Scrap steel briquettes for electric arc furnace steelmaking and their preparation method
By designing a gradient structure of an outer reduction zone and an inner slag-forming zone in scrap steel briquettes for electric arc furnace steelmaking, combined with conical through holes and an anti-oxidation coating, an orderly reaction of reduction followed by slag-forming is achieved. This solves the problems of slow melting speed and delayed metallurgical reaction in traditional scrap steel briquettes for electric arc furnace steelmaking, thereby improving metal yield and metallurgical efficiency.
Patent Information
- Application Number
- CN202611334965.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional scrap steel briquettes have a slow melting rate, high unit power consumption, and severe metal oxidation and burning loss in electric arc furnace steelmaking. In addition, the slag formation reaction is delayed, which affects the steel yield and smelting cycle.
Design a scrap steel briquette for electric arc furnace steelmaking. The outer reduction zone contains carbonaceous and metallic reducing agents, and the inner slag-forming zone contains slag-forming agents. Conical through holes are set, and asymmetric through holes are formed by gradient material distribution and high-pressure forming. An anti-oxidation coating is applied to achieve reaction control of reduction followed by slag formation.
It improved metal yield, shortened smelting cycle, reduced power consumption, improved metallurgical reaction efficiency and steel purification capacity, and reduced dust emissions.
Smart Images

Figure CN123108230A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of scrap steel smelting technology, specifically relating to a scrap steel briquette for electric arc furnace steelmaking and its preparation method. Background Technology
[0002] Electric arc furnace steelmaking is a key process in the modern steel industry for utilizing scrap steel resources. However, traditional scrap steel briquettes only change the physical form. In actual production, these briquettes often exhibit problems such as slow melting speed, high unit power consumption, and severe metal oxidation and burning loss in electric arc furnaces, especially significantly affecting the yield of molten steel. At the same time, the metallurgical reactions required for slag formation are often delayed, prolonging the overall furnace smelting cycle.
[0003] Chinese patent application number 202111560113.3 discloses a structure that adds fuel and creates through holes inside scrap steel balers, intending to accelerate melting by increasing the heat exchange area and supplementing heat. While this solution improves heat transfer efficiency to some extent, it essentially remains a simple physical mixture of fuel and scrap steel. The two react almost simultaneously at high temperatures, failing to differentiate and optimize the timing of the two key stages in electric arc furnace smelting: reduction and slag formation. Specifically, the slag-forming agent (such as calcium oxide) and the reducing agent (such as carbonaceous materials) come into contact too early inside the baler, easily undergoing a solid-phase reaction during heating, weakening their independent roles in the molten pool and reducing reaction efficiency. Furthermore, the simple through-hole design has limited effect on guiding and organizing airflow within the furnace, making it difficult to fully utilize the advantages of airflow stirring and heat transfer.
[0004] This invention provides a scrap steel briquette for electric arc furnace steelmaking and its preparation method, particularly concerning how to improve metal yield. Summary of the Invention
[0005] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention provides a scrap steel briquette for electric arc furnace steelmaking, with the purpose of improving metal recovery.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a scrap steel briquette for electric arc furnace steelmaking, comprising an outer reduction zone and an inner slag-forming zone arranged sequentially from the outside to the inside; the outer reduction zone contains a carbonaceous reducing agent and a metallic reducing agent, and the inner slag-forming zone contains a slag-forming agent and a carbonaceous reducing agent; the scrap steel briquette is provided with at least one conical through hole, which extends from the surface of the outer reduction zone to the inner slag-forming zone.
[0007] The mass ratio of the outer reduction zone to the inner slag-forming zone is (3:7) to (4:6).
[0008] The raw material composition of the outer reduction zone, by mass percentage, includes: 85%~90% scrap steel, 5%~10% carbonaceous reducing agent, 0~2% slag-forming agent, 1.5%~3% metal reducing agent, and 0.2%~1% binder.
[0009] The raw material composition of the inner slag-forming zone, by mass percentage, includes: 80%~85% scrap steel, 1%~3% carbonaceous reducing agent, 12%~16% slag-forming agent, 0~1% metal reducing agent, and 0.2%~1% binder.
[0010] The large end diameter of the tapered through hole is 30mm to 50mm, the small end diameter is 10mm to 30mm, and the depth of the tapered through hole is 60% to 95% of the thickness of the scrap steel briquettes.
[0011] The total raw material composition of the scrap steel briquettes, by mass percentage, includes: 80%–92% scrap steel raw materials, 3%–10% carbonaceous reducing agent, 4%–8% slag-forming agent, 0.5%–2% metal reducing agent, and 0.5%–1% binder.
[0012] The inner wall of the tapered through-hole is coated with an antioxidant coating, which contains a metal reducing agent and a binder.
[0013] The carbonaceous reducing agent is coke powder, anthracite powder, or graphite powder; the slag-forming agent is a mixture of quicklime and fluorite; in the inner slag-forming zone, the mass ratio of quicklime to fluorite is (10~12):(1.5~2);
[0014] The metal reducing agent is ferrosilicon powder or aluminum powder;
[0015] The binder is a composite of hydrolyzed starch and nano-bentonite, and the mass ratio of hydrolyzed starch to nano-bentonite is (2:1) to (3:1).
[0016] The number of tapered through holes is two.
[0017] This invention also provides a method for preparing scrap steel briquettes for electric arc furnace steelmaking, comprising the following steps:
[0018] Raw material pretreatment: Preheating the scrap steel raw material;
[0019] Gradient material distribution: The preheated scrap steel raw material and auxiliary materials are added to the briquetting mold in layers according to the ratio of the outer reduction zone and the inner slag-forming zone. The mixture that constitutes the outer reduction zone is added first, and then the mixture that constitutes the inner slag-forming zone is added.
[0020] High-pressure forming and channel preparation: pressing and forming under pressure, while simultaneously forming asymmetrically distributed tapered through holes;
[0021] Curing process: Curing the pressed blocks after they have been formed.
[0022] The preheating temperature is 200℃~400℃; the pressing pressure is 1200 MPa~1500 MPa, and the holding time is 10 seconds~20 seconds; the curing treatment is to cure at 80℃~120℃ for 2 hours~4 hours.
[0023] After the curing process, the method further includes the step of forming an antioxidant coating on the inner wall of the tapered through hole: preparing a slurry by mixing a metal reducing agent and a binder, and applying it to the inner wall of the tapered through hole to form the antioxidant coating.
[0024] The scrap steel briquettes for electric arc furnace steelmaking of the present invention have an outer reduction zone that reacts first, effectively suppressing the oxidation and burning loss of the entire briquette and improving the metal yield. The inner slag-forming agent melts out at the appropriate time, quickly forming functional slag and shortening the smelting cycle. Attached Figure Description
[0025] This manual includes the following figures, which illustrate the following:
[0026] Figure 1 This is a schematic diagram of the structure of scrap steel briquettes for electric arc furnace steelmaking according to the present invention;
[0027] The markings in the diagram are: 100 - scrap steel briquettes; 110 - outer reduction zone; 120 - inner slag-forming zone; 130 - conical through-hole. Detailed Implementation
[0028] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings, in order to help those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solutions of the present invention, and to facilitate its implementation.
[0029] It should be noted that in the following embodiments, the terms "first," "second," and "third" do not represent an absolute distinction in structure and / or function, nor do they represent the order of execution; they are merely for the convenience of description.
[0030] Firstly, such as Figure 1 As shown, this embodiment of the invention provides a scrap steel briquette 100 for electric arc furnace steelmaking, comprising an outer reduction zone 110 and an inner slag-forming zone 120 arranged sequentially from the outside to the inside, with the outer reduction zone 110 enclosing the inner slag-forming zone 120. The outer reduction zone 110 contains a carbonaceous reducing agent and a metallic reducing agent, while the inner slag-forming zone 120 contains a slag-forming agent and a carbonaceous reducing agent. The scrap steel briquette 100 is provided with at least one conical through hole 130, which extends from the surface of the outer reduction zone 110 to the inner slag-forming zone 120.
[0031] Specifically, the scrap steel briquette 100 provided in this embodiment of the invention is designed with a gradient functional structure including an outer reduction zone 110 and an inner slag-forming zone 120, aiming to achieve orderly reaction control of "reduction first, slag formation later". Specifically, the outer reduction zone 110 rapidly releases carbonaceous reducing agent and metallic reducing agent in the early stage of high temperature, creating a strong reducing atmosphere, inhibiting the oxidation of iron and providing chemothermal activity; after the initial reaction in the outer reduction zone 110, the high proportion of slag-forming agent contained in the inner slag-forming zone 120 can melt out at an appropriate time, rapidly forming functional slag, thereby improving the melting rate, metal yield and metallurgical refining effect.
[0032] The preferred mass ratio of the outer reduction zone 110 to the inner slag-forming zone 120 is 3:7 to 4:6. By controlling the mass ratio of the outer reduction zone 110 to the inner slag-forming zone 120, the reducing capacity provided by the outer reduction zone 110 in the early stage of melting and the rate of slag formation by the inner slag-forming zone 120 in the later stage of melting can be adjusted to match their timing. In one specific embodiment of the present invention, the mass ratio of the outer reduction zone 110 to the inner slag-forming zone 120 is 4:6; in another specific embodiment of the present invention, the mass ratio of the outer reduction zone 110 to the inner slag-forming zone 120 is 3:7.
[0033] Furthermore, the concentrations of both carbonaceous and metallic reducing agents in the outer reduction zone 110 are higher than those in the inner slagging zone 120, while the concentration of slagging agent in the inner slagging zone 120 is higher than that in the outer reduction zone 110. In other words, carbonaceous and metallic reducing agents are concentrated in the outer layer, while slagging agents are concentrated in the inner layer. This concentration gradient distribution can be achieved through gradient material distribution, allowing the briquettes to initially receive the reducing atmosphere from the outer layer after entering the furnace, followed by the slagging function from the inner layer.
[0034] Specifically, the raw materials in the outer reduction zone 110, by mass percentage, include: 85-90% scrap steel, 5-10% carbonaceous reducing agent, 0-2% slagging agent, 1.5-3% metallic reducing agent, and 0.2-1% binder. Since the outer reduction zone 110 is the first to come into contact with the high-temperature furnace gas and is directly exposed to the oxidizing atmosphere, the carbonaceous reducing agent content in the outer reduction zone 110 is relatively high to achieve a rapid reaction, quickly generating a large amount of CO gas and forming a strong reducing atmosphere, effectively inhibiting the oxidation and burning loss of iron elements on the briquette surface. Simultaneously, the oxidation reaction of carbon releases chemical heat, providing additional energy for the initial melting stage, helping to reduce the power consumption per ton of steel in the electric arc furnace, and further lowering the melting point of the scrap steel by enhancing the carburizing effect on the scrap steel surface, thus promoting its rapid melting.
[0035] Moreover, the content of metal reducing agent in the outer reduction zone 110 is relatively high. Since the metal reducing agent has a stronger reducing ability, it can preferentially react with oxygen at high temperatures, further consolidating the local strong reducing environment. This process not only generates dense oxides such as SiO2 or Al2O3 to form a protective film and reduce the oxidation loss of metallic iron, but also has a significant exothermic effect (e.g., Si + O2 → SiO2, with an exothermic heat of 28314 kJ / kg), which replenishes the system with heat and improves energy utilization efficiency.
[0036] Furthermore, to ensure that the core function of the outer reduction zone 110, which is reduction protection, is not interfered with, the slag-forming agent content needs to be controlled at an extremely low level (0~2%), or even omitted altogether. This avoids premature adverse side reactions between the slag-forming agent (such as CaO) and the carbonaceous reducing agent (e.g., CaO + C → Ca + CO), resulting in waste of the reducing agent. Simultaneously, it prevents premature slag formation that would coat unmelted scrap steel, hindering heat transfer and mass diffusion, and affecting the overall melting rate. Conversely, a low slag-forming agent content helps maintain a lower melting point in the outer reduction zone 110, thereby accelerating its melting process, forming the initial molten pool as early as possible, and creating conditions for subsequent metallurgical reactions.
[0037] The outer reduction zone 110 has a high scrap steel content, which not only provides a sufficient source of metal material, improving the overall density and quality stability of the briquettes, but more importantly, it endows them with good mechanical strength. This ensures that the briquettes maintain their structural integrity during transportation, stacking, and feeding, thus providing physical protection for the inner slag-forming zone 120. When the outer reduction zone 110 melts rapidly, the resulting molten metal pool effectively isolates the inner slag-forming zone 120 from the direct impact of the high-temperature airflow, preventing the functional components of the inner slag-forming zone 120 from participating in the reaction prematurely, and ensuring the smooth implementation of the timing control strategy of reduction followed by slag formation.
[0038] Correspondingly, the raw materials in the inner slag-forming zone 120, by mass percentage, include: 80-85% scrap steel, 1-3% carbonaceous reducing agent, 12-16% slag-forming agent, 0-1% metallic reducing agent, and 0.2-1% binder. The slag-forming agent content in the inner slag-forming zone 120 is significantly higher than that in the outer reduction zone 110, enabling the slag-forming agent to rapidly participate in the reaction after the scrap steel has basically melted, quickly forming a high-basicity, highly fluid slag. This effectively promotes metallurgical refining processes such as dephosphorization and desulfurization, and enhances the slag's adsorption capacity for non-metallic inclusions, achieving efficient slag formation and deep purification.
[0039] Furthermore, since the inner slag-forming zone 120 is within the protective atmosphere formed by the outer reduction zone 110, the environment already possesses strong reducing conditions, thus significantly reducing the need for additional reducing capacity. Therefore, the content of carbonaceous reducing agent is controlled at a low level, providing only a small amount of carbon source to maintain a weak reducing atmosphere. This avoids adverse reactions between carbon and the slag-forming agent (such as the reaction of C and CaO to generate CO gas, leading to splashing or energy loss), and also facilitates precise control of the final carbon content of the molten steel, meeting the stringent requirements of the smelting process for composition control.
[0040] Correspondingly, since a sufficient protective atmosphere has been formed in the outer reduction zone 110, the amount of metal reducing agent added in the inner slag-forming zone 120 is also extremely small. The small amount of metal reducing agent added is only used to prevent the risk of local oxidation; in addition, the addition of trace amounts of ferrosilicon to the metal reducing agent can also participate in adjusting the slag composition, optimizing its physicochemical properties, and at the same time helping to reduce the cost of alloys used in the smelting process.
[0041] To ensure the realization of the above refining functions, the scrap steel content in the inner slag-forming zone 120 is appropriately reduced, thus reserving sufficient space for the introduction of a large amount of slag-forming agent. The generated slag can promptly cover the surface of the newly formed molten steel, playing multiple roles of heat preservation, oxygen isolation, and impurity adsorption, preventing secondary oxidation of the molten steel, and avoiding the problem of insufficient basicity or sluggish reaction caused by excessive scrap steel diluting the concentration of the slag-forming agent.
[0042] In embodiments of the present invention, such as Figure 1 As shown, the conical through-hole 130 is a conical hole with a large end and a small end at its two ends. The large end of the conical through-hole 130 is located on the outer surface of the outer reduction zone 110, and the small end is located inside the inner slag-forming zone 120. The conical through-hole 130 is used to guide the gas flow in the furnace into the interior of the scrap steel briquette 100. The diameter of the large end of the conical through-hole 130 is 30mm to 50mm, and the diameter of the small end is 10mm to 30mm. The depth of the conical through-hole 130 (i.e., the total length of the conical through-hole 130) is 60% to 95% of the thickness of the scrap steel briquette 100. The thickness of the scrap steel briquette 100 refers to the distance between two opposite outer surfaces in the thickness direction of the outer reduction zone 110.
[0043] In this embodiment of the invention, the number of tapered through holes 130 can be one, two, or more, with two holes in an asymmetrical distribution being more effective. Asymmetrical distribution means that the central axes of the through holes are not parallel and are asymmetrical with respect to the geometric center of the pressing block, thereby creating vortices when the airflow passes through the furnace.
[0044] In this embodiment of the invention, the inner wall of the tapered through-hole 130 is coated with an anti-oxidation coating, which includes a metal reducing agent and a binder. The metal reducing agent can be aluminum powder or ferrosilicon powder, and the binder can be water glass or hydrolyzed starch. The coating's function is to preferentially oxidize at the initial high temperature of the electric furnace, delaying the collapse of the pore structure, thereby maintaining the through-hole's guiding effect on airflow.
[0045] In this embodiment of the invention, the total raw material ratio of the scrap steel briquettes 100, by mass percentage, includes: 80%–92% scrap steel raw materials, 3%–10% carbonaceous reducing agent, 4%–8% slag-forming agent, 0.5%–2% metal reducing agent, and 0.5%–1% binder. This total ratio is a comprehensive superposition of the components of the outer reduction zone 110 and the inner slag-forming zone 120, taking into account the overall requirements of reduction and slag formation.
[0046] In this embodiment of the invention, the carbonaceous reducing agent can be coke powder, anthracite powder, or graphite powder; the slag-forming agent is a mixture of quicklime and fluorite, and the mass ratio of quicklime to fluorite is (5-8):1. Preferably, in the inner slag-forming zone 120, the mass ratio of quicklime to fluorite is (10-12):(1.5-2). The high proportion of quicklime effectively constructs a high-alkalinity slag environment (R = CaO / SiO2 = 2.8-3.2), significantly improving dephosphorization and desulfurization capabilities (dephosphorization rate ≥85%), stabilizing slag foaming, enhancing the electric arc submersion effect, and thus improving thermal energy utilization efficiency. Simultaneously, fluorite (CaF2) effectively lowers the melting point of the slag and improves its fluidity, promotes the dissolution and dispersion of lime particles, accelerates the slag-forming kinetics process, and enhances the slag's ability to adsorb and remove non-metallic inclusions in molten steel, achieving deep purification.
[0047] In this embodiment of the invention, the metal reducing agent is ferrosilicon powder or aluminum powder; the binder is a composite of hydrolyzed starch and nano-bentonite, and the mass ratio of hydrolyzed starch to nano-bentonite is (2:1) to (3:1).
[0048] In one specific embodiment of the present invention, coke powder is used as a carbonaceous reducing agent, quicklime and fluorite are mixed at a ratio of 6:1, ferrosilicon powder is selected as the metal reducing agent, and the ratio of hydrolyzed starch to nano-bentonite in the binder is 2.5:1.
[0049] In one specific embodiment of the present invention, such as Figure 1 As shown, there are two tapered through holes 130.
[0050] Secondly, embodiments of the present invention also provide a method for preparing scrap steel briquettes 100 for electric arc furnace steelmaking, comprising the following steps:
[0051] S1. Raw material pretreatment: Preheating of scrap steel raw materials;
[0052] S2, Gradient feeding: The preheated scrap steel raw material and auxiliary materials are added to the briquetting mold in layers according to the ratio of the outer reduction zone 110 and the inner slag-forming zone 120. The mixture that constitutes the outer reduction zone 110 is added first, and then the mixture that constitutes the inner slag-forming zone 120 is added.
[0053] S3, High-pressure forming and channel preparation: Pressing and forming under pressure, and forming asymmetrically distributed tapered through holes 130 at the same time;
[0054] S4. Curing treatment: Curing the pressed blocks.
[0055] In step S1 above, the scrap steel raw material is preheated at a temperature of 200℃ to 400℃. For example, the preheating temperature can be 250℃, 300℃, or 350℃. The preheating time is determined based on the amount of scrap steel and equipment capacity, generally 2 to 4 hours. Preheating removes moisture and creates a slight oxide layer on the surface of the scrap steel, which is beneficial for subsequent bonding with the reducing agent. Furthermore, the carbonaceous reducing agent, slagging agent, and metal reducing agent are each pulverized to a particle size of less than 2mm to facilitate uniform mixing and subsequent pressing and molding.
[0056] In step S2 above, the preheated scrap steel raw material and auxiliary materials are added to the briquetting mold in layers according to the ratio of the outer reduction zone 110 and the inner slag-forming zone 120. Specifically, the mixture constituting the outer reduction zone 110 is added first, spread out, and then the mixture constituting the inner slag-forming zone 120 is added. During gradient material distribution, the mass ratio of the mixture in the outer reduction zone 110 to the inner slag-forming zone 120 is 3:7 to 4:6. Furthermore, the content of carbonaceous reducing agent and metallic reducing agent in the mixture in the outer reduction zone 110 is higher than that in the mixture in the inner slag-forming zone 120, and the content of slag-forming agent in the mixture in the inner slag-forming zone 120 is higher than that in the mixture in the outer reduction zone 110. This concentration difference can be achieved by preparing mixtures with different component contents separately.
[0057] In step S3 above, the material is pressed and formed under pressure, simultaneously creating asymmetrically distributed tapered through-holes 130. The pressing pressure is preferably 1200 MPa to 1500 MPa, and the holding time is 10 to 20 seconds. The tapered through-holes 130 are achieved by setting corresponding tapered mandrels in the mold. The large-end diameter, small-end diameter, and height of the mandrel are set according to the required hole diameter and depth. After pressing, the material is demolded to obtain a green compact with tapered through-holes 130.
[0058] In step S4 above, the pressed green block is cured. The curing treatment is preferably performed at a temperature of 80℃ to 120℃ for 2 to 4 hours. For example, the green block is cured at 110℃ for 3 hours. During the curing process, the hydrolyzed starch in the composite binder gelatinizes, and nano-bentonite fills the micropores, improving the cold and hot strength of the block.
[0059] The method for preparing scrap steel briquettes 100 for electric arc furnace steelmaking according to an embodiment of the present invention further includes the following steps:
[0060] S5. Forming an anti-oxidation coating on the inner wall of the tapered through hole 130: Prepare a slurry by mixing a metal reducing agent and a binder, and apply it to the inner wall of the tapered through hole 130 to form an anti-oxidation coating.
[0061] In step S5 above, the metal reducing agent and binder are mixed to form a slurry, which is then coated onto the inner wall of the conical through-hole 130 on the green briquette. Specifically, aluminum powder or ferrosilicon powder can be mixed with water glass or hydrolyzed starch in a certain proportion to form a slurry, which is then coated onto the conical inner wall of the conical through-hole 130 by spraying or dipping, and then naturally dried or dried at low temperature to form the final scrap steel briquette 100.
[0062] The scrap steel briquettes 100 for electric arc furnace steelmaking and their preparation method according to embodiments of the present invention have the following advantages:
[0063] 1. Achieving a sequential reaction of "reduction first, slag formation later". Since the reducing agent is enriched in the outer layer and the slag-forming agent in the inner layer, the outer layer reacts first after the briquettes are put into the furnace, forming a localized reducing atmosphere around the briquettes, inhibiting the oxidation and burn-off of iron elements, and simultaneously releasing chemical heat to accelerate melting. After the outer layer melts and peels off, the inner slag-forming agent enters the molten pool in large quantities. At this time, the molten pool has sufficient temperature and steel volume, and the slag-forming agent quickly forms slag and participates in the dephosphorization and desulfurization reactions. This sequential control avoids the problem of premature contact and solid-phase reaction between the reducing agent and slag-forming agent in existing technologies, resulting in mutual consumption. Practical application shows that using the briquettes of this invention can improve the overall scrap steel recovery rate and shorten the smelting cycle.
[0064] 2. Enhanced mass and heat transfer. Compared to ordinary circular straight holes, the asymmetrically distributed conical through-holes (130mm diameter) can guide the airflow in the furnace to generate eddies and localized turbulence, increasing the convective heat transfer coefficient. The conical structure itself also increases the heat transfer area. The anti-oxidation coating on the inner wall of the channels preferentially oxidizes at the initial high temperature, delaying channel collapse and extending the effective heat transfer time of the through-holes. Combined with scrap steel preheating and chemical heat supplementation of the reducing agent, the power consumption per ton of steel can be significantly reduced.
[0065] 3. Good structural stability. The composite binder of hydrolyzed starch and nano-bentonite, combined with preheating treatment and high-pressure molding, gives the briquettes high cold and hot strength. They are not easy to break or delaminate during transportation, stacking, and initial furnace loading, thus ensuring the integrity of the gradient functional structure.
[0066] 4. Significant environmental and economic benefits. Due to increased metal yield, shorter smelting cycle, and reduced electricity consumption, the production cost per ton of steel can be reduced, while the total amount of slag and dust emissions are also reduced.
[0067] To further illustrate the technical effects of the present invention, a comparative example is also provided, as follows.
[0068] Comparative Example
[0069] In the comparative example, the scrap steel briquette 100 also includes an outer reduction zone 110 and an inner slag-forming zone 120 with a mass ratio of 4:6. It also has two frustum-shaped channels and an anti-oxidation coating. The large diameter end of the channel has a diameter of 40 mm, the small diameter end has a diameter of 20 mm, and the depth is 80% of the thickness of the briquette. The inner wall of the channel is also coated with an anti-oxidation coating.
[0070] In the comparative example, the raw materials in the outer reduction zone 110, by mass percentage, include: 93% scrap steel, 4% carbonaceous reducing agent, 1% slagging agent, 1.5% metal reducing agent, and 0.5% binder. The raw materials in the inner slagging zone 120, by mass percentage, include: 77% scrap steel, 3.5% carbonaceous reducing agent, 18% slagging agent, 0.5% metal reducing agent, and 1% binder.
[0071] Comparative tests on smelting performance show that, as shown in Table 1, in terms of the melting process, the outer layer of the example reacts rapidly and the flame is strong and uniform within 0-2 minutes, while the outer layer reaction of the control group is weak; within 4-6 minutes, the foamy slag of the example is stable and has good heat transfer, while the control group's slag is too thick, has poor heat transfer, and splashes. The complete melting time of the example is 6 minutes and 15 seconds, while that of the control group is as long as 9 minutes and 8 seconds, an increase of 46.1%.
[0072] Table 1 Comparison of Melting Processes
[0073]
[0074] As shown in Table 2, in terms of metallurgical performance, the metal yield of the example reached 96.5%, while that of the comparative example was only 92.3%, a decrease of 4.2 percentage points; the endpoint [C] of the example was controlled at 0.19%±0.008, while that of the comparative example was 0.23%±0.042, with a fluctuation of more than 5 times; the dephosphorization rate of the example was 87.5%, while that of the comparative example was 76.8%; the foam slag index of the example was 1.8, while that of the comparative example was 0.8; the free CaO in the slag of the example was <3%, while that of the comparative example was as high as 14~18%.
[0075] Table 2 Quantitative Comparison of Metallurgical Performance
[0076]
[0077] Analysis revealed that the comparative example, with only 4% carbonaceous reducing agent in the outer layer, failed to create an effective CO reducing atmosphere, resulting in a C / O atomic ratio of only 0.62. This led to the failure of the outer layer's reducing function and severe iron oxidation. Furthermore, the comparative example's 18% inner layer slag-forming agent resulted in excessive lime, high free CaO levels, and overly thick slag, hindering heat transfer. The 3.5% inner layer carbonaceous reducing agent also caused uncontrolled carbon release. This rendered the gradient synergy of the comparative example completely ineffective, with each functional component interfering with the others, ultimately leading to a comprehensive economic loss of 171.1 yuan / ton of steel, as shown in Table 3. This clearly demonstrates that the proportioning range, gradient structure, pore design, and coating protection in the embodiments of this invention constitute a complete technical solution. Deviation from any single element will significantly reduce the overall effect, highlighting the synergistic relationship between the various technical features in the embodiments of this invention.
[0078] Table 3 Quantitative Comparison of Metallurgical Performance
[0079]
[0080] The present invention has been described above by way of example with reference to the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-described manner. Any non-substantial improvements made using the inventive concept and technical solution; or the direct application of the inventive concept and technical solution to other situations without modification, are all within the protection scope of the present invention.
Claims
1. A scrap steel briquettes for electric arc furnace steelmaking, characterized in that, It includes an outer reduction zone and an inner slag-forming zone arranged sequentially from the outside to the inside; the outer reduction zone contains carbonaceous reducing agent and metallic reducing agent, and the inner slag-forming zone contains slag-forming agent and carbonaceous reducing agent; the scrap steel briquette is provided with at least one conical through hole, which extends from the surface of the outer reduction zone to the inner slag-forming zone.
2. The scrap steel briquettes for electric arc furnace steelmaking according to claim 1, characterized in that, The mass ratio of the outer reduction zone to the inner slag-forming zone is (3:7) to (4:6).
3. The scrap steel briquettes for electric arc furnace steelmaking according to claim 1, characterized in that, The raw material composition of the outer reduction zone, by mass percentage, includes: 85%~90% scrap steel, 5%~10% carbonaceous reducing agent, 0~2% slag-forming agent, 1.5%~3% metal reducing agent, and 0.2%~1% binder.
4. The scrap steel briquettes for electric arc furnace steelmaking according to claim 1, characterized in that, The raw material composition of the inner slag-forming zone, by mass percentage, includes: 80%~85% scrap steel, 1%~3% carbonaceous reducing agent, 12%~16% slag-forming agent, 0~1% metal reducing agent, and 0.2%~1% binder.
5. The scrap steel briquettes for electric arc furnace steelmaking according to claim 1, characterized in that, The inner wall of the tapered through-hole is coated with an antioxidant coating, which contains a metal reducing agent and a binder.
6. The scrap steel briquettes for electric arc furnace steelmaking according to claim 5, characterized in that, The carbonaceous reducing agent is coke powder, anthracite powder, or graphite powder; the slag-forming agent is a mixture of quicklime and fluorite; in the inner slag-forming zone, the mass ratio of quicklime to fluorite is (10~12):(1.5~2); The metal reducing agent is ferrosilicon powder or aluminum powder; The binder is a composite of hydrolyzed starch and nano-bentonite, and the mass ratio of hydrolyzed starch to nano-bentonite is (2:1) to (3:1).
7. The scrap steel briquettes for electric arc furnace steelmaking according to any one of claims 1 to 3, characterized in that, The number of tapered through holes is two.
8. A method for preparing scrap steel briquettes for electric arc furnace steelmaking as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Raw material pretreatment: Preheating the scrap steel raw material; Gradient material distribution: The preheated scrap steel raw material and auxiliary materials are added to the briquetting mold in layers according to the ratio of the outer reduction zone and the inner slag-forming zone. The mixture that constitutes the outer reduction zone is added first, and then the mixture that constitutes the inner slag-forming zone is added. High-pressure forming and channel preparation: pressing and forming under pressure, while simultaneously forming asymmetrically distributed tapered through holes; Curing process: Curing the pressed blocks after they have been formed.
9. The method for preparing scrap steel briquettes for electric arc furnace steelmaking according to claim 8, characterized in that, The preheating temperature is 200℃~400℃; the pressing pressure is 1200 MPa~1500 MPa, and the holding time is 10 seconds~20 seconds; the curing treatment is to cure at 80℃~120℃ for 2 hours~4 hours.
10. The method for preparing scrap steel briquettes for electric arc furnace steelmaking according to claim 8 or 9, characterized in that, After the curing process, the method further includes the step of forming an antioxidant coating on the inner wall of the tapered through hole: preparing a slurry by mixing a metal reducing agent and a binder, and applying it to the inner wall of the tapered through hole to form the antioxidant coating.
Citation Information
Patent Citations
Scrap steel packing block and manufacturing method and steelmaking method thereof
CN114231693A