Adhesive composition, adhesive sheet having an adhesive layer formed from the adhesive composition
By using an adhesive composition of block copolymers and acrylic oligomers, the problems of insufficient adhesion and heat resistance to low-polarity substrates are solved, achieving stable adhesion and good appearance in high-temperature environments.
Patent Information
- Application Number
- CN202610648963.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, adhesive compositions have poor adhesion, heat resistance, and coating appearance to low-polarity substrates such as PP resin, and are prone to peeling and displacement, especially in high-temperature environments.
An adhesive composition comprising block copolymers and acrylic oligomers is used. The block copolymers are hard segments composed of styrene elastomers and vinyl aromatic compounds, and the acrylic oligomers are a mixture of monomers with high glass transition temperatures. These are combined with a tackifying resin to form an adhesive layer.
It improves adhesion to low-polarity substrates, heat-resistant adhesion, and coating appearance, ensuring that it is not easy to peel off or shift in high-temperature environments, and has excellent heat retention.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to adhesive compositions and adhesive sheets having an adhesive layer formed from the adhesive composition. Background Technology
[0002] Adhesive sheets with an adhesive layer formed by an adhesive are easy to handle and are therefore widely used in labeling, medical applications, and other fields. The substrates that can be adhered to in adhesive sheets vary depending on the application; sometimes high-polarity substrates such as SUS and polyesters are used, as well as low-polarity substrates such as polyolefins. However, low-polarity substrates generally tend to be difficult to bond, requiring adhesives that can ensure adhesion to resins such as polyolefins. Furthermore, adhesives intended for use in various environments such as marking films, window films, automotive parts, and optical displays require coating transparency, excellent coating appearance that prevents lifting or peeling at the adhesive interface between the substrate and the adhesive layer during processing, excellent heat-resistant adhesion that does not peel or shift even at high temperatures, and heat-resistant holding power.
[0003] As an example, adhesives used to bond decorative sheets to substrates are employed in applications where designed films (decorative sheets) are used to decorate the exterior surfaces of molded products such as automotive interior and exterior parts, keyboards, home appliances, smartphones, building materials, furniture, musical instruments, and Shinkansen window frames. The decoration of molded products using decorative sheets typically requires a heating process, thus necessitating various levels of durability under high temperatures. Furthermore, in recent years, there has been an increasing use of polypropylene resin (hereinafter referred to as PP resin), which has a low specific gravity and excellent thermoforming properties, as the substrate for decorative sheets; therefore, a tight bond with PP resin is also required.
[0004] Patent Document 1 discloses a double-sided adhesive sheet for decorative molding, which comprises an olefin elastomer, a tackifying resin, an oil component and a silane coupling agent. The olefin elastomer has blocks obtained by polymerizing α-olefins as hydrogenated compounds and blocks composed of styrene polymers.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-139099 Summary of the Invention
[0008] The technical problem that the invention aims to solve
[0009] The inventors conducted research and found that the adhesive composition described in Patent Document 1 could not achieve satisfactory performance for PP resin, which is a low-polarity adherend.
[0010] That is, to date, no adhesive composition has been developed that exhibits excellent adhesion to low-polarity substrates, heat-resistant adhesion, heat retention, and a superior coating appearance after processing.
[0011] Solutions for solving technical problems
[0012] In order to solve the above-mentioned technical problems, the inventors conducted repeated and in-depth research, and as a result, completed this invention.
[0013] The adhesive composition and adhesive sheet of the present invention have the following [1] to
[11] .
[0014] [1] An adhesive composition comprising a block copolymer (A) and an acrylic oligomer (B), wherein the block copolymer (A) contains a styrene elastomer (A1) having soft segments composed of at least one of polybutadiene and polyisoprene, and hard segments composed of polymers of vinyl aromatic compounds, and the acrylic oligomer (B) is a copolymer comprising a mixture of monomers including (meth)acrylic monomers (b1) with a glass transition temperature of 60°C or higher, and the acrylic oligomer (B) has a weight-average molecular weight in the range of 0.5 million to 200,000.
[0015] [2] According to the adhesive composition of [1], wherein the diblock ratio in 100% by mass of the block copolymer (A) is 10 to 80% by mass.
[0016] [3] According to the adhesive composition of [1] or [2], wherein the glass transition temperature of the acrylic oligomer (B) is above 30°C and below 180°C.
[0017] [4] The adhesive composition according to any one of [1] to [3], wherein the (meth)acrylic monomer (b1) of the homopolymer having a glass transition temperature of 60°C or higher is a (meth)acrylic monomer having a cyclic structure.
[0018] [5] The adhesive composition according to any one of [1] to [4], wherein the monomer mixture constituting the acrylic oligomer (B) further comprises a monomer (b2) having a functional group.
[0019] [6] According to the adhesive composition of [5], wherein the content of a monomer (b2) having a functional group is 0.01 to 10% by mass in 100% by mass of the monomer mixture constituting the acrylic oligomer (B).
[0020] [7] The adhesive composition according to any one of [1] to [6], wherein the content of acrylic oligomer (B) is 1 to 100 parts by mass relative to 100 parts by mass of block copolymer (A).
[0021] [8] The adhesive composition according to any one of [1] to [7] further comprises a tackifying resin (C) in the amount of 1 to 150 parts by weight relative to 100 parts by weight of the block copolymer (A).
[0022] [9] The adhesive composition according to [8], wherein the tackifying resin (C) comprises a hydrocarbon resin.
[0023]
[10] The adhesive composition according to [9], wherein the hydrocarbon resin contains at least one of unhydrogenated aromatic petroleum resin and hydrogenated aromatic petroleum resin.
[0024]
[11] An adhesive sheet having an adhesive layer formed from any one of the adhesive compositions described in [1] to
[10] .
[0025] Invention Effects
[0026] According to the present invention, an adhesive composition exhibiting excellent adhesion to low-polarity adherents, heat-resistant adhesion, heat-retaining strength, and a superior coating appearance after processing can be provided, as well as an adhesive sheet having an adhesive layer formed from the adhesive composition. It has been found that when an adhesive layer is formed from an adhesive composition containing a specified block copolymer (A) and an acrylic oligomer (B), excellent adhesion to low-polarity adherents, heat-resistant adhesion, and heat-retaining strength are achieved, along with a superior coating appearance after processing. Detailed Implementation
[0027] Hereinafter, the adhesive composition of the present invention and the adhesive sheet having an adhesive layer formed from the adhesive composition will be described, but are not limited thereto.
[0028] It should be noted that in this specification, (meth)acrylic monomers refer to (meth)acrylates, and (meth)acrylates refer to both acrylates and methacrylates. (Methacryl)acryloyl groups include acryloyl and methacryloyl groups. Monomers refer to monomers having olefinically unsaturated groups.
[0029] In this specification, the numerical range defined by “~” includes the range of values recorded before and after “~” as the lower and upper limits.
[0030] Unless otherwise specified, each ingredient mentioned in this instruction manual may be used independently or in combination with two or more ingredients.
[0031] The weight-average molecular weight (Mw) is the weight-average molecular weight of polystyrene determined by gel permeation chromatography (GPC).
[0032] It should be noted that in this invention, the terms "film" and "sheet" are not distinguished based on thickness. In other words, the term "sheet" in this specification also includes thin film-like sheets, and the term "film" in this specification also includes sheet-like films with thickness. Furthermore, both "sheet" and "film" also include laminates.
[0033] Furthermore, the adhered object refers to the object to which the adhesive layer of the adhesive sheet is attached.
[0034] Adhesive Compositions
[0035] The adhesive composition of the present invention is characterized in that it contains a block copolymer (A) and an acrylic oligomer (B), wherein the block copolymer (A) contains a styrene elastomer (A1) having soft segments composed of at least one of polybutadiene and polyisoprene, and hard segments composed of polymers of vinyl aromatic compounds; the acrylic oligomer (B) is a copolymer of monomer mixtures comprising a (meth)acrylic monomer (b1) with a glass transition temperature of 60°C or higher; and the acrylic oligomer (B) has a weight-average molecular weight in the range of 0.5 million to 200,000.
[0036] The following is a description of each component.
[0037] <Block copolymer (A)>
[0038] The block copolymer (A) comprises a styrene-based elastomer (A1) having soft segments composed of at least one of polybutadiene and polyisoprene, and hard segments composed of polymers of vinyl aromatic compounds.
[0039] When the soft segments constituting the styrene-based elastomer (A1) are designated as (X) and the hard segments as (Y), the molecular structure of the styrene-based elastomer (A1) can be linear, branched, radial, or any combination thereof. For example, it can be a block polymer with structures such as XY (diblock), YXY (triblock), (YX-)n, and YXYXY (multiblock). Furthermore, n is an integer of 2 or more.
[0040] There are no particular limitations on styrene-based elastomers (A1) as long as they are commonly used substances. Examples include triblock polymers such as styrene-isoprene-styrene (SIS) and styrene-butadiene-styrene (SBS), diblock copolymers such as styrene-isoprene (SI), styrene-butadiene (SB), and styrene-(ethylene-butene) (SEB), and hydrides of block polymers such as styrene-(ethylene-propylene)-styrene (SEPS) and styrene-(ethylene-butene)-styrene (SEBS). By including styrene-based elastomers (A1), adhesion and heat retention properties become good. They can be used alone or in combination of two or more.
[0041] Specific examples of styrene-based elastomers (A1) include, for example, styrene-isoprene-styrene (SIS), the Kraton D series from Kraton Corporation and the Quintac series from ZEON Corporation of Japan, which preferably contain styrene-isoprene (SI) as a diblock component. Additionally, for styrene-butene-styrene (SBS), the Kraton D series from Kraton Corporation and the TUFPRENE series from Asahi Kasei Corporation are examples, which preferably contain styrene-butene (SB) as a diblock component. Furthermore, for styrene-(ethylene-butene)-styrene (SEBS), the Kraton G series from Kraton Corporation and the TUFTEC series from Asahi Kasei Corporation are examples, which preferably contain styrene-(ethylene-butene) (SEB) as a diblock component. Finally, for styrene-(ethylene-propylene)-styrene (SEPS), the Kraton G series from Kraton Corporation and the SEPTON series from Kuraray Corporation are examples, which preferably contain styrene-(ethylene-propylene) (SEP) as a diblock component.
[0042] The block copolymer (A) may contain other block copolymers (A2) besides styrene-based elastomers (A1). As other block copolymers (A2), any thermoplastic block copolymer having soft segments (X) and hard segments (Y) is acceptable, such as styrene-based elastomers, olefin-based elastomers, polyester-based elastomers, vinyl chloride resin-based elastomers, acrylic elastomers, urethane elastomers, polyamide elastomers, etc., other than (A1). Preferably, it is a styrene-based elastomer or acrylic elastomer other than (A1) that is a block copolymer having soft segments mainly composed of structural units from conjugated diene compounds and hard segments mainly composed of structural units from vinyl aromatic compounds.
[0043] As a soft segment of a styrene-based elastomer other than (A1), a conjugated diene compound is preferred. Examples include isobutene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, isoprene, 3-butyl-1,3-octadiene, and phenyl-1,3-butadiene. The soft segment can be a block with partially hydrogenated unsaturated bonds of the conjugated diene compound, or it can be a fully hydrogenated block.
[0044] As compounds comprising the hard segments of styrene-based elastomers other than (A1), vinyl aromatic compounds are preferred. Examples include α-methylstyrene, vinyltoluene, p-tert-butylstyrene, divinylbenzene, p-methylstyrene, and 1,1-diphenylstyrene, among which styrene is more preferred due to its good heat retention.
[0045] In 100% by mass of block copolymer (A), the content of block copolymer (A2) is preferably less than 10% by mass. If the content of other block copolymers is less than 10% by mass, good compatibility can be easily obtained, and moderate adhesion can be easily achieved.
[0046] The diblock ratio in 100% by mass of the block copolymer (A) is preferably 10-80% by mass, more preferably 20-75% by mass, and even more preferably 30-70% by mass. By making the diblock ratio in 100% by mass of the block copolymer (A) 10% by mass or more, the flexibility of the coating film is improved, and the adhesion and heat-resistant adhesion to olefin-based substrates are better. By making the diblock ratio of the block copolymer (A) 80% by mass or less, the cohesiveness of the coating film is improved, and the heat retention is better.
[0047] When block copolymer (A) contains multiple block copolymers with different diblock ratios, the diblock ratio in 100% by mass of block copolymer (A) is calculated by summing the products of the diblock ratios of each material and their contents. For example, if block copolymer (A) consists of 80 parts by mass of block copolymer with a diblock ratio of 20% by mass and 20 parts by mass of block copolymer with a diblock ratio of 60% by mass, the diblock ratio in 100% by mass of block copolymer (A) is calculated as 20 × 0.8 + 60 × 0.2 = 28% by mass.
[0048] The content of structural units derived from vinyl aromatic compounds in the block copolymer (A) is preferably 5 to 70% by mass, more preferably 10 to 50% by mass, in 100% by mass of the block copolymer (A). By making the content of structural units derived from vinyl aromatic compounds in the block copolymer (A) 5% by mass or more, the cohesiveness of the coating film is improved, and the heat retention is better. By making the content of structural units derived from vinyl aromatic compounds in the block copolymer (A) 70% by mass or less, the flexibility of the coating film is improved, and the adhesion to low-polarity raw materials such as PP resin is better. The content of structural units derived from vinyl aromatic compounds is determined by calculating the mass proportion of vinyl aromatic compounds in the total mass of the block copolymer (A). When the vinyl aromatic compound is styrene, the content of structural units derived from vinyl aromatic compounds refers to the styrene content. The styrene content can be confirmed from the manufacturer's catalog value.
[0049] The weight-average molecular weight of the block copolymer (A) is preferably 10,000 to 500,000, more preferably 30,000 to 250,000. By making the weight-average molecular weight of the block copolymer (A) 10,000 or more, the cohesiveness of the coating film is improved, and the heat retention is better. By making the weight-average molecular weight of the block copolymer (A) 500,000 or less, the wettability to the substrate is improved, and the adhesion to olefin-based substrates is better.
[0050] <Acrylic oligomer (B)>
[0051] Acrylic oligomer (B) is a copolymer of monomer mixtures containing a homopolymer of (meth)acrylic monomer (b1) with a glass transition temperature of 60°C or higher, and a weight average molecular weight in the range of 0.5 million to 200,000. In addition to the acrylic monomer (b1), the monomer mixture constituting acrylic oligomer (B) may also contain monomers with functional groups (b2) and other monomers besides (b1) and (b2). It should be noted that in this specification, monomers with functional groups are classified as monomers with functional groups (b2) even if the glass transition temperature of the homopolymer is 60°C or higher.
[0052] <The homopolymer is a (meth)acrylic acid monomer (b1) with a glass transition temperature above 60°C>
[0053] The homopolymer has a glass transition temperature of 60°C or higher. The (meth)acrylic acid monomer (b1) (hereinafter also referred to as monomer (b1)) contributes to the wettability of low polarity substrates and the cohesiveness at high temperatures, i.e., adhesion and heat-resistant adhesion.
[0054] (Meth)acrylic monomers (b1) with a glass transition temperature (Tg) of 60°C or higher as homopolymers include methyl methacrylate (MMA, Tg: 103°C), ethyl methacrylate (EMA, Tg: 65°C), isopropyl methacrylate (IPMA, Tg: 81°C), isobutyl methacrylate (IBMA, Tg: 67°C), tert-butyl methacrylate (TBMA, Tg: 107°C), cyclohexyl methacrylate (CHMA, Tg: 66°C), isobornyl methacrylate (IBXMA, Tg: 180°C), and isobornyl acrylate (IBXA, Tg: 97°C). Among them, as a monomer (b1), from the viewpoint of balancing cohesiveness and wettability to low-polarity adherents, it is preferably selected from at least one of methyl methacrylate (MMA, Tg: 103°C), ethyl methacrylate (EMA, Tg: 65°C), cyclohexyl methacrylate (CHMA, Tg: 66°C), isobornyl methacrylate (IBXMA, Tg: 180°C), and isobornyl acrylate (IBXA, Tg: 97°C). From the viewpoint of being able to further improve the balance between cohesiveness and wettability to low-polarity adherents, it is more preferably a (meth)acrylic monomer with a cyclic structure such as cyclohexyl methacrylate (CHMA, Tg: 66°C), isobornyl methacrylate (IBXMA, Tg: 180°C), and isobornyl acrylate (IBXA, Tg: 97°C).
[0055] The content of monomer (b1) in the monomer mixture constituting the acrylic oligomer (B) is preferably 45% by mass or more and 99.99% by mass or less, more preferably 55% by mass or more and 99.5% by mass or less, and even more preferably 60% by mass or more and 99.5% by mass or less. By setting the content of monomer (b1) in the monomer mixture constituting the acrylic oligomer (B) to 40% by mass or more, cohesiveness can be imparted, and by setting the content of monomer (b1) to 95% by mass or less, wettability to low-polarity adherents can be improved.
[0056] <Single with functional groups (b2)>
[0057] There are no particular restrictions on the number of functional groups (b2) a monomer may have, as long as it has hydroxyl, carboxyl, amino, amide, or glycidyl groups.
[0058] By including a monomer (b2) with functional groups (hereinafter also referred to as monomer (b2)), there is a tendency for excessive miscibility between the acrylic oligomer (B) and the block copolymer (A). Therefore, when forming the adhesive layer, the acrylic oligomer (B) is moderately and locally present on the surface of the adhesive layer. If the acrylic oligomer (B) is moderately and locally present on the surface of the adhesive layer, the wettability with the substrate is improved, resulting in an excellent appearance of the processed coating.
[0059] Examples of monomers containing hydroxyl groups include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate.
[0060] Examples of monomers containing carboxyl groups include acrylic acid, methacrylic acid, and monomers represented by the following formula (Formula 1).
[0061] Equation 1 CH2=CR1-CO-O-(C2H4-COO-)nH
[0062] Here, R1 represents hydrogen or methyl, and n represents an integer greater than or equal to 1.
[0063] Examples of monomers containing amino groups include 2-(dimethylamino)methyl methacrylate, 2-(diethylamino)ethyl methacrylate, 3-(dimethylamino)propyl methacrylate, and 2-(dimethylamino)dimethylaminoethyl methacrylate.
[0064] Monomers with amide groups include N-vinyl lactone, N-vinyl caprolactam, N-vinyl pyrrolidone, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, etc.; cyclic amides such as vinylmorpholine and (meth)acryloylmorpholine; N-vinyl carboxylic amides such as N-vinylformamide and N-vinylacetamide; (meth)acrylamide; and (meth)acrylamides such as substituted (meth)acrylamide.
[0065] Examples of monomers containing glycidyl groups include glycidyl (meth)acrylate.
[0066] Other monomers with functional groups include cyclic amines such as vinylpyridine, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, and vinyloxazole.
[0067] Among them, as monomer (b2), from the viewpoint of compatibility and adhesion to the substrate, it is preferable to include at least one monomer selected from monomers having hydroxyl groups, monomers having amino groups, monomers having carboxyl groups, and monomers having amide groups. As monomers having amide groups, (meth)acrylamides are preferred.
[0068] The content of monomer (b2) in the monomer mixture constituting the acrylic oligomer (B) is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 8% by mass or less, and even more preferably 0.5% by mass or more and 5% by mass or less. By setting the content of monomer (b2) in the monomer mixture constituting the acrylic oligomer (B) to 0.01% by mass or more, the substrate adhesion is improved, and the coating appearance after processing is excellent. By setting the content of monomer (b2) to 10% by mass or less, the compatibility is improved, and the adhesion becomes good.
[0069] <Other monomers (b3)>
[0070] The monomer mixture constituting the acrylic oligomer (B) may contain other monomers besides the aforementioned monomers (b1) and (b2) as an arbitrary component, without impairing the effects of the invention. Examples include (meth)acrylic acid monomers, vinyl acetate, styrene, and other vinyl monomers with a glass transition temperature (Tg) below 60°C in the homopolymer; these may be used alone or in combination of two or more.
[0071] Among these, monomers (b3) are preferably, from the viewpoint of improving wettability to low-polarity adherents, methyl acrylate (MA, Tg: 6°C), ethyl acrylate (EA, Tg: -27°C), butyl acrylate (BA, Tg: -54°C), isobutyl acrylate (IBA, Tg: -26°C), 2-ethylhexyl methacrylate (2EHMA, Tg: -10°C), n-butyl acrylate (n-BA, Tg: -57°C), and 2-ethylhexyl acrylate (2EHA, Tg: -7°C). The monomers are (meth)acrylic acid monomers with a glass transition temperature (Tg) of less than 60°C for homopolymers such as 6°C, n-octyl acrylate (Tg: -80°C), and 2-octyl acrylate (Tg: -47°C), preferably selected from at least one of ethyl acrylate (EA, Tg: -27°C), 2-ethylhexyl methacrylate (2EHMA, Tg: -10°C), and n-butyl acrylate (n-BA, Tg: -57°C), more preferably 2-ethylhexyl methacrylate (2EHMA, Tg: -10°C).
[0072] The content of other monomers (b3) is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, in 100% by mass of the monomer mixture constituting the acrylic oligomer (B). If the content of other monomers (b3) is 45% by mass or less in 100% by mass of the monomer mixture constituting the acrylic oligomer (B), the adhesion to low-polarity substrates and the cohesiveness of the adhesive layer can be improved, and moderate adhesion can be easily obtained.
[0073] <Weight-average molecular weight (Mw)>
[0074] The acrylic oligomer (B) has a weight-average molecular weight (Mw) in the range of 0.5 million to 200,000, preferably in the range of 10,000 to 150,000, and more preferably in the range of 10,000 to 50,000. When the weight-average molecular weight (Mw) of the acrylic oligomer (B) is 0.5 million or more, the adhesive composition can exhibit appropriate cohesive strength.
[0075] Furthermore, when the weight-average molecular weight (Mw) of acrylic oligomers (B) is below 200,000, their wettability with the substrate becomes good, thus the adhesive layer adheres to the substrate with high adhesion. Therefore, the adhesive layer can exhibit high adhesion.
[0076] The weight-average molecular weight (Mw) of acrylic oligomers (B) can be adjusted to the desired value by changing the reaction temperature, reaction time, type of organic solvent, amount of organic solvent used, type of polymerization initiator, and amount of polymerization initiator used.
[0077] Glass transition temperature (Tg)
[0078] The glass transition temperature (Tg) of the acrylic oligomer (B) is preferably 30°C or higher and lower than 180°C, more preferably 55°C or higher and lower than 180°C, and even more preferably 70°C or higher and lower than 180°C. When the glass transition temperature (Tg) of the acrylic oligomer (B) is 30°C or higher and lower than 180°C, the decrease in viscoelasticity (i.e., the decrease in cohesive strength) caused by high-temperature heating is suppressed. The adhesive layer, by having moderate viscoelasticity, can exhibit high heat retention.
[0079] The glass transition temperature (Tg) of acrylic oligomer (B) is obtained by converting the absolute temperature (K) calculated according to Formula 1 below into Celsius (°C).
[0080] 1 / Tg=m1 / Tg1+m2 / Tg2+…+m(k-1) / Tg(k-1)+mk / Tgk (Formula 1)
[0081] In Formula 1, Tg1, Tg2, ..., Tg(k-1) and Tgk represent the glass transition temperatures (Tg) expressed in absolute temperature (K) when the monomers constituting the acrylic oligomer (B) are made into homopolymers. m1, m2, ..., m(k-1) and mk represent the mole fractions of the monomers constituting the acrylic oligomer (B), and m1 + m2 + ... + m(k-1) + mk = 1.
[0082] It should be noted that by subtracting 273 from the absolute temperature (K), the absolute temperature (K) can be converted to the Celsius temperature (°C), and by adding 273 to the Celsius temperature (°C), the Celsius temperature (°C) can be converted to the absolute temperature (K).
[0083] "Glass transition temperature (Tg) when producing homopolymer" refers to the glass transition temperature (Tg) of the homopolymer produced by homopolymerizing the monomer. It can be obtained from information from various monomer vendors or from the values recorded in "Polymer Handbook 3rd Edition" (AWILEY-INTER SCIENCE PUBLICATION, 1989).
[0084] Regarding the glass transition temperature (Tg) of homopolymers expressed in Celsius (°C), it is 180°C for isobornyl methacrylate (IBXMA), 97°C for isobornyl acrylate (IBXA), 103°C for methyl methacrylate (MMA), 65°C for ethyl methacrylate (EMA), 163°C for acrylic acid (AA), 18°C for dimethylaminoethyl methacrylate (DM), 55°C for 2-hydroxyethyl methacrylate (HEMA), 100°C for styrene (St), and -10°C for 2-ethylhexyl methacrylate (2-EHMA).
[0085] The glass transition temperature (Tg) of acrylic oligomers (B) can be appropriately adjusted, for example, by using monomers with different glass transition temperatures (Tg) when making homopolymers.
[0086] The content of acrylic oligomer (B) relative to 100 parts by weight of the block copolymer (A) is preferably 1 to 100 parts by weight, more preferably 1 to 50 parts by weight, and even more preferably 1 to 30 parts by weight. By making the content of acrylic oligomer (B) 1 part by weight or more relative to 100 parts by weight of the block copolymer (A), the acrylic oligomer (B) is adequately and locally present on the surface of the adhesive layer. If the acrylic oligomer (B) is adequately and locally present on the surface of the adhesive layer, the wettability with the adherend is improved, so the adhesive layer can adhere to the adherend with high adhesion. Therefore, the adhesive layer can exhibit high heat-resistant adhesion. In addition, when the content of acrylic oligomer (B) is 100 parts by weight or less relative to 100 parts by weight of the block copolymer (A), the block copolymer (A) and the acrylic oligomer (B) maintain adequate compatibility, thus preventing, for example, the reduction in adhesion caused by low compatibility, and resulting in an excellent coating appearance after processing.
[0087] <Manufacturing of Acrylic Oligopolymer (B)>
[0088] Acrylic oligomers (B) can be manufactured by polymerizing the above-mentioned mixture of acrylic monomers.
[0089] The polymerization can be carried out using known polymerization methods such as solution polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization, with solution polymerization being preferred. Solvents used in solution polymerization are preferably acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, cyclohexanone, etc. The polymerization temperature is preferably a boiling point reaction temperature of 60–120 °C. Furthermore, the polymerization time is preferably approximately 5–12 hours.
[0090] The polymerization initiator used in the polymerization is preferably a free radical polymerization initiator. Free radical polymerization initiators are typically peroxides and azo compounds.
[0091] Examples of peroxides include di-tert-butyl peroxide, dicumyl peroxide, tert-butylcumyl peroxide, α,α'-bis(tert-butylperoxide-m-isopropyl)benzene, 2,5-di(tert-butylperoxide)hexyne-3, and other dialkyl peroxides; tert-butyl peroxide, tert-butyl peracetate, 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane, and other peroxide esters; cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, and other ketone peroxides; 2,2-bis(4,4-di-tert-butylperoxide)cyclohexanone, etc. Peroxide ketals such as hexyl propane, 1,1-bis(tert-butylperoxide)3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxide)cyclohexane, and n-butyl-4,4-bis(tert-butylperoxide)valerate; hydroperoxides such as cumene hydroperoxide, dicumene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; and peroxide dicarbonates such as bis(tert-butylcyclohexyl) peroxide dicarbonate.
[0092] Examples of azo compounds include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylbutyronitrile), etc.; 2,2'-azobis(4-methoxy-2,4-dimethylpentanitrile), 2,2'-azobis(2,4-dimethylpentanitrile), etc.; 2,2'-azobis(2-hydroxymethylpropionitrile), etc.; and 1,1'-azobis(cyclohexane-1-formonitrile), etc.
[0093] Relative to 100 parts by weight of the monomer mixture mentioned above, the polymerization initiator is preferably used in amounts of 0.01 to 10 parts by weight, more preferably 0.1 to 2 parts by weight.
[0094] After polymerizing the acrylic oligomer (B), the solvent can be appropriately evaporated to achieve solvent-free polymerization. As a method of solvent-free polymerization, the acrylic oligomer (B) solution can be heated above the boiling point of the solvent to evaporate the solvent, thus obtaining solvent-free acrylic oligomer (B). A reduced pressure device can be used when evaporating the solvent.
[0095] This adhesive composition preferably includes a tackifying resin (C) in addition to a block copolymer (A) and an acrylic oligomer (B).
[0096] <Tackifying Resin (C)>
[0097] Examples of tackifying resins (C) include aliphatic petroleum resins (C5 series petroleum resins), aromatic petroleum resins (C9 series petroleum resins or styrene-based petroleum resins), alicyclic petroleum resins (dicyclopentadiene-based petroleum resins), aliphatic / aromatic copolymer petroleum resins, alicyclic / aromatic copolymer petroleum resins, aliphatic / alicyclic copolymer petroleum resins, hydrogenated petroleum resins derived from the above-mentioned petroleum resins, phenolic resins, modified phenolic resins, terpene phenolic resins, hydrogenated terpene phenolic resins, xylene phenolic resins, xylene resins, dicyclopentadiene-phenolic resins, phenol-modified petroleum resins, rosin ester resins, modified rosin ester resins, terpene resins, and hydrogenated terpene resins. These can be used alone or in combination of two or more.
[0098] From the viewpoint of good compatibility and improved adhesion to low-polarity raw materials such as PP resin, hydrocarbon resins, rosin ester resins, terpene phenolic resins, and hydrogenated terpene phenolic resins are preferred, with hydrocarbon resins and hydrogenated terpene phenolic resins being more preferred, and hydrocarbon resins being even more preferred. Among hydrocarbon resins, those containing at least one of unhydrogenated aromatic petroleum resins and hydrogenated aromatic petroleum resins are particularly preferred.
[0099] There are no particular limitations on tackifying resins (C) as long as they are commonly used. For example, as aromatic petroleum resins, examples include Eastman's Endex series, Kristalex series, and Mitsui Chemicals' FTR series. In addition, as hydrogenated aromatic petroleum resins, examples include Arakawa Chemicals' ARKON series and Eastman's Regalite series.
[0100] The softening point of the tackifying resin (C) is preferably 80~160℃, more preferably 100℃~155℃. By ensuring that the softening point of the tackifying resin (C) is within the above range, the cohesiveness of the coating film is improved, resulting in an adhesive layer with superior heat retention. It should be noted that the softening point of this invention is obtained based on the ring and ball method and represents the value measured according to JIS K5902.
[0101] The content of tackifying resin (C) relative to 100 parts by weight of the block copolymer (A) is preferably 1 to 150 parts by weight, more preferably 10 to 150 parts by weight, and even more preferably 10 to 100 parts by weight. By setting the tackifying resin (C) to 1 part by weight or more relative to 100 parts by weight of the block copolymer (A), excellent heat retention is achieved, and by setting the tackifying resin to 150 parts by weight or less, excellent coating appearance can be maintained after processing.
[0102] In addition to the block copolymer (A), acrylic oligomer (B), and tackifying resin (C), this adhesive composition may contain, as needed, any additives such as solvents, other resins besides the block copolymer (A), curing agents, plasticizers, silane coupling agents, leveling agents, inorganic and / or organic microparticles, ultraviolet absorbers, light stabilizers, and antioxidants. The amount of these additives added can be appropriately selected within the range that yields the effects of this invention.
[0103] Other resins besides the block copolymer (A) include known thermoplastic resins such as low-density polyethylene, ultra-low-density polyethylene, low-crystallinity (amorphous) polyolefins, ionomer resins, ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid-maleic anhydride copolymers, ethylene-glycidyl methacrylate copolymers, and other ethylene copolymers; as well as thermoplastic polyesters and polyamide copolymers, polyurethanes, polystyrene resins, celluloid, polyacrylonitrile, and vinyl chloride-vinyl acetate copolymers, and other polyvinyl chloride resins. These resins can be used alone or in combination of two or more. The content of these other resins in the solids component of this adhesive composition is preferably less than 10% by mass. If the content of these resins is less than 10% by mass, good compatibility is easily obtained, and moderate adhesive strength can be readily achieved.
[0104] As a curing agent, it is preferable to form bonds by reacting with the functional groups in the acrylic oligomer (B) through heat or the like. For example, considering the reactivity with the functional groups of the acrylic oligomer (B) in the adhesive composition, one or more known curing agents can be selected from epoxy curing agents, isocyanate curing agents, oxazoline curing agents, aziridine curing agents, carbodiimide curing agents, metal chelate curing agents, melamine curing agents, etc. From the viewpoint of heat-resistant adhesion, it is preferable to include an isocyanate curing agent. The curing agent is preferably 0.1 to 5 parts by weight, more preferably 0.1 to 2 parts by weight, relative to 100 parts by weight of the acrylic oligomer (B).
[0105] <Method for manufacturing adhesive composition>
[0106] A method for manufacturing the adhesive composition will be described. However, the present invention is not limited to the following manufacturing method. It can be manufactured by dissolving a block copolymer (A), an acrylic oligomer (B), and a desired tackifying resin (C) in a solvent such as toluene, and mixing in any additives. It should be noted that it can also be manufactured by softening granular rubber containing the block copolymer (A) by heating it, and then mixing it with the acrylic oligomer (B) and any additives using a mixer, kneader, or similar method.
[0107] Adhesive film
[0108] The adhesive sheet has an adhesive layer formed from the adhesive composition of the present invention.
[0109] The adhesive sheet of the present invention preferably has a release film adhered to at least one side of the adhesive layer. Specifically, it is either a configuration in which a release film is formed on both sides of the adhesive layer or a configuration in which a release film is formed on one side of the adhesive layer and a light-transmitting substrate is provided on the other side of the adhesive, and the adhesive layer is an adhesive layer formed from the adhesive composition of the present invention.
[0110] The thickness of the adhesive layer is preferably 2~1000μm, more preferably 5~500μm, further preferably 10~100μm, and most preferably 20~50μm. It should be noted that the adhesive layer can be a single layer or any of two or more layers stacked together.
[0111] Examples of substrates include polyester (polyethylene terephthalate, polyethylene naphthalate), polycarbonate, polymethyl methacrylate, polyethylene, polypropylene, cyclic olefins, polyvinyl chloride, polyurethane, polyamide, ethylene-vinyl acetate copolymer, etc., as well as inorganic materials such as glass plates, non-woven fabrics, and paper.
[0112] When applying this adhesive composition to a substrate, a solvent may be added; any suitable solvent may be used. Examples of solvents include methyl acetate, ethyl acetate, propyl acetate, n-butyl acetate, isobutyl acetate, toluene, xylene, hexane, acetone, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, n-propanol, and isopropanol. These organic solvents may be used alone or in combination. The viscosity of the adhesive composition may be adjusted by adding these organic solvents, or the viscosity may be reduced by heating the adhesive composition. From a solubility point of view, propyl acetate, n-butyl acetate, isobutyl acetate, toluene, xylene, hexane, methyl ethyl ketone, and isopropanol are preferred; propyl acetate, n-butyl acetate, isobutyl acetate, toluene, and hexane are more preferred.
[0113] There are no particular limitations on the coating method; various methods can be used, such as Mayer stick coating, applicator coating, brush coating, spray coating, roller coating, gravure coating, stencil coating, smear coating, corner wheel coating, doctor blade coating, reverse coating, spin coating, etc. Furthermore, there are no particular limitations on the drying and curing method; methods using hot air drying, infrared radiation, depressurization, and active energy rays can be listed. From the viewpoint of resistance to gas release, heating with hot air or steam at 60~180°C is preferred.
[0114] The adhesive composition of the present invention exhibits excellent adhesion to low-polarity substrates, heat-resistant adhesion, and heat retention, and can impart excellent coating appearance in cross-cut tests. Therefore, the adhesive sheet of the present invention can be suitably used as a decorative sheet.
[0115] <Decorative Piece>
[0116] The decorative sheet comprises a substrate and an adhesive layer formed by this adhesive composition. If necessary, the exposed surface of the adhesive layer can be covered with a release liner. It should be noted that the release liner is peeled off when the adhesive sheet is adhered to the object. There are no particular limitations on the substrate; examples include plastic films, paper, and metal foils. The substrate can be a laminate with any one or more layers stacked on at least one side. Corona discharge treatment and anchoring agent coating, or other easy-adhesion treatments, can be applied to any side of the substrate forming the adhesive layer, as needed. There are no particular limitations on the release liner; known release liners with known release treatments, such as release agent coating, applied to the surface of a resin sheet or paper substrate can be used.
[0117] Examples of substrates used in decorative films include polyester (polyethylene terephthalate, polyethylene naphthalate), polycarbonate, polymethyl methacrylate, polyethylene, polypropylene, cyclic olefins, polyvinyl chloride, polyurethane, polyamide, ethylene-vinyl acetate copolymer and other plastic films, inorganic materials such as glass plates, non-woven fabrics, and paper.
[0118] <Resting Film>
[0119] There are no particular restrictions on the use of a release film, and a transparent plastic substrate is preferred. Examples of raw materials for transparent plastic substrates include polyesters such as polyethylene terephthalate (PET), acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose, polysulfone, polyarylate, and polycyclic olefins. It should be noted that two or more plastic materials can be used alone or in combination.
[0120] As a release film, among the aforementioned transparent plastic substrates, a transparent plastic substrate with excellent heat resistance is preferred, that is, a transparent plastic substrate that inhibits or prevents deformation under harsh conditions such as high temperature and high humidity. PET film or sheet is particularly preferred as a transparent plastic substrate.
[0121] The thickness of the transparent plastic substrate is not particularly limited, but is preferably 10 to 200 μm, and more preferably 25 to 150 μm.
[0122] Decorative sheets using this adhesive composition are suitable for attachment to substrates using vacuum forming and vacuum air forming methods. Conventionally known methods can be appropriately applied in vacuum forming and vacuum air forming.
[0123] <Manufacturing Method of Decorative Sheets>
[0124] A method for manufacturing a decorative sheet having an adhesive layer formed from this adhesive composition will be described. However, conventionally known methods can be appropriately used, and the present invention is not limited to the following manufacturing methods. For example, when using an adhesive composition manufactured by dissolving it in a solvent, a coating film is formed on a sheet on which a surface layer and a decorative layer are formed by applying the solvent-diluted adhesive composition using methods such as knife coating, bar coating, blade coating, doctor coating, roller coating, or cast coating. Then, it is heated and dried as needed, thereby forming an adhesive layer on the sheet. On the other hand, when using an adhesive composition manufactured by a heat-based mixing method, a hot melt coating machine capable of softening the adhesive composition by preheating is used, thereby forming an adhesive layer on the sheet. Decorative sheets having an adhesive layer formed from this adhesive composition exhibit moderate adhesion at room temperature (e.g., 25°C) and excellent adhesion at high temperatures (e.g., 100-150°C), thus maintaining their properties for extended periods at high temperatures (e.g., 80°C for 7 days). Therefore, decorative sheets having an adhesive layer formed from this adhesive composition are suitable for applications such as interior and exterior decoration of aircraft, automobiles, and building materials, as well as in the nursing and medical fields, electrification products, electronic components, smartphones, furniture, musical instruments, and Shinkansen window frames, etc., based on three-dimensional surface decoration (Three-dimensional Overlay Method: TOM molding) as a type of vacuum compression molding.
[0125] <Decorative Structures and Their Manufacturing Methods>
[0126] Decorative sheets having an adhesive layer formed from this adhesive composition can be attached to a substrate to form a decorative structure. There are no particular limitations on the shape of the substrate; various shapes of substrates (e.g., three-dimensional molded articles) can be used.
[0127] More specifically, the decorative structure may sequentially include a surface layer, a decorative layer, and an adhesive layer. The surface layer is the layer that forms the surface of the decorative molded article, and layers conventionally known in the field of decorative sheets can be appropriately used. As the surface layer, it may be composed of various resins such as acrylic resins, polyurethanes, fluoropolymers, and polyvinyl chloride. Furthermore, the exposed surface of the surface layer may be embossed. The decorative layer is used to decorate the decorative object, and various materials can be used depending on the intended use. The decorative layer may, for example, contain at least one resin selected from olefin resins, styrene resins, and vinyl chloride resins. In addition, the decorative layer may further include other layers such as design layers, bulk layers, and bonding layers as arbitrary elements. The number of decorative sheets, the type, arrangement, and thickness of each layer can be appropriately selected and are not particularly limited. The adhesive layer is the layer used to attach the decorative sheet to the substrate (e.g., a molded article formed into a three-dimensional shape), and can be formed by cross-linking the adhesive composition (e.g., after coating onto a substrate) by drying or irradiation with ultraviolet light.
[0128] Example
[0129] The present invention will be described in more detail below through examples, but the present invention is not limited to these examples. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". In addition, the amount of formulation in the table is parts by mass, and the values other than solvent are conversion values of non-volatile components. In addition, empty columns in the table indicate no formulation.
[0130] It should be noted that the method for determining the weight-average molecular weight of the block copolymer (A) and the acrylic oligomer (B) is as follows.
[0131] Determination of weight-average molecular weight (Mw)
[0132] Weight-average molecular weight (Mw) was determined by gel permeation chromatography (GPC). The apparatus used was a Shimadzu Corporation GPC system: the "Prominence" LC-GPC system. Two TSKgel α-M columns were connected in series, manufactured by Tosoh Corporation. N,N-dimethylformamide (DMF) was used as the eluent, and the determination was performed at 40°C. Mw was determined by conversion using polystyrene, a known standard reference material, as the reference material.
[0133] <Determination of softening point>
[0134] The softening point of the tackifying resin (C) is a publicly available value obtained using the ring and ball method (JIS K5902) or from literature, product manuals, etc. When the publicly available value is set as a temperature range, the average of the lower and upper limits is taken.
[0135] <Example of manufacturing acrylic oligomer (B)>
[0136] (Acrylic oligomer (B-1))
[0137] Using a reaction apparatus equipped with a stirrer, reflux condenser, nitrogen inlet pipe, thermometer, and dropping pipe, 100 parts of isobornyl methacrylate (IBXMA) as monomer (b1), 0.02 parts of 2,2-azobisisobutyronitrile (AIBN) as polymerization initiator, and 150 parts of methyl ethyl ketone (MEK) as solvent were added to a reaction vessel. Polymerization was carried out at 70°C for 5 hours under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain an acrylic oligomer solution (B-1) with a non-volatile content of 40.0 ± 0.5%. The weight-average molecular weight (Mw) of the obtained acrylic oligomer is shown in the table.
[0138] (Acrylic oligomers (B-2~B-19), other oligomers (B'-1~B'-4))
[0139] The composition and proportions (parts by mass) were changed to those shown in Table 1, and the solvent amount was adjusted appropriately. Otherwise, acrylic oligomers (B-2 to B-19) and other oligomers (B'-1 to B'-4) were synthesized using the same method as that used for the production of acrylic oligomers (B-1). The weight-average molecular weight and glass transition temperature of the obtained oligomers are shown in Tables 1 to 3.
[0140] [Table 1]
[0141]
[0142] [Table 2]
[0143]
[0144] [Table 3]
[0145]
[0146] The details of each monomer recorded in Tables 1 to 3 above are as follows.
[0147] "IBXMA": Isoborneol methacrylate (homopolymer Tg: 180℃)
[0148] "IBXA": Isobornyl acrylate (homopolymer Tg: 97℃)
[0149] "MMA": Methyl methacrylate (Tg of homopolymer: 103℃)
[0150] “EMA”: Ethyl methacrylate (Tg: 65℃ for homopolymer)
[0151] "AA": Acrylic acid (homopolymer Tg: 163℃)
[0152] “DAM”: 2-(dimethylamino)ethyl methacrylate (Tg of homopolymer: 18℃)
[0153] "HEMA": 2-Hydroxyethyl methacrylate (Tg: 55℃ for homopolymer)
[0154] “St”: Styrene (Tg of homopolymer: 100℃)
[0155] "2EHMA": 2-Ethylhexyl methacrylate (homopolymer Tg: -10℃)
[0156] <Preparation of Adhesive Compositions>
[0157] (Example 1)
[0158] 100 parts of A1-3 (Kraton D1119, manufactured by Kraton, a styrene-isoprene-styrene (SIS) block polymer), which serves as a styrene-based elastomer (A1), and 10 parts of an acrylic oligomer (B-1) were dissolved in toluene and stirred until homogeneous to obtain an adhesive composition with a solids content of 40% by mass. The mixture was stirred at 23°C for 3 hours. It should be noted that the solids content refers to the total amount of components excluding toluene.
[0159] (Examples 2-33, Comparative Examples 1-4)
[0160] As shown in Tables 4-6 and Table 8, the adhesive composition was obtained by changing the types and amounts of styrene-based elastomer (A1) and acrylic oligomer (B), otherwise operating in the same manner as in Example 1.
[0161] (Example 34)
[0162] 100 parts of A1-3 (Kraton D1119, Kraton Corporation, a styrene-isoprene-styrene (SIS) block polymer), serving as a styrene-based elastomer (A1), 10 parts of an acrylic oligomer (B-17), and C-3 (ARKON P-140, Arakawa Chemical Co., Ltd., a fully hydrogenated aromatic petroleum resin), serving as a tackifying resin (C), were dissolved in toluene and stirred until homogeneous to obtain an adhesive composition with a solids content of 40% by mass. The mixture was stirred at 23°C for 3 hours. It should be noted that the solids content refers to the total amount of components excluding toluene.
[0163] (Examples 35-44, Comparative Example 5)
[0164] As shown in Tables 7 and 8, the adhesive composition was obtained by changing the types and amounts of styrene-based elastomer (A1), acrylic oligomer (B), and tackifying resin (C), except for the same procedure as in Example 34.
[0165] [Table 4]
[0166]
[0167] [Table 5]
[0168]
[0169] [Table 6]
[0170]
[0171] [Table 7]
[0172]
[0173] [Table 8]
[0174]
[0175] The details of the materials in Tables 4 to 8 are as follows.
[0176] (Block copolymer (A))
[0177] [Styrene-based elastomers (A1)]
[0178] • A1-1: Kraton D1160; Kraton Corporation, styrene-isoprene-styrene (SIS) block polymer, Mw = 117,000, styrene content 19% by mass, diblock percentage 0% by mass.
[0179] • A1-2: Kraton D1161; Kraton Corporation, styrene-isoprene-styrene (SIS) block polymer, Mw = 220,000, styrene content 15% by mass, diblock ratio 10% by mass.
[0180] • A1-3: Kraton D1119; Kraton Corporation, styrene-isoprene-styrene (SIS) block polymer, Mw = 50,000, styrene content 22% by mass, diblock ratio 66% by mass.
[0181] • A1-4: Kraton D1118; Kraton Corporation, styrene-butadiene-styrene (SBS) block polymer, Mw = 80,000, styrene content 33% by mass, diblock ratio 78% by mass.
[0182] • A1-5: Kraton G1657; Kraton Corporation, styrene-ethylene-butene-styrene (SEBS) block polymer, Mw = 115,000, styrene content 13% by mass, diblock ratio 30% by mass.
[0183] • A1-6: SEPTON 2063; manufactured by Asahi Kasei Corporation, a styrene-ethylene-propylene-styrene (SEPS) block polymer, Mw = 100,000, styrene content 13% by mass, diblock ratio 60% by mass.
[0184] [Other block copolymers besides (A1) (A2)]
[0185] • A2-1: KURARITY LA2140; manufactured by Kuraray, a polymethyl methacrylate (PMMA)-polybutyl acrylate (PBA)-PMMA block polymer, Mw = 69,000, PMMA content 20% by mass, diblock ratio 0% by mass
[0186] (Tackifying Resin (C))
[0187] • C-1: YS Polyster TH 130; manufactured by Anwha Chemical Co., Ltd., hydrogenated terpene phenolic resin, softening point 130℃
[0188] • C-2: YS Polyster T80; manufactured by Anwha Chemical Co., Ltd., a terpene phenolic resin, softening point 80℃.
[0189] • C-3: ARKON P-140; manufactured by Arakawa Chemical Co., Ltd., a fully hydrogenated aromatic petroleum resin with a softening point of 140°C.
[0190] • C-4: Endex 155; manufactured by Eastman, an aromatic petroleum resin with a softening point of 153°C.
[0191] • C5: YS PolysterT160; manufactured by Anwha Chemical Co., Ltd., a terpene phenolic resin, softening point 160℃.
[0192] (Making of adhesive sheets)
[0193] The adhesive composition was coated onto a 38 μm thick polyethylene terephthalate (PET) release sheet using a corner-cutting wheel coater to a dried thickness of 50 μm. The coated sheet was then dried at 100°C for 2 minutes to obtain the release sheet. Next, a single side of a 100 μm thick polyethylene terephthalate film (hereinafter referred to as PET film, product name: A-4300, manufactured by Toyobo Co., Ltd.) was bonded to the adhesive side of the release sheet to create a laminate consisting of a release sheet / adhesive layer / PET film, thus obtaining the experimental release sheet.
[0194] <Physical Property Evaluation of Adhesive Compositions>
[0195] The adhesion, heat resistance, heat retention, and cross-cut test of the obtained adhesive composition to low-polarity substrates, as well as the evaluation of the appearance of the processed coating, are assessed by the following methods.
[0196] <Adhesion>
[0197] A test piece, 25 mm wide and 150 mm long, was cut from the adhesive sheet prepared by the above method. The peelable sheet was peeled off from the cut decorative sheet to expose the adhesive layer. This adhesive layer was then pressed onto a polypropylene (PP) sheet (the substrate) by passing a 2 kg pressing roller back and forth once, resulting in the test piece. After the test piece was left to stand in a constant temperature chamber at 23°C for 24 hours, its 180-degree peel strength (peel speed: 300 mm / min) was measured in the same chamber at 23°C, and this strength was used as the adhesion strength.
[0198] [Evaluation Criteria]
[0199] ◎(Excellent): 20N / 25mm or higher
[0200] ○ (Good): 15N / 25mm or more and less than 20N / 25mm
[0201] △(Applicable): 5N / 25mm or more but less than 15N / 25mm
[0202] × (Not applicable): Less than 5N / 25mm
[0203] <Heat-resistant adhesion>
[0204] Test pieces were obtained using the same method as for evaluating adhesion. Next, the test pieces were left to stand in a constant temperature chamber at 80°C for 1 hour, and then the 180-degree peel strength (peel speed: 300 mm / min) of the test pieces was measured in an atmosphere at 80°C as the heat-resistant adhesion.
[0205] [Evaluation Criteria]
[0206] ◎(Excellent): 20N / 25mm or higher
[0207] ○ (Good): 15N / 25mm or more and less than 20N / 25mm
[0208] △(Applicable): 5N / 25mm or more but less than 15N / 25mm
[0209] × (Not applicable): Less than 5N / 25mm
[0210] <Heat retention>
[0211] A test piece, 25 mm wide and 80 mm long, is cut from the adhesive sheet prepared by the above method. The peelable sheet is then peeled off from the cut decorative sheet to expose the adhesive layer. This adhesive layer is pressed onto the polypropylene (PP) sheet (the substrate) by applying a 1 kg pressing roller back and forth once, resulting in a bonding area of 25 mm × 25 mm. The test piece is then placed in an 80°C atmosphere for 20 minutes, followed by an 80°C oven with a 1 kg load applied parallel to the adhesive layer. The length (mm) of displacement from the original position is measured 24 hours after the load is applied to evaluate the heat retention.
[0212] [Evaluation Criteria]
[0213] ◎(Excellent): 0mm (No offset)
[0214] 〇 (Good): Exceeding 0mm and less than 5mm
[0215] △(Practical): 5mm and above but less than 25mm
[0216] × (Not applicable): 25mm and above
[0217] <Cross-grid test>
[0218] The experimental laminate obtained above was installed in the mold frame of a TOM molding machine (manufactured by Fuse Vacuum Co., Ltd., NGF molding machine), and a PP resin mortar cup with an inner diameter of 68 mm × outer diameter of 70 mm × height of 38 mm was placed inside the frame. Then, the decorative structure was formed by covering the PP resin mortar cup with the experimental laminate. For this decorative structure, the top surface and curved surface were cut into cross shapes with a cutter, and after being placed in an environment of 80°C for 1000 hours, the presence of lifting or peeling was visually checked, and evaluated according to the following criteria.
[0219] [Evaluation Criteria]
[0220] ◎(Excellent): No floating or peeling was found.
[0221] 〇 (Good): Confirmed that at least one of the floating and peeling is less than 0.5 mm in size or distance.
[0222] △(Practical): Confirm at least one of foaming, floating and peeling, with a size or distance exceeding 0.5mm and less than 1mm.
[0223] × (Not applicable): Identify at least one of foaming, floating, and peeling, with a size or distance exceeding 1 mm but less than 1.5 mm.
[0224] This invention is not limited to the above-described embodiments and examples. As long as the spirit of this invention is not departed, appropriate design changes can be made.
[0225] As shown in Examples 1 to 44 of Tables 4 to 7, the adhesive compositions of the present invention exhibit excellent adhesion to low-polarity substrates, heat-resistant adhesion, heat-resistant retention, and the appearance of the processed coating (cross-cut test).
[0226] On the other hand, the adhesive composition shown in Comparative Example 1 of Table 8 is a block copolymer (A) that does not contain styrene-based elastomer (A1), and has poor adhesion and heat resistance to low polarity substrates.
[0227] Furthermore, the adhesive compositions shown in Comparative Examples 2 and 3 in Table 8, which do not contain homopolymers and have a glass transition temperature of 60°C or higher (meth)acrylic monomers (b1), exhibit poor cross-cut adhesion, poor adhesion to low-polarity substrates, and poor heat-resistant adhesion.
[0228] In addition, the adhesive compositions shown in Comparative Examples 4 and 5 in Table 8 are of an acrylic oligomer (B) with a weight-average molecular weight outside the range of 0.5 million to 200,000, and have poor heat retention or adhesion to low polarity substrates, as well as poor heat-resistant adhesion.
[0229] Industrial availability
[0230] The adhesive composition of the present invention exhibits excellent adhesion to low-polarity substrates, heat-resistant adhesion, heat retention, and cross-cut adhesion (appearance of the coating after molding). Therefore, it is also suitable for applications such as decoration of aircraft, automobiles, railways, interior and exterior building materials, nursing and medical fields, and electrification products.
Claims
1. An adhesive composition comprising a block copolymer (A) and an acrylic oligomer (B), wherein, The block copolymer (A) contains a styrene-based elastomer (A1), said styrene-based elastomer (A1) having soft segments composed of at least one of polybutadiene and polyisoprene, and hard segments composed of polymers of vinyl aromatic compounds. Acrylic oligomer (B) is a copolymer of monomer mixtures containing homopolymers of (meth)acrylic monomers (b1) with a glass transition temperature of 60°C or higher. The weight-average molecular weight of acrylic oligomers (B) ranges from 0.5 million to 200,000.
2. The adhesive composition according to claim 1, wherein, The diblock ratio in 100% by mass of the block copolymer (A) is 10-80% by mass.
3. The adhesive composition according to claim 1, wherein, The glass transition temperature of acrylic oligomer (B) is above 30°C and below 180°C.
4. The adhesive composition according to claim 1, wherein, The homopolymer has a glass transition temperature of 60°C or higher. The (meth)acrylic monomer (b1) is a (meth)acrylic monomer with a cyclic structure.
5. The adhesive composition according to claim 1, wherein, The monomer mixture constituting the acrylic oligomer (B) also includes monomers (b2) having functional groups.
6. The adhesive composition according to claim 5, wherein, In 100% by mass of the monomer mixture constituting acrylic oligomer (B), the content of monomer (b2) with functional groups is 0.01 to 10% by mass.
7. The adhesive composition according to claim 1, wherein, The content of acrylic oligomer (B) is 1 to 100 parts by mass relative to 100 parts by mass of block copolymer (A).
8. The adhesive composition according to claim 1, wherein, It further comprises 1 to 150 parts by weight of tackifying resin (C) relative to 100 parts by weight of block copolymer (A).
9. The adhesive composition according to claim 8, wherein, Tackifying resins (C) include hydrocarbon resins.
10. The adhesive composition according to claim 9, wherein, The hydrocarbon resin contains at least one of unhydrogenated aromatic petroleum resin and hydrogenated aromatic petroleum resin.
11. An adhesive sheet having an adhesive layer formed from the adhesive composition of any one of claims 1 to 10.
Citation Information
Patent Citations
Double-sided adhesive sheet for decorative molding, laminate adhesive sheet for decorative molding and decorative molding laminate