Anti-PID polyolefin encapsulating film and its preparation method and BC photovoltaic module
By using an anti-PID polyolefin encapsulating film in BC photovoltaic modules and constructing a high-efficiency ion-trapping network using silane coupling agent-modified ion trapping agents, the PID problem of BC modules was solved, achieving the power retention rate requirement without the need for light restoration, thus improving the stability and power generation efficiency of the modules.
Patent Information
- Application Number
- CN202611575763.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
Back-contact (BC) photovoltaic modules are susceptible to potential-induced degradation (PID) during long-term outdoor operation. Existing technologies have significant limitations in improving anti-PID performance in BC module applications, especially in addressing passivation interface failure and power degradation caused by ion migration.
An anti-PID polyolefin encapsulation film is used. By introducing an ion trapping agent modified with a silane coupling agent into the polyolefin elastomer matrix, an ion exchange mechanism is constructed to actively capture and fix migrating ions, forming a highly efficient ion trapping network and preventing ions from reaching the passivation interface on the back of the battery.
Without the need for light recovery, the power retention rate of BC modules is significantly improved, meeting the PID test requirements of IEC 62804 standard. This solves the problem of power generation loss caused by insufficient light recovery and ensures the stability of the modules under low light and cloudy conditions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic encapsulation materials technology, and more specifically, to an anti-PID polyolefin encapsulation film, its preparation method, and BC photovoltaic modules. Background Technology
[0002] Photovoltaic modules face the severe challenge of potential-induced degradation (PID) during long-term outdoor operation. This phenomenon mainly stems from the migration of mobile ions in the encapsulation material to the cell passivation interface under the influence of an electric field, leading to surface passivation failure and intensified carrier recombination. Back-contact (BC) cells, due to their unique electrode structure design, are particularly sensitive to the PID effect, as their passivation interface is directly exposed within the encapsulation system and is more susceptible to the influence of ion migration.
[0003] Currently, the industry's technical approaches to improving the anti-PID performance of modules mainly revolve around the encapsulation film material system: on the one hand, polyolefin elastomers (POE) are used to replace traditional ethylene-vinyl acetate copolymer (EVA) films, utilizing the intrinsic high volume resistivity of POE's non-polar molecular chain structure to reduce ion migration rates; on the other hand, ion-capturing agents such as zeolites and metal oxide acid removers are added to the EVA system to capture free sodium ions through chemical adsorption or ion exchange mechanisms. These two technical approaches have achieved certain application results in conventional PERC modules, but have revealed significant limitations in BC module applications.
[0004] Therefore, there is an urgent need to develop a POE encapsulation film suitable for BC modules that can capture and immobilize migrating ions from the source, so that BC modules can meet the power retention rate index without light recovery after PID testing, completely eliminating the dependence on light recovery.
[0005] In view of this, the present invention is proposed. Summary of the Invention
[0006] The purpose of this invention is to provide an anti-PID polyolefin encapsulating film and its preparation method, as well as a BC photovoltaic module, to improve the above-mentioned technical problems.
[0007] This invention is implemented as follows: In a first aspect, the present invention provides an anti-PID polyolefin encapsulating film, comprising, by weight, the following components: 95.0~99.3 parts of polyolefin elastomer matrix resin; 0.2-2.0 parts of ion-scavenging agent surface-modified with silane coupling agent; Crosslinking agent 0.3~1.0 parts; 0.1-0.5 parts of crosslinking agent; 0.3~1.0 parts of silane coupling agent; Antioxidant 0.1-0.5 parts; and 0.1 to 0.3 parts of light stabilizer.
[0008] In an optional embodiment, it comprises the following components by mass: 96.0~99 parts of polyolefin elastomer matrix resin; 0.5-1.5 parts of ion-scavenging agent surface-modified with silane coupling agent; Crosslinking agent 0.4~0.8 parts; 0.1 to 0.3 parts of crosslinking agent; 0.3-0.7 parts of silane coupling agent; Antioxidant 0.2-0.5 parts; and 0.1 to 0.2 parts of light stabilizer.
[0009] In an optional embodiment, the ion trapping agent modified with the silane coupling agent is selected from at least one of surface-modified zirconium hydrogen phosphate, lanthanum ion-exchange zeolite, and modified hydrotalcite. And / or, the average particle size of the ion trap is 0.5 μm to 5 μm, preferably 1 μm to 3 μm.
[0010] In an optional embodiment, the ion scavenger modified with silane coupling agent is prepared by the following method: mixing and stirring the ion scavenger powder with the silane coupling agent in a high-speed mixer, so that the silane coupling agent is chemically bonded to the surface of the powder. Preferably, the mass ratio of the ion-scavenging agent powder to the silane coupling agent is 100:2 to 100:8; Preferably, the mixing temperature is 80℃~100℃ and the time is 15min~30min.
[0011] In an optional embodiment, the silane coupling agent is selected from at least one of vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane; And / or, the crosslinking agent is a peroxide-based crosslinking agent selected from at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and dicumyl peroxide, preferably 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0012] And / or, the co-crosslinking agent is selected from at least one of trimethylolpropane triacrylate and triallyl isocyanurate; And / or, the antioxidant is a compound system of hindered phenolic antioxidants and phosphite antioxidants; And / or, the light stabilizer is a hindered amine light stabilizer selected from at least one of Tinuvin 770 and Tinuvin 622.
[0013] In an optional embodiment, the polyolefin elastomer matrix resin is an ethylene-octene copolymer with a density of 0.865 g / cm³ to 0.885 g / cm³, a melt index of 2.0 g / 10min to 10.0 g / 10min, and a total residual metal ion content of less than 10 ppm.
[0014] In an optional embodiment, the visible light transmittance of the anti-PID polyolefin encapsulating film is greater than or equal to 91%, the glass interface peel force is greater than or equal to 80 N / cm, and the gelation rate is greater than or equal to 85%.
[0015] Secondly, the present invention provides a method for preparing an anti-PID polyolefin encapsulating film as described in any of the foregoing embodiments, comprising: mixing the polyolefin elastomer matrix resin, the ion trap modified with a silane coupling agent, the crosslinking agent, the co-crosslinking agent, the silane coupling agent, the antioxidant, and the light stabilizer in a uniform ratio to obtain a mixture, which is then melt-extruded at 80°C to 120°C using an extruder, cast and cooled, and wound up to obtain the anti-PID polyolefin encapsulating film.
[0016] Thirdly, the present invention provides a BC photovoltaic module, comprising photovoltaic glass, a first encapsulating film, a BC cell, a second encapsulating film, and a backsheet stacked sequentially from top to bottom; the first encapsulating film and the second encapsulating film are both anti-PID polyolefin encapsulating films according to any of the foregoing embodiments; the BC cell has a back passivation layer, and the back passivation layer is in direct contact with the adjacent encapsulating film; after the BC photovoltaic module undergoes PID testing according to IEC 62804 standard and without light recovery treatment, its power retention rate is greater than or equal to 95%.
[0017] In an optional embodiment, the BC cell is an IBC cell or a TBC cell.
[0018] The present invention has the following beneficial effects: This invention completely blocks ion migration at its source, eliminating dependence on the photorecovery effect. By introducing an ion trap modified with a silane coupling agent into a POE matrix with low metal residue, its compatibility and dispersion uniformity with nonpolar POE are significantly improved, effectively eliminating the risk of leakage caused by agglomeration. Furthermore, this trap can, through an ion exchange mechanism, remove permeated Na+. + Ca² +By firmly locking cations within the film, the number of ions reaching the passivation interface on the back of the BC cell is significantly reduced, fundamentally solving the field passivation failure problem caused by positive charge accumulation. Unlike traditional passive strategies that rely solely on increasing bulk resistance to slow migration rates, this solution actively captures and fixes cations, effectively blocking the migration path. This allows the BC module to directly meet power retention requirements after PID testing without requiring light recovery, completely overcoming the problem of power generation loss due to insufficient light recovery under low-light and cloudy conditions. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0020] Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible subranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the range referred to.
[0021] In the description of this invention, the terms "comprising," "including," etc., mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships may exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than one" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.
[0022] The following is a detailed description of the anti-PID polyolefin encapsulating film, its preparation method, and the BC photovoltaic module provided by the present invention.
[0023] The anti-PID polyolefin encapsulating film provided by the embodiments of the present invention is based on the mechanism of "active capture and fixation" to block ion migration from the source, thereby completely eliminating the dependence on photorecovery effect.
[0024] Specifically, the anti-PID polyolefin encapsulating film comprises, by weight, the following components: 95.0-99.3 parts of polyolefin elastomer matrix resin; 0.2-2.0 parts of ion trapping agent surface modified with silane coupling agent; 0.3-1.0 parts of crosslinking agent; 0.1-0.5 parts of co-crosslinking agent; 0.3-1.0 parts of silane coupling agent; 0.1-0.5 parts of antioxidant; and 0.1-0.3 parts of light stabilizer.
[0025] In a preferred embodiment, the proportions of the components can be further optimized as follows: 96.0-99 parts of polyolefin elastomer matrix resin; 0.5-1.5 parts of ion-trapping agent surface-modified with silane coupling agent; 0.4-0.8 parts of crosslinking agent; 0.1-0.3 parts of co-crosslinking agent; 0.3-0.7 parts of silane coupling agent; 0.2-0.5 parts of antioxidant; and 0.1-0.2 parts of light stabilizer. This preferred proportion maximizes ion-trapping efficiency while ensuring the basic physical properties and long-term reliability of the film.
[0026] The polyolefin elastomer matrix resin is preferably an ethylene-octene copolymer. Its density can be selected from 0.865 g / cm³, 0.870 g / cm³, 0.875 g / cm³, 0.880 g / cm³, or 0.885 g / cm³, with a preferred range of 0.865 g / cm³ to 0.885 g / cm³. The melt index (190℃ / 2.16kg) can be selected from 2.0 g / 10min, 4.0 g / 10min, 6.0 g / 10min, 8.0 g / 10min, or 10.0 g / 10min, with a preferred range of 2.0 g / 10min to 10.0 g / 10min. Crucially, the resin is low in metal residues, with the total residual amount of metal ions such as sodium, aluminum, calcium, and zinc being less than 10 ppm, for example, less than 9 ppm, 7 ppm, 5 ppm, or 3 ppm. Selecting a matrix resin with low metal residue is the basis for achieving high temperature and high volume resistivity of the film, providing a clean background environment for the ion scavenger to perform its active defense function, and avoiding the contribution of inferior raw material ion contamination to PID attenuation.
[0027] The surface-modified ion scavenger is the core functional component for achieving the technical effects of this invention. It is selected from at least one of surface-modified zirconium hydrogen phosphate, lanthanum ion-exchange zeolite, and modified hydrotalcite. These materials have unique layered or porous structures, enabling them to firmly fix sodium ions, calcium ions, and other cations that permeate into the membrane within the membrane matrix through an ion exchange mechanism. This significantly reduces the total amount of ions reaching the passivation interface on the back of the BC battery, fundamentally avoiding the field passivation failure problem caused by the accumulation of positive charges at the interface. The particle size of the ion scavenger directly affects its dispersibility and scavenging efficiency. Its average particle size can be selected as 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, or 5 μm, preferably 1 μm to 3 μm. If the particle size is too small, such as below 0.5 μm, the powder is prone to agglomeration and difficult to disperse uniformly in the matrix; if the particle size is too large, such as exceeding 5 μm, it may affect the light transmittance and mechanical properties of the membrane. The amount of ion scavenger added is crucial. The addition amount can be selected as 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, or 2.0 parts. When the addition amount is less than 0.2 parts, there are insufficient ion-capturing sites, which cannot effectively capture all migrating ions, causing the BC module to still rely on light recovery to restore power after PID testing. When the addition amount is greater than 2.0 parts, the excessive inorganic filler is more difficult to disperse in the POE matrix, and is prone to agglomeration to form microscopic defects, which become potential leakage channels, resulting in a decrease in the volume resistivity and light transmittance of the film at 85°C; at the same time, excessive ionic filler may release free ions under high temperature and high humidity PID testing conditions, which will degrade the anti-PID performance. Therefore, adopting the preferred range of 0.5 to 1.5 parts can achieve the best balance between capture efficiency and overall film performance.
[0028] However, simply blending the ion scavenger cannot achieve the above-mentioned effects; surface modification is a crucial step that determines the success or failure of this invention. Unmodified ion scavengers are rich in hydroxyl groups and exhibit strong hydrophilicity, making them thermodynamically incompatible with the non-polar POE matrix, which can lead to severe interfacial defects and filler agglomeration.
[0029] This invention, through a specific surface modification process, has completely changed this situation, and its decisive impact is reflected in the following three aspects: First, the fundamental problems of dispersibility and interfacial compatibility are solved. The specific method involves adding ion-scavenging agent powder and silane coupling agent to a high-speed mixer at a mass ratio of 100:2 to 100:8, for example, ratios of 100:2, 100:4, 100:5, 100:6, or 100:8. The mixture is then stirred at high speed for 15 to 30 minutes (e.g., 80°C, 90°C, or 100°C) at a temperature of 80°C to 100°C. During this process, one end of the silane coupling agent chemically bonds with the hydroxyl groups on the surface of the ion-scavenging agent through hydrolyzed silanol groups, firmly anchoring it to the powder surface; the other end carries organic functional groups such as vinyl or methacryloxy groups, transforming the surface of the ion-scavenging agent from hydrophilic to hydrophobic, thus achieving thermodynamic compatibility with the non-polar POE matrix. This transformation enables the capture agent particles to be uniformly dispersed in the matrix at the nano or micron scale, effectively eliminating potential leakage channels caused by interfacial incompatibility and particle agglomeration. This is a prerequisite for ensuring the high volume resistivity and insulation performance of the film.
[0030] Secondly, a synergistic "capture-fixation" defense system was constructed. The uniformly dispersed modified ion trapping agent forms a dense ion-capturing network within the POE matrix. When external sodium ions, calcium ions, etc., penetrate into the membrane under the drive of an electric field, they are rapidly captured and firmly fixed by these exposed trapping sites through an ion exchange mechanism. Without surface modification, the trapping agent suffers a significant loss of effective specific surface area due to aggregation, with most of its ion exchange sites embedded within the aggregates, unable to contact migrating ions, rendering the "active capture" function ineffective. Therefore, surface modification is the core guarantee for activating the ion trapping agent function and constructing an efficient "capture-fixation" system by achieving nanoscale dispersion.
[0031] Third, a balance between the optical and mechanical properties of the encapsulant film is achieved. Agglomerated scavenging particles become light scattering centers, severely reducing the film's transmittance and directly affecting the photoelectric conversion efficiency of the solar cell. Simultaneously, large agglomerates are also mechanically weak points, deteriorating the peel strength between the film and glass. The uniform dispersion achieved through surface modification eliminates these macroscopic defects, allowing the film to maintain a high transmittance of ≥91% and a peel strength of ≥80 N / cm while possessing excellent anti-PID performance, thus meeting the stringent comprehensive requirements of photovoltaic modules for the optical, mechanical, and electrical properties of encapsulation materials.
[0032] Furthermore, in some embodiments of the present invention, whether used for surface modification of ion traps or added directly as a component, the silane coupling agent may be selected from at least one of vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane.
[0033] In the encapsulant film composition, in addition to the silane coupling agent used for surface modification of the ion scavenger, an additional silane coupling agent is added, with a dosage of 0.3~0.7 parts, which can be selected as 0.3 parts, 0.5 parts, or 0.7 parts, etc., mainly for the following three purposes: (1) The additional silane coupling agent will migrate to the interface between the encapsulant film and the photovoltaic glass during the encapsulant film lamination process. The silanol groups at one end chemically bond with the silanol groups on the glass surface, while the vinyl and other organic functional groups at the other end participate in the crosslinking reaction of the POE matrix. This molecular bridge effect can significantly improve the peel force of the encapsulant film to the glass, ensuring that it reaches a performance index of greater than or equal to 80 N / cm, thereby ensuring the structural reliability of the module in long-term outdoor service. (2) In the surface modification step of the ion scavenger, the silane coupling agent has been chemically bonded to the surface of the scavenger powder. However, in the subsequent high-temperature extrusion and lamination process, some coupling agents may fail due to thermal degradation or shearing. Adding an extra silane coupling agent to the formulation can serve as a supplementary reserve, dynamically repairing and renewing the inorganic-organic interface, ensuring that the entire film system always maintains a good interfacial bonding state. (3) The extra silane coupling agent has unsaturated double bonds, which can participate in the construction of the crosslinking network of POE molecular chains as auxiliary crosslinking sites in the free radical reaction initiated by the peroxide crosslinking agent. This helps to further improve the crosslinking density and gel rate of the film, enhance the cohesive strength and heat resistance of the film body, and enable the film to maintain excellent mechanical properties and dimensional stability at high temperatures.
[0034] Furthermore, in some embodiments of the present invention, the crosslinking agent is a peroxide-based crosslinking agent, selected from at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (bis(2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) and dicumyl peroxide (DCP), preferably 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. Its dosage can be selected as 0.3 parts, 0.5 parts, 0.7 parts, or 1.0 parts. The crosslinking agent enables the POE molecular chains to form a three-dimensional network structure, significantly improving the mechanical strength, heat resistance, and creep resistance of the film.
[0035] In some embodiments, the co-crosslinking agent is selected from at least one of trimethylolpropane triacrylate (TMPTA) and triallyl isocyanurate (TAIC), and its amount can be selected as 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, or 0.5 parts. The co-crosslinking agent can improve the crosslinking efficiency, suppress side reactions, and make the crosslinking network more complete.
[0036] In some embodiments, the antioxidant is a combination system of hindered phenolic antioxidants and phosphite antioxidants, such as a combination of Irganox 1010 and Irgafos 168. The dosage can be selected as 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, or 0.5 parts. This combination of primary and secondary antioxidants can exert a synergistic effect, effectively capturing free radicals and decomposing hydrogen peroxides during processing and long-term use, preventing thermo-oxidative degradation of the film.
[0037] In some embodiments, the light stabilizer is a hindered amine light stabilizer (HALS), selected from at least one of Tinuvin 770 and Tinuvin 622, and its amount can be selected as 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts or 0.3 parts. It can capture free radicals generated during photoaging, giving the film excellent UV aging resistance.
[0038] Through the synergistic effect of the above components, the anti-PID polyolefin encapsulating film prepared according to the embodiments of the present invention exhibits excellent comprehensive performance. Its visible light transmittance is greater than or equal to 91%, for example, reaching 91.5%, 92%, or higher, ensuring the light energy absorption efficiency of the solar cell; its peel force to the glass interface is greater than or equal to 80 N / cm, for example, reaching 85 N / cm, 90 N / cm, or higher, ensuring the long-term structural reliability of the module; and its gelation rate is greater than or equal to 85%, for example, reaching 87%, 90%, or higher, indicating the formation of a sufficiently cross-linked network.
[0039] Some embodiments of the present invention also provide a method for preparing the above-mentioned anti-PID polyolefin encapsulating film, which includes: adding all the above components into a high-speed mixer according to the proportions, mixing at room temperature for 5 to 10 minutes to obtain a uniform mixture. Subsequently, feeding the mixture into a single-screw or twin-screw extruder, melting and extruding it at a temperature of 80°C to 120°C (e.g., 80°C, 90°C, 100°C, 110°C, or 120°C), casting it through a T-die, cooling it on a cooling roller at 20°C to 40°C, and finally drawing and winding it to obtain an anti-PID polyolefin encapsulating film with a thickness of 0.3 mm to 0.6 mm.
[0040] Some embodiments of the present invention also provide a BC photovoltaic module, the structure of which, from top to bottom, includes: photovoltaic glass, a first encapsulating film, a BC cell, a second encapsulating film, and a backsheet. The first and second encapsulating films are both the anti-PID polyolefin encapsulating films described above in this invention. The BC cell can be an IBC cell or a TBC cell, and its back passivation layer is in direct contact with the adjacent encapsulating film.
[0041] During the module lamination process, the lamination temperature is controlled between 135℃ and 150℃, for example, 140℃ or 145℃; the lamination time is controlled between 8 minutes and 15 minutes, for example, 10 minutes or 12 minutes. Under these conditions, the encapsulant film fully cross-links and cures, forming an integral whole with the solar cells, glass, and backsheet. The key advantage of this BC photovoltaic module is that, after undergoing PID testing according to IEC 62804 standard (85℃ / 85%RH, -1500V, 96h) without any light recovery treatment, its power retention rate is greater than or equal to 95%, and can even reach 97% or higher. This breakthrough completely solves the industry problem of continuous power generation loss caused by insufficient light recovery under conditions such as low light and cloudy days, which is a common issue in traditional solutions.
[0042] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0043] Example 1 This embodiment provides an anti-PID polyolefin encapsulating film, with the following formulation by weight: POE matrix (ethylene-octene copolymer, density 0.870 g / cm³, MI=5.0 g / 10min, total metal residue <5 ppm) 98.0 parts; silane-modified zirconium hydrogen phosphate (α-ZrP, particle size 1.5μm, silane dosage 5%) 1.0 part; bis(2,5-diphenyltrimethoxysilane) 0.6 parts; TMPTA 0.2 parts; vinyltrimethoxysilane 0.5 parts; Irganox 1010 0.2 parts; Irgafos 168 0.2 parts; Tinuvin 770 0.1 parts.
[0044] Its preparation method includes the following steps: S1. Surface modification of ion scavenger: The ion scavenger powder is put into a high-speed mixer, preheated to 90°C, sprayed with silane coupling agent (5% of the powder mass), stirred at high speed for 20 minutes, discharged and cooled to obtain a surface-modified ion scavenger.
[0045] S2. Ingredient Mixing: Add POE matrix resin, surface modified ion scavenger, crosslinking agent, co-crosslinking agent, silane coupling agent, antioxidant, and light stabilizer to a high-speed mixer according to the formula, and mix at room temperature for 8 minutes to obtain a uniform mixture.
[0046] S3. Extrusion Casting: The mixture is fed into a single-screw or twin-screw extruder at an extrusion temperature of 100°C. It is then cast through a T-die, cooled by a roller at 30°C, and wound up to obtain a POE encapsulation film with a thickness of 0.45 mm.
[0047] Example 2 The only difference between this embodiment and Example 1 is that, by weight, its formulation is as follows: 98.5 parts of POE matrix (same as Example 1); 0.5 parts of silane-modified lanthanum exchange zeolite (particle size 2.0 μm, silane content 4%); 0.6 parts of bis(2,5-diphenyltrimethylammonium chloride); 0.2 parts of TMPTA; 0.5 parts of vinyltrimethoxysilane; 0.4 parts of antioxidant compound (same as Example 1); and 0.1 parts of HALS.
[0048] The preparation method is the same as in Example 1, and the film thickness is 0.45 mm.
[0049] Example 3 The only difference between this embodiment and Example 1 is that, by weight, its formulation is as follows: 97.5 parts of POE matrix (same as Example 1); 1.5 parts of silane-modified hydrotalcite (LDH, particle size 2.5 μm, silane content 6%); 0.6 parts of bis(2,5-diphenyltrimethoxysilane); 0.2 parts of TMPTA; 0.5 parts of vinyltrimethoxysilane; 0.4 parts of antioxidant compound; and 0.1 parts of HALS.
[0050] The preparation method is the same as in Example 1, and the film thickness is 0.45 mm.
[0051] Comparative Example 1 The only difference between this comparative example and Example 1 is that, by weight, its formulation is: 99.0 parts of POE matrix (same as Example 1); 0.6 parts of bis(2,5-diphenyltrimethylammonium chloride); 0.2 parts of TMPTA; 0.5 parts of vinyltrimethoxysilane; 0.4 parts of antioxidant compound; and 0.1 parts of HALS.
[0052] The preparation method is the same as in Example 1.
[0053] Comparative Example 2 The only difference between this comparative example and Example 1 is that, by weight, its formulation is: 96.5 parts of EVA resin (VA content 28%); 2.0 parts of unmodified zeolite powder; 0.6 parts of crosslinking agent; 0.3 parts of co-crosslinking agent; 0.5 parts of silane coupling agent; 0.3 parts of antioxidant; and 0.1 parts of light stabilizer.
[0054] The preparation method is the same as in Example 1, with an extrusion temperature of 100°C.
[0055] Comparative Example 3 The only difference between this comparative example and Example 1 is that the modified ion trapping agent used is zirconium hydrogen phosphate, which has not been modified with silane surface.
[0056] The preparation method is the same as in Example 1.
[0057] Comparative Example 4 The only difference between this comparative example and Example 1 is that the formulation contains 95.0 parts of POE matrix (same as Example 1), 3.5 parts of silane-modified zirconium hydrogen phosphate, and the remaining additives are the same as in Example 1.
[0058] The preparation method is the same as in Example 1.
[0059] Comparative Example 5 The only difference between this comparative example and Example 1 is the formulation (parts by weight): POE matrix (ethylene-octene copolymer, density 0.870 g / cm³, MI=5.0 g / 10min, total metal residue <5 ppm) 98.0 parts; silane-modified zirconium hydrogen phosphate (α-ZrP, particle size 1.5 μm, silane dosage 5%) 1.0 part; bis(2,5-diphenyltrioxide) 0.6 parts; TMPTA 0.2 parts; Irganox 1010 0.2 parts; Irgafos 168 0.2 parts; Tinuvin 770 0.1 parts.
[0060] The preparation method is the same as in Example 1.
[0061] Performance testing The encapsulating films used in the examples and comparative examples were used to encapsulate BC battery modules. Specifically, the photovoltaic glass, encapsulating film, BC battery cells, encapsulating film, and backsheet, arranged sequentially, were encapsulated using a lamination process at a lamination temperature of 142°C and a lamination time of 12 minutes. The passivation layer on the back of the BC battery cells was in direct contact with the encapsulating film.
[0062] The performance of the BC battery module was tested, and the specific testing methods are as follows: (1) Transmittance: The average transmittance of visible light (380~780 nm) was tested according to GB / T 2410-2008; (2) Peel strength: According to GB / T 2790-1995, the peel strength of the adhesive film at 180° to the soda-lime glass was tested; (3) Degree of crosslinking: Extracted by reflux with xylene according to Appendix A of GB / T 29848-2013; (4) PID test: According to IEC 62804-1, place the BC module in an environment of 85℃ / 85%RH and apply a bias voltage of -1500V for 96h; immediately after the test (within 2h, without any light or baking recovery treatment), test the maximum power of the module and calculate the power retention rate.
[0063] The test results are shown in Table 1.
[0064] Table 1
[0065] Note: Power retention rate after PID is the measured value within 2 hours after the test, without any light recovery processing. A power retention rate of ≥95% is considered to meet the reliability index.
[0066] The data in Table 1 shows that: (1) After PID testing, the power retention rate of the BC components in Examples 1 to 3 without light recovery was ≥95%, which met the reliability requirements and proved the effectiveness of the technical solution of the present invention.
[0067] (2) The power retention rate of Comparative Example 1 (pure POE, without ion trapping agent) after PID was only 91.3%, which required photorecovery to meet the standard. This shows that the intrinsic high volume resistivity of POE alone cannot completely block ion migration, which verifies the necessity of introducing ion trapping agent.
[0068] (3) The power retention rate of Comparative Example 2 (EVA+zeolite) after PID was 92.1%, indicating that the intrinsic high temperature insulation performance of the EVA system is poor, and even with the addition of ion scavengers, it is difficult to meet the high reliability requirements of BC components.
[0069] (4) The power retention rate of Comparative Example 3 (POE + unmodified α-ZrP) after PID was 91.7%, and it still required light recovery. This indicates that the unmodified filler has poor dispersibility in POE, is easy to agglomerate and form leakage channels, which verifies the key role of silane surface modification.
[0070] (5) The power retention rate after PID in Comparative Example 4 (excessive ion capture agent, 3.5 parts) was 92.2%, indicating that excessive addition led to performance degradation, which verified the rationality of setting the upper limit of the addition amount to 2.0 parts in this invention.
[0071] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A PID-resistant polyolefin encapsulating film, characterized in that, By mass, it comprises the following components: 95.0~99.3 parts of polyolefin elastomer matrix resin; 0.2-2.0 parts of ion-scavenging agent surface-modified with silane coupling agent; Crosslinking agent 0.3~1.0 parts; 0.1-0.5 parts of crosslinking agent; 0.3~1.0 parts of silane coupling agent; Antioxidant 0.1~0.5 parts; as well as 0.1 to 0.3 parts of light stabilizer.
2. The anti-PID polyolefin encapsulating film according to claim 1, characterized in that, By mass, it comprises the following components: 96.0~99 parts of polyolefin elastomer matrix resin; 0.5-1.5 parts of ion-scavenging agent surface-modified with silane coupling agent; Crosslinking agent 0.4~0.8 parts; 0.1-0.3 parts of crosslinking agent; 0.3-0.7 parts of silane coupling agent; Antioxidant 0.2~0.5 parts; as well as 0.1 to 0.2 parts of light stabilizer.
3. The anti-PID polyolefin encapsulating film according to claim 1, characterized in that, The ion-scavenging agent modified by the silane coupling agent is selected from at least one of the following: surface-modified zirconium hydrogen phosphate, lanthanum ion-exchange zeolite, and modified hydrotalcite. And / or, the average particle size of the ion trap is 0.5 μm to 5 μm, preferably 1 μm to 3 μm.
4. The anti-PID polyolefin encapsulating film according to any one of claims 1 to 3, characterized in that, The ion scavenger modified with silane coupling agent is prepared by the following method: mixing and stirring the ion scavenger powder with the silane coupling agent in a high-speed mixer, so that the silane coupling agent is chemically bonded to the surface of the powder. Preferably, the mass ratio of the ion-scavenging agent powder to the silane coupling agent is 100:2 to 100:8; Preferably, the mixing temperature is 80℃~100℃ and the time is 15min~30min.
5. The anti-PID polyolefin encapsulating film according to any one of claims 1 to 3, characterized in that, The silane coupling agent is selected from at least one of vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane; And / or, the crosslinking agent is a peroxide-based crosslinking agent selected from at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and dicumyl peroxide, preferably 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. And / or, the co-crosslinking agent is selected from at least one of trimethylolpropane triacrylate and triallyl isocyanurate; And / or, the antioxidant is a compound system of hindered phenolic antioxidants and phosphite antioxidants; And / or, the light stabilizer is a hindered amine light stabilizer selected from at least one of Tinuvin 770 and Tinuvin 622.
6. The anti-PID polyolefin encapsulating film according to any one of claims 1 to 3, characterized in that, The polyolefin elastomer matrix resin is an ethylene-octene copolymer with a density of 0.865 g / cm³ to 0.885 g / cm³, a melt index of 2.0 g / 10 min to 10.0 g / 10 min, and a total residual metal ion content of less than 10 ppm.
7. The anti-PID polyolefin encapsulating film according to any one of claims 1 to 3, characterized in that, The anti-PID polyolefin encapsulating film has a visible light transmittance greater than or equal to 91%, a glass interface peel force greater than or equal to 80 N / cm, and a gelation rate greater than or equal to 85%.
8. A method for preparing an anti-PID polyolefin encapsulating film as described in any one of claims 1 to 7, characterized in that, It includes: The mixture of the polyolefin elastomer matrix resin, the ion trap modified with silane coupling agent, the crosslinking agent, the co-crosslinking agent, the silane coupling agent, the antioxidant, and the light stabilizer is uniformly mixed in a certain proportion and then melt-extruded at 80°C to 120°C using an extruder. After casting and cooling, the mixture is then wound up to obtain the anti-PID polyolefin encapsulation film.
9. A BC photovoltaic module, characterized in that, The photovoltaic module comprises, from top to bottom, photovoltaic glass, a first encapsulating film, a BC solar cell, a second encapsulating film, and a backsheet, stacked sequentially. Both the first and second encapsulating films are anti-PID polyolefin encapsulating films according to any one of claims 1 to 7. The BC solar cell has a back passivation layer, which is in direct contact with the adjacent encapsulating film. After undergoing PID testing according to IEC 62804 standard and without light recovery treatment, the BC photovoltaic module has a power retention rate greater than or equal to 95%.
10. The BC photovoltaic module according to claim 9, characterized in that, The BC battery cell is either an IBC battery or a TBC battery.