Hybrid surface protection composition using composite organic admixtures and ceramic-based inorganic admixtures, and eco-friendly surface protection construction method for concrete and steel structures using the same

The hybrid surface protection composition addresses the limitations of conventional materials by using a ceramic-based inorganic and organic admixture to prevent corrosion and cracking in concrete and steel structures, enhancing durability and safety.

KR103046460B1Active Publication Date: 2026-11-11CABLETEC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020260086302
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-05-13
Publication Date
2026-11-11
Estimated Expiration
2046-05-13

AI Technical Summary

Technical Problem

Conventional surface protection materials for concrete and steel structures fail to prevent corrosion, cracking, and deterioration due to environmental factors such as acid rain, chloride ions, and ultraviolet rays, and do not effectively cope with structural shrinkage and expansion, leading to reduced durability and maintenance issues.

Method used

A hybrid surface protection composition comprising a ceramic-based inorganic admixture and a composite organic admixture, including specific components like calcium carbonate, tungsten carbide, and methyl methacrylate, which provides adhesion, thermal expansion compatibility, and resistance to environmental changes, fire, and chemical erosion.

Benefits of technology

The composition prevents corrosion, cracking, and deterioration of concrete and steel structures by flexibly responding to environmental changes, offering excellent durability, heat resistance, and resistance to ultraviolet rays, while being eco-friendly and safe for human health.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention comprises 5 to 75 weight% of a ceramic-based inorganic admixture and 25 to 95 weight% of a composite organic admixture, wherein the ceramic-based inorganic admixture comprises 100 weight parts of calcium carbonate; 5 to 20 weight parts of aluminum silicate; 5 to 20 weight parts of Inconel; 5 to 20 weight parts of vermiculite; 5 to 20 weight parts of aluminum hydroxide; 0.5 to 15 weight parts of tungsten carbide; 0.5 to 15 weight parts of titanium dioxide; 0.5 to 15 weight parts of silica sol; and 0.5 to 15 weight parts of a filler pigment; and the composite organic admixture comprises 100 weight parts of methyl methacrylate; and 30 to 50 weight parts of 1,4-butanediol dimethacrylate. By comprising 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of styrene-butyl acrylic acid copolymer; 0.1 to 20 parts by weight of decamethylcyclopentasiloxane; 0.1 to 20 parts by weight of sodium phytate; 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; 0.1 to 20 parts by weight of alkoxysilane; and 0.1 to 20 parts by weight of diisocyanate, The present invention relates to a hybrid surface protection material composition using a composite organic admixture and a ceramic-based inorganic admixture, which can prevent corrosion caused by chemical erosion of concrete and steel structures under harsh environments, has excellent adhesion to the surface of concrete and steel structures and a similar coefficient of thermal expansion, can flexibly respond to shrinkage and expansion caused by external environmental changes such as changes in humidity and temperature, vibration / behavior, and impact from external loads to prevent cracking and delamination, has excellent durability by blocking ultraviolet rays and deterioration factors, can protect concrete and steel structures from fire due to excellent heat resistance, and possesses excellent water permeability, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance, as well as being safe for the human body as there is no leaching of harmful heavy metals, and an eco-friendly surface protection construction method for concrete and steel structures using the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, which can prevent corrosion caused by chemical erosion of concrete and steel structures under harsh environments, has excellent adhesion to the surface of concrete and steel structures and a similar coefficient of thermal expansion, can flexibly respond to shrinkage and expansion caused by external environmental changes such as changes in humidity and temperature, vibration / behavior, and impact from external loads to prevent cracking and delamination, has excellent durability by blocking ultraviolet rays and deterioration factors, can protect concrete and steel structures from fire due to excellent heat resistance, and possesses excellent water permeability, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance, as well as being safe for the human body as there is no leaching of harmful heavy metals, and an eco-friendly surface protection construction method for concrete and steel structures using the same. Background Technology

[0003] In general concrete structures, concrete deteriorates due to a combination of factors including carbonation, salt damage, frost damage, chemical erosion, alkali-aggregate reaction, fatigue, weathering, and fire. This deterioration progresses from the surface inward, accelerating the corrosion of rebar within the concrete and causing the rebar to expand. This expanded rebar accelerates stress within the concrete structure, inducing cracks and degrading its physical performance through reduced bond strength, spalling of the cover concrete, and a decrease in rebar strength.

[0004] Furthermore, steel structures also suffer increasingly severe damage from harsh environmental conditions. Steel, widely used in the construction sector for steel structures, bridges, decks, elevated roads, and steel frame structures, is not only a finite Earth resource but also possesses the inevitable drawback of corrosion. The primary influencing factors that accelerate steel corrosion are environmental factors; atmospheric pollutants such as sulfur dioxide (SO2), hydrogen sulfide (H2S), and sea salt particles, as well as meteorological factors like temperature and humidity, generally promote corrosion.

[0005] Therefore, surface protection materials based on epoxy, urethane, alkyd, and acrylic resins have been developed and used to physically and chemically protect and repair the surfaces of concrete and steel structures, thereby preventing corrosion and deterioration of durability caused by external environmental factors.

[0006] However, conventional surface protection materials have had problems such as deterioration due to various environmental factors, particularly acid rain, nitrogen oxides and sulfur oxides from automobile exhaust, and chloride ions in marine environments; failure to cope with the shrinkage and expansion of structures caused by changes in the external environment (humidity, temperature, vibration, and shock), resulting in cracks or separation of the coating film from the structure; and rapid reduction in service life due to yellowing, cracking, and swelling caused by ultraviolet rays. Prior art literature

[0008] Registered Patent No. 10-1956633 Registered Patent No. 10-2256238 Registered Patent No. 10-1952152 The problem to be solved

[0009] The present invention has been devised to solve the aforementioned problems. One embodiment of the present invention aims to provide a hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, which prevents corrosion of concrete and steel structures, improves durability by blocking ultraviolet rays and deterioration factors, and prevents cracking, peeling, etc., by flexibly responding to the shrinkage and expansion of structures due to changes in the external environment (humidity, temperature, vibration, and shock), and an eco-friendly surface protection construction method for concrete and steel structures using the same.

[0010] The various problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem

[0012] One embodiment of the present invention comprises 5 to 75 weight% of a ceramic-based inorganic admixture and 25 to 95 weight% of a composite organic admixture, wherein

[0013] The ceramic-based inorganic admixture comprises 100 parts by weight of calcium carbonate; 5 to 20 parts by weight of aluminum silicate; 5 to 20 parts by weight of Inconel; 5 to 20 parts by weight of vermiculite; 5 to 20 parts by weight of aluminum hydroxide; 0.5 to 15 parts by weight of tungsten carbide; 0.5 to 15 parts by weight of titanium dioxide; 0.5 to 15 parts by weight of silica sol; and 0.5 to 15 parts by weight of a filler pigment;

[0014] The above composite organic admixture comprises 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of styrene-butyl acrylic acid copolymer; 0.1 to 20 parts by weight of decamethylcyclopentasiloxane; 0.1 to 20 parts by weight of sodium phytate; 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; and 0.1 to 20 parts by weight of alkoxysilane. A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture is provided, comprising 0.1 to 20 parts by weight of diisocyanate.

[0015] The above tungsten carbide is

[0016] It is tungsten carbide with a modified oxide layer formed, and

[0017] The method comprises the steps of: preparing tungsten carbide with an oxide layer formed thereon by immersing 100 parts by weight of tungsten carbide in 400 to 600 parts by weight of an acidic solution prepared by mixing hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1 and maintaining it for 10 to 30 minutes to produce tungsten carbide with an oxide layer formed on its surface; and preparing tungsten carbide with an oxide layer formed thereon by mixing 100 parts by weight of the tungsten carbide with an oxide layer formed on its surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and 1 to 10 parts by weight of a glucopyranoside-based compound. Manufactured,

[0018] The above glucopyranoside compound may be one or more selected from the group consisting of 2-ethylhexylglucopyranoside (CAS No. 125590-73-0), methyl-D-glucopyranoside (CAS No. 3149-68-6), and mixtures thereof.

[0019] The tungsten carbide with the above modified oxide layer formed is

[0020] It is a tungsten carbide-titanium carbide composite with a modified oxide layer formed thereon, and

[0021] A method comprising the steps of: preparing a tungsten carbide-titanium carbide composite having a modified oxide layer formed thereon by immersing 100 parts by weight of a carbide composite, in which tungsten carbide and titanium carbide are mixed in a weight ratio of 1:0.1 to 0.5, in 400 to 600 parts by weight of an acidic solution mixed with hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1, and maintaining the mixture for 10 to 30 minutes to produce a tungsten carbide-titanium carbide composite having an oxide layer formed on its surface; and preparing a tungsten carbide-titanium carbide composite having a modified oxide layer formed thereon by mixing 100 parts by weight of the tungsten carbide-titanium carbide composite having an oxide layer formed on its surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and 1 to 10 parts by weight of a glucopyranoside-based compound. It can be manufactured.

[0022] The above composite organic admixture is

[0023] It further contains 0.1 to 3 parts by weight of a cyanoethyl-based compound per 100 parts by weight of methyl methacrylate, and

[0024] The above cyanoethyl compound may be one or more selected from the group consisting of cyanoethylpullulan (CAS No. 77466-56-9), cyanoethylcellulose (CAS No. 9004-41-5), cyanoethylsucrose (CAS No. 29253-78-9), and mixtures thereof.

[0025] In addition, another embodiment of the present invention is an eco-friendly surface protection construction method for concrete and steel structures using a hybrid surface protection composition utilizing a composite organic admixture and a ceramic-based inorganic admixture, wherein

[0026] The present invention provides an eco-friendly surface protection construction method for concrete and steel structures, comprising the steps of: removing and cleaning impurities or foreign substances from the surface, and, if necessary, applying a putty material to form a base surface; forming a primer layer on the base surface; applying and curing a hybrid surface protection composition using the composite organic admixture and a ceramic-based inorganic admixture on the primer layer to form a surface protection layer; and applying a surface finishing composition on the surface protection layer to form a surface finishing layer.

[0027] The above surface finishing composition is

[0028] 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; 0.1 to 20 parts by weight of cyanoethyl compound; 0.1 to 20 parts by weight of alkoxysilane; 0.1 to 20 parts by weight of aluminum silicate; 0.1 to 20 parts by weight of Inconel; 0.1 to 20 parts by weight of vermiculite; 0.1 to 20 parts by weight of titanium dioxide; It may include 0.1 to 20 parts by weight of silica sol. Effects of the invention

[0030] According to a hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture according to one embodiment of the present invention, and an eco-friendly surface protection construction method for concrete and steel structures using the same, corrosion caused by chemical erosion of concrete and steel structures under harsh environments can be prevented, thereby enabling the extension of service life, reduction of maintenance costs, and improvement of constructability.

[0031] In addition, it has excellent adhesion to the surfaces of concrete and steel structures and a similar coefficient of thermal expansion. It is effective in preventing cracks and spalling by flexibly responding to shrinkage and expansion caused by external environmental changes, such as changes in humidity and temperature, vibration / behavior, and impact from external loads.

[0032] Furthermore, it offers excellent durability by blocking ultraviolet rays and degradation factors, and its superior heat resistance protects concrete and steel structures from fire. In addition, it exhibits excellent water resistance, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance, and is an eco-friendly product that is safe for the human body as it does not leach harmful heavy metals.

[0033] Therefore, it can be usefully applied to underground structures such as sewer pipes, sewer culverts, underground power conduits, and underground utility tunnels, as well as marine concrete structures, underwater concrete structures, waterproofing structures, and concrete and steel structures in environments with severe chemical erosion or poor conditions. Specific details for implementing the invention

[0035] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0036] One embodiment of the present invention comprises 5 to 75 weight% of a ceramic-based inorganic admixture and 25 to 95 weight% of a composite organic admixture, wherein

[0037] The ceramic-based inorganic admixture comprises 100 parts by weight of calcium carbonate; 5 to 20 parts by weight of aluminum silicate; 5 to 20 parts by weight of Inconel; 5 to 20 parts by weight of vermiculite; 5 to 20 parts by weight of aluminum hydroxide; 0.5 to 15 parts by weight of tungsten carbide; 0.5 to 15 parts by weight of titanium dioxide; 0.5 to 15 parts by weight of silica sol; and 0.5 to 15 parts by weight of a filler pigment;

[0038] The above composite organic admixture comprises 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of styrene-butyl acrylic acid copolymer; 0.1 to 20 parts by weight of decamethylcyclopentasiloxane; 0.1 to 20 parts by weight of sodium phytate; 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; and 0.1 to 20 parts by weight of alkoxysilane. A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture is provided, comprising 0.1 to 20 parts by weight of diisocyanate.

[0039] According to one embodiment of the present invention, the hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, and the eco-friendly surface protection construction method for concrete and steel structures using the same, can prevent corrosion caused by chemical erosion of concrete and steel structures under harsh environments, thereby enabling the extension of service life, reduction of maintenance costs, and improvement of constructability. Furthermore, it has excellent adhesion to the surfaces of concrete and steel structures and similar coefficients of thermal expansion. It also has the effect of preventing cracks and delamination by flexibly responding to shrinkage and expansion caused by external environmental changes, such as changes in humidity and temperature, vibration / movement, and impact from external loads. In addition, it has excellent durability by blocking ultraviolet rays and deterioration factors, and can protect concrete and steel structures from fire due to its excellent heat resistance. Moreover, it exhibits excellent water permeability, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance, and is an eco-friendly product that is safe for the human body as there is no leaching of harmful heavy metals. Therefore, it can be usefully applied to underground structures such as sewer pipes, sewer culverts, underground power conduits, and underground utility tunnels, as well as marine concrete structures, underwater concrete structures, waterproofing structures, and concrete and steel structures in environments with severe chemical erosion or poor conditions.

[0040] More specifically, a hybrid surface protection material composition using a composite organic admixture and a ceramic-based inorganic admixture according to one embodiment of the present invention comprises 5 to 75 weight% of a ceramic-based inorganic admixture and 25 to 95 weight% of a composite organic admixture.

[0041] The above ceramic-based inorganic admixture exhibits excellent strength, heat resistance, water permeability, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance. In particular, it prevents corrosion by blocking chemical erosion of concrete and steel structures in harsh environments, such as marine and underwater environments, and improves durability by blocking ultraviolet rays and deterioration factors. Furthermore, it serves an eco-friendly role that is safe for the human body as there is no leaching of harmful heavy metals. Considering the aforementioned improvement effects, it is preferable that the above ceramic-based inorganic admixture be contained in a range of 5 to 75 weight percent in a hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture according to one embodiment of the present invention.

[0042] More specifically, the ceramic-based inorganic admixture may preferably be used comprising 100 parts by weight of calcium carbonate; 5 to 20 parts by weight of aluminum silicate; 5 to 20 parts by weight of Inconel; 5 to 20 parts by weight of vermiculite; 5 to 20 parts by weight of aluminum hydroxide; 0.5 to 15 parts by weight of tungsten carbide; 0.5 to 15 parts by weight of titanium dioxide; 0.5 to 15 parts by weight of silica sol; and 0.5 to 15 parts by weight of a filler pigment.

[0043] The above calcium carbonate plays a role in achieving excellent watertightness, workability, and durability.

[0044] Hereinafter, the content of other components constituting the ceramic-based inorganic admixture is based on 100 parts by weight of calcium carbonate.

[0045] The above aluminum silicate (CAS No. 14504-95-1) ensures crack resistance and penetration resistance in environments with significant external changes, safely protects structures in case of fire with excellent heat resistance, and permanently protects structures from salt damage and carbonation with chemical and stain resistance.

[0046] It is preferable that the above aluminum silicate be contained in a range of 5 to 20 parts by weight per 100 parts by weight of the above calcium carbonate. If the content of the above aluminum silicate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above aluminum silicate is too high, there is a problem that the adhesion strength may be reduced.

[0047] The aforementioned Inconel protects structures from salt damage and carbonation caused by chemical and thermal loads applied to the surface through its excellent strength, watertightness, hardness, waterproofing performance, and chemical and stain resistance, and plays a role in maintaining corrosion and oxidation resistance under harsh environments such as marine and underwater environments.

[0048] The above Inconel may be products such as Inconel 600, Inconel 625, and Inconel 718, and it is preferable to use Inconel 600, which is a nickel-chromium alloy containing about 72 weight% or more of nickel and about 14 to 17 weight% of chromium.

[0049] It is preferable that the above Inconel be contained in a range of 5 to 20 parts by weight per 100 parts by weight of calcium carbonate. If the content of the above Inconel is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above Inconel is too high, there is a problem that crack resistance may be reduced.

[0050] The above-mentioned vermiculite (CAS No. 1318-00-9) plays a role in enhancing durability by improving strength, watertightness, hardness, water resistance, chemical resistance, and stain resistance through excellent adhesion and increased density of the coating film. In addition, it blocks heat by reducing heat transfer due to its layered structure and expansiveness, and reduces the weight of the surface protection material due to its low density.

[0051] It is preferable that the vermiculite be contained in a range of 5 to 20 parts by weight per 100 parts by weight of calcium carbonate. If the content of the vermiculite is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the vermiculite is too high, there is a problem that the initial film formation may be delayed.

[0052] The above aluminum hydroxide has excellent hygroscopicity, which prevents material separation and enhances adhesion to the substrate, thereby playing a role in realizing functionality and durability such as excellent strength performance, watertightness, hardness, acid resistance, resistance to accelerated neutralization, resistance to chloride ion penetration, and heat resistance.

[0053] It is preferable that the aluminum hydroxide be contained in a range of 5 to 20 parts by weight per 100 parts by weight of the calcium carbonate. If the content of the aluminum hydroxide is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the aluminum hydroxide is too high, there is a problem that workability may be reduced or price competitiveness may be reduced.

[0054] The above tungsten carbide plays a role in rapidly increasing the hardness of the coating surface to improve wear and scratch resistance, and to ensure stability in fire and high-temperature environments.

[0055] In addition, to further enhance the aforementioned improvement effects and further improve excellent crack resistance and carbonation resistance, tungsten carbide with a modified oxide layer formed thereon may be used.

[0056] Specifically, the method comprises the steps of: preparing tungsten carbide with an oxide layer formed thereon by immersing 100 parts by weight of tungsten carbide in 400 to 600 parts by weight of an acidic solution prepared by mixing hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1 and maintaining it for 10 to 30 minutes to produce tungsten carbide with an oxide layer formed on its surface; and preparing tungsten carbide with an oxide layer formed thereon by mixing 100 parts by weight of the tungsten carbide with an oxide layer formed on its surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and 1 to 10 parts by weight of a glucopyranoside-based compound. It can be manufactured.

[0057] The above glycidyloxypropyl trimethoxysilane and glucopyranoside-based compounds serve to improve the dispersibility of tungsten carbide and its miscibility with the components of the complex organic admixture. At this time, the glucopyranoside-based compounds may be one or more selected from the group consisting of 2-ethylhexylglucopyranoside (CAS No. 125590-73-0), methyl-D-glucopyranoside (CAS No. 3149-68-6), and mixtures thereof.

[0058] In addition, to further enhance the aforementioned improvement effects and safely protect structures in the event of a fire with excellent heat resistance, and to improve long-term durability by maintaining strong corrosion protection performance even in harsh environments such as marine and underwater environments, a tungsten carbide-titanium carbide composite with a modified oxide layer formed thereon may be used.

[0059] Specifically, the tungsten carbide-titanium carbide composite having the modified oxide layer formed thereon comprises the step of preparing a tungsten carbide-titanium carbide composite having an oxide layer formed on its surface by immersing 100 parts by weight of a carbide composite, in which tungsten carbide and titanium carbide are mixed in a weight ratio of 1:0.1 to 0.5, in 400 to 600 parts by weight of an acidic solution mixed with hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1, and maintaining it for 10 to 30 minutes; A method comprising the step of preparing a tungsten carbide-titanium carbide composite with a modified oxide layer by mixing 100 parts by weight of a tungsten carbide-titanium carbide composite with an oxide layer formed on the surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and 1 to 10 parts by weight of a glucopyranoside-based compound. It can be manufactured.

[0060] The above tungsten carbide may be contained in a range of 0.5 to 15 parts by weight per 100 parts by weight of calcium carbonate. If the content of the above tungsten carbide is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above tungsten carbide is too high, there is a problem that material separation may occur or workability may be reduced.

[0061] The above titanium dioxide provides excellent functionality such as stain resistance and antibacterial properties, and serves to block ultraviolet rays and chemical corrosion.

[0062] The titanium dioxide may be contained in a range of 0.5 to 15 parts by weight per 100 parts by weight of the calcium carbonate. If the content of the titanium dioxide is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the titanium dioxide is too high, there is a problem that the strength performance may be reduced.

[0063] The aforementioned silica sol ensures strong adhesion and crack resistance, and through its excellent strength, watertightness, hardness, perfect waterproofing, and chemical and stain resistance, it permanently protects structures from salt damage and carbonation, while serving to fundamentally block ultraviolet rays and chemical erosion. Furthermore, its superior heat resistance safely protects structures in the event of a fire, enhancing long-term durability, and it maintains robust anti-corrosion performance even under harsh conditions such as marine and underwater environments.

[0064] The above silica sol may be contained in a range of 0.5 to 15 parts by weight per 100 parts by weight of the calcium carbonate. If the content of the silica sol is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the silica sol is too high, there is a problem that material separation may occur or crack resistance may be reduced.

[0065] The above-mentioned extender pigment provides color and functions to realize excellent strength reinforcement, watertightness, workability, and other functionalities.

[0066] The above-mentioned extender pigments are commonly used in the field and are not specifically limited in type, but non-limiting examples of the above-mentioned extender pigments include talc, light charcoal, heavy charcoal, silicon-based fillers, clay, mica, barium sulfate, etc.

[0067] The above-mentioned extender pigment may be contained in a range of 0.5 to 15 parts by weight per 100 parts by weight of the calcium carbonate. If the content of the above-mentioned extender pigment is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above-mentioned extender pigment is too high, there is a problem that material separation may occur or crack resistance may be reduced.

[0068] In addition, the composite organic admixture according to the present invention has excellent adhesion to the surface of concrete and steel structures and a similar coefficient of thermal expansion. It also plays a role in preventing cracks, delamination, etc. by flexibly responding to shrinkage and expansion caused by external environmental changes such as changes in humidity and temperature, vibration / movement, and impact due to external loads. Furthermore, it plays a role in realizing elasticity, water resistance, corrosion resistance, chemical resistance, acid resistance, water permeability, resistance to carbonation acceleration, resistance to chloride ion penetration, heat resistance, flexural resistance, weather resistance, and stain resistance. Additionally, it plays a role in realizing an eco-friendly effect that is safe for the human body by blocking ultraviolet rays and deterioration factors, thereby providing excellent durability, and preventing the leaching of harmful heavy metals. Considering the aforementioned improvement effects, it is preferable that such a composite organic admixture be contained in a range of 25 to 95 weight percent in a hybrid surface protection material composition using a composite organic admixture and a ceramic-based inorganic admixture according to one embodiment of the present invention.

[0069] More specifically, the composite organic admixture comprises 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of styrene-butyl acrylic acid copolymer; 0.1 to 20 parts by weight of decamethylcyclopentasiloxane; 0.1 to 20 parts by weight of sodium phytate; 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; and 0.1 to 20 parts by weight of alkoxysilane. It is preferable to use a composition comprising 0.1 to 20 parts by weight of diisocyanate.

[0070] The above methyl methacrylate serves to provide excellent adhesion strength, water resistance, corrosion resistance, chemical resistance, acid resistance, water permeability, resistance to chloride ion penetration and neutralization, weather resistance, UV resistance, wear resistance, and hardness.

[0071] Hereinafter, the content of other components constituting the above-mentioned composite organic admixture is based on 100 parts by weight of the above-mentioned methyl methacrylate.

[0072] The above 1,4-butanediol dimethacrylate improves chemical resistance and water resistance by increasing crosslinking density and inhibiting the penetration of chloride ions, moisture, and carbon dioxide, and strengthens the hardness, wear resistance, adhesion, and tensile strength of the coating film to prevent surface damage and peeling.

[0073] The above 1,4-butanediol dimethacrylate may be contained in a range of 30 to 50 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above 1,4-butanediol dimethacrylate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above 1,4-butanediol dimethacrylate is too high, there is a problem that flexibility is reduced and peeling and microcracks may occur.

[0074] The above cellulose acetate propionate (CAS No. 9004-39-1) acts as an integral part of the concrete structure due to its excellent penetration and adhesion, thereby improving water resistance, chemical resistance, acid resistance, durability, weather resistance, and strength. In addition, it enables faster application and drying through excellent workability without material separation even in wet conditions.

[0075] The above cellulose acetate propionate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above cellulose acetate propionate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above cellulose acetate propionate is too high, there is a problem that workability may be reduced.

[0076] The above polycyclohexylene dimethylene terephthalate (PCHDT, CAS No. 24936-69-4) prevents cracking by increasing tensile strength, impact strength, and elongation, and provides resistance to ultraviolet rays, moisture, and chemicals, thereby preventing carbonation, salt damage, and deterioration of concrete and enabling long-term durability.

[0077] The above polycyclohexylenedimethylene terephthalate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above polycyclohexylenedimethylene terephthalate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above polycyclohexylenedimethylene terephthalate is too high, there is a problem that workability may be reduced.

[0078] The above styrene-butyl acrylic acid copolymer serves to provide excellent adhesion strength, water resistance, corrosion resistance, chemical resistance, acid resistance, water permeability, and resistance to chloride ion penetration and neutralization.

[0079] The above styrene-butyl acrylic acid copolymer may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above styrene-butyl acrylic acid copolymer is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above styrene-butyl acrylic acid copolymer is too high, there is a problem that weather resistance may be reduced.

[0080] The above-mentioned decamethylcyclopentasiloxane (CAS No. 541-02-6) acts as an integral part of the concrete structure with excellent adhesion, elasticity, and toughness to achieve resistance to carbonation, weather resistance, and strength, and plays a role in enabling faster application and drying even in wet conditions.

[0081] The above decamethylcyclopentasiloxane may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above decamethylcyclopentasiloxane is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above decamethylcyclopentasiloxane is too high, there is a problem that the deformation resistance may be reduced.

[0082] The above sodium phytate (CAS No. 14306-25-3) not only prevents oxidation of the ceramic-based inorganic admixture of the present invention and improves dispersion stability, but also provides UV / thermal oxidation resistance, thereby improving long-term storage stability.

[0083] The sodium phytate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the methyl methacrylate. If the content of the sodium phytate is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the sodium phytate is too high, it is difficult to expect further performance improvement effects, and there is a problem that price competitiveness may be reduced.

[0084] The above tetrahexyl ascorbate (CAS No. 183476-82-6) inhibits the decomposition of the composite organic admixture by UV, heat, and oxygen, and prevents yellowing and fading of the coating film, thereby providing long-term durability.

[0085] The above tetrahexyl ascorbate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above tetrahexyl ascorbate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above tetrahexyl ascorbate is too high, it is difficult to expect further performance improvement effects, and there is a problem that price competitiveness may be reduced.

[0086] The above alkoxysilane functions to provide excellent adhesion strength, wear resistance, hardness, corrosion resistance, chemical resistance, acid resistance, resistance to chloride ion penetration and neutralization, weather resistance, and stain resistance.

[0087] The above-mentioned alkoxysilanes are commonly used in the field and are not specifically limited in type, but non-limiting examples include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, triphenylmethoxysilane, triphenylethoxysilane, ethyltriethoxysilane, propylethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltripropoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltrimethoxysilane. N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltripropoxysilane, 3-acryloxypropylmethylbis(trimethoxy)silane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, Chloropropyltrimethoxysilane, chloropropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, etc. can be used.

[0088] More preferable alkoxysilanes can be used, which are one or more selected from the group consisting of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltrimethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltripropoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and mixtures thereof, thereby ensuring even better chemical resistance.

[0089] The above alkoxysilane may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above alkoxysilane is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above alkoxysilane is too high, there is a problem that corrosion resistance may be reduced.

[0090] The above diisocyanate functions to promote reactivity and provide excellent elasticity, impact resistance, flexural resistance, internal adhesion strength, wear resistance, hardness, water resistance, corrosion resistance, chemical resistance, acid resistance, water permeability, and resistance to chloride ion penetration and neutralization.

[0091] The above-mentioned diisocyanates are commonly used in the field and are not specifically limited in type, but non-limiting examples include toluene diisocyanate (TDI), methylene diphenyl diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), dicyclohexylmethane diisocyanate (H12MDI), hexamethylene diisocyanate trimer (HDT), toluene diisocyanate trimer (TDI), and isophorone diisocyanate trimer.

[0092] The above diisocyanate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above diisocyanate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above diisocyanate is too high, there is a problem that crack resistance may be reduced.

[0093] In addition, the above composite organic admixture may further contain 0.1 to 3 parts by weight of a cyanoethyl-based compound per 100 parts by weight of the methyl methacrylate.

[0094] The above cyanoethyl compound improves strong bonding strength with the surface, water resistance, wear resistance, heat resistance, and chemical resistance, thereby preventing cracking and peeling of the coating film.

[0095] The above cyanoethyl compound may be one or more selected from the group consisting of cyanoethylpullulan (CAS No. 77466-56-9), cyanoethylcellulose (CAS No. 9004-41-5), cyanoethylsucrose (CAS No. 29253-78-9), and mixtures thereof.

[0096] In addition, the above-mentioned composite organic admixture may further include additives commonly used in the field, such as crosslinking accelerators, concentration regulators, film adhesion agents, antifreeze agents, fluidizing agents, preservatives, defoaming agents, etc. Considering the respective improvement effects, these additives may be included in a range of 0.001 to 1 part by weight per 100 parts by weight of the above-mentioned methyl methacrylate.

[0097] More specifically, the crosslinking promoter functions to promote crosslinking between the polymers. These above-mentioned crosslinking accelerators are commonly used in the field and are not particularly limited in type; however, non-limiting examples of the above-mentioned crosslinking agents include benzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, t-butylcumyl peroxide, methyl ethyl ketone peroxide, cumene hydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,3-bis(t-butylperoxypropyl)benzene, di-t-butylperoxy-diisopropylbenzene, t-butylperoxybenzene, 2,4-dichlorobenzoyl peroxide, and 1,1-dibutylperoxy-3,3,5-trimethylsiloxane. Organic peroxides such as n-butyl-4,4-di-t-butylperoxyvalerate; tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), dithiodimorpholine, etc. may be used.

[0098] In addition, the concentration regulator functions to improve workability by controlling the viscosity of the composition and to prevent material separation. The concentration regulator is generally used in the field and is not specifically limited in type, but non-limiting examples of the concentration regulator may include cellulose-based, acrylic-based, polyacrylamide-based, urethane-based, polyvinyl alcohol, polyvinyl acetate, etc., such as methylcellulose, carboxymethylcellulose, methylcellulose acetate, and ethylcellulose.

[0099] In addition, the above-mentioned film adhesive has the function of further improving the adhesion of the film. The above-mentioned film adhesive is generally used in the field and is not specifically limited in type, but non-limiting examples of the above-mentioned film adhesive include organometallic compounds such as dibutyltin dilorate, dibutyltin diacetate, dibutyltin dioctoeate, tin acetate, etc.

[0100] In addition, the above-mentioned antifreeze prevents the phenomenon of the coating film being destroyed due to freezing at low temperatures and improves the low-temperature stability of the composition. The above-mentioned antifreeze is generally used in the field and is not particularly limited in type, but non-limiting examples of the above-mentioned antifreeze include glycol-based antifreezes such as ethylene glycol and propylene glycol.

[0101] In addition, the above-mentioned fluidizing agent enhances dispersion to improve the fluidity and workability of the composition, and ultimately functions to improve watertightness, strength, and durability. Such fluidizing agents are generally used in the field and are not specifically limited in type; however, non-limiting examples of such fluidizing agents include melamine-based and polycarboxylic acid-based fluidizing agents.

[0102] In addition, the above preservative functions to prevent the composition from decaying or the coating from collapsing due to the action of microorganisms (bacteria), and to improve the long-term preservation stability of the composition. The above preservative is generally used in the field and is not specifically limited in type, but a non-limiting example of the above preservative is sodium styrene sulfonate.

[0103] In addition, the above-mentioned defoamer functions to improve strength and durability by removing bubbles from the composition. The above-mentioned defoamer is generally used in the field and is not specifically limited in type, but non-limiting examples of the above-mentioned defoamer include alcohol-based defoamers such as glycol; silicone-based defoamers such as dimethyl silicone oil, polyorganosiloxane, fluorosilicone oil; fatty acid-based defoamers such as stearic acid, oleic acid; oil-based defoamers such as kerosene, animal and vegetable oil, castor oil; ester-based defoamers such as solitol trioleate, glycerol monoricinoleate; and oxyalkylene-based defoamers such as polyoxyalkylene, acetylene ethers, polyoxyalkylene fatty acid esters, and polyoxyalkylene alkylamines.

[0104] A hybrid surface protection composition using the composite organic admixture and the ceramic-based inorganic admixture according to one embodiment of the present invention can be prepared by mixing 5 to 75 weight% of the ceramic-based inorganic admixture and 25 to 95 weight% of the composite organic admixture for a predetermined time (e.g., 1 to 10 minutes) using a forced mixer or a continuous mixer.

[0105] Meanwhile, another embodiment of the present invention is an eco-friendly surface protection construction method for concrete and steel structures using a hybrid surface protection material composition utilizing a composite organic admixture and a ceramic-based inorganic admixture, wherein

[0106] The present invention provides an eco-friendly surface protection construction method for concrete and steel structures, comprising the steps of: removing and cleaning impurities or foreign substances from the surface, and, if necessary, applying a putty material to form a base surface; forming a primer layer on the base surface; applying and curing a hybrid surface protection composition using the composite organic admixture and a ceramic-based inorganic admixture on the primer layer to form a surface protection layer; and applying a surface finishing composition on the surface protection layer to form a surface finishing layer.

[0107] In the specification of the present invention, the term "concrete structure" may be used to include structures made of concrete, such as chemical plants, food factories, livestock barn floors, marine concrete structures, underwater concrete structures, waterproofing structures, underground structures, sewer pipes, road surfaces, bridge decks, concrete slabs of bridges, and bridge expansion joints; and the term "steel structure" may be used to include structures made of steel, such as steel bridges, deck plates, deck plates, and steel bridge facilities.

[0108] First, the step of forming the base surface can be performed by removing and cleaning impurities or foreign substances on the surface using a high-pressure water washer, power tool, shot blaster, etc., and then, if necessary, applying putty material. In addition, if there are deteriorated areas on the surface, the base surface can be formed by removing and cleaning the affected area using a grinder, planer, etc., and then applying putty material.

[0109] At this time, the putty material is generally used in the field and is not specifically limited in type, but as a non-limiting example, one or more types selected from the group consisting of epoxy putty, urethane putty, cement-based putty, and mixtures thereof may be used.

[0110] In addition, the step of forming a primer layer on the substrate may be performed to further improve the adhesion of the hybrid surface protection composition using the composite organic admixture and ceramic-based inorganic admixture of the present invention, further suppress water penetration and chloride ion penetration, and further improve water resistance and water resistance. At this time, the primer layer is not particularly limited in type as it is generally used in the field, but as a non-limiting example, it may include one or more selected from the group consisting of styrene-butadiene latex, ethylene vinyl acetate, polyacrylate, acrylic, methyl methacrylate, the polymer composite of the present invention, and mixtures thereof.

[0111] In addition, in the step of forming a surface protection layer by applying and curing the hybrid surface protection composition using the composite organic admixture and the ceramic-based inorganic admixture of the present invention on the upper surface of the primer layer, the application may be performed using a brush, roller, airless sprayer, spray equipment, etc. In addition, the hybrid surface protection composition using the composite organic admixture and the ceramic-based inorganic admixture may be applied 1 to 3 times.

[0112] In addition, the step of forming a surface finishing layer by applying a surface finishing composition on top of the surface protection layer described above not only allows the hybrid surface protection composition using the composite organic admixture and ceramic-based inorganic admixture of the present invention to be attached and integrated with excellent adhesion, but also has the effect of further improving functionality and durability such as excellent elasticity, impact resistance, adhesion strength, chemical resistance, acid resistance, water permeability, resistance to accelerated neutralization, resistance to chloride ion penetration, heat resistance, flexibility, weather resistance, and stain resistance.

[0113] The above-mentioned surface finishing composition is commonly used in the field and is not particularly limited in type. For example, the above-mentioned surface finishing composition comprises 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; a cyanoethyl compound; 0.1 to 20 parts by weight of alkoxysilane; 0.1 to 20 parts by weight of aluminum silicate; 0.1 to 20 parts by weight of Inconel; and 0.1 to 20 parts by weight of vermiculite. The above-mentioned improvement effect can be further enhanced by using a composition comprising 0.1 to 20 parts by weight of titanium dioxide and 0.1 to 20 parts by weight of silica sol.

[0114] The above methyl methacrylate serves to provide excellent adhesion strength, water resistance, corrosion resistance, chemical resistance, acid resistance, water permeability, resistance to chloride ion penetration and neutralization, weather resistance, UV resistance, wear resistance, and hardness.

[0115] Hereinafter, the content of other components constituting the surface finishing composition is based on 100 parts by weight of the methyl methacrylate.

[0116] The above 1,4-butanediol dimethacrylate improves chemical resistance and water resistance by increasing crosslinking density and inhibiting the penetration of chloride ions, moisture, and carbon dioxide, and strengthens the hardness, wear resistance, adhesion, and tensile strength of the coating film to prevent surface damage and peeling.

[0117] The above 1,4-butanediol dimethacrylate may be contained in a range of 30 to 50 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above 1,4-butanediol dimethacrylate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above 1,4-butanediol dimethacrylate is too high, there is a problem that flexibility is reduced and peeling and microcracks may occur.

[0118] The above cellulose acetate propionate acts as an integral part of the concrete structure due to its excellent penetration and adhesion, thereby improving water resistance, chemical resistance, acid resistance, durability, weather resistance, and strength. In addition, it enables faster application and drying through excellent workability without material separation even in wet conditions.

[0119] The above cellulose acetate propionate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above cellulose acetate propionate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above cellulose acetate propionate is too high, there is a problem that workability may be reduced.

[0120] The above polycyclohexylene dimethylene terephthalate (PCHDT, CAS No. 24936-69-4) prevents cracking by increasing tensile strength, impact strength, and elongation, and provides resistance to ultraviolet rays, moisture, and chemicals, thereby preventing carbonation, salt damage, and deterioration of concrete and enabling long-term durability.

[0121] The above polycyclohexylenedimethylene terephthalate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above polycyclohexylenedimethylene terephthalate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above polycyclohexylenedimethylene terephthalate is too high, there is a problem that workability may be reduced.

[0122] The above tetrahexyl ascorbate (CAS No. 183476-82-6) inhibits the decomposition of the composite organic admixture by UV, heat, and oxygen, and prevents yellowing and fading of the coating film, thereby providing long-term durability.

[0123] The above tetrahexyl ascorbate may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above tetrahexyl ascorbate is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above tetrahexyl ascorbate is too high, it is difficult to expect further performance improvement effects, and there is a problem that price competitiveness may be reduced.

[0124] The above cyanoethyl compound improves strong bonding strength with the surface, water resistance, wear resistance, heat resistance, and chemical resistance, thereby preventing cracking and peeling of the coating film.

[0125] The above cyanoethyl compound may be one or more selected from the group consisting of cyanoethylpullulan (CAS No. 77466-56-9), cyanoethylcellulose (CAS No. 9004-41-5), cyanoethylsucrose (CAS No. 29253-78-9), and mixtures thereof.

[0126] The above cyanoethyl compound may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above cyanoethyl compound is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above cyanoethyl compound is too high, it is difficult to expect further performance improvement effects and there is a problem that price competitiveness may be reduced.

[0127] The above alkoxysilane functions to provide excellent adhesion strength, wear resistance, hardness, corrosion resistance, chemical resistance, acid resistance, resistance to chloride ion penetration and neutralization, weather resistance, and stain resistance.

[0128] The above-mentioned alkoxysilanes are commonly used in the field and are not specifically limited in type, but non-limiting examples include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, triphenylmethoxysilane, triphenylethoxysilane, ethyltriethoxysilane, propylethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltripropoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltrimethoxysilane. N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltripropoxysilane, 3-acryloxypropylmethylbis(trimethoxy)silane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, Chloropropyltrimethoxysilane, chloropropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, etc. can be used.

[0129] More preferable alkoxysilanes can be used, which are one or more selected from the group consisting of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltrimethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltripropoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and mixtures thereof, thereby ensuring even better chemical resistance.

[0130] The above alkoxysilane may be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above alkoxysilane is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above alkoxysilane is too high, there is a problem that corrosion resistance may be reduced.

[0131] The above aluminum silicate (CAS No. 14504-95-1) ensures crack resistance and penetration resistance in environments with significant external changes, safely protects structures in case of fire with excellent heat resistance, and permanently protects structures from salt damage and carbonation with chemical and stain resistance.

[0132] It is preferable that the aluminum silicate be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the methyl methacrylate. If the content of the aluminum silicate is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the aluminum silicate is too high, there is a problem that the adhesion strength may be reduced.

[0133] The aforementioned Inconel protects structures from salt damage and carbonation caused by chemical and thermal loads applied to the surface through its excellent strength, watertightness, hardness, waterproofing performance, and chemical and stain resistance, and plays a role in maintaining corrosion and oxidation resistance under harsh environments such as marine and underwater environments.

[0134] The above Inconel may be products such as Inco's Inconel 600, Inconel 625, and Inconel 718, and it is preferable to use Inconel 600, which is a nickel-chromium alloy containing 72 weight% or more of nickel and 14 to 17 weight% of chromium.

[0135] It is preferable that the above Inconel be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the above Inconel is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the above Inconel is too high, there is a problem that crack resistance may be reduced.

[0136] The above-mentioned vermiculite (CAS No. 1318-00-9) plays a role in enhancing durability by improving strength, watertightness, hardness, water resistance, chemical resistance, and stain resistance through excellent adhesion and increased density of the coating film. In addition, it blocks heat by reducing heat transfer due to its layered structure and expansiveness, and reduces the weight of the surface protection material due to its low density.

[0137] It is preferable that the vermiculite be contained in a range of 0.1 to 20 parts by weight per 100 parts by weight of the methyl methacrylate. If the content of the vermiculite is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the vermiculite is too high, there is a problem that the initial film formation may be delayed.

[0138] The above titanium dioxide provides excellent functionality such as stain resistance and antibacterial properties, and serves to block ultraviolet rays and chemical corrosion.

[0139] The titanium dioxide may be contained in a range of 0.1 to 15 parts by weight per 100 parts by weight of the methyl methacrylate. If the content of the titanium dioxide is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the titanium dioxide is too high, there is a problem that the strength performance may be reduced.

[0140] The aforementioned silica sol ensures strong adhesion and crack resistance, and through its excellent strength, watertightness, hardness, perfect waterproofing, and chemical and stain resistance, it permanently protects structures from salt damage and carbonation, while serving to fundamentally block ultraviolet rays and chemical erosion. Furthermore, its superior heat resistance safely protects structures in the event of a fire, enhancing long-term durability, and it maintains robust anti-corrosion performance even under harsh conditions such as marine and underwater environments.

[0141] The above silica sol may be contained in a range of 0.1 to 15 parts by weight per 100 parts by weight of the above methyl methacrylate. If the content of the silica sol is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the silica sol is too high, there is a problem that material separation may occur or crack resistance may be reduced.

[0142] In addition, the surface finishing composition may further include additives commonly used in the field, such as crosslinking accelerators, concentration regulators, film adhesion agents, antifreeze agents, fluidizing agents, preservatives, defoaming agents, etc. Considering the respective improvement effects, these additives may be included in a range of 0.01 to 5 parts by weight per 100 parts by weight of the methyl methacrylate.

[0143] A more specific description of the crosslinking accelerator, concentration regulator, film adhesion agent, antifreeze, fluidizing agent, preservative, and defoaming agent as the above-mentioned additives is the same as that described in the additives of the above-mentioned composite organic admixture.

[0144] According to one embodiment of the present invention, the hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, and the eco-friendly surface protection construction method for concrete and steel structures using the same, can prevent corrosion caused by chemical erosion of concrete and steel structures under harsh environments, thereby enabling the extension of service life, reduction of maintenance costs, and improvement of constructability. Furthermore, it has excellent adhesion to the surfaces of concrete and steel structures and similar coefficients of thermal expansion. It also has the effect of preventing cracks and delamination by flexibly responding to shrinkage and expansion caused by external environmental changes, such as changes in humidity and temperature, vibration / movement, and impact from external loads. In addition, it has excellent durability by blocking ultraviolet rays and deterioration factors, and can protect concrete and steel structures from fire due to its excellent heat resistance. Moreover, it exhibits excellent water permeability, stain resistance, neutralization resistance, chloride ion penetration resistance, and chemical resistance, and is an eco-friendly product that is safe for the human body as there is no leaching of harmful heavy metals. Therefore, it can be usefully applied to underground structures such as sewer pipes, sewer culverts, underground power conduits, and underground utility tunnels, as well as marine concrete structures, underwater concrete structures, waterproofing structures, and concrete and steel structures in environments with severe chemical erosion or poor conditions.

[0145] Although preferred embodiments of the present invention have been described in detail above, the present invention is not limited to the above embodiments, and various modifications are possible by those skilled in the art within the scope of the technical concept of the present invention.

[0147] [Preparation Example 1] Tungsten carbide with a modified oxide layer

[0148] Tungsten carbide with an oxide layer formed on its surface was prepared by immersing 100 parts by weight of tungsten carbide in 500 parts by weight of an acidic solution of hydrochloric acid (HCl) and nitric acid (HNO3) mixed in a ratio of 3:1 for 25 minutes. Subsequently, tungsten carbide with a modified oxide layer formed on its surface was prepared by mixing 100 parts by weight of the tungsten carbide with the oxide layer formed on its surface, 13 parts by weight of glycidyloxypropyl trimethoxysilane, and 5 parts by weight of 2-ethylhexylglucopyranoside (CAS No. 125590-73-0) for 1 hour.

[0150] [Preparation Example 2] Tungsten carbide-titanium carbide composite with a modified oxide layer

[0151] A tungsten carbide-titanium carbide composite with an oxide layer formed on its surface was prepared by immersing 100 parts by weight of a carbide composite, in which tungsten carbide and titanium carbide were mixed in a weight ratio of 1:0.3, in 500 parts by weight of an acidic solution in which hydrochloric acid (HCl) and nitric acid (HNO3) were mixed in a ratio of 3:1 for 25 minutes. Subsequently, a tungsten carbide-titanium carbide composite with an oxide layer formed on its surface was prepared by mixing 100 parts by weight of the tungsten carbide-titanium carbide composite with an oxide layer formed on its surface, 13 parts by weight of glycidyloxypropyl trimethoxysilane, 3 parts by weight of 2-ethylhexylglucopyranoside (CAS No. 125590-73-0), and 3 parts by weight of methyl-D-glucopyranoside (CAS No. 3149-68-6) for 1 hour.

[0153] [Examples 1 to 3 and Comparative Examples 1 and 2]

[0154] Preparation of a hybrid surface protection material composition using a composite organic admixture and a ceramic-based inorganic admixture

[0155] A hybrid surface protection composition and a comparative composition using a composite organic admixture and a ceramic-based inorganic admixture were prepared by mixing the components and content as shown in Table 1 below in a forced mixer and stirring for about 2 minutes.

[0156] division Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Ceramic-based inorganic admixtures 35 35 35 35 35 weight part calcium carbonate 100 100 100 100 100 Aluminum Silicate [CAS No. 14504-95-1] 8 8 8 - 8 Inconel 7 7 7 - - Vermiculite [CAS No. 1318-00-9] 10 10 10 - - aluminum hydroxide 12 12 12 - 12 Tungsten carbide 4 4 [Manufacturing Example 1] 4 [Manufacturing Example 2] - - tungsten - - - - 4 titanium dioxide 2 2 2 2 2 silica sol 2 2 2 2 2 Body pigment 0.6 0.6 0.6 0.6 0.6 Composite organic admixture 65 65 65 65 65 weight part Methyl methacrylate 100 100 100 10 100 1,4-butanediol dimethacrylate 35 35 35 - 35 Cellulose acetate propionate [CAS No. 9004-39-1] 12 12 12 - - Polycyclohexylenedimethylene terephthalate [CAS No. 24936-69-4] 10 10 10 - - Styrene-butyl acrylic acid copolymer [CAS No. 25767-47-9] 10 10 10 100 10 Decamethylcyclopentasiloxane [CAS No. 541-02-6] 7 7 7 - - Sodium Phytate [CAS No. 14306-25-3] 5 5 5 - - Tetrahexyl ascorbate [CAS No. 183476-82-6] 5 5 5 - - 3-Aminopropyltriethoxysilane 3 3 3 3 3 Hexamethylene diisocyanate (HDI) 6 6 6 6 6 Cyanoethylfluran [CAS No. 77466-56-9] - 0.5 0.3 - - Cyanoethylcellulose [CAS No. 9004-41-5] - - 0.2 - - Benzoyl peroxide 0.05 0.05 0.05 0.05 0.05 polyvinyl acetate 0.05 0.05 0.05 0.05 0.05 Dibutyltin diacetate 0.05 0.05 0.05 0.05 0.05 Ethylene glycol 0.05 0.05 0.05 0.05 0.05 Polycarboxylic acid-based fluidizing agents 0.05 0.05 0.05 0.05 0.05 Sodium styrene sulfonate 0.05 0.05 0.05 0.05 0.05 Polyorganosiloxane 0.05 0.05 0.05 0.05 0.05 Solitol trioleate 0.05 0.05 0.05 0.05 0.05 Inconel: Inconel 600 product

[0158] The following test examples show experimental results comparing the characteristics of the embodiments according to the present invention with those of comparative examples 1 and 2, so that the characteristics of embodiments 1 to 3 according to the present invention can be more easily identified.

[0160] [Test Example 1]

[0161] For the hybrid surface protection material compositions using composite organic admixtures and ceramic-based inorganic admixtures prepared according to Examples 1 to 3 of the present invention and the comparative compositions prepared according to Comparative Examples 1 and 2, an accelerated neutralization test was performed according to KS F 4936, a salt spray test was performed according to KS D 9502, an accelerated weathering test was performed according to KS M 2274, tests for adhesion strength, film formation appearance, water permeability, chloride ion penetration resistance, and moisture permeability were performed according to KS F 4936, a chemical resistance test (sulfuric acid, hydrochloric acid, sodium hydroxide) was performed according to KS M ISO 2812, a flexural resistance test was performed according to KS M 5000, an impact resistance test was performed according to KS D 6711, a stain resistance test was performed according to the Korea Housing Corporation Specialized Specification-2006, and KS M ISO 11507 (acceleration of paints Weathering test was performed by fluorescence exposure to UV, and the results are shown in Table 2.

[0162] item Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Neutering promotion (mm) 0 0 0 0.5 0.3 salt spray No issues No issues No issues discoloration No issues Accelerated weathering No issues No issues No issues discoloration discoloration Adhesion strength (MPa) After standard curing 2.2 2.3 2.5 1.4 1.8 After accelerated weathering 2.1 2.2 2.4 1.2 1.5 After alternating hot and cold 2.0 2.0 2.2 1.0 1.4 alkali resistance after 2.0 2.1 2.2 1.0 1.4 After saline tolerance 1.9 2.0 2.3 1.1 1.5 Film formation surface appearance After standard curing No issues No issues No issues No issues No issues After accelerated weathering No issues No issues No issues discoloration discoloration After alternating hot and cold No issues No issues No issues No issues No issues alkali resistance after No issues No issues No issues No issues No issues After saline tolerance No issues No issues No issues discoloration No issues Endurance Not a pitcher Not a pitcher Not a pitcher Pitcher occurrence Not a pitcher Chloride ion penetration resistance (C) 30 26 21 87 69 moisture permeability 1.1 0.9 0.7 2.3 1.9 Chemical resistance sulfuric acid No issues No issues No issues swelling swelling hydrochloric acid No issues No issues No issues swelling No issues Sodium hydroxide No issues No issues No issues No issues No issues Flexibility No issues No issues No issues No issues No issues Impact resistance No issues No issues No issues offshoot Final payment due Stain resistance No issues No issues No issues No issues No issues Weather resistance (168 hours, △ 0.34 0.29 0.26 1.42 0.81

[0163] As shown in Table 2 above, it was confirmed that the hybrid surface protection composition using the composite organic admixture and ceramic-based inorganic admixture prepared according to Examples 1 to 3 had very excellent performance compared to the comparative composition prepared according to Comparative Examples 1 and 2.

[0165] [Examples 4 to 6 and Comparative Examples 3 and 4]

[0166] Preparation of a surface finishing composition

[0167] A surface finishing composition and a comparative coating composition were prepared by mixing the components and contents as shown in Table 3 below in a forced mixer and stirring for about 2 minutes.

[0168] division Example 4 Example 5 Example 6 Comparative Example 3 Comparative Example 4 Methyl methacrylate 100 100 100 100 100 1,4-butanediol dimethacrylate 35 35 35 - 35 Cellulose acetate propionate [CAS No. 9004-39-1] 12 12 12 - - Polycyclohexylenedimethylene terephthalate [CAS No. 24936-69-4] 10 10 10 - - Tetrahexyl ascorbate [CAS No. 183476-82-6] 7 7 7 - - Cyanoethylfluran [CAS No. 77466-56-9] 3 - 1 - - Cyanoethylcellulose [CAS No. 9004-41-5] - 2 1 - - Cyanoethyl sucrose [CAS No. 29253-78-9] - 1 1 - - 3-Aminopropyltriethoxysilane - 4 4 - 4 3-Acryloxypropyltriethoxysilane 5 1 1 5 1 Aluminum Silicate [CAS No. 14504-95-1] 3 3 3 - - Inconel [Inconel 600 product] 1 1 1 - - Vermiculite [CAS No. 1318-00-9] 2 2 2 - - titanium dioxide 2 2 2 2 2 silica sol 2 2 2 2 2 Benzoyl peroxide 0.05 0.05 0.05 0.05 0.05 polyvinyl acetate 0.05 0.05 0.05 0.05 0.05 Dibutyltin diacetate 0.05 0.05 0.05 0.05 0.05 Ethylene glycol 0.05 0.05 0.05 0.05 0.05 Polycarboxylic acid-based fluidizing agents 0.05 0.05 0.05 0.05 0.05 Sodium styrene sulfonate 0.05 0.05 0.05 0.05 0.05 Polyorganosiloxane 0.05 0.05 0.05 0.05 0.05 Solitol trioleate 0.05 0.05 0.05 0.05 0.05

[0169] The following test examples show experimental results comparing the characteristics of the embodiments according to the present invention with those of comparative examples 3 and 4, so that the characteristics of embodiments 4 to 6 according to the present invention can be more easily identified.

[0171] [Test Example 2]

[0172] In order to comparatively evaluate the physical properties of the surface finishing composition of the present invention, for each test specimen on which a surface finishing layer was formed by applying and curing the hybrid surface protection composition using the composite organic admixture and ceramic-based inorganic admixture prepared according to Examples 1 to 3 and the comparative composition prepared according to Comparative Examples 1 and 2, respectively, the surface finishing composition prepared according to Examples 4 to 6 and the comparative coating composition prepared according to Comparative Examples 3 and 4 were respectively applied, an accelerated neutralization test was performed according to KS F 4936, a salt spray test was performed according to KS D 9502, an accelerated weathering test was performed according to KS M 2274, tests for adhesion strength, film formation appearance, water permeability, chloride ion penetration resistance, and moisture permeability were performed according to KS F 4936, and a chemical resistance test (sulfuric acid, hydrochloric acid, sodium hydroxide) was performed according to KS M ISO 2812, and KS M Flexural strength tests were performed according to 5000, impact resistance tests according to KS D 6711, stain resistance tests according to Housing Corporation Specialized Specification-2006, and weathering tests according to KS M ISO 11507 (Accelerated Weathering Test of Paints - Fluorescent Exposure to UV), and the respective results are shown in Table 4 below.

[0173] item Example 4 Example 5 Example 6 Comparative Example 3 Comparative Example 4 Neutering promotion (mm) 0 0 0 0.4 0.2 salt spray No issues No issues No issues No issues No issues Accelerated weathering No issues No issues No issues No issues No issues Adhesion strength (MPa) After standard curing 2.3 2.5 2.8 1.5 1.9 After accelerated weathering 2.2 2.4 2.7 1.3 1.6 After alternating hot and cold 2.1 2.2 2.5 1.1 1.4 alkali resistance after 2.2 2.3 2.3 1.1 1.5 After saline tolerance 2.1 2.3 2.4 1.2 1.5 Film formation surface appearance After standard curing No issues No issues No issues No issues No issues After accelerated weathering No issues No issues No issues No issues No issues After alternating hot and cold No issues No issues No issues No issues No issues alkali resistance after No issues No issues No issues No issues No issues After saline tolerance No issues No issues No issues No issues No issues Endurance Not a pitcher Not a pitcher Not a pitcher Not a pitcher Not a pitcher Chloride ion penetration resistance (C) 22 20 18 76 54 moisture permeability 1.0 0.8 06 2.2 1.8 Chemical resistance sulfuric acid No issues No issues No issues swelling No issues hydrochloric acid No issues No issues No issues swelling No issues Sodium hydroxide No issues No issues No issues No issues No issues Flexibility No issues No issues No issues No issues No issues Impact resistance No issues No issues No issues No issues No issues Stain resistance No issues No issues No issues No issues No issues Weather resistance (168 hours, △ 0.31 0.27 0.25 1.30 0.73

[0174] As shown in Table 4 above, it was confirmed that the test specimens using the surface finishing compositions prepared according to Examples 4 to 6 had very excellent performance compared to the comparative coating compositions according to Comparative Examples 3 and 4.

[0176] As explained above, those skilled in the art to which the present invention pertains will understand that the present invention may be implemented in other specific forms without altering its technical concept or essential features. Therefore, all embodiments described above should be understood as illustrative and not restrictive. The scope of the present invention should be interpreted as including all modified or altered forms derived from the meaning and scope of the claims set forth below and their equivalents, rather than from the detailed description above.

Claims

Claim 1 The composition comprises 5 to 75 weight% of a ceramic-based inorganic admixture and 25 to 95 weight% of a composite organic admixture, wherein the ceramic-based inorganic admixture comprises 100 weight parts of calcium carbonate; 5 to 20 weight parts of aluminum silicate; 5 to 20 weight parts of Inconel alloy, which is a nickel-based alloy; 5 to 20 weight parts of vermiculite; 5 to 20 weight parts of aluminum hydroxide; 0.5 to 15 weight parts of tungsten carbide; 0.5 to 15 weight parts of titanium dioxide; 0.5 to 15 weight parts of silica sol; and 0.5 to 15 weight parts of a filler pigment; and the composite organic admixture comprises 100 weight parts of methyl methacrylate; and 30 to 50 weight parts of 1,4-butanediol dimethacrylate. A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, characterized by comprising: 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of styrene-butyl acrylic acid copolymer; 0.1 to 20 parts by weight of decamethylcyclopentasiloxane; 0.1 to 20 parts by weight of sodium phytate; 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; 0.1 to 20 parts by weight of alkoxysilane; and 0.1 to 20 parts by weight of diisocyanate. Claim 2 A method according to claim 1, wherein the tungsten carbide is tungsten carbide with a modified oxide layer formed thereon, comprising the steps of: preparing tungsten carbide with an oxide layer formed on its surface by immersing 100 parts by weight of tungsten carbide with a modified oxide layer formed thereon in 400 to 600 parts by weight of an acidic solution obtained by mixing hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1 and maintaining it for 10 to 30 minutes; and preparing tungsten carbide with a modified oxide layer formed thereon by mixing 100 parts by weight of tungsten carbide with an oxide layer formed on its surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and 1 to 10 parts by weight of a glucopyranoside-based compound. A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, characterized in that the glucopyranoside-based compound is manufactured and is one or more selected from the group consisting of 2-ethylhexylglucopyranoside (CAS No. 125590-73-0), methyl-D-glucopyranoside (CAS No. 3149-68-6), and mixtures thereof. Claim 3 In claim 2, the tungsten carbide with the modified oxide layer formed thereon is a tungsten carbide-titanium carbide composite with the modified oxide layer formed thereon, and the tungsten carbide-titanium carbide composite with the modified oxide layer formed thereon comprises the step of preparing a tungsten carbide-titanium carbide composite with an oxide layer formed on its surface by immersing 100 parts by weight of a carbide composite in which tungsten carbide and titanium carbide are mixed in a weight ratio of 1:0.1 to 0.5 into 400 to 600 parts by weight of an acidic solution mixed with hydrochloric acid (HCl) and nitric acid (HNO3) in a ratio of 3:1 for 10 to 30 minutes; and 100 parts by weight of the tungsten carbide-titanium carbide composite with the oxide layer formed on its surface, 10 to 30 parts by weight of glycidyloxypropyl trimethoxysilane, and A method comprising the step of preparing a tungsten carbide-titanium carbide composite with a modified oxide layer formed by mixing 1 to 10 parts by weight of a glucopyranoside-based compound. A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, characterized by being manufactured. Claim 4 A hybrid surface protection composition using a composite organic admixture and a ceramic-based inorganic admixture, wherein the composite organic admixture further contains 0.1 to 3 parts by weight of a cyanoethyl-based compound per 100 parts by weight of methyl methacrylate, and the cyanoethyl-based compound is one or more selected from the group consisting of cyanoethylpullulan (CAS No. 77466-56-9), cyanoethylcellulose (CAS No. 9004-41-5), cyanoethylsucrose (CAS No. 29253-78-9), and mixtures thereof. Claim 5 An eco-friendly surface protection construction method for concrete and steel structures using a hybrid surface protection composition utilizing a composite organic admixture and a ceramic-based inorganic admixture according to any one of claims 1 to 4, comprising the steps of: removing and washing impurities or foreign substances from the surface, and if deteriorated areas exist on the surface, removing and washing the relevant areas using a grinder, planer, etc., and then applying a putty material to form a base surface; forming a primer layer on the base surface; applying and curing the hybrid surface protection composition utilizing the composite organic admixture and the ceramic-based inorganic admixture on the primer layer to form a surface protection layer; and applying a surface finishing composition on the surface protection layer to form a surface finishing layer. Claim 6 In claim 5, the surface finishing composition comprises 100 parts by weight of methyl methacrylate; 30 to 50 parts by weight of 1,4-butanediol dimethacrylate; 0.1 to 20 parts by weight of cellulose acetate propionate; 0.1 to 20 parts by weight of polycyclohexylenedimethylene terephthalate (PCHDT); 0.1 to 20 parts by weight of tetrahexyldecyl ascorbate; 0.1 to 20 parts by weight of a cyanoethyl compound; 0.1 to 20 parts by weight of alkoxysilane; 0.1 to 20 parts by weight of aluminum silicate; 0.1 to 20 parts by weight of Inconel alloy, which is a nickel-based alloy; and 0.1 to 20 parts by weight of vermiculite. An eco-friendly surface protection construction method for concrete and steel structures, characterized by comprising 0.1 to 20 parts by weight of titanium dioxide; and 0.1 to 20 parts by weight of silica sol.

Citation Information

Patent Citations

  • Functional surface protect-reinforce composition for concrete and steel structure with elastic polymer modifier and surface protecting-reinforcing construction method for surface of concrete and steel structure using the same

    KR102543960B1

  • Composite thermal insulation coating with heat shielding properties and construction method thereof

    KR102804144B1

  • Compositions for golf equipment

    US20110130222A1