Methods for optimizing the stability of grinding fluid

By selecting appropriate abrasives and controlling the surface charge of abrasive particles, the mechanical and chemical properties of the polishing slurry were optimized, solving the problem of unstable polishing slurry in the CMP process and improving polishing effect and product yield.

CN123107545APending Publication Date: 2026-11-17SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611079868.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The instability of the polishing slurry in the CMP process leads to process instability, affecting the polishing effect and product yield.

Method used

By selecting abrasives with suitable particle size, distribution, and solid content, and by incorporating a single batch of abrasives into a chemical solution while controlling the surface charge of the abrasive particles, the mechanical and chemical properties of the grinding fluid can be optimized.

Benefits of technology

It improves the stability and polishing effect of the polishing slurry, thereby increasing the product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107545A_ABST
    Figure CN123107545A_ABST
Patent Text Reader

Abstract

This invention discloses a method for optimizing the stability of polishing slurry, comprising: Step 1, selecting abrasives based on particle size, distribution, and solid content to ensure that the selected abrasives meet the acceptable particle size, distribution, and solid content requirements. Step 2, incorporating a single batch of the selected abrasives into a chemical solution to form a polishing slurry; the abrasive particles have surface charges, and the deviation of the surface charge count of each particle in the polishing slurry is controlled by adjusting the batch size. Step 3, testing the stability of the polishing slurry and selecting polishing slurries that pass the test. Step 4, supplying the selected polishing slurry to the wafer fab production line to ensure the stability of the polishing slurry during production. This invention optimizes the stability of polishing slurries and thereby improves polishing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing semiconductor integrated circuits, and more particularly to a method for optimizing the stability of polishing slurry. Background Technology

[0002] CMP (Continuous Metallurgy Process) requires the use of polishing slurry, which is a mixture of abrasive particles and a chemical solution. CMP achieves the polishing of the film layer on the substrate through both mechanical and chemical actions using the polishing slurry. Therefore, the performance of the polishing slurry has a significant impact on the CMP process. If the polishing slurry is unstable, the CMP process will inevitably be unstable. Thus, the instability of the polishing slurry can have a significant impact on the CMP process, making the optimization and improvement of polishing slurry stability an urgent matter. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide a method for optimizing the stability of polishing slurry, which can optimize the stability of polishing slurry and thereby improve the polishing effect.

[0004] To solve the above-mentioned technical problems, the method for optimizing the stability of grinding slurry provided by the present invention includes: Step 1: Select abrasives based on particle size, distribution, and solid content to ensure that the selected abrasives meet the requirements in terms of particle size, distribution, and solid content.

[0005] Step 2: The selected abrasive particles in a single batch are incorporated into a chemical solution to form the polishing slurry; the abrasive particles have surface charges, and the deviation of the surface charge number of each abrasive particle in the polishing slurry is controlled by the single batch.

[0006] Step 3: Test the stability of the polishing slurry and select the polishing slurry that passes the test.

[0007] Step 4: Supply the selected polishing slurry to the wafer fab production line to ensure the stability of the polishing slurry during production.

[0008] A further improvement is that the abrasive comprises silica sol abrasive.

[0009] A further improvement is that the chemical solution includes: a pH adjuster, a polishing accelerator, and a surfactant.

[0010] A further improvement is that, in the wafer fab, the polishing slurry is used to supply CMP equipment and implement the CMP process.

[0011] A further improvement is that, in the CMP process, the material film layer polished using the polishing slurry includes a silicon oxide layer.

[0012] A further improvement is that, in the CMP process, the silicon oxide layer is formed on the substrate and the substrate is placed on the polishing head, the polishing slurry flows into the surface of the polishing pad, and the polishing head controls the contact between the substrate and the polishing pad and applies pressure and rotation to achieve polishing.

[0013] A further improvement is that, in step three, the test includes the following sub-steps: The CMP process is performed on the test substrate using the polishing slurry.

[0014] After the CMP process is completed, the polishing effect on the test substrate is tested. If the polishing effect meets the requirements, the test result is considered qualified.

[0015] A further improvement is that, during the process of using the line in the wafer fab, the polishing slurry is used to perform the CMP process on the product substrate.

[0016] Before forming the polishing slurry, this invention first selects the abrasive. By selecting the abrasive, it ensures that the particle size, distribution, and solid content of the abrasive do not deviate significantly. Secondly, by using a single batch of abrasive to incorporate into the chemical solution, the deviation of the surface charge number of the abrasive particles can be controlled. The particle size, distribution, and solid content of the abrasive are related to the mechanical polishing performance in the CMP process, while the surface charge number of the abrasive particles is related to the chemical polishing performance in the CMP process. By simultaneously optimizing the particle size, distribution, solid content, and surface charge number of the abrasive, this invention can simultaneously optimize the mechanical and chemical polishing performance in the CMP process. Therefore, this invention can simultaneously optimize the polishing slurry from both mechanical and chemical performance aspects, thus optimizing the overall stability of the polishing slurry and improving the polishing effect, ultimately increasing the product yield. Attached Figure Description

[0017] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments: Figure 1 This is a flowchart of a method for optimizing the stability of grinding fluid according to an embodiment of the present invention; Figure 2 These are photographs of the abrasives selected in the method for optimizing the stability of the grinding fluid in this embodiment of the invention. Figure 3 This is a schematic diagram illustrating the two aspects of the mechanical and chemical effects on the CMP process in the method for optimizing the stability of the grinding fluid according to an embodiment of the present invention. Figure 4 This is a comparison table showing the effects of a single batch of abrasive and a mixed batch of abrasive from existing methods on the mechanical, chemical, and polishing effects of the CMP process, based on the method for optimizing the stability of the polishing slurry according to embodiments of the present invention. Figure 5 This is a schematic diagram of the CMP process being performed in the method for optimizing the stability of the polishing slurry according to an embodiment of the present invention, at the beginning of the CMP process; Figure 6 This is a schematic diagram of the CMP process performed in the method for optimizing the stability of the grinding fluid according to an embodiment of the present invention, and after the CMP process is completed. Detailed Implementation

[0018] like Figure 1 The diagram shown is a flowchart of a method for optimizing the stability of a polishing slurry according to an embodiment of the present invention; the method for optimizing the stability of a polishing slurry according to an embodiment of the present invention includes: Step 1: Select abrasives based on particle size, distribution, and solid content to ensure that the selected abrasives meet the requirements in terms of particle size, distribution, and solid content.

[0019] In this embodiment of the invention, the abrasive includes silica sol abrasive. In other embodiments, other types of abrasives may be selected according to the requirements of the film layer to be ground.

[0020] In this embodiment of the invention, the particle size, distribution, and solid content of the abrasive are related to the mechanical grinding performance in the CMP process. By pre-selecting the abrasive, the deviations in particle size, distribution, and solid content of the abrasive in the subsequently formed grinding slurry can meet the requirements. In this application, the particle size refers to the diameter of the abrasive particles, and the abrasive distribution refers to the distribution of particles of different diameters within the abrasive.

[0021] like Figure 2 The image shown is a photograph of the abrasive selected in the method for optimizing the stability of the grinding fluid according to an embodiment of the present invention. Figure 2 The particles 101 in the text are particles of the abrasive. It can be seen that the particle size of each particle 101 is good and the distribution is uniform.

[0022] Step 2: The selected abrasive particles in a single batch are incorporated into a chemical solution to form the polishing slurry; the abrasive particles have surface charges, and the deviation of the surface charge number of each abrasive particle in the polishing slurry is controlled by the single batch.

[0023] In this embodiment of the invention, the chemical solution includes: a pH adjuster, a polishing accelerator, and a surfactant.

[0024] like Figure 3 The diagram shown illustrates the two aspects of the mechanical and chemical effects on the CMP process in the method for optimizing the stability of the grinding fluid according to an embodiment of the present invention. Figure 3 The diagram shows the mechanical action indicated by label 102 and the chemical action indicated by label 104, which are required for phase equilibrium in CMP.

[0025] Box 103 shows the factors related to mechanical action, namely: the particle size, distribution, and solid content of the abrasive. This is achieved through the preceding step one, namely, selecting the abrasive, for example, optimizing the silica sol abrasive.

[0026] Box 105 shows the factors related to the chemical reaction: abrasive surface charge, pH adjuster, polishing accelerator, and surfactant. The abrasive surface charge is related to the abrasive itself, while the pH adjuster, polishing accelerator, and surfactant are all related to the chemical solution.

[0027] In this embodiment of the invention, step two aims to improve the uniformity of the surface charge on the abrasive, that is, to ensure good uniformity of the surface charge on each particle of the abrasive. This is achieved by using a single batch of the abrasive to form the polishing slurry. Figure 4 The table shown compares the effects of a single batch of abrasive (using the method for optimizing the stability of the polishing slurry according to an embodiment of the present invention) and a mixed batch of abrasive (using existing methods) on the mechanical, chemical, and polishing effects of the CMP process. It can be seen that the curves for the mechanical, chemical, and polishing effects corresponding to a single batch of abrasive show less fluctuation than those corresponding to a mixed batch of abrasive. The chemical effect corresponds to the uniformity of the surface charge of the abrasive; therefore, using a single batch of abrasive can improve the uniformity of the surface charge, ultimately improving the stability of the polishing slurry.

[0028] Step 3: Test the stability of the polishing slurry and select the polishing slurry that passes the test.

[0029] Step 4: Supply the selected polishing slurry to the wafer fab production line to ensure the stability of the polishing slurry during production.

[0030] In this embodiment of the invention, in the wafer fab, the polishing slurry is used to supply CMP equipment for use in implementing the CMP process.

[0031] In the CMP process, the material film layer polished using the polishing slurry includes a silicon oxide layer.

[0032] In the CMP process, the silicon oxide layer is formed on a substrate, and the substrate is placed on a polishing head. The polishing slurry flows onto the surface of the polishing pad. The polishing head controls the contact between the substrate and the polishing pad, applying pressure and rotation to achieve polishing. Figure 5The diagram shown is a schematic representation of the CMP process performed in the method for optimizing the stability of the polishing slurry according to an embodiment of the present invention, specifically at the beginning of the CMP process. Mark 201 indicates the surface of the silicon oxide layer formed on the substrate that needs to be polished; the circle corresponding to mark 202 represents the particles of the abrasive; and mark 203 represents the surface of the polishing pad. It can be seen that at the beginning of the CMP process, the surface corresponding to mark 201 is uneven. Figure 5 The molecular structures of the silicon oxide layer and the abrasive are also shown. Figure 6 The diagram shown is a schematic of the CMP process performed in the method for optimizing the stability of the polishing slurry according to an embodiment of the present invention, and after the CMP process is completed; it can be seen that after the CMP process is completed, the surface corresponding to mark 201 is flat.

[0033] In some embodiments, step three above includes the following sub-steps: The CMP process is performed on the test substrate using the polishing slurry.

[0034] After the CMP process is completed, the polishing effect on the test substrate is tested. If the polishing effect meets the requirements, the test result is considered qualified.

[0035] In this embodiment of the invention, during the process of using the polishing slurry on the production line of the wafer fab, the polishing slurry is used to perform the CMP process on the product substrate.

[0036] Before forming the polishing slurry, the present invention first selects the abrasive. By selecting the abrasive, it ensures that the particle size, distribution, and solid content of the abrasive do not deviate significantly. Secondly, a single batch of abrasive is incorporated into the chemical solution. Using a single batch of abrasive allows for control of the deviation in the surface charge number of the abrasive particles. The particle size, distribution, and solid content of the abrasive are related to the mechanical polishing performance in the CMP process, while the surface charge number of the abrasive particles is related to the chemical polishing performance in the CMP process. By simultaneously optimizing the particle size, distribution, solid content, and surface charge number of the abrasive, the present invention can simultaneously optimize the mechanical and chemical polishing performance in the CMP process. Therefore, the present invention can simultaneously optimize the polishing slurry from both mechanical and chemical performance aspects, thus optimizing the overall stability of the polishing slurry and improving the polishing effect, ultimately increasing the product yield.

[0037] This invention optimizes the polishing effect and improves the stability of the polishing slurry by optimizing the selection of polishing slurry raw materials, standardizing batches of silica sol abrasives, and reducing particle distribution and charge deviation on particles. Using an oxide polishing slurry as an example, the optimized oxide polishing slurry significantly improves both offline and online stability, resulting in increased product yield.

[0038] The present invention has been described in detail above through specific embodiments, but these are not intended to limit the invention. Many modifications and improvements can be made by those skilled in the art without departing from the principles of the invention, and these should also be considered within the scope of protection of the present invention.

Claims

1. A method of optimizing stability of a polishing liquid, characterized by, include: Step 1: Select abrasives based on particle size, distribution, and solid content to ensure that the selected abrasives meet the requirements in terms of particle size, distribution, and solid content. Step 2: The selected abrasive particles in a single batch are incorporated into a chemical solution to form the polishing slurry; the abrasive particles have surface charges, and the deviation of the surface charge number of each particle in the polishing slurry is controlled by the single batch. Step 3: Test the stability of the polishing slurry and select the polishing slurry that passes the test; Step 4: Supply the selected polishing slurry to the wafer fab production line to ensure the stability of the polishing slurry during production.

2. The method of polishing fluid stability optimization of claim 1, wherein: The abrasive includes silica sol abrasive.

3. The method of polishing fluid stability optimization of claim 1, wherein: The chemical solution includes: pH adjuster, polishing accelerator, and surfactant.

4. The method of polishing fluid stability optimization of claim 2, wherein: In the wafer fab, the polishing slurry is used to supply CMP equipment and implement the CMP process.

5. The method of polishing fluid stability optimization of claim 4, wherein: In the CMP process, the material film layer polished using the polishing slurry includes a silicon oxide layer.

6. The method of polishing fluid stability optimization of claim 5, wherein: In the CMP process, the silicon oxide layer is formed on the substrate and the substrate is placed on the polishing head. The polishing slurry flows into the surface of the polishing pad. The polishing head controls the contact between the substrate and the polishing pad and applies pressure and rotation to achieve polishing.

7. The method of polishing fluid stability optimization of claim 6, wherein: Step three includes the following sub-steps: The CMP process is performed on the test substrate using the polishing slurry. After the CMP process is completed, the polishing effect on the test substrate is tested. If the polishing effect meets the requirements, the test result is considered qualified.