%.
[0014] The acidic catalyst is dilute hydrochloric acid with a concentration of 0.1 mol / L.
[0015] Another objective of this invention is to provide a method for preparing the above-mentioned hydrophobic and dustproof coating for photovoltaic modules, which is simple to process and can be mass-produced.
[0016] To achieve the above objectives, the technical solution adopted is as follows:
[0017] The above-mentioned method for preparing a hydrophobic and dust-resistant coating includes the following steps:
[0018] S1: Nano-silica is uniformly dispersed in n-heptane, n-butyl acetate and anhydrous ethanol to obtain a silica suspension;
[0019] After uniformly mixing the acidic catalyst, water, and anhydrous ethanol, a silane modifier was added, and hydrolysis was carried out to obtain a pre-hydrolyzed solution.
[0020] S2: The pre-hydrolyzed solution is added dropwise to the silica suspension. After the addition is complete, the temperature is raised to 55-65℃, and the mixture is stirred for 2-2.5 hours. Then, it is naturally cooled to room temperature to obtain a modified silica dispersion.
[0021] S3: After dissolving methyl MQ silicone resin in n-butyl acetate, add a crosslinking agent, mix evenly, add the modified silica dispersion, stir until evenly mixed, and obtain a hydrophobic and dustproof coating.
[0022] S4: After applying the hydrophobic and dustproof coating to a clean photovoltaic glass surface, allow it to dry at room temperature for 10-15 minutes, then dry it at 80-85℃ for 20-30 minutes, and finally cure it at 110-130℃ for 2.5-3.5 hours to obtain the hydrophobic and dustproof coating for the photovoltaic module.
[0023] Furthermore, in step S1, the mass ratio of anhydrous ethanol in the silica suspension and the pre-hydrolyzed solution is 5:10-15; the amount of n-butyl acetate in the silica suspension is 1 / 2 of the total mass of n-butyl acetate.
[0024] In step S2, the temperature is raised to 60°C and the reaction is stirred for 2 hours.
[0025] Furthermore, in step S1, the hydrolysis time is 30-40 minutes;
[0026] The silane modifier was added and mixed in the following order: tetraethyl orthosilicate, tetramethoxysilane, and hexadecyltrimethoxysilane.
[0027] Furthermore, in step S3, a small amount of the modified silica dispersion is first added, and after stirring and pre-activation, the remaining modified silica dispersion is added.
[0028] Furthermore, the amount of modified silica dispersion added during the pre-activation process does not exceed 4% of the total mass of the modified silica dispersion.
[0029] Furthermore, in step S3, after adding the modified silica dispersion, the mixture is first magnetically stirred for 30-40 minutes, and then ultrasonically treated for 5-8 minutes.
[0030] In step S4, the coating method is spin coating or spray coating.
[0031] Furthermore, the spin coating speed is 2000-2500 r / min, and the time is 30s.
[0032] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0033] The technical solution of this invention is based on the principle of multisilane stepwise pre-hydrolysis grafting and MQ resin crosslinking film formation. Through the stepwise hydrolysis of HDTMS, TEOS, and TMOS and the condensation of hydroxyl groups on the SiO2 surface, combined with MTMS crosslinking with MQ resin to construct a three-dimensional network, a balance between hydrophobic and dustproof functions and high light transmittance is achieved. Specific key points and beneficial effects are as follows:
[0034] 1. Hydrophobic modification mechanism based on polysilane step-by-step pre-hydrolysis. TEOS and TMOS are first hydrolyzed to form an oligomeric silanol network, providing a cross-linking framework; HDTMS is then hydrolyzed to provide C16 long-chain alkyl groups. The three are synergistically grafted onto the SiO2 surface, forming a micro / nano structure of "inner cross-linked framework + outer long-chain hydrophobic layer," endowing the coating with excellent hydrophobic properties. This step-by-step pre-hydrolysis process avoids the self-polymerization of TMOS due to excessively rapid hydrolysis, resulting in white spots, while ensuring that the HDTMS long chains are fully grafted and arranged on the outermost layer, significantly improving hydrophobic durability.
[0035] 2. Film-enhancing effect based on MTMS crosslinking with MQ resin. After film formation, MTMS condenses with MQ resin and the silanol groups on the SiO2 surface at high temperature, forming a dense three-dimensional network, improving adhesion and weather resistance. MQ resin, as the film-forming matrix, has excellent compatibility with modified SiO2 particles, forming a dense, uniform, and highly stable hydrophobic film after crosslinking with MTMS. This organic-inorganic composite system combines the mechanical strength of inorganic nanoparticles with the flexibility of organosilicon resin, giving the coating strong adhesion to the photovoltaic glass surface and resistance to wind and sand erosion and rain washing.
[0036] 3. The evaporation gradient regulation effect of the n-heptane / n-butyl acetate / ethanol system based on composite solvents. n-Heptane evaporates quickly, preventing sagging; n-butyl acetate evaporates slowly, preventing pinholes; ethanol acts as a co-solvent to improve polarity matching. The combination of these three components allows for precise control of slurry viscosity and evaporation rate, ensuring uniform solvent evaporation during coating and film formation, avoiding film whitening, cracking, or pinholes, ensuring coating density and surface smoothness, while maintaining high light transmittance (≥92%).
[0037] 4. Ensuring Hydrophobic Durability and Light Transmittance Based on Staged Curing Process. The staged curing process ensures long-chain arrangement and full cross-linking: room temperature surface drying allows low-boiling-point solvents to evaporate smoothly; 80°C pre-baking removes residual polar solvents to prevent high-temperature bubbling; and 120°C high-temperature curing promotes complete dehydration and condensation of silanol groups, forming a dense cross-linked network. This process improves the hydrophobic durability and light transmittance of the coating, avoiding coating defects caused by direct high-temperature curing.
[0038] 5. Weather resistance assurance for desert and Gobi environments. This invention employs a composite system of inorganic nano-SiO2 and organosilicon MQ resin, which, after curing, forms a three-dimensional network structure with high cross-linking density. This structure exhibits excellent resistance to wind and sand abrasion, capable of withstanding the erosion of strong winds and sandstorms in desert and Gobi regions. MQ resin provides excellent temperature resistance (-40~85℃) and UV resistance; the coating exhibits excellent resistance to UV radiation and does not yellow or degrade under long-term outdoor exposure. The coating can withstand drastic temperature changes from -40℃ to 85℃ without cracking or peeling under thermal cycling conditions. Attached Figure Description
[0039] Figure 1 This is a water contact angle test diagram of the hydrophobic and dustproof coating of Example 1.
[0040] Figure 2 This is a transmittance test diagram of the hydrophobic and dustproof coating of Example 1.
[0041] Figure 3 This is a SEM image of the hydrophobic and dustproof coating of Example 1.
[0042] Figure 4The water contact angle test diagram is for the hydrophobic and dustproof coating of Comparative Example 1.
[0043] Figure 5 The water contact angle test diagram is for the hydrophobic and dustproof coating of Comparative Example 3.
[0044] Figure 6 This represents the contact angle of the sample after temperature cycling.
[0045] Figure 7 This is a transmittance test graph of the sample after temperature cycling.
[0046] Note: Sample 1 is the hydrophobic and dustproof coating of Example 1, and Sample 2 is the hydrophobic and dustproof coating after temperature difference cycling. Detailed Implementation
[0047] To further illustrate the hydrophobic and dust-resistant coating for photovoltaic modules and its preparation method according to the present invention, and to achieve the intended purpose of the invention, the following detailed description, in conjunction with preferred embodiments, details the specific implementation, structure, features, and effects of the hydrophobic and dust-resistant coating for photovoltaic modules and its preparation method according to the present invention. In the following description, different "embodiments" or "embodiments" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable manner.
[0048] The following will provide a more detailed description of a hydrophobic and dust-resistant coating for photovoltaic modules and its preparation method, using specific embodiments as examples:
[0049] This invention utilizes a multi-silane stepwise pre-hydrolysis process to generate stable hydrophobic groups, which are then combined with MTMS crosslinked MQ resin to construct a micro-nano rough structure. This, coupled with a composite solvent-controlled and staged curing process, results in a coating with excellent hydrophobic self-cleaning properties and a light transmittance of ≥92%. When applied to the surface of photovoltaic modules, this coating effectively reduces dust adhesion and enables rainwater self-cleaning, providing a complete technical solution for dust protection of photovoltaic modules in arid environments.
[0050] The technical solution adopted in this invention is as follows:
[0051] A hydrophobic and dust-proof coating for photovoltaic modules is formed by applying a coating liquid to the surface of photovoltaic glass and then curing it.
[0052] The coating liquid comprises: nano-silica, methyl MQ silicone resin, crosslinking agent, silane modifier, composite organic solvent, acidic catalyst, and deionized water;
[0053] The crosslinking agent is methyltrimethoxysilane;
[0054] The silane modifier includes: hexadecyltrimethoxysilane, tetraethyl orthosilicate, and tetramethoxysilane;
[0055] The composite organic solvent includes: n-heptane, n-butyl acetate, and anhydrous ethanol.
[0056] In the above technical solution, anhydrous ethanol is not merely a diluent solvent; it plays multiple roles in the system. Because the surface of nano-silica is rich in silanol groups and exhibits strong polarity, it is prone to agglomeration and sedimentation in non-polar n-heptane. Anhydrous ethanol in the suspension component improves the surface wettability of nano-silica particles and weakens interparticle hydrogen bonding. Combined with ultrasonic treatment, this results in a stable silica suspension. Anhydrous ethanol in the pre-hydrolyzed liquid component acts as a co-solvent, enabling deionized water, dilute hydrochloric acid catalyst, and the three silane modifiers to form a homogeneous liquid phase. This ensures that the tetraethyl orthosilicate, tetramethoxysilane, and hexadecyltrimethoxysilane are added sequentially for stepwise hydrolysis, avoiding self-polymerization caused by excessively rapid tetramethoxysilane hydrolysis and ensuring effective grafting of long-chain alkylsilanes onto the silica particle surface. During the staged curing process, anhydrous ethanol smoothly escapes from the film layer during the room temperature surface drying and low temperature pre-baking stages, avoiding the solvent being trapped inside the film and causing bubbling and whitening, ensuring that the film is dense and smooth, and ultimately achieving the comprehensive performance of high light transmittance and hydrophobic and dustproof coating.
[0057] Preferably, the coating liquid comprises, by weight: 0.1-0.2 parts of nano-silica, 25-35 parts of n-heptane, 15-25 parts of n-butyl acetate, 10-15 parts of anhydrous ethanol, 0.5-0.7 parts of hexadecyltrimethoxysilane, 0.2-0.4 parts of tetraethyl orthosilicate, 0.08-0.15 parts of tetramethoxysilane, 0.15-0.25 parts of crosslinking agent, 1.0-1.5 parts of methyl MQ silicone resin, 0.2-0.3 parts of deionized water, and 0.05-0.1 parts of acidic catalyst.
[0058] Preferably, the nano-silica has a particle size of 15-20 nm and a purity of ≥99.5%.
[0059] The acidic catalyst is dilute hydrochloric acid with a concentration of 0.1 mol / L.
[0060] The above-mentioned method for preparing a hydrophobic and dust-resistant coating includes the following steps:
[0061] S1: Nano-silica is uniformly dispersed in n-heptane, n-butyl acetate and anhydrous ethanol to obtain a silica suspension;
[0062] After uniformly mixing the acidic catalyst, water, and anhydrous ethanol, a silane modifier was added, and hydrolysis was carried out to obtain a pre-hydrolyzed solution.
[0063] S2: The pre-hydrolyzed solution is added dropwise to the silica suspension. After the addition is complete, the temperature is raised to 55-65℃, and the mixture is stirred for 2-2.5 hours. Then, it is naturally cooled to room temperature to obtain a modified silica dispersion.
[0064] S3: After dissolving methyl MQ silicone resin in n-butyl acetate, add a crosslinking agent, mix evenly, add the modified silica dispersion, stir until evenly mixed, and obtain a hydrophobic and dustproof coating.
[0065] S4: After applying the hydrophobic and dustproof coating to a clean photovoltaic glass surface, allow it to dry at room temperature for 10-15 minutes, then dry it at 80-85℃ for 20-30 minutes, and finally cure it at 110-130℃ for 2.5-3.5 hours to obtain the hydrophobic and dustproof coating for the photovoltaic module.
[0066] Preferably, in step S1, the mass ratio of anhydrous ethanol in the silica suspension and the pre-hydrolyzed solution is 5:10-15; the amount of n-butyl acetate in the silica suspension is 1 / 2 of the total mass of n-butyl acetate.
[0067] In step S2, the temperature is raised to 60°C and the reaction is stirred for 2 hours.
[0068] Preferably, in step S1, the hydrolysis time is 30-40 min;
[0069] The silane modifier was added and mixed in the following order: tetraethyl orthosilicate, tetramethoxysilane, and hexadecyltrimethoxysilane.
[0070] In the above technical solution, mixing the silane modifiers in sequence is more conducive to complete hydrolysis.
[0071] Preferably, in step S3, a small amount of the modified silica dispersion is added first, and after stirring and pre-activation, the remaining modified silica dispersion is added.
[0072] More preferably, the amount of modified silica dispersion added during the pre-activation process does not exceed 4% of the total mass of the modified silica dispersion.
[0073] Preferably, in step S3, after adding the modified silica dispersion, the mixture is first magnetically stirred for 30-40 minutes, and then ultrasonically treated for 5-8 minutes.
[0074] In step S4, the coating method is spin coating or spray coating.
[0075] More preferably, the spin coating speed is 2000-2500 r / min and the time is 30s.
[0076] In this invention, the preparation methods are all conventional unless otherwise specified, and the raw materials used can be obtained from publicly available commercial sources unless otherwise specified. All parts refer to parts by weight, and the temperature is in degrees Celsius (°C).
[0077] All raw materials used in this invention are commercially available conventional industrial raw materials, and their purity meets the requirements for experimental and industrial preparation, without the need to limit specific manufacturers.
[0078] The particle size of nano-silica is 15-20nm, and the purity is ≥99.5%.
[0079] Example 1.
[0080] The raw materials are: 0.15 g nano SiO2, 28 g n-heptane, 20 mL n-butyl acetate (17.6 g), 13 mL anhydrous ethanol (10.3 g), 0.25 mL deionized water (0.25 g), 0.05 mL dilute hydrochloric acid (0.1 mol / L) (0.05 g), 0.3 mL tetraethyl orthosilicate (0.28 g), 0.11 mL tetramethoxysilane (0.112 g), 0.6 mL hexadecyltrimethoxysilane (0.534 g), 1.3 g methyl MQ silicone resin, and 0.2 mL methyltrimethoxysilane (0.19 g).
[0081] The specific steps are as follows:
[0082] S1: Nano-silica dispersion
[0083] 0.15 g of nano-SiO2 was added to a composite organic solvent consisting of 28 g of n-heptane, 10 mL of n-butyl acetate, and 5 mL of anhydrous ethanol, and sonicated at room temperature for 50 min to obtain a uniformly dispersed SiO2 suspension.
[0084] S2: Polysilane stepwise prehydrolysis
[0085] Mix 8 mL of anhydrous ethanol, 0.25 mL of deionized water, and 1 drop of 0.1 M dilute hydrochloric acid (approximately 0.05 mL). First, add 0.3 mL of tetraethyl orthosilicate (TEOS) and stir under sealed conditions at room temperature for 5 min. Then, add 0.11 mL of tetramethoxysilane (TMOS) and stir for 5 min. Finally, add 0.6 mL of hexadecyltrimethoxysilane (HDTMS) and stir for 20 min to obtain the pre-hydrolyzed solution.
[0086] S3: In-situ grafting
[0087] The pre-hydrolyzed solution was slowly added dropwise to the SiO2 suspension. After the addition was complete, the temperature was raised to 60°C, and the mixture was stirred in a sealed container for 2 hours. The mixture was then allowed to cool naturally to room temperature to obtain the modified SiO2 dispersion.
[0088] S4: MQ / MTMS adhesive preparation
[0089] Dissolve 1.3 g of MQ resin in 10 mL of n-butyl acetate, stir until clear, then add 0.2 mL of methyltrimethoxysilane (MTMS) and stir for 15 min.
[0090] Add 2 mL of the modified SiO2 dispersion from step S3 and stir for 5 min for pre-activation.
[0091] S5: Co-coating
[0092] The pre-activated mixture obtained in step S4 is then slowly dripped into the modified SiO2 dispersion obtained in the remaining step S3, magnetically stirred for 30 min, and gently sonicated for 5 min to obtain a hydrophobic and dustproof coating.
[0093] The hydrophobic and dust-repellent coating was spin-coated onto the clean photovoltaic glass surface at a spin speed of 2000-2500 rpm for 30 seconds.
[0094] S6: Stage Curing
[0095] The prepared glass-coated component was surface-dried at room temperature for 15 min, baked at 80℃ for 30 min, and cured at 120℃ for 3 h to obtain a hydrophobic and dustproof coating 1 for photovoltaic modules.
[0096] Example 2.
[0097] The raw materials are: 0.10 g nano SiO2, 25 g n-heptane, 15 g n-butyl acetate, 12 g anhydrous ethanol, 0.20 mL (0.20 g) deionized water, 0.05 mL (0.05 g) dilute hydrochloric acid (0.1 mol / L), 0.21 g tetraethyl orthosilicate, 0.08 g tetramethoxysilane, 0.6 g hexadecyltrimethoxysilane, 1.0 g methyl MQ silicone resin, and 0.15 g methyltrimethoxysilane.
[0098] The specific steps are as follows:
[0099] S1: Nano-silica dispersion
[0100] 0.10 g of nano-SiO2 was added to a composite organic solvent consisting of 25 g of n-heptane, 7.5 g of n-butyl acetate, and 6 g of anhydrous ethanol, and sonicated at room temperature for 40 min to obtain a uniformly dispersed SiO2 suspension.
[0101] S2: Polysilane stepwise prehydrolysis
[0102] Mix 6 g of anhydrous ethanol, 0.20 mL of deionized water, and 1 drop of 0.1 M dilute hydrochloric acid (approximately 0.05 mL). First, add 0.21 g of tetraethyl orthosilicate (TEOS) and stir under sealed conditions at room temperature for 5 min. Then, add 0.08 g of tetramethoxysilane (TMOS) and stir for 5 min. Finally, add 0.6 g of hexadecyltrimethoxysilane (HDTMS) and stir for 20 min to obtain the pre-hydrolyzed solution.
[0103] S3: In-situ grafting
[0104] The pre-hydrolyzed solution was slowly added dropwise to the SiO2 suspension. After the addition was complete, the temperature was raised to 55°C, and the mixture was stirred in a sealed container for 2.5 h. The mixture was then allowed to cool naturally to room temperature to obtain the modified SiO2 dispersion.
[0105] S4: MQ / MTMS adhesive preparation
[0106] Dissolve 1.0 g of MQ resin in 7.5 g of n-butyl acetate, stir until clear, then add 0.15 g of methyltrimethoxysilane (MTMS) and stir for 15 min.
[0107] Add 2g of the modified SiO2 dispersion from step S3 and stir for 5 min for pre-activation.
[0108] S5: Co-coating
[0109] The pre-activated mixture obtained in step S4 is then slowly dripped into the modified SiO2 dispersion obtained in the remaining step S3, magnetically stirred for 30 min, and gently sonicated for 5 min to obtain a hydrophobic and dustproof coating.
[0110] The hydrophobic and dust-repellent coating was spin-coated onto the clean photovoltaic glass surface at a spin speed of 2000-2500 rpm for 30 seconds.
[0111] S6: Stage Curing
[0112] The prepared glass-coated component was surface-dried at room temperature for 10 min, baked at 80℃ for 30 min, and cured at 110℃ for 3.5 h to obtain a hydrophobic and dustproof coating 2 for photovoltaic modules.
[0113] Example 3.
[0114] The raw materials are: 0.2g nano SiO2, 35g n-heptane, 25g n-butyl acetate, 25g anhydrous ethanol, 0.30 mL (0.30g) deionized water, 0.10 mL (0.10g) dilute hydrochloric acid (0.1 mol / L), 0.4g tetraethyl orthosilicate, 0.15g tetramethoxysilane, 0.7g hexadecyltrimethoxysilane, 1.5g methylMQ silicone resin, and 0.25g methyltrimethoxysilane.
[0115] The specific steps are as follows:
[0116] S1: Nano-silica dispersion
[0117] 0.20 g of nano-SiO2 was added to a composite organic solvent consisting of 35 g of n-heptane, 12.5 g of n-butyl acetate, and 8 g of anhydrous ethanol, and sonicated at room temperature for 60 min to obtain a uniformly dispersed SiO2 suspension.
[0118] S2: Polysilane stepwise prehydrolysis
[0119] Mix 17g of anhydrous ethanol, 0.30 mL of deionized water, and 2 drops of 0.1M dilute hydrochloric acid (approximately 0.1 mL). First, add 0.4g of tetraethyl orthosilicate (TEOS) and stir under sealed conditions at room temperature for 8 minutes. Then, add 0.15g of tetramethoxysilane (TMOS) and stir for 8 minutes. Finally, add 0.7g of hexadecyltrimethoxysilane (HDTMS) and stir for 24 minutes to obtain the pre-hydrolyzed solution.
[0120] S3: In-situ grafting
[0121] The pre-hydrolyzed solution was slowly added dropwise to the SiO2 suspension. After the addition was complete, the temperature was raised to 65°C, and the mixture was stirred in a sealed container for 2.5 h. The mixture was then allowed to cool naturally to room temperature to obtain the modified SiO2 dispersion.
[0122] S4: MQ / MTMS adhesive preparation
[0123] Dissolve 1.5 g of MQ resin in 12.5 g of n-butyl acetate, stir until clear, then add 0.25 g of methyltrimethoxysilane (MTMS) and stir for 15 min.
[0124] Add 2 mL of the modified SiO2 dispersion from step S3 and stir for 5 min for pre-activation.
[0125] S5: Co-coating
[0126] The pre-activated mixture obtained in step S4 is then slowly dripped into the modified SiO2 dispersion obtained in the remaining step S3, magnetically stirred for 40 min, and gently sonicated for 8 min to obtain a hydrophobic and dustproof coating.
[0127] The hydrophobic and dust-repellent coating was spin-coated onto the clean photovoltaic glass surface at a spin speed of 2000-2500 rpm for 30 seconds.
[0128] S6: Stage Curing
[0129] The prepared glass-coated component was surface-dried at room temperature for 15 min, baked at 85℃ for 25 min, and cured at 130℃ for 2.5 h to obtain a hydrophobic and dustproof coating 3 for photovoltaic modules.
[0130] Example 4.
[0131] The raw materials are: 0.13 g nano SiO2, 30 g n-heptane, 18 g n-butyl acetate, 15 g anhydrous ethanol, 0.20 mL (0.20 g) deionized water, 0.05 mL (0.05 g) dilute hydrochloric acid (0.1 mol / L), 0.30 g tetraethyl orthosilicate, 0.10 g tetramethoxysilane, 0.6 g hexadecyltrimethoxysilane, 1.2 g methyl MQ silicone resin, and 0.18 g methyltrimethoxysilane.
[0132] The specific steps are as follows:
[0133] S1: Nano-silica dispersion
[0134] 0.13 g of nano-SiO2 was added to a composite organic solvent consisting of 30 g of n-heptane, 9 g of n-butyl acetate, and 5 g of anhydrous ethanol, and sonicated at room temperature for 45 min to obtain a uniformly dispersed SiO2 suspension.
[0135] S2: Polysilane stepwise prehydrolysis
[0136] Mix 10g anhydrous ethanol, 0.20mL deionized water, and 1 drop of 0.1M dilute hydrochloric acid (approximately 0.05mL). First, add 0.30g tetraethyl orthosilicate (TEOS) and stir under sealed conditions at room temperature for 5 min. Then, add 0.10g tetramethoxysilane (TMOS) and stir for 5 min. Finally, add 0.6g hexadecyltrimethoxysilane (HDTMS) and stir for 25 min to obtain the pre-hydrolyzed solution.
[0137] S3: In-situ grafting
[0138] The pre-hydrolyzed solution was slowly added dropwise to the SiO2 suspension. After the addition was complete, the temperature was raised to 60°C, and the mixture was stirred in a sealed container for 2 hours. The mixture was then allowed to cool naturally to room temperature to obtain the modified SiO2 dispersion.
[0139] S4: MQ / MTMS adhesive preparation
[0140] Dissolve 1.2 g of MQ resin in 9 g of n-butyl acetate, stir until clear, then add 0.18 g of methyltrimethoxysilane (MTMS) and stir for 15 min.
[0141] Add 2 mL of the modified SiO2 dispersion from step S3 and stir for 5 min for pre-activation.
[0142] S5: Co-coating
[0143] The pre-activated mixture obtained in step S4 is then slowly dripped into the modified SiO2 dispersion obtained in the remaining step S3, magnetically stirred for 30 min, and gently sonicated for 5 min to obtain a hydrophobic and dustproof coating.
[0144] A hydrophobic and dust-resistant coating is sprayed onto the clean surface of the photovoltaic glass.
[0145] S6: Stage Curing
[0146] The prepared glass-coated component was surface-dried at room temperature for 15 min, baked at 80℃ for 20 min, and cured at 110℃ for 3.5 h to obtain a hydrophobic and dustproof coating 4 for photovoltaic modules.
[0147] Example 5: Performance Testing
[0148] The hydrophobic and dust-resistant coating for photovoltaic modules prepared in Example 1 was tested as follows:
[0149] (1) Water contact angle: Referring to GB / T 30447-2013 standard, the water contact angle of the coating surface was measured using a contact angle measuring instrument. The results are as follows: Figure 1 As shown.
[0150] (2) Total light transmittance: Measured using a spectrophotometer (wavelength 380-1100 nm) according to GB / T 30984.1-2015 standard. The results are as follows: Figure 2 As shown.
[0151] (3) Dustproof performance: Prickly heat powder was used as simulated dust and evenly sprinkled on the sample surface. After the dustproof test (without wiping), the transmittance was directly measured and the transmittance retention rate was calculated.
[0152] The test results are shown in Table 1 below:
[0153] Table 1
[0154]
[0155] As shown in Table 1, the water contact angle of the hydrophobic and dustproof coating of the present invention reaches 97.7°, exhibiting excellent hydrophobic self-cleaning performance; the total light transmittance reaches 93.2%, and the light transmittance retention rate after the dustproof test is ≥90.5%, indicating that the coating has good dustproof performance while maintaining high light transmittance.
[0156] (4) Drastic temperature changes
[0157] Methods: The coating prepared in Example 1 was placed in a high and low temperature test chamber and subjected to temperature shock test according to GB / T 2423.22. After holding at -40℃ for 30 min, the temperature was switched to 85℃ for 30 min, which was recorded as 1 cycle. A total of 100 cycles were performed. The water contact angle and total light transmittance of the coating were measured before and after the test, and the surface condition of the coating was observed.
[0158] Result: As Figure 6-7 As shown, after 100 cycles of severe temperature difference, the coating surface showed no cracks or peeling; the water contact angle decreased from 97.7° to 95.8°, and the total light transmittance decreased from 93.2% to 92.8%, with no significant attenuation, indicating that the coating can withstand severe temperature changes from -40℃ to 85℃.
[0159] (5) Water contact angle
[0160] The water contact angle of the photovoltaic module hydrophobic and dustproof coatings obtained in Examples 2-3 was measured using a contact angle measuring instrument in accordance with GB / T 30447-2013 standard.
[0161] Results: The left and right contact angles of the hydrophobic and dustproof coating for photovoltaic modules obtained in Example 2 were 98.108 and 97.67, respectively, and the left and right contact angles of the hydrophobic and dustproof coating for photovoltaic modules obtained in Example 3 were 95.88 and 96.34, respectively.
[0162] Comparative Example 1.
[0163] The operating steps of Comparative Example 1 are the same as those of Example 1, except that no silane modifier is used.
[0164] The specific steps are as follows:
[0165] S1: Nano-silica dispersion
[0166] 0.15 g of nano-SiO2 was added to a composite organic solvent consisting of 28 g of n-heptane, 10 mL of n-butyl acetate, and 5 mL of anhydrous ethanol, and sonicated at room temperature for 50 min to obtain a uniformly dispersed SiO2 suspension.
[0167] S2: Preparation of pretreatment solution
[0168] Mix 10 g of anhydrous ethanol, 0.25 g of deionized water, and 1 drop of 0.1 mol / L dilute hydrochloric acid (approximately 0.05 g) to obtain the pretreatment solution.
[0169] S3: In-situ grafting
[0170] The pretreatment solution was slowly added dropwise to the SiO2 suspension. After the addition was complete, the temperature was raised to 60°C, and the mixture was stirred in a sealed container for 2 hours. The mixture was then allowed to cool naturally to room temperature to obtain the modified SiO2 dispersion.
[0171] S4: MQ / MTMS adhesive preparation
[0172] Dissolve 1.3 g of MQ resin in 10 mL of n-butyl acetate, stir until clear, then add 0.2 mL of methyltrimethoxysilane (MTMS) and stir for 15 min.
[0173] Add 2 mL of the modified SiO2 dispersion from step S3 and stir for 5 min for pre-activation.
[0174] S5: Co-coating
[0175] The pre-activated mixture obtained in step S4 is then slowly dripped into the modified SiO2 dispersion obtained in the remaining step S3, magnetically stirred for 30 min, and gently sonicated for 5 min to obtain a hydrophobic and dustproof coating.
[0176] The hydrophobic and dust-repellent coating was spin-coated onto the clean photovoltaic glass surface at a spin speed of 2000-2500 rpm for 30 seconds.
[0177] S6: Stage Curing
[0178] The prepared glass coating component was surface dried at room temperature for 20 min, baked at 80℃ for 30 min, and cured at 120℃ for 3 h to obtain a hydrophobic and dustproof coating 5 for photovoltaic modules.
[0179] The photovoltaic modules were coated with hydrophobic dustproof coating 5 and tested for water contact angle, total light transmittance, and dustproof performance in the same manner as in Example 1. Results: Figure 4 As shown, the water contact angle is 66.8°, the total light transmittance is 93.0%, and the transmittance retention rate after the dustproof test is 76.5%. Therefore, the coating is not hydrophobic and has poor dustproof performance.
[0180] The results show that the silane modifier used in this invention has a significant impact on the hydrophobic properties. The mechanism is as follows: TEOS and TMOS first hydrolyze to form an oligomeric silanol network, providing a cross-linking framework; HDTMS then hydrolyzes and provides C16 long-chain alkyl groups. All three are synergistically grafted onto the SiO2 surface, forming a micro / nano structure of "inner cross-linked framework + outer long-chain hydrophobic layer," endowing the coating with excellent hydrophobic properties. This step-by-step pre-hydrolysis process avoids the formation of white spots due to excessively rapid TMOS self-polymerization, while ensuring that the HDTMS long chains are fully grafted and arranged on the outermost layer, significantly improving hydrophobic durability.
[0181] Comparative Example 2: Composite Organic Solvent
[0182] The operating procedures for Comparative Example 2 were the same as those for Example 1, except for the choice of organic solvent. The selection and results are shown in Table 2.
[0183] Table 2
[0184]
[0185] As shown in Table 2, the selection of composite organic solvents in this invention avoids sagging and pinholes. The combination of the three ensures uniform solvent evaporation during the coating process, preventing whitening, cracking, or pinholes in the film, ensuring coating density and surface smoothness, while maintaining high light transmittance.
[0186] Comparative Example 3: Curing
[0187] The specific operation steps are as follows: The operation steps of Comparative Example 3 are the same as those of Example 1, except that in step S6: After coating, without room temperature surface drying and 80°C pre-baking, it is directly placed at 120°C for 3 hours to obtain the hydrophobic and dustproof coating 6 for photovoltaic modules.
[0188] The photovoltaic module was coated with hydrophobic and dust-resistant coating 6 and subjected to the same water contact angle and total light transmittance tests as in Example 1. The surface morphology was also observed. Results: Figure 5 As shown, the coating surface exhibits whitening, micropores, and localized blistering. The water contact angle is 88.9°, and the total light transmittance is 91.5%.
[0189] The results show that when high-temperature curing is performed directly without staged curing, the low-boiling-point solvent evaporates rapidly, leading to defects such as bubbles and micropores in the film layer. The long-chain hydrophobic groups are also disordered, resulting in a significant decrease in both the hydrophobicity and light transmittance of the coating. In contrast, this invention employs a process of surface drying at room temperature, pre-baking at 80-85℃, and staged curing at 110-130℃. This ensures stable solvent evaporation, orderly arrangement of long chains, and sufficient dehydration and condensation of silanol groups, thereby obtaining a dense, highly transparent, and durable hydrophobic coating.
[0190] As can be seen from the embodiments of this invention, this invention addresses the technical bottlenecks of traditional coatings, such as easy dust accumulation, difficulty in dust removal, and severe attenuation of light transmittance in strong winds and arid environments like deserts and wastelands, by proposing a hydrophobic surface coating design scheme. This invention uses 15-20nm SiO2 nanoparticles as a substrate, employing a stepwise pre-hydrolysis of hexadecyltrimethoxysilane (HDTMS), tetraethyl orthosilicate (TEOS), and tetramethoxysilane (TMOS) to form a composite silanol in an acidic ethanol aqueous solution, which then condenses and grafts with hydroxyl groups on the SiO2 surface. Then, using methyl MQ silicone resin as the film-forming matrix, methyl trimethoxysilane (MTMS) as the crosslinking agent, and n-heptane / n-butyl acetate / ethanol as the composite solvent, a hydrophobic and dust-resistant coating is formed after blending, coating, and staged curing. The coating of this invention has a water contact angle ≥90°, and possesses high light transmittance, strong adhesion, weather resistance, and wind and sand resistance. The preparation process is simple, cost-controllable, and suitable for large-scale mass production.
[0191] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A hydrophobic and dust repellent coating for photovoltaic modules, characterized in that, The hydrophobic and dustproof coating is formed by applying a coating liquid to the surface of photovoltaic glass and then curing it. The coating liquid comprises: nano-silica, methyl MQ silicone resin, crosslinking agent, silane modifier, composite organic solvent, acidic catalyst, and deionized water; The crosslinking agent is methyltrimethoxysilane; The silane modifier includes: hexadecyltrimethoxysilane, tetraethyl orthosilicate, and tetramethoxysilane; The composite organic solvent includes: n-heptane, n-butyl acetate, and anhydrous ethanol.
2. The hydrophobic and dustproof coating according to claim 1, characterized in that, The coating solution comprises, by weight, 0.1-0.2 parts of nano-silica, 25-35 parts of n-heptane, 15-25 parts of n-butyl acetate, 10-15 parts of anhydrous ethanol, 0.5-0.7 parts of hexadecyltrimethoxysilane, 0.2-0.4 parts of tetraethyl orthosilicate, 0.08-0.15 parts of tetramethoxysilane, 0.15-0.25 parts of crosslinking agent, 1.0-1.5 parts of methyl MQ silicone resin, 0.2-0.3 parts of deionized water, and 0.05-0.1 parts of acidic catalyst.
3. The hydrophobic and dustproof coating according to claim 1, characterized in that, The nano-silica has a particle size of 15-20 nm and a purity of ≥99.5%. The acidic catalyst is dilute hydrochloric acid with a concentration of 0.1 mol / L.
4. Process for the production of a hydrophobic dirt-repellent coating according to any one of claims 1 to 3, characterized in that Includes the following steps: S1: Nano-silica is uniformly dispersed in n-heptane, n-butyl acetate and anhydrous ethanol to obtain a silica suspension; After uniformly mixing the acidic catalyst, water, and anhydrous ethanol, a silane modifier was added, and hydrolysis was carried out to obtain a pre-hydrolyzed solution. S2: The pre-hydrolyzed solution is added dropwise to the silica suspension. After the addition is complete, the temperature is raised to 55-65℃, and the mixture is stirred for 2-2.5 hours. Then, it is naturally cooled to room temperature to obtain a modified silica dispersion. S3: After dissolving methyl MQ silicone resin in n-butyl acetate, add a crosslinking agent, mix evenly, add the modified silica dispersion, stir until evenly mixed, and obtain a hydrophobic and dustproof coating. S4: After applying the hydrophobic and dustproof coating to a clean photovoltaic glass surface, allow it to dry at room temperature for 10-15 minutes, then dry it at 80-85℃ for 20-30 minutes, and finally cure it at 110-130℃ for 2.5-3.5 hours to obtain the hydrophobic and dustproof coating for the photovoltaic module.
5. The preparation method according to claim 4, characterized in that, In step S1, the mass ratio of anhydrous ethanol in the silica suspension and the pre-hydrolyzed solution is 5:10-15; the amount of n-butyl acetate in the silica suspension is 1 / 2 of the total mass of n-butyl acetate. In step S2, the temperature is raised to 60°C and the reaction is stirred for 2 hours.
6. The preparation method according to claim 4, characterized in that, In step S1, the hydrolysis time is 30-40 min; The silane modifier was added and mixed in the following order: tetraethyl orthosilicate, tetramethoxysilane, and hexadecyltrimethoxysilane.
7. The preparation method according to claim 4, characterized in that, In step S3, a small amount of the modified silica dispersion is first added, and after stirring and pre-activation, the remaining modified silica dispersion is added.
8. The preparation method according to claim 7, characterized in that, The amount of modified silica dispersion added during the pre-activation process shall not exceed 4% of the total mass of the modified silica dispersion.
9. The preparation method according to claim 4, characterized in that, In step S3, after adding the modified silica dispersion, the mixture is first magnetically stirred for 30-40 minutes, and then ultrasonically treated for 5-8 minutes. In step S4, the coating method is spin coating or spray coating.
10. The preparation method according to claim 9, characterized in that, The spin coating is performed at a speed of 2000-2500 r / min for 30 seconds.