A high-temperature resistant and flame-retardant polyester fabric-based adhesive tape and its preparation method

By setting a flame-retardant anchoring base coating and an organosilicon pressure-sensitive adhesive layer on a polyester fabric substrate, and combining phosphate-modified polyurethane and expandable graphite electron beam irradiation crosslinking technology, the problem of easy combustion of polyester fabric-based tape at high temperatures is solved, achieving halogen-free flame retardancy and maintaining peel strength at high temperatures, thus achieving a V-0 flame retardant rating.

CN123107559APending Publication Date: 2026-11-17YANZHOU (JIANGSU) ADHESIVE PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611350226.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyester fabric-based tapes are easily flammable in high-temperature or open-flame environments, failing to meet the flame-retardant safety requirements of wiring harnesses for electronic and electrical equipment and new energy vehicles. Furthermore, the use of flame retardants in existing technologies leads to a decrease in the cohesive strength and peel strength of the adhesive layer. Additionally, halogen-free flame retardants have poor compatibility with silicone pressure-sensitive adhesives, making them prone to migration and precipitation, and the undercoating layer cannot form an effective flame-retardant barrier.

Method used

The flame-retardant anchoring base coating is composed of phosphate-modified polyurethane, ammonium polyphosphate, melamine cyanurate and isocyanate curing agent. It is combined with an organosilicon pressure-sensitive adhesive layer, expandable graphite and fumed silica, and cross-linked by electron beam irradiation to form an adhesive layer with a gel mass fraction of not less than 80%, forming a flame-retardant anchoring barrier and an adhesive layer structure that is stable at high temperature.

Benefits of technology

It achieves halogen-free flame retardancy of the tape, with a vertical burning rating of V-0 and a peel strength retention rate of no less than 85% in an environment of 150℃. It solves the problems of decreased cohesive strength and peel strength attenuation of the adhesive layer at high temperatures, and improves the flame retardancy consistency and mechanical properties of the adhesive layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107559A_ABST
    Figure CN123107559A_ABST
Patent Text Reader

Abstract

This invention discloses a high-temperature resistant, flame-retardant polyester fabric-based adhesive tape and its preparation method, belonging to the field of adhesive tape technology. The tape includes a polyester fabric substrate layer, with a flame-retardant anchoring primer layer and an organosilicon pressure-sensitive adhesive layer sequentially disposed on one side of the polyester fabric substrate layer. The flame-retardant anchoring primer layer is formed by curing a primer liquid composed of phosphate-modified polyurethane, ammonium polyphosphate, melamine cyanurate, isocyanate curing agent, and organic solvent. The preparation method includes: preparing the primer liquid and applying it to the surface of the polyester fabric substrate layer, drying and curing to form the primer layer; preparing the adhesive composition, applying it to the surface of the primer layer, and drying it in sections to form the adhesive layer; subjecting the adhesive layer to electron beam irradiation crosslinking, followed by winding, curing, and slitting to obtain the finished product. This invention achieves halogen-free flame retardancy, high temperature resistance, and high peel strength retention in the tape through the synergistic flame-retardant design of the primer layer and adhesive layer, electron beam irradiation crosslinking enhancement, and sectioned drying process, making it suitable for electronic and electrical insulation wrapping and automotive wiring harness fixing and sealing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of adhesive tape technology, and in particular to a high-temperature resistant, flame-retardant polyester fabric-based adhesive tape and its preparation method. Background Technology

[0002] Polyester fabric-based tapes are widely used for insulation and sealing in fields such as electronics, automotive wiring harnesses, and building decoration due to their excellent mechanical properties, dimensional stability, and cost advantages. However, the base material and adhesive layer of ordinary polyester fabric-based tapes are both flammable materials with poor flame retardant properties. They are prone to burning and dripping in high-temperature or open-flame environments, failing to meet the stringent flame-retardant safety requirements of electronic and electrical equipment and new energy vehicle wiring harnesses.

[0003] Existing flame-retardant fabric-based tapes typically add large amounts of halogenated flame retardants to the substrate or adhesive layer. While this achieves a certain flame-retardant effect, it releases toxic and harmful gases and corrosive fumes during combustion, failing to meet environmental regulations. In halogen-free flame-retardant technologies, excessive addition of inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide leads to decreased cohesive strength and peel strength of the adhesive layer. Furthermore, these agents have poor compatibility with silicone pressure-sensitive adhesives, easily migrating and precipitating, resulting in insufficient tape durability.

[0004] Existing base coats for cloth-based adhesive tapes typically only enhance adhesion and do not provide flame retardancy. When flames penetrate from the edge of the adhesive layer or the back of the substrate, the base coat fails to form an effective flame-retardant barrier, allowing the flames to rapidly penetrate the substrate and cause the entire layer to fail. Current methods have not established a base coat system that combines flame retardancy and anchoring properties.

[0005] Existing silicone pressure-sensitive adhesive layers are typically crosslinked using thermosetting or room-temperature vulcanization methods, resulting in limited crosslinking density and low gel mass fraction. In high-temperature environments above 150°C, silicone molecular chains are prone to slippage and creep, causing a sharp decrease in the cohesive strength of the pressure-sensitive adhesive. This leads to severe attenuation of the tape's peel strength, loss of holding power, and a short high-temperature protective lifespan.

[0006] Existing methods for laminating expandable graphite with silicone pressure-sensitive adhesives typically employ simple mechanical mixing. However, expandable graphite has low density and a hydrophobic surface, resulting in weak interfacial bonding with the silicone matrix, uneven dispersion, and a tendency to form agglomerates and defects in the adhesive layer, affecting the mechanical properties and flame retardant consistency of the layer. Current methods do not utilize additives such as fumed silica to improve the dispersion stability of expandable graphite.

[0007] Current electron beam irradiation crosslinking technology for pressure-sensitive adhesives typically does not optimize the absorbed dose. Insufficient dose results in low crosslinking degree and limited improvement in high-temperature performance; excessive dose leads to breakage and degradation of the silicone backbone, causing the adhesive layer to become brittle and reducing initial tack and peel strength. Existing methods have not established a matching relationship between absorbed dose, gel mass fraction, and high-temperature peel strength retention. Summary of the Invention

[0008] Therefore, embodiments of the present invention provide a high-temperature resistant, flame-retardant polyester fabric-based adhesive tape and its preparation method.

[0009] On the one hand, a high-temperature resistant flame-retardant polyester fabric-based tape is provided, including a polyester fabric substrate layer, wherein a flame-retardant anchoring primer layer and an organosilicon pressure-sensitive adhesive layer are sequentially disposed on one side of the polyester fabric substrate layer;

[0010] The flame-retardant anchoring primer is formed by curing a primer liquid on the surface of the polyester fabric substrate layer. The primer liquid comprises, by weight, 45-65 parts of phosphate ester modified polyurethane, 15-25 parts of ammonium polyphosphate, 8-15 parts of melamine cyanurate, 1-4 parts of isocyanate curing agent and 40-70 parts of organic solvent.

[0011] The silicone pressure-sensitive adhesive layer is formed by curing the adhesive composition on the surface of the flame-retardant anchoring base coating and cross-linking it under electron beam irradiation. The adhesive composition includes 100 parts of silicone pressure-sensitive adhesive, 8-20 parts of expandable graphite and 3-8 parts of fumed silica by weight.

[0012] The gel mass fraction of the silicone pressure-sensitive adhesive layer is not less than 80%.

[0013] On the other hand, a method for preparing high-temperature resistant flame-retardant polyester fabric-based adhesive tape is also proposed, including the following steps.

[0014] Step 1: Dissolve the phosphate-modified polyurethane in an organic solvent, add ammonium polyphosphate, melamine cyanurate and isocyanate curing agent, stir and disperse evenly, filter to obtain the primer liquid;

[0015] Step 2: Apply the primer liquid to one side of the polyester fabric substrate layer, dry and cure to form a flame-retardant anchoring primer coating.

[0016] Step 3: Mix the silicone pressure-sensitive adhesive, expandable graphite and fumed silica, stir and disperse evenly to obtain the adhesive composition;

[0017] Step 4: Apply the adhesive composition to the surface of the flame-retardant anchoring base coating, and dry it in sections to form an adhesive layer;

[0018] Step 5: The adhesive layer is cross-linked by electron beam irradiation, wound up, cured, and cut to obtain the high-temperature resistant flame-retardant polyester fabric-based adhesive tape.

[0019] Beneficial effects

[0020] The beneficial effects of the technical solutions provided in the embodiments of the present invention include at least the following:

[0021] This invention solves the technical problem of poor flame retardant properties of ordinary cloth-based tapes in the prior art, which cannot meet the flame retardant safety requirements in the fields of electronics, electrical engineering, and automotive wiring harnesses. It achieves the technical effect of halogen-free flame retardancy of the tape and a vertical burning rating of V-0 through the synergistic flame retardancy of the base coating and adhesive layer. The flame retardant anchoring base coating is formed by curing a primer liquid composed of phosphate ester modified polyurethane, ammonium polyphosphate, melamine cyanurate, isocyanate curing agent and organic solvent. The silicone pressure-sensitive adhesive layer is formed by curing an adhesive composition composed of silicone pressure-sensitive adhesive, expandable graphite and fumed silica and undergoing electron beam irradiation cross-linking.

[0022] This invention uses phosphate-modified polyurethane as the film-forming material in the flame-retardant anchoring base coating. The mass of the phosphate polyol accounts for 10% to 20% of the sum of the mass of the polyester polyol and the phosphate polyol. Ammonium polyphosphate and melamine cyanurate are used as flame-retardant synergists. This solves the technical problem in the prior art where the base coating only enhances adhesion and does not impart flame-retardant function, resulting in easy flame penetration of the substrate. It achieves the technical effect of forming a flame-retardant anchoring barrier on the substrate surface through the synergistic effect of the phosphate-modified polyurethane film-forming material and the intumescent flame retardant.

[0023] This invention utilizes an organosilicon pressure-sensitive adhesive layer formed by the condensation of hydroxyl-terminated polydimethylsiloxane and MQ silicone resin, with a mass ratio of MQ silicone resin to hydroxyl-terminated polydimethylsiloxane of 1.2–1.8:1. Expandable graphite and fumed silica are added to the adhesive composition. After crosslinking by electron beam irradiation, the gel mass fraction is not less than 80%. This invention solves the technical problems of limited crosslinking density and severe peel strength attenuation caused by molecular chain slippage at high temperatures in existing organosilicon pressure-sensitive adhesives. It achieves the technical effects of increasing the gel mass fraction through electron beam irradiation crosslinking, enhancing cohesive strength through MQ silicone resin, and maintaining a peel strength retention rate of not less than 85% after being placed in an environment of 150°C for 500 hours.

[0024] This invention improves the dispersion stability of expandable graphite in organosilicon pressure-sensitive adhesives by adding fumed silica to the adhesive composition and utilizing the thickening and thixotropic effects of fumed silica. This solves the technical problems of weak interfacial bonding between expandable graphite and organosilicon matrix, uneven dispersion, and easy formation of agglomerates and defects in the prior art. It achieves the technical effect of improving the flame retardant consistency and mechanical properties of the adhesive layer through synergistic dispersion of fumed silica.

[0025] This invention addresses the technical problems in existing technologies, such as the mismatch between the expansion temperature of expandable graphite and the temperature resistance of organosilicon pressure-sensitive adhesives, and insufficient cross-linking or main chain breakage due to unoptimized electron beam dose. These problems are achieved by using expandable graphite with an initial expansion temperature of 180–220℃, an expansion ratio of 200–300 mL / g, a particle size of 50–150 μm, and an absorbed dose of 40–80 kGy for electron beam irradiation cross-linking. The invention achieves the technical effect of forming a heat-insulating carbon layer by expanding expandable graphite before organosilicon softens, and balancing the degree of cross-linking and mechanical properties by optimizing the irradiation dose.

[0026] This invention solves the technical problem in the prior art where one-time high-temperature drying leads to excessive solvent evaporation, forming bubbles or surface skin, by using segmented drying, including a first drying stage at 70-90°C, a second drying stage at 100-120°C, and a third drying stage at 130-150°C, with a curing temperature of 40-60°C and a time of 48-72 hours. It achieves the technical effects of achieving gradient solvent evaporation through segmented drying, releasing residual stress through low-temperature long-term curing, and improving the density of the adhesive layer and the adhesion of the interface. Attached Figure Description

[0027] Figure 1 A flowchart provided for an embodiment of this application. Detailed Implementation

[0028] To make the technical problems, technical solutions and advantages of the present invention clearer, a detailed description will be given below in conjunction with the accompanying drawings and specific embodiments.

[0029] like Figure 1 As shown, a high-temperature resistant and flame-retardant polyester fabric-based tape includes a polyester fabric substrate layer, wherein a flame-retardant anchoring primer layer and an organosilicon pressure-sensitive adhesive layer are sequentially disposed on one side of the polyester fabric substrate layer.

[0030] The flame-retardant anchoring primer is formed by curing a primer liquid on the surface of the polyester fabric substrate layer. The primer liquid comprises, by weight, 45-65 parts of phosphate ester modified polyurethane, 15-25 parts of ammonium polyphosphate, 8-15 parts of melamine cyanurate, 1-4 parts of isocyanate curing agent and 40-70 parts of organic solvent.

[0031] The silicone pressure-sensitive adhesive layer is formed by curing the adhesive composition on the surface of the flame-retardant anchoring base coating and cross-linking it under electron beam irradiation. The adhesive composition includes 100 parts of silicone pressure-sensitive adhesive, 8-20 parts of expandable graphite and 3-8 parts of fumed silica by weight.

[0032] The gel mass fraction of the silicone pressure-sensitive adhesive layer is not less than 80%.

[0033] It should be noted that the wiring harness in the engine compartment of a car is in a high-temperature environment of 150°C for a long time. Existing polyester cloth-based tape has three problems in this environment: First, the small molecular components in the adhesive layer migrate to the interface between the substrate and the adhesive layer when heated, leaving adhesive residue after being torn off; second, both the substrate and the adhesive layer are flammable organic materials, which continue to burn when exposed to an open flame; and third, the cohesive strength of the adhesive layer decreases at high temperatures, causing the wiring harness to loosen at the binding points. The various layers of this invention address the aforementioned problems: Phosphate-modified polyurethane decomposes upon heating to generate polyphosphoric acid, catalyzing the dehydration of polyester fibers and film-forming resin into carbon; melamine cyanurate sublimates upon heating and decomposes to release non-flammable gases, diluting the concentration of combustible gases and oxygen. These two components form a phosphorus-nitrogen synergistic system, solving the flame retardancy problem; the phosphate groups in the phosphate-modified polyurethane interact with the ester groups on the polyester surface, forming an anchoring interface between the substrate and the adhesive layer in the flame-retardant anchoring base coating, inhibiting the migration of small molecules in the adhesive layer at high temperatures, thus solving the residue problem; the main chain of the organosilicon pressure-sensitive adhesive is a silicon-oxygen bond, which, combined with the three-dimensional network formed by electron beam irradiation crosslinking, prevents creep flow in the adhesive layer at 150°C when the gel mass fraction is not less than 80%, solving the high-temperature adhesion problem; expandable graphite expands upon heating and forms a carbon layer on the adhesive layer surface, blocking heat transfer to the interior of the adhesive layer and delaying thermal failure; fumed silica forms a thixotropic structure in the adhesive composition, inhibiting the sedimentation of expandable graphite before coating. (Gel mass fraction) The determination method is as follows: Take the irradiated adhesive layer sample, reflux extract with toluene for 24 h, dry at 80 °C for 4 h to constant weight, and the gel mass fraction is the mass of insoluble matter after extraction. Compared with the sample mass before extraction The ratio, i.e. The weight percentages of each component in the primer are determined by calculating the mass fraction of phosphorus in the primer layer: Mass fraction of phosphorus in the primer layer. According to the formula Calculate, where This refers to the total mass fraction of the primer solids, specifically the weight fraction of the phosphate-modified polyurethane. Ammonium polyphosphate (parts by weight) 1 part by weight of melamine cyanurate With isocyanate curing agent (parts by weight) The sum, with a coefficient of 0.32, represents the mass fraction of phosphorus in ammonium polyphosphate, calculated from the ratio of the relative atomic mass of phosphorus (31) to the relative molecular mass (97) of the repeating unit in ammonium polyphosphate. The coefficient 0.02 represents the representative value of the mass fraction of phosphorus in phosphate-modified polyurethane, the calculation process of which is given in the primer composition refinement section; substituting the values ​​results in the combination that minimizes the mass fraction of phosphorus. , , , Calculated Substitute the combination that yields the highest mass fraction of phosphorus. , , , Calculated When the mass fraction of phosphorus in the base coating is in the range of 6.9% to 10.0%, the afterburning time of the tape after two fire removals, measured by the vertical burning method, does not exceed 10 seconds, and no dripping material ignites the degreased cotton.

[0034] As an optional embodiment, the polyester fabric substrate layer is woven from polyester low-elasticity yarn with a linear density of 8-12 tex, a warp density of 300-420 threads / 10cm, a weft density of 300-420 threads / 10cm, a weight of 60-110 g / m², and a thickness of 0.10-0.18 mm.

[0035] The polyester fabric substrate layer undergoes heat setting treatment at a temperature of 170–200°C for 30–90 seconds.

[0036] It should be noted that the weight is calculated based on weaving parameters, and the number of warp threads within a 1m width is the warp density. 10 times, The unit is threads / 10cm, the length of a single warp yarn is 1m, and the warp yarn linear density is... The unit is tex, which is the weight in grams per kilometer of yarn. Therefore, the total weight of all warp yarns within 1 m² is... g, and similarly, the total mass of all weft yarns is g. g, For dense latitude, Weft yarn linear density, weight per gram That is, according to the formula Calculations were performed; substituting both warp and weft density as 360 yarns / 10cm and warp and weft linear density as 10tex, the calculated basis weight was 72g / m², falling within the 60-110g / m² range. The endpoints of this basis weight range correspond to two types of failure scenarios: below 60g / m², the substrate's mechanical strength is insufficient, leading to breakage under binding tension; above 110g / m², the tape's flexibility decreases, making it unable to adhere to the irregular curved surfaces of the yarn bundle; the 60-110g / m² range balances binding strength and adhesion. The heat setting temperature was determined as follows: polyester's glass transition temperature is 78-81℃, and its melting point is 255-260℃. The heat setting temperature must be higher than the glass transition temperature to allow molecular chain rearrangement and crystallization, while simultaneously being lower than the melting point to prevent fiber agglomeration; within the 170-200℃ range, the warp thermal shrinkage rate of the substrate was measured to be less than 2%, ensuring no shrinkage or loosening at the binding point during service.

[0037] As an optional embodiment, the phosphate-modified polyurethane is prepared by polycondensation of polyester polyol, diisocyanate and phosphate polyol, wherein the mass of the phosphate polyol accounts for 10% to 20% of the sum of the mass of the polyester polyol and the phosphate polyol;

[0038] The organic solvent is a mixture of butanone and toluene;

[0039] The isocyanate curing agent is hexamethylene diisocyanate trimer.

[0040] It should be noted that the mass fraction of phosphorus in phosphate-modified polyurethane... Equal to the mass fraction of phosphorus in phosphate ester polyols The proportion of phosphate ester polyols The product of, i.e. ; The mass percentage of phosphoric acid in the feed for the preparation of phosphate ester polyols is calculated to be 16%. The ratio of phosphate ester polyol to the sum of the masses of polyester polyol and phosphate ester polyol is substituted into... The interval endpoints 10% and 20% are calculated as follows: The phosphorus content ranges from 1.6% to 3.2%, and the representative value of 2% for phosphorus in phosphate-modified polyurethane in the aforementioned calculation of the phosphorus content of the base coating falls within this range. The endpoints of the phosphate polyol content are inferred from the failure scenarios: when the content is below 10%, the amount of polyphosphoric acid released by the resin decomposition upon heating is insufficient, the char-forming catalytic effect is weak, and the flame-retardant effect of the base coating fails; when the content is above 20%, the proportion of flexible ester segments in the resin main chain decreases, the base coating becomes brittle, and cracks during winding and slitting; within the 10% to 20% range, the char-forming catalytic ability and anchoring strength of the base coating are simultaneously established. The selection of methyl ethyl ketone (MEK) and toluene as organic solvents is based on the following: both MEK and toluene have the ability to dissolve phosphate-modified polyurethane; MEK has a boiling point of 79.6℃, and toluene has a boiling point of 110.6℃. The boiling points of the two solvents are offset, and the solvents evaporate in stages during the drying process, preventing the base coating surface from forming a skin. The basis for selecting hexamethylene diisocyanate trimer as the isocyanate curing agent is as follows: the isocyanate group in the trimer structure has a functionality of 3, which reacts with the hydroxyl groups in the polyurethane to form a three-dimensional cross-linked network, and the primer does not soften at the service temperature of 150℃.

[0041] As an optional embodiment, the solid content of the primer is 35% to 50%;

[0042] The dry film thickness of the flame-retardant anchoring primer is 6–15 μm.

[0043] It should be noted that: dry film thickness Equal to the dry base coating amount of the primer With the dry film density of the base coating The ratio, i.e. , The unit is g / m², and the dry coating amount is the product of the wet coating amount and the solid content. The density of each component in the base coating, weighted by mass fraction, is 1.3 g / cm³; substituting... The values ​​are 8.8 g / m² and 20 g / m², respectively. The thicknesses are 6.8 μm and 15.4 μm, respectively, with a dry film thickness ranging from 6 to 15 μm. The determination of the solid content range is based on the following: when the solid content is below 35%, the dry film deposition in a single coating cannot reach the lower limit of the dry film thickness, requiring repeated coating; when the solid content is above 50%, the viscosity of the primer increases, resulting in insufficient leveling after coating and thickness deviation in the primer layer. The endpoints of the dry film thickness also correspond to failure scenarios: below 6 μm, the total amount of flame retardant in the primer layer is insufficient, and the afterflame time in the vertical burning test exceeds 10 seconds; above 15 μm, the overall flexibility of the tape decreases, and the edges curl up when wrapping the wire harness; the 6–15 μm range achieves a balance between the total amount of flame retardant and the wrapability of the tape.

[0044] As an optional embodiment, the silicone pressure-sensitive adhesive is formed by the condensation of hydroxyl-terminated polydimethylsiloxane and MQ silicone resin, wherein the mass ratio of MQ silicone resin to hydroxyl-terminated polydimethylsiloxane is 1.2 to 1.8:1.

[0045] It should be noted that: with This indicates the mass ratio of MQ silicone resin to hydroxyl-terminated polydimethylsiloxane; the endpoints of the range are determined experimentally. When the ratio is less than 1.2:1, the cohesive strength of the adhesive layer is insufficient, and creep slippage occurs in the adhesive layer during the 150℃ holding test; When the ratio is greater than 1.8:1, the initial adhesion of the adhesive layer decreases, the 180° peel strength is less than 6N / 25mm, and curling occurs when wrapping the wire harness; When the ratio is in the range of 1.2 to 1.8:1, the tack performance at 150°C and the peel strength at 180°C simultaneously meet the requirements for wire harness bundling. This mass ratio is crucial because the silanol groups of hydroxyl-terminated polydimethylsiloxane and MQ silicone resin condense under heating conditions to form a cross-linked structure with silicon-oxygen-silicon bonds as the main chain. The bond energy of the silicon-oxygen bond is 460 kJ / mol, which is higher than the carbon-carbon bond energy of 348 kJ / mol. This bond energy difference ensures that the main chain of the adhesive layer does not break at the service temperature of 150°C, which is the structural basis for the high-temperature resistance of the tape.

[0046] As an optional embodiment, the expandable graphite has an initial expansion temperature of 180–220°C, an expansion ratio of 200–300 mL / g, and a particle size of 50–150 μm.

[0047] It should be noted that the mass of expandable graphite per unit area of ​​the adhesive layer is... According to the formula Accounting, in the formula This refers to the thickness of the carbon layer formed after expandable graphite expands due to heat. For a unit area of ​​1m², The expansion ratio of expandable graphite is given; the lower limit of the carbon layer thickness (1.2 mm) is determined by the back temperature test, and the temperature on the back of the tape tends to stabilize when the carbon layer thickness reaches 1.2 mm; the upper limit of the carbon layer thickness (2.5 mm) is determined by the initial tack test, and the initial tack of the adhesive layer decreases when it exceeds 2.5 mm; substituting... mm mL / g, calculated g / m², substitute into mm mL / g, calculated The adhesive layer density is 58 g / m², which translates to 6.9–21.6 parts of expandable graphite per 100 parts by weight of silicone pressure-sensitive adhesive. Based on the initial tack retention test results, the expandable graphite weight is estimated to be 8–20 parts. The initial expansion temperature range is derived as follows: the long-term service temperature of automotive engine compartment wiring harnesses is 150℃, and the initial expansion temperature must be higher than 150℃ to prevent premature expansion of expandable graphite during service, which could damage the adhesive layer structure. Simultaneously, it must be lower than the melting point of polyester, 255℃. Thermogravimetric analysis shows that the initial expansion temperature range of expandable graphite meeting these conditions is 180–220℃. The particle size and dosage are related: the expandable graphite particle size is larger than the dry film thickness of the adhesive layer. The expanded graphite worms extend along the thickness direction and are anchored in the carbon layer. The particle size of 50-150μm matches the dry film thickness of 40-70μm of the adhesive layer. The carbon layer completely covers the surface of the adhesive layer. The heat of the external flame is blocked by the carbon layer. The internal temperature of the adhesive layer is lower than its failure temperature. Flame retardancy and adhesion retention are achieved simultaneously.

[0048] As an optional embodiment, the absorbed dose of the electron beam irradiation crosslinking is 40–80 kGy.

[0049] It should be noted that the determination of the absorbed dose range is based on the following: When the absorbed dose is below 40 kGy, the gel mass fraction measured by the aforementioned toluene reflux extraction method is below 80%, the cross-linked network of the adhesive layer is incomplete, and cohesive failure occurs during the 150°C holding strength test; when the absorbed dose is above 80 kGy, the polyester molecular chains undergo irradiation degradation, the substrate tensile strength retention rate is below 85%, and the substrate breaks under binding tension; when the absorbed dose is in the range of 40–80 kGy, both the gel mass fraction and the substrate tensile strength retention rate meet the requirements. The significance of the dose window is to limit the degree of irradiation cross-linking to the balance point between the cohesive strength of the adhesive layer and the mechanical strength of the substrate, so that the high-temperature holding strength and binding strength of the tape are both achieved, without sacrificing the strength of the substrate in pursuit of cross-linking density.

[0050] As an optional embodiment, the dry film thickness of the silicone pressure-sensitive adhesive layer is 40–70 μm;

[0051] The tape has a 180° peel strength of 6-12 N / 25 mm against the steel plate, a vertical burning rating of V-0, and a peel strength retention rate of no less than 85% after being placed in an environment of 150°C for 500 hours.

[0052] It should be noted that: the test method for vertical flammability rating is as follows: A 125mm × 13mm sample is applied to the lower end of the sample for 10 seconds, then removed. The afterflame time and whether the dripping material ignites the cotton 300mm below are recorded. The flame is applied again for 10 seconds, and the recording is repeated. If the afterflame time does not exceed 10 seconds after both removals and no dripping material ignites the cotton, it is recorded as V-0. The test method for 180° peel strength is as follows: Using a 304 stainless steel plate as the test plate, the peel angle is 180°, the tensile speed is 300mm / min, and 5 samples are tested in each group, with the average value taken. Adhesive layer dry film thickness. Equal to the dry coating amount of the adhesive composition With adhesive layer density The ratio, i.e. , It is 1.05 g / cm³, substitute into The concentration is 42–74 g / m², resulting in a dry film thickness of 40–70 μm. Peel strength retention rate. This is the ratio of the peel strength after aging to the peel strength before aging, i.e. , The peel strength at 180° after being placed in an environment of 150°C for 500 hours. The peel strength is 180° before aging. The above performance indicators correspond to the long-term service conditions of automotive engine compartment wiring harnesses: when the peel strength retention rate is not less than 85% under aging conditions of 150℃ and 500h, the tape will not delaminate during the service life of the entire vehicle, and the flame retardant, anchoring and temperature resistance effects of each layer structure are thus unified into verifiable product performance.

[0053] As an optional embodiment, the following steps are included.

[0054] Step 1: Dissolve the phosphate-modified polyurethane in an organic solvent, add ammonium polyphosphate, melamine cyanurate and isocyanate curing agent, stir and disperse evenly, filter to obtain the primer liquid;

[0055] Step 2: Apply the primer liquid to one side of the polyester fabric substrate layer, dry and cure to form a flame-retardant anchoring primer coating.

[0056] Step 3: Mix the silicone pressure-sensitive adhesive, expandable graphite and fumed silica, stir and disperse evenly to obtain the adhesive composition;

[0057] Step 4: Apply the adhesive composition to the surface of the flame-retardant anchoring base coating, and dry it in sections to form an adhesive layer;

[0058] Step 5: The adhesive layer is cross-linked by electron beam irradiation, wound up, cured, and cut to obtain the high-temperature resistant flame-retardant polyester fabric-based adhesive tape.

[0059] It should be noted that the steps are connected as follows: In step one, the phosphate-modified polyurethane is added before the flame-retardant powder. After the resin is fully dissolved, ammonium polyphosphate and melamine cyanurate are dispersed to avoid powder agglomeration. A 200-300 mesh filter is used to remove undispersed particles, preventing defects in the flame-retardant anchoring base coating. In step two, the drying and curing temperature is 90-120℃. This temperature range is higher than the boiling point of methyl ethyl ketone (79.6℃) and toluene (110.6℃), allowing the organic solvent to completely evaporate and the isocyanate groups and hydroxyl groups to complete the cross-linking reaction. It is also lower than the lower limit of the heat-setting temperature (170℃), ensuring no change in the substrate dimensions. In step three, expandable graphite is added after the silicone pressure-sensitive adhesive, and fumed silica is added last, utilizing its thixotropic structure to inhibit the sedimentation of expandable graphite. In step five, electron beam irradiation cross-linking is completed before winding, ensuring the absorbed dose is evenly applied to the adhesive layer. Curing is performed after winding, releasing the internal stress of the adhesive layer. The order of each step in this method corresponds one-to-one with the formation order of the product structure. The anchoring interface is formed first, and then the adhesive layer is formed, ensuring that the anchoring effect of the base layer is not destroyed during the adhesive application process.

[0060] As an optional embodiment, the segmented drying includes a first drying segment, a second drying segment, and a third drying segment performed sequentially;

[0061] The temperature of the first drying section is 70-90℃, the temperature of the second drying section is 100-120℃, and the temperature of the third drying section is 130-150℃;

[0062] The ripening temperature is 40–60°C, and the time is 48–72 hours.

[0063] It should be noted that the segmented drying temperature range is derived as follows: the solvent in the adhesive composition is toluene, with a boiling point of 110.6℃; the temperature of the first drying stage is below the boiling point of toluene, allowing the solvent below the surface to slowly migrate to the surface, preventing surface skinning and blistering; the temperature of the second drying stage exceeds the boiling point of toluene, serving as the main volatile stage, where the solvent fully evaporates; the temperature of the third drying stage is 130–150℃, removing residual solvent and promoting the initial condensation of hydroxyl-terminated polydimethylsiloxane with the silanol groups of MQ silicone resin. The curing temperature and time are determined based on the following: curing homogenizes the cross-linked network formed by electron beam irradiation and releases the internal stress generated during coating and winding; the curing time of 48–72 h is measured from the time required for the peel strength to reach a stable value; the curing temperature of 40–60℃ is higher than the ambient temperature of the workshop but lower than the flow temperature of the adhesive layer, ensuring that the adhesive layer does not overflow during winding. After adopting the above drying and curing conditions, no air bubbles are generated inside the adhesive layer, the peel strength test data has small dispersion, the bonding performance of the tape is consistent throughout, and there are no local delamination points after the wire harness is bundled.

[0064] The technical solution of the present invention will be described in detail below with reference to the embodiments. The scope of protection of the present invention is not limited to the following embodiments. The raw materials used in the following embodiments are all commercially available industrial-grade products, and the performance test data are the average values ​​of 5 samples.

[0065] Phosphate-modified polyurethane was prepared as follows: Polybutylene adipate diol and phosphate polyol were added to a reaction vessel. The hydroxyl value of polybutylene adipate diol was 56 mg KOH / g, and the phosphate polyol was prepared by esterification of phosphoric acid with trimethylolpropane, with a hydroxyl value of 280 mg KOH / g and a phosphorus element mass fraction of 16%. The temperature was raised to 75–85 °C, and isophorone diisocyanate was added dropwise. The molar ratio of isocyanate groups to hydroxyl groups was 0.9:1. Simultaneously, diisocyanate was added... Dibutyltin lauryl ester was used as a catalyst at a concentration of 0.05% of the total mass of the reactants. After the addition was complete, the reaction was maintained at a constant temperature for 3 hours, and then the temperature was raised to 90°C for another 2 hours. The isocyanate group content was measured, and the material was cooled and discharged when the content dropped below 0.5%. Hydroxyl-terminated phosphate-modified polyurethane was obtained, with a viscosity of 8000–12000 mPa·s at 25°C. The proportions of phosphate polyol to the sum of the masses of polybutylene adipate diol and phosphate polyol in each example are given.

[0066] Example 1;

[0067] Weigh 55 kg of the phosphate-modified polyurethane prepared according to the above method and add it to the reactor. The phosphate polyol accounts for 15% of the total mass of polybutylene adipate diol and phosphate polyol. The resulting resin has a phosphorus content of 2.4%. Add 30 kg of methyl ethyl ketone and 25 kg of toluene and stir until the resin is completely dissolved. Add 20 kg of type II ammonium polyphosphate with a degree of polymerization greater than 1000 and a phosphorus content of 32%. Add 12 kg of melamine cyanurate, with a D50 of 6.5 μm measured by a laser particle size analyzer. Add 2 kg of hexamethylene diisocyanate trimer with an isocyanate group content of 21.8%. Disperse at 800 r / min for 40 min. The slurry fineness is less than 25 μm. Filter through a 250-mesh filter and adjust the solid content to 42% with methyl ethyl ketone. The primer solution has no sedimentation after standing for 24 h.

[0068] The polyester fabric substrate is woven from 10tex low-elastic polyester yarn, with a warp and weft density of 360 threads / 10cm; weight per square meter. According to the formula Accounting, in the formula , The units are warp and weft density, expressed as roots / 10cm. , The linear density of the warp and weft yarns is expressed in tex, with a calculated value of 72 g / m², an actual measured weight of 72.6 g / m², and a thickness of 0.14 mm. The fabric is subjected to stretch heat setting at 185℃ for 60 seconds, with a warp tension of 12 N / cm.

[0069] The primer was applied to one side of the substrate using a comma-shaped scraper at a speed of 15 m / min, with a dry coating amount of 13.4 g / m². It was then dried at 110℃ for 90 s to form a flame-retardant anchoring primer with a dry film thickness of 10.3 μm. The phosphorus content of the primer was [not specified]. According to the formula The calculated rate is 8.7%, where... The phosphorus content of the phosphate-modified polyurethane is 2.4% by mass. , These represent the feed amounts of phosphate-modified polyurethane and ammonium polyphosphate, respectively. The total solid feed amount of the primer liquid is 89 kg, and the coefficient 0.32 represents the mass fraction of phosphorus in ammonium polyphosphate.

[0070] Take 100 kg of silicone pressure-sensitive adhesive, which is prepared by condensation of hydroxyl-terminated polydimethylsiloxane and MQ silicone resin in toluene. The viscosity of hydroxyl-terminated polydimethylsiloxane at 25℃ is 15000~25000 mPa·s. The molar ratio of M unit to Q unit of MQ silicone resin is 0.8:1, the mass fraction of hydroxyl group is 1.2%, the mass ratio of the two is 1.5:1, and the solid content of the adhesive solution is 60%. Add 14 kg of expandable graphite with an initial expansion temperature of 200℃, an expansion ratio of 250 mL / g, and a particle size of 80 μm. Finally, add 5 kg of hydrophobic fumed silica with a specific surface area of ​​200 m² / g. Disperse at 600 r / min for 30 min. The resulting adhesive composition shows no graphite sedimentation after standing for 12 h.

[0071] The adhesive composition was coated on the surface of the flame-retardant anchoring primer with a dry coating amount of 58 g / m². It was then dried in three stages at 80°C, 110°C and 140°C, with dwell times of 40 s, 50 s and 60 s respectively. The resulting adhesive layer had a dry film thickness of 55 μm and no bubbles or crystal points on the surface.

[0072] The adhesive layer was cross-linked by electron beam irradiation with an accelerating voltage of 200 kV, nitrogen protection, and an oxygen content below 200 ppm. The beam current and vehicle speed were adjusted to achieve an absorbed dose of 60 kGy. After irradiation, the gel mass fraction was 85.7%. The mass of insoluble matter in the sample after reflux extraction with toluene for 24 hours and drying at 80°C for 4 hours to constant weight. Compared with the sample mass before extraction The ratio, i.e. After winding, the tape is cured at 50°C for 60 hours, then slit to obtain the finished tape.

[0073] Example 2 and Example 3

[0074] The preparation processes of Examples 2 and 3 are the same as those of Example 1, and the differences are listed in Table 1. Example 2 corresponds to the lower limit combination of each parameter range, and Example 3 corresponds to the upper limit combination, which is used to check the feasibility of the interval endpoints.

[0075] In Example 2, the phosphorus content of the primer coating was calculated using the same formula as in Example 1, with a resin phosphorus content of 1.6% and a total solids content of 69 kg, resulting in a phosphorus content of 8.0%. In Example 3, the resin phosphorus content was 3.2%, and the total solids content of the primer coating was 109 kg, resulting in a phosphorus content of 9.2%. After irradiation, the meridional tensile strength retention rate of the substrate in Example 3 was 86.5%, and no embrittlement was observed.

[0076] Comparative Examples 1 to 4;

[0077] Comparative Example 1: No flame-retardant anchoring base coating was applied; the adhesive composition was directly coated onto the polyester fabric substrate, and the other conditions were the same as in Example 1.

[0078] Comparative Example 2: No expandable graphite was added to the adhesive composition, the amount of fumed silica remained unchanged, and the other conditions were the same as in Example 1.

[0079] Comparative Example 3: No electron beam irradiation crosslinking was performed. The adhesive layer was dried and then directly entered the curing process. The other conditions were the same as in Example 1.

[0080] Comparative Example 4: 32 parts by weight of ammonium polyphosphate were used as the flame retardant in the primer liquid without the addition of melamine cyanurate. The mass fraction of phosphorus in the primer layer was calculated to be 13.0% according to the same formula. The other conditions were the same as in Example 1.

[0081] Performance testing;

[0082] The performance testing methods for the tapes obtained in each embodiment and comparative example are as follows: Vertical flammability rating was determined using the vertical flammability method. The sample size was 125mm × 13mm. A flame was applied to the lower end of the sample for 10 seconds and then removed. The afterflame time and whether the dripping material ignited the cotton 300mm below were recorded. The flame was applied again for 10 seconds, and the recording was repeated. A sample with an afterflame time not exceeding 10 seconds after both removals of the flame and no dripping material igniting the cotton was recorded as V-0. A sample with an afterflame time not exceeding 30 seconds and no dripping material igniting the cotton was recorded as V-1. A sample with dripping material igniting the cotton was recorded as V-2. The oxygen index was determined by maintaining the sample's flammability. The minimum oxygen volume fraction required for a given length is indicated; the 180° peel strength is determined using a 304 stainless steel plate as the test plate, with a peel angle of 180° and a tensile speed of 300 mm / min; initial adhesion is achieved using the inclined plane rolling ball method, indicated by the largest ball number adhered to by the sample; the high-temperature holding test involves a 25 mm × 25 mm adhesive area, a 1 kg load, and a test temperature of 150°C, recording the time when slippage exceeds 1 mm or the sample detaches; the heat aging test involves placing the tape adhered to the stainless steel plate in a 150°C forced-air oven for 500 h, removing it, cooling it to room temperature, and then retesting the 180° peel strength, with the peel strength retention rate... Peel strength after aging Peel strength before aging The ratio, i.e. The residual adhesive was determined by removing the tape after the heat aging test and visually inspecting the surface of the test board. The tensile strength retention rate was determined by tensile testing using the strip method, measuring the longitudinal tensile strength of the substrate before and after irradiation, and expressed as a percentage of the ratio before and after irradiation.

[0083] The test results are listed in Table 2.

[0084] Experimental Phenomenon Recording and Result Analysis

[0085] In the vertical burning test, it was observed that after the samples of Examples 1 to 3 were removed from the fire, the char layer continued to adhere to the surface of the substrate, the afterburning time was less than 2 seconds, and there was no dripping. In Comparative Example 1, the flame spread upward along the adhesive layer, the adhesive layer melted and dripped down and ignited the degreased cotton. Although the phosphorus content of the base coating of Comparative Example 4 reached 13.0%, which was higher than 8.7% in Example 1, the char layer was loose and brittle, and the afterburning time exceeded 10 seconds. This indicates that the combination of ammonium polyphosphate and melamine cyanurate has a direct impact on the strength of the char layer, and is not a simple superposition of the amount of flame retardant.

[0086] When the tape was removed after the heat aging test, it was observed that a continuous adhesive film remained on the surface of the test panel of Comparative Example 1, and strip-shaped adhesive residue remained on the surface of Comparative Example 4. No visible residue was observed on the surface of the test panels of Examples 1 to 3. The only difference between Comparative Example 1 and Example 1 was the base coating, indicating that the base coating performed the function of anchoring the adhesive layer at high temperatures.

[0087] The vertical burning rating of Comparative Example 2 was reduced to V-1, and the peel strength retention rate after thermal aging was 65.9%. It held for 5.2 hours at 150℃, indicating that the carbon layer formed by the thermal expansion of expandable graphite has a direct effect on blocking the transfer of heat to the adhesive layer. Without this component, even if the base coating is intact, the adhesive layer still fails prematurely at high temperature.

[0088] The gel mass fraction of Comparative Example 3 was only 44.8%, and it slipped as a whole after 0.4 hours of holding test at 150℃. After heat aging, the adhesive layer overflowed from the winding edge, indicating that the three-dimensional network formed by irradiation crosslinking is a prerequisite for the high-temperature holding of the adhesive layer. The vertical burning rating of Comparative Example 3 was still V-0, indicating that irradiation crosslinking solves the problem of high-temperature holding rather than the problem of flame retardancy. The problems solved by each technical feature are distinct from each other.

[0089] Examples 2 and 3 respectively take the lower limit and upper limit combination of each parameter range. The finished products all reach V-0 level and the peel strength retention rate after heat aging is not less than 85%. The endpoints of the range are supported by the examples. The phosphorus element mass fraction of the base coating of Examples 1, 2 and 3 is 8.7%, 8.0% and 9.2% respectively, all of which fall within the range calculated according to the composition range.

[0090] The above test data is an example record. The data in the formal application documents should be replaced with the actual test records, while keeping the test conditions, sample quantity and value taking method unchanged.

[0091] Obviously, those skilled in the art can make various modifications and variations to this application without departing from the scope of this application. Therefore, if such modifications and variations fall within the scope of the claims of this application and their equivalents, this application also intends to include such modifications and variations.

Claims

1. A high-temperature resistant, flame-retardant polyester fabric-based adhesive tape, characterized in that, The product includes a polyester fabric substrate layer, one side of which is sequentially provided with a flame-retardant anchoring primer coating and an organosilicon pressure-sensitive adhesive layer; The flame-retardant anchoring primer is formed by curing a primer liquid on the surface of the polyester fabric substrate layer. The primer liquid comprises, by weight, 45-65 parts of phosphate ester modified polyurethane, 15-25 parts of ammonium polyphosphate, 8-15 parts of melamine cyanurate, 1-4 parts of isocyanate curing agent and 40-70 parts of organic solvent. The silicone pressure-sensitive adhesive layer is formed by curing the adhesive composition on the surface of the flame-retardant anchoring base coating and cross-linking it under electron beam irradiation. The adhesive composition includes 100 parts of silicone pressure-sensitive adhesive, 8-20 parts of expandable graphite and 3-8 parts of fumed silica by weight. The gel mass fraction of the silicone pressure-sensitive adhesive layer is not less than 80%.

2. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 1, characterized in that, The polyester fabric substrate layer is woven from polyester low-elasticity yarn with a linear density of 8-12 tex, a warp density of 300-420 threads / 10cm, a weft density of 300-420 threads / 10cm, a weight of 60-110 g / m², and a thickness of 0.10-0.18 mm. The polyester fabric substrate layer undergoes heat setting treatment at a temperature of 170–200°C for 30–90 seconds.

3. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 1, characterized in that, The phosphate-modified polyurethane is prepared by polycondensation of polyester polyol, diisocyanate and phosphate polyol, wherein the mass of the phosphate polyol accounts for 10% to 20% of the sum of the mass of the polyester polyol and the phosphate polyol; The organic solvent is a mixture of butanone and toluene; The isocyanate curing agent is hexamethylene diisocyanate trimer.

4. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 3, characterized in that, The solid content of the primer is 35% to 50%; The dry film thickness of the flame-retardant anchoring primer is 6–15 μm.

5. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 1, characterized in that, The silicone pressure-sensitive adhesive is formed by the condensation of hydroxyl-terminated polydimethylsiloxane and MQ silicone resin, wherein the mass ratio of MQ silicone resin to hydroxyl-terminated polydimethylsiloxane is 1.2 to 1.8:

1.

6. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 5, characterized in that, The expandable graphite has an initial expansion temperature of 180–220℃, an expansion ratio of 200–300 mL / g, and a particle size of 50–150 μm.

7. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 6, characterized in that, The absorbed dose of the electron beam irradiation crosslinking is 40–80 kGy.

8. The high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to claim 7, characterized in that, The dry film thickness of the organosilicon pressure-sensitive adhesive layer is 40–70 μm; The tape has a 180° peel strength of 6-12 N / 25 mm against the steel plate, a vertical burning rating of V-0, and a peel strength retention rate of no less than 85% after being placed in an environment of 150°C for 500 hours.

9. The method for preparing high-temperature resistant flame-retardant polyester fabric-based adhesive tape according to any one of claims 1 to 8, characterized in that, It includes the following steps. Step 1: Dissolve the phosphate-modified polyurethane in an organic solvent, add ammonium polyphosphate, melamine cyanurate and isocyanate curing agent, stir and disperse evenly, filter to obtain the primer liquid; Step 2: Apply the primer liquid to one side of the polyester fabric substrate layer, dry and cure to form a flame-retardant anchoring primer coating. Step 3: Mix the silicone pressure-sensitive adhesive, expandable graphite and fumed silica, stir and disperse evenly to obtain the adhesive composition; Step 4: Apply the adhesive composition to the surface of the flame-retardant anchoring base coating, and dry it in sections to form an adhesive layer; Step 5: The adhesive layer is cross-linked by electron beam irradiation, wound up, cured, and cut to obtain the high-temperature resistant flame-retardant polyester fabric-based adhesive tape.

10. The preparation method according to claim 9, characterized in that, The segmented drying process includes a first drying segment, a second drying segment, and a third drying segment performed sequentially. The temperature of the first drying section is 70-90℃, the temperature of the second drying section is 100-120℃, and the temperature of the third drying section is 130-150℃; The ripening temperature is 40–60°C, and the time is 48–72 hours.