A method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel
By precisely controlling the amount of magnesium added and RH vacuum treatment, combined with aluminum slag ball modification and rare earth treatment in the crystallizer, the problems of precipitate dispersion and inclusion control in low-carbon titanium-containing steel were solved, achieving fine dispersion of precipitates in the steel and high-efficiency anti-scaling performance, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202611449228.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively control the fine dispersion of precipitates in low-carbon titanium-containing steel, which poses a risk of carbon increase. The particle size control of inclusions is unclear, the effect of magnesium treatment is unstable, and the effect of rare earth treatment is not fully realized. It is difficult to improve strength, formability and resistance to hydrogen-induced cracking at the same time.
By precisely controlling the amount and yield of magnesium, combined with RH vacuum treatment, aluminum slag ball modification of ladle top slag and rare earth treatment in the crystallizer, fine MgO·Al2O3 and rare earth compounds are generated as heterogeneous nucleation cores, which promote the dispersion of titanium-containing precipitates such as TiN, TiC, and Ti4C2S2, thereby reducing the oxygen content and the number of inclusions in the steel.
It achieves high dispersion of titanium-containing precipitates in low-carbon steel, with inclusions of ≤5μm accounting for ≥70% of the total, significantly reducing oxygen content in the steel, significantly improving anti-scaling performance, simplifying the process, reducing costs, and providing excellent comprehensive mechanical properties.
Smart Images

Figure REF-OBJ-1789638366029-000001
Abstract
Description
Technical Field
[0001] This invention relates to the field of iron and steel metallurgy, specifically to a method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel. The low-carbon titanium-containing steel is particularly suitable for enamel steel, and can also be used in fields requiring control of inclusion and precipitate dispersion, such as automotive structural steel, pipeline steel, and hydrogen storage container steel. Background Technology
[0002] Low-carbon titanium-containing steel is widely used in enamel products, automotive structures, pipeline transportation, and hydrogen storage containers. As the base material for enamel products, enamel steel must possess sufficient hydrogen storage capacity to prevent blistering defects. Blistering is a phenomenon where hydrogen atoms absorbed by the steel plate during the firing process aggregate into hydrogen molecules at the interface, generating internal pressure that causes the enamel layer to blister and peel off; this has been a long-standing technical challenge in the enamel industry. The hydrogen storage performance of ferritic low-carbon enamel steel depends on the number and distribution of hydrogen traps; the most effective way to improve hydrogen storage performance is to increase the content and dispersion of second-phase particles.
[0003] Currently, titanium-containing precipitates (TiN, TiC, Ti4C2S2, etc.) are the most widely used hydrogen traps in enamel steel due to their ability to form irreversible hydrogen traps. Both domestically and internationally, a low-carbon, high-titanium, sulfur-containing approach is commonly adopted, with Ti4C2S2 as the primary hydrogen trap. Titanium treatment can refine inclusions, and its deoxidation products can act as nucleation sites for manganese sulfide, improving the microstructure and properties of the steel. In automotive structural steel, pipeline steel, and hydrogen storage container steel, it is also necessary to control the size, morphology, and distribution of inclusions and precipitates through elements such as Ti, Mg, and rare earth elements to improve strength, toughness, formability, and resistance to hydrogen-induced cracking.
[0004] However, existing technologies have several shortcomings: hydrogen traps are singular and have poor stability; strength, formability, and anti-explosion properties are difficult to control synergistically; high titanium and high sulfur content increases the difficulty of smelting and continuous casting; TiN particles larger than 5 μm become crack initiators, and existing technologies struggle to balance their quantity and dispersion; the LF+RH process carries the risk of carbon increase, which is detrimental to the production of low-carbon steel with a carbon content below 0.065 wt%; and calcium treatment has limited effectiveness. In particular, existing magnesium treatment processes lack a systematic and quantitative description of the relationship between magnesium addition and yield; the particle size control range of oxide inclusions after magnesium treatment is unclear; and the synergistic nucleation mechanism between MgO·Al2O3 and titanium-containing precipitates is not fully elucidated, resulting in insufficient stability and repeatability of magnesium treatment effects. Meanwhile, existing rare earth treatments for crystallizers mostly emphasize the generation of rare earth sulfur oxides, failing to clarify the differentiated alteration effects of rare earths on two types of inclusions: Al-Ca-Mg-Ti-O composite oxides and titanium-containing precipitates. They also fail to demonstrate the significant reduction in the total number of inclusions, the substantial decrease in oxygen content in the steel, and the improved cleanliness achieved by making large inclusions difficult to detect under a metallographic microscope after rare earth treatment. Therefore, a method is urgently needed that can avoid carbon gain while simultaneously achieving dual dispersion control of oxide inclusions and titanium-containing precipitates. Summary of the Invention
[0005] The purpose of this invention is to provide a method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel. This method addresses the shortcomings of existing technologies, which cannot simultaneously achieve both low carbon content (C: 0.04wt%~0.07wt%) and fine dispersion control of titanium-containing precipitates. Furthermore, existing technologies suffer from problems such as carbon increase in LF treatment, blockage during calcium treatment, and excessive precipitate size. This invention provides a method that precisely controls the amount and yield of magnesium addition, clarifies the particle size range of oxide inclusions after magnesium treatment, and establishes the synergistic nucleation mechanism of MgO·Al2O3 and TiN. This method achieves a ≥70% proportion of inclusions with a particle size ≤5μm in the titanium-containing precipitates, while simultaneously precisely controlling the carbon content in the steel to 0.04wt%~0.07wt%.
[0006] To achieve the above objectives, the basic solution provided by this invention is: a method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel, comprising the following steps: S1: Hot metal pretreatment and converter smelting The molten iron is pretreated for desulfurization, and the sulfur content of the molten iron after desulfurization is controlled to be ≤0.005wt%. The desulfurized molten iron is then transferred to a converter for smelting, and the carbon content of the tapped steel is controlled to be 0.04wt%~0.08wt%, and the tapping temperature is 1620~1650℃.
[0007] S2: Ladle top slag modification During or after tapping, aluminum slag balls with an aluminum content of ≥28wt% are added to the ladle at a rate of 1.0–2.0 kg / t of steel to reduce the (FeO+MnO) content in the top slag to below 5wt%.
[0008] S3: RH vacuum treatment and composition adjustment The ladle is transported to the RH vacuum degassing unit and circulated under a vacuum of ≤133Pa: First, it is decarburized under RH vacuum and the composition is finely adjusted by adding a carbon raiser to precisely adjust the carbon content of the molten steel to 0.04wt%~0.07wt%; then aluminum particles are added for deoxidation, with an addition amount of 0.25~0.3kg / t steel; after adding, it is circulated for 8 minutes, and then high-grade ferrotitanium with a titanium content of ≥70wt% is added to adjust the titanium content of the molten steel to 0.03wt%~0.04wt%; after adding, it is circulated for another 5 minutes.
[0009] S4: Magnesium Treatment and Soft Blowing Five minutes after adding ferrotitanium in step S3, aluminum-magnesium alloy cored wire is fed into the molten steel. The cored wire consists of low-carbon steel strip encasing core powder. Based on the total mass of the core powder, the magnesium content is 10wt%–15wt%, the aluminum content is 40wt%–50wt%, and the remainder is Fe and unavoidable impurities. For a steel volume of 120t, the total wire feeding length is calculated based on the steel volume and a magnesium recovery rate of 25%–30%, controlling the magnesium content in the steel to be 0.0010wt%–0.0025wt%. The protective effect of aluminum on magnesium in the aluminum-magnesium alloy cored wire lowers the vapor pressure of magnesium, resulting in a milder heat of dissolution effect compared to pure magnesium, and allowing the magnesium recovery rate to remain stable at 25%–30%.
[0010] After the wire feeding is completed, the bottom of the ladle is immediately blown with argon for soft blowing and stirring. The soft blowing time is 10 to 12 minutes. After soft blowing, the magnesium content in the steel is controlled at 0.0010wt% to 0.0025wt%.
[0011] After magnesium treatment, the oxide inclusions in the steel are transformed from the original Al2O3 inclusions into finely dispersed MgO·Al2O3 or Al-Ca-Mg-Ti-O composite oxides. The particle size characteristics are as follows: the particle size of the inclusions is mainly 0.5-5μm, and the number of inclusions with a particle size ≤5μm accounts for ≥70%.
[0012] S5: Modification treatment of rare earth inclusions in continuous casting After soft blowing, slab continuous casting is carried out, with argon gas protection throughout the casting process. During continuous casting, lanthanum-cerium mixed rare earth cored wire is fed into the crystallizer. The lanthanum content in the cored wire is 40 wt% and the cerium content is 60 wt% based on the total mass of rare earth elements. The total lanthanum and cerium content in the steel is controlled to reach 0.0012 wt% to 0.0020 wt%, and the rare earth recovery rate is ≥80%. After the rare earth cored wire is fed in, lanthanum and cerium react rapidly with oxygen and sulfur in the steel to generate fine spherical RE2O2S, RE2S3, RE1O3, etc., where RE represents lanthanum and cerium mixed rare earth. The strong deoxidizing and desulfurizing effects of rare earth elements significantly reduce the total oxygen content in steel, causing a large number of inclusions to float and be removed. Under a metallographic microscope, the number of inclusions is greatly reduced, and large inclusions ≥5μm are difficult to detect. Residual fine rare earth compounds act as heterogeneous nucleation sites for titanium-containing precipitates during solidification, synergistically interacting with the MgO·Al2O3 core generated in step S4 to promote highly dispersed precipitation of the titanium-containing phase. Some rare earth compounds form a core-shell structure with MgO·Al2O3 as the core and RE2O2S as the shell, or vice versa.
[0013] The chemical composition of the obtained low-carbon steel plate, in wt%, is as follows: C: 0.04wt%~0.07wt%, Ti: 0.03wt%~0.04wt%, Mn: 0.60wt%~0.70wt%, P≤0.018wt%, S≤0.005wt%, Al: 0.020wt%~0.045wt%, N≤0.0050wt%, La+Ce: 0.0012wt%~0.0020wt%, Mg: 0.0010wt%~0.0025wt%, with the balance being Fe and unavoidable impurities.
[0014] The principle of this invention is as follows: This method first lays the foundation for pure molten steel through deep desulfurization of molten iron and fixed-carbon smelting in a converter. Then, it creates a low-oxidation metallurgical environment by modifying the ladle top slag with aluminum slag balls. Precise carbon adjustment and aluminum deoxidation are achieved in a RH vacuum environment, generating fine, dispersed Al2O3 particles as a heterogeneous nucleation substrate. Titanium alloying then precipitates the primary nuclei containing titanium phases. Subsequently, trace amounts of magnesium are used to modify Al2O3 into finely dispersed MgO·Al2O3, which has a small critical nucleation radius, a small wetting angle with the molten steel, and is less prone to aggregation and growth. The trace amounts of Mg ensure that MgO·Al2O3 exists stably in the steel and becomes a solidification nucleus for TiN during the cooling process of the molten steel, promoting the dispersed distribution of TiN inclusions and reducing the formation of large-sized TiN particles. A prolonged bottom-blowing argon process in the ladle achieves uniform dispersion of inclusions. Finally, a mixture of lanthanum and cerium rare earth elements is introduced into the crystallizer to further modify the inclusions and supplement nucleation sites. Rare earth elements accumulate at the solidification front, reacting with O and S to generate fine compounds such as RE2O2S, RE2S3, and REA1O3. These compounds perform final-stage modification and surface alteration on the Al-Ca-Mg-Ti-O composite oxide, reducing the interfacial energy of inclusions, inhibiting their aggregation and growth, and promoting spheroidization. Simultaneously, the total number of inclusions is significantly reduced, and the oxygen content in the steel is significantly lowered, making large inclusions difficult to detect under a metallographic microscope. The rare earth compounds, together with MgO·Al2O3, serve as heterogeneous nucleation cores for TiN, TiC, Ti(C,N), and Ti4C2S2, promoting highly dispersed precipitation of titanium-containing phases and reducing the formation of large-sized TiN. The synergistic effect of multiple components guides the uniform and fine spheroidization of titanium-containing phases and oxide inclusions, achieving precise control over the size and distribution of precipitates from the metallurgical source.
[0015] The table below shows a comparison of the changes in inclusions between rare earth-treated and untreated inclusions:
[0016] The present invention has the following beneficial effects: Achieving precise low-carbon control: By completely eliminating the LF refining process and avoiding electrode carbonization, the carbon content of molten steel can be stably controlled within the range of 0.04wt% to 0.07wt%, meeting the production requirements of low-carbon titanium-containing steel.
[0017] High dispersion of titanium-containing precipitates: Through a chain-like progressive nucleation process of "Al2O3 dispersed particles → MgO·Al2O3 dispersed cores → rare earth compounds → titanium-containing precipitates", the proportion of particles with a size ≤5μm in the inclusions of titanium-containing precipitates such as TiN, TiC, and Ti4C2S2 is ≥70%, and the number density of precipitates per unit volume is increased by more than 50% compared with conventional processes.
[0018] Magnesium treatment results are stable and controllable: Through the protective effect of aluminum on magnesium in aluminum-magnesium alloy cored wire and the wire feeding process, the magnesium yield is stable at 25% to 30%, and the magnesium content in the steel is precisely controlled within the range of 0.0010wt% to 0.0025wt%. After magnesium treatment, the particle size of MgO·Al2O3 inclusions is mainly 0.5 to 5μm, and the proportion of inclusions with a particle size ≤5μm is ≥70%.
[0019] Significant improvements in final rare earth modification and cleanliness: After feeding La / Ce mixed rare earth into the crystallizer, the Al-Ca-Mg-Ti-O composite oxide in the steel transforms from large-sized irregular inclusions into 0.5–5 μm spherical / near-spherical REA1O3, RE2O2S, and RE2S3, partially forming a core-shell structure with MgO·Al2O3 as the core and REA1O3 and / or RE2O2S as the shell, with ≤5μm accounting for ≥75%. Simultaneously, the strong deoxidation and desulfurization effects of rare earth significantly reduce the total oxygen content in the steel, drastically reducing the total number of inclusions; large inclusions ≥5μm are difficult to detect under a metallographic microscope. Titanium-containing precipitates diffusely precipitate with rare earth compounds and MgO·Al2O3 as the core, with ≤5μm accounting for ≥70%, increasing the number density by more than 50%, thereby increasing the number of irreversible hydrogen traps and improving resistance to scaling.
[0020] Significantly improved resistance to hydrogen splattering: hydrogen penetration time ≥22 min for 1.8 mm thick steel plate, hydrogen penetration time ≥26.8 min for 2.0 mm thick steel plate, normalized hydrogen penetration value TH ≥6.7 min / mm 2 It meets the industry's requirements for resistance to scale bursts.
[0021] Simplified process and reduced cost: Eliminating the LF refining and calcium treatment processes shortens the smelting cycle by 35-45 minutes, reduces power consumption and refractory material consumption, and avoids the nozzle nodule problem caused by calcium treatment, enabling stable continuous casting of multiple furnaces.
[0022] Excellent comprehensive mechanical properties: The dispersed titanium-containing particles play a role in grain refinement and precipitation reinforcement. The yield strength of the obtained hot-rolled plate is ≥350MPa and the elongation after fracture is ≥30%, which combines high strength and good formability. Detailed Implementation
[0023] The following description of a preferred embodiment of the present invention is for illustrative purposes and does not constitute a limitation on the scope of protection of the present invention.
[0024] A preferred embodiment of the method of the present invention is as follows: S1: Blast furnace molten iron is desulfurized by KR to a sulfur content of 0.003wt%, then transferred to a 120t top and bottom combined blowing converter, with the final carbon content controlled at 0.08wt%, and the tapping temperature at 1630℃.
[0025] S2: 1.5 kg / t of aluminum slag balls are added during the tapping process. Based on the total mass of the aluminum slag balls, the composition of the aluminum slag balls is Al2O3: 42 wt%, metallic Al: 28 wt%, CaO: 15 wt%, and the remaining component is lightly calcined dolomite. The (FeO+MnO) content in the top slag is reduced to 4.2 wt%.
[0026] S3: RH vacuum degree 90Pa, adjust carbon to 0.060wt%, add aluminum granules 0.3kg / t, circulate for 8min; add high-grade ferrotitanium with titanium content of 70wt%, control the Ti of molten steel to 0.035wt%~0.040wt%, and continue to circulate the molten steel for 6min.
[0027] S4: After adding ferrotitanium for 5 minutes, feed in aluminum-magnesium alloy cored wire with a steel volume of 120t, a total wire feeding length of 250 meters, a wire feeding speed of 2.8m / s, and control the Mg content in the steel to 0.0015wt% after soft blowing. After feeding the wire, perform bottom blowing with argon for 10 minutes.
[0028] S5: Continuous casting with argon protection throughout the process, feeding lanthanum-cerium mixed rare earth cored wire (La: 40wt%, Ce: 60wt% by total mass of rare earth elements) into the crystallizer, with a wire feeding speed of 5.0m / s, rare earth recovery rate ≥80%, and controlling the total La+Ce content in the steel to be 0.0012wt%~0.0020wt%. After rare earth treatment: the total oxygen content in the steel is significantly reduced, the total number of inclusions is greatly reduced, and large inclusions ≥5μm are difficult to detect under a metallographic microscope; the size of Al-Ca-Mg-Ti-O composite oxides is mainly 0.5~5μm, with ≤5μm accounting for ≥75%, and the morphology changes from angular to spherical / near spherical, with some forming a MgO·Al2O3 core and RE2O3 shell; and a MgO·Al2O3 core with RE2O2S shell encapsulation structure; titanium-containing precipitates TiN, TiC, Ti(C,N), and Ti4C2S2 precipitate with rare earth compounds and / or MgO·Al2O3 as the core, with ≤5μm accounting for ≥70%, average size ≤3μm, and number density increased by ≥50%.
[0029] In the low-carbon titanium-containing steel produced by the above method: the particle size of MgO-Al2O3 inclusions is mainly 0.5-5μm, and the proportion of inclusions with a particle size ≤5μm is ≥70%; the hydrogen penetration time of the 1.8mm thick steel plate is ≥22min, the hydrogen penetration time of the 2.0mm thick steel plate is ≥26.8min, and the normalized hydrogen penetration value TH is ≥6.7min / mm 2 The steel plate meets the industry's anti-scaling requirements, with a yield strength ≥350MPa and an elongation ≥30%. The chemical composition of the obtained steel plate, in wt%, is as follows: C: 0.04wt%~0.07wt%, Ti: 0.03wt%~0.04wt%, Mn: 0.60wt%~0.70wt%, P≤0.018wt%, S≤0.005wt%, Al: 0.020wt%~0.045wt%, N≤0.0050wt%, La+Ce: 0.0012wt%~0.0020wt%, Mg: 0.0010wt%~0.0025wt%, with the balance being Fe and unavoidable impurities.
[0030] The above description is merely a preferred embodiment of the present invention, and common knowledge regarding specific structures and characteristics is not described in detail here. It should be noted that those skilled in the art can make several improvements without departing from the structure of the present invention, and these should also be considered within the scope of protection of the present invention. These improvements will not affect the effectiveness of the present invention or the practicality of the patent. The scope of protection claimed in this application shall be determined by the content of its claims.
Claims
1. A method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel, characterized in that, Includes the following steps: S1: The molten iron is pretreated to desulfurize it to a sulfur content of ≤0.005wt%, and then it is smelted in a converter. The carbon content of the tapped steel is controlled to be 0.04wt%~0.08wt%, and the tapping temperature is 1620~1650℃. S2: During or after tapping, aluminum slag balls with an aluminum content ≥28wt% are added to the ladle at a rate of 1.0~2.0kg / t steel to reduce the FeO+MnO content in the top slag to below 5wt%. S3: Transport the ladle to the RH vacuum degassing unit and perform circulation treatment under a vacuum degree ≤133Pa. First, adjust the carbon content of the molten steel to 0.04wt%~0.07wt%. Then, add 0.25~0.3kg / t of aluminum particles for deoxidation and circulate for 8min. Add high-grade ferrotitanium with a titanium content ≥70wt% to adjust the titanium content of the molten steel to 0.03wt%~0.04wt%. After adding, continue circulation treatment for 5~6min. S4: After adding ferrotitanium in step S3 for 5-6 minutes, feed aluminum-magnesium alloy cored wire into the molten steel in the ladle. The cored wire is composed of low-carbon strip steel wrapped with core powder. Based on the total mass of the core powder, the magnesium content in the core powder is 10wt%-15wt%, the aluminum content is 40wt%-50wt%, and the balance is Fe and unavoidable impurities. For 120t of molten steel, the magnesium recovery rate is controlled at 25%-30%, and the magnesium content in the steel is controlled at 0.0010wt%-0.0025wt%. After the wire feeding is completed, perform bottom blowing of argon in the ladle for 10-12 minutes. S5: After soft blowing, continuous casting is carried out under argon protection throughout the process. Lanthanum-cerium mixed rare earth cored wire is fed into the crystallizer. The cored wire contains 40wt% lanthanum and 60wt% cerium by total mass of rare earth elements. The total lanthanum and cerium content in the steel is controlled to be 0.0012wt%~0.0020wt%, and the rare earth recovery rate is ≥80%. After the rare earth cored wire is fed in, lanthanum and cerium react rapidly with oxygen and sulfur in the steel to generate fine spherical RE2O2S, RE2S3, REA1O3, etc., which perform final-stage modification on the Al-Ca-Mg-Ti-O composite oxide in the steel, significantly reducing the total number of inclusions and the oxygen content in the steel. Large inclusions are difficult to detect under a metallographic microscope. The residual fine rare earth compounds and MgO·Al2O3 work together as heterogeneous nucleation cores for titanium-containing precipitates, promoting highly dispersed precipitation of titanium-containing precipitates.
2. The method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel according to claim 1, characterized in that, After magnesium treatment in step S4, the particle size of MgO·Al2O3 inclusions in the steel is mainly 0.5-5 μm, with inclusions ≤5 μm accounting for ≥70%. After rare earth treatment in the crystallizer, the total number of Al-Ca-Mg-Ti-O composite oxide inclusions in the steel is significantly reduced, and the total oxygen content in the steel is reduced by ≥30% compared to before rare earth treatment. Large inclusions ≥5 μm are difficult to detect under a metallographic microscope. The Al-Ca-Mg-Ti-O composite oxide is transformed into one or more of REAlO3, RE2O3, RE2O2S, and RE2S3, and partially... The structure is formed with MgO·Al2O3 as the core and RE2O2S as the shell, or with MgO·Al2O3 as the core and RE2O2S as the shell. The particle size is mainly 0.5-5μm, and the proportion of particles ≤5μm is ≥75%. The titanium-containing precipitates include one or more of TiN, TiC, Ti(C,N), and Ti4C2S2. After rare earth treatment, the titanium-containing precipitates are precipitated with rare earth compounds and MgO·Al2O3 as heterogeneous nucleation cores. The proportion of particles ≤5μm is ≥70%, the average size is ≤3μm, and the number density is ≥50% higher than that of untreated particles.
3. The method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel according to claim 1, characterized in that, The method eliminates the LF refining process.
4. The method for controlling the dispersion of titanium-containing precipitates and inclusions in ultra-low carbon enamel steel according to claim 1, characterized in that, The chemical composition of the obtained low-carbon steel plate, by mass percentage, is as follows: C: 0.04wt%~0.07wt%, Ti: 0.03wt%~0.04wt%, Mn: 0.60wt%~0.70wt%, P≤0.018wt%, S≤0.005wt%, Al: 0.020wt%~0.045wt%, N≤0.0050wt%, La+Ce: 0.0012wt%~0.0020wt%, Mg: 0.0010wt%~0.0025wt%, with the balance being Fe and unavoidable impurities.