A method for controlling transverse wrinkles on thin-gauge hot-rolled steel with a strength of 355MPa.

By optimizing processes such as RH vacuum denitrification and Ti microalloying, combined with KR desulfurization, converter smelting, and low-temperature coiling, the problems of surface transverse fold defects and long production cycles of 355MPa strength grade thin-gauge hot-rolled steel have been solved, achieving efficient production of high-quality hot-rolled steel.

CN123108239APending Publication Date: 2026-11-17HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611330220.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing 355MPa strength grade thin-gauge hot-rolled steel is prone to surface transverse crease defects during the smelting process, and the production cycle is long, making it difficult to meet the requirements of high surface quality and cost control.

Method used

By using RH vacuum denitrification and Ti microalloying, the N content in the steel is controlled to be ≤0.0055%. Combined with KR desulfurization, converter smelting, argon station slag washing and high-alumina pre-melted slag washing, the slag basicity and the Mn/S ratio of the molten steel are controlled. With the help of dynamic light reduction and low temperature coiling, the center segregation and center porosity of the slab are optimized, and the low temperature control of the finishing rolling and coiling steps is achieved.

Benefits of technology

It effectively suppresses surface transverse crease defects, significantly shortens the production cycle, improves the surface quality and production efficiency of products, and meets the high strength and aesthetic requirements of thin-gauge hot-rolled steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108239A_ABST
    Figure CN123108239A_ABST
Patent Text Reader

Abstract

This invention provides a method for controlling transverse wrinkles on the surface of 355MPa strength-grade thin-gauge hot-rolled steel, comprising the following steps: RH vacuum denitrification treatment of molten steel, followed by Ti microalloying to obtain refined molten steel; continuous casting of the refined molten steel to obtain a slab, wherein the center segregation and center porosity of the slab are both ≤C1.5; heating the slab to 1150~1230℃, performing rough rolling and finish rolling respectively, followed by ultra-rapid cooling and laminar flow cooling respectively, and finally coiling to obtain a steel coil. The control method of this invention is simple, easy to operate, significantly shortens the production cycle of thin-gauge hot-rolled steel, and the surface quality of the obtained product meets the usage requirements, with good appearance and promising prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hot-rolled steel production technology, and in particular to a 355MPa strength grade thin-gauge hot-rolled steel and a method for controlling surface transverse wrinkles. Background Technology

[0002] Low-alloy high-strength structural steel with a strength grade of 355MPa, as an important variety of hot-rolled coil, is characterized by high strength, good toughness, and excellent weldability, and is widely used in construction, bridges, and machinery manufacturing. With increasing competition in the steel market and rising cost control requirements from downstream users, the "hot rolling over cold rolling" process for thin-gauge hot-rolled products has become a significant industry trend. This involves directly replacing the traditional long-process "hot rolling + cold rolling + pickling" with hot rolling, while ensuring surface quality and performance, thereby significantly shortening the production cycle and reducing manufacturing costs. However, in the smelting process of 355MPa strength grade thin-gauge hot-rolled steel and the process of reducing alloy costs, surface quality control faces severe challenges, with transverse crease defects becoming a bottleneck restricting the quality improvement of this type of product.

[0003] Transverse crease defects are crease-like defects on the surface of thin-gauge hot-rolled strip steel, perpendicular or nearly perpendicular to the rolling direction. They typically appear gradually during the uncoiling process as the coil diameter decreases and the curvature increases, severely affecting the surface aesthetics and downstream performance of the product. Studies have shown that the presence of a yield plateau in the material's stress-strain curve and high nitrogen content in the molten steel are the main internal causes of transverse crease defects. For example, the yield plateau causes concentrated plastic deformation, while high nitrogen content exacerbates the pinning effect of Cotillard atmospheres on dislocations, further extending the yield plateau length. Currently, for thin-gauge products with high surface quality requirements, the industry commonly uses cold rolling and pickling processes to eliminate transverse crease defects. However, this process has drawbacks such as long production cycles, high energy consumption, and increased material costs. Based on this, this invention provides a method for controlling transverse creases on the surface of 355MPa strength-grade thin-gauge hot-rolled steel, to solve the problems of easy generation of transverse crease defects and long production cycles in existing thin-gauge hot-rolled steel. Summary of the Invention

[0004] The main objective of this invention is to provide a method for controlling transverse wrinkles on the surface of 355MPa strength grade thin-gauge hot-rolled steel, aiming to solve the technical problems of easy generation of transverse wrinkle defects and long production cycle of existing thin-gauge hot-rolled steel.

[0005] To achieve the above objectives, the present invention provides a method for controlling transverse wrinkles on the surface of thin-gauge hot-rolled steel with a strength of 355MPa, comprising the following steps: S1: The molten steel is subjected to RH vacuum denitrification treatment and Ti is added for microalloying to obtain refined molten steel.

[0006] S2: The refined molten steel is continuously cast to obtain a slab, wherein the center segregation and center porosity of the slab are both ≤C1.5.

[0007] S3: The slab is heated to 1150~1230℃, and then subjected to rough rolling and finish rolling in sequence, followed by ultra-fast cooling and laminar flow cooling, and finally coiled to obtain a steel coil.

[0008] The finishing rolling temperature is 810~850℃.

[0009] The winding temperature is 480~550℃.

[0010] The chemical composition of the refined steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the remainder being iron and other unavoidable impurities.

[0011] The thickness of thin-gauge hot-rolled steel with a strength of 355MPa is ≤4mm.

[0012] According to the embodiments of this application, the vacuum degree of the RH vacuum denitrification treatment is 100~133Pa, and after circulating for 6~8 minutes, Ti is added and circulated for 2~3 minutes. After breaking the vacuum, the mixture is gently blown and stirred for 8~12 minutes to obtain the refined molten steel.

[0013] The nitrogen content in the refined steel is ≤0.0050%.

[0014] The Ti / N mass ratio in the refined steel is ≥2.8.

[0015] According to the embodiments of this application, the steel preparation steps include: after KR desulfurization of molten iron, it is smelted in a converter, and then slag washed in an argon station to obtain the molten steel.

[0016] The iron-to-metal ratio is ≥75%.

[0017] The slag basicity (CaO / SiO2) after steelmaking in the converter is 4-7.

[0018] The mass ratio of Mn / S in the molten steel is ≥30.

[0019] According to the embodiments of this application, the S content in the molten iron after KR desulfurization is ≤0.005%.

[0020] Before tapping, add 1.5~3.0 kg / t of lime to the ladle. 50~75 seconds before tapping is complete, add 1.5~3.5 kg / t of lime and high-alumina pre-melted slag.

[0021] The composition of the lime, by mass fraction, includes: CaO≥90%, SiO2≤5%, MgO 4~8%, moisture≤0.5%, with the balance being unavoidable impurities.

[0022] The composition of the high-alumina pre-melted slag, by mass fraction, includes: Al2O3 20~30%, CaO 50~60%, SiO2 ≤15%, MgO 4~8%, with the balance being unavoidable impurities.

[0023] According to an embodiment of this application, the casting superheat of the continuous casting is 10~25°C.

[0024] The continuous casting employs dynamic light reduction, with a reduction amount of 4~6mm.

[0025] The casting speed is 4.0~4.5m / min.

[0026] According to the embodiments of this application, the furnace exit temperature of the slab after heating is 1170~1220℃.

[0027] The feed temperature of the roughing mill is ≤980℃.

[0028] The inlet temperature of the finishing mill is 830~870℃.

[0029] According to an embodiment of this application, the ultra-fast cooling rate is 20~30℃ / s.

[0030] The laminar flow cooling rate is 10~15℃ / s.

[0031] According to an embodiment of this application, the thickness of the 355MPa strength grade thin-gauge hot-rolled steel is 1.5~4mm.

[0032] The steel coil is naturally cooled to an uncoiling temperature of ≤50℃.

[0033] This invention provides a 355MPa strength grade thin-gauge hot-rolled steel, which is prepared according to the above-mentioned method for controlling the transverse wrinkles on the surface of the 355MPa strength grade thin-gauge hot-rolled steel.

[0034] According to the embodiments of this application, the chemical composition of the 355MPa strength grade thin-gauge hot-rolled steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the balance being Fe and unavoidable impurities.

[0035] The yield strength of the 355MPa strength grade thin-gauge hot-rolled steel is 380~450MPa.

[0036] The tensile strength of the 355MPa strength grade thin-gauge hot-rolled steel is 500~580MPa.

[0037] The elongation of the 355MPa strength grade thin-gauge hot-rolled steel is ≥22%.

[0038] The yield plateau length of the 355MPa strength grade thin-gauge hot-rolled steel is ≤3.5mm, and the surface is free of transverse creases.

[0039] Compared with the prior art, the beneficial effects of the present invention are as follows: The aforementioned method for controlling transverse wrinkles on the surface of 355 MPa strength-grade thin-gauge hot-rolled steel achieves effective suppression of transverse wrinkles and a significant reduction in production cycle through synergistic regulation of composition and process. Specifically, RH vacuum denitrification treatment strictly controls the N content in the steel to ≤0.0055%, and adds Ti for microalloying. Ti preferentially combines with N to form fine and stable TiN, effectively reducing the N content dissolved in ferrite and the formation of coarse TiN precipitates at grain boundaries. This reduces the pinning effect of Cotillard atmospheres formed by C and N interstitial atoms on dislocations, thereby shortening the yield plateau length YPE in the tensile curve and reducing the risk of transverse wrinkles during stamping. Through KR desulfurization, converter smelting, argon station slag washing, and washing with tapping lime and high-alumina pre-melted slag, along with controlling slag basicity and the Mn / S ratio of molten steel, the cleanliness of the molten steel is effectively improved, reducing the number and size of inclusions and minimizing transverse wrinkle defects induced by stress concentration around inclusions. By controlling the center segregation and porosity of the slab to ≤C1.5, the uniformity and density of the internal structure of the slab are significantly improved, thus enhancing the surface quality of thin-gauge hot-rolled steel. Furthermore, this invention utilizes vacuum denitrification to control the yield plateau length of the material at low temperatures during the finishing rolling and coiling steps.

[0040] The control method of this invention is simple and easy to operate, requiring no additional post-processing steps such as offline annealing, surface grinding, or repeated leveling. The process flow is concise, significantly shortening the production cycle of thin-gauge hot-rolled steel and improving production line efficiency and yield. This control method is particularly suitable for the production of thin-gauge 355 MPa grade hot-rolled steel with a thickness ≤4mm. The resulting products meet usage requirements in terms of surface quality and have a good aesthetic appearance, demonstrating promising prospects for industrial application. Attached Figure Description

[0041] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0042] Figure 1 This is a photograph of the 355MPa strength grade thin-gauge hot-rolled steel obtained in Example 1; Figure 2 This is a photograph of the hot-rolled steel produced in Comparative Example 1.

[0043] The realization of the objective, functional characteristics and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0044] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0045] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.

[0046] To achieve the above objectives, the present invention provides a method for controlling transverse wrinkles on the surface of thin-gauge hot-rolled steel with a strength of 355MPa, comprising the following steps: S1: The molten steel is subjected to RH vacuum denitrification treatment and Ti is added for microalloying to obtain refined molten steel.

[0047] S2: The refined molten steel is continuously cast to obtain a slab, wherein the center segregation and center porosity of the slab are both ≤C1.5.

[0048] S3: The slab is heated to 1150~1230℃, and then subjected to rough rolling and finish rolling in sequence, followed by ultra-fast cooling and laminar flow cooling, and finally coiled to obtain a steel coil.

[0049] The finishing rolling temperature is 810~850℃.

[0050] The winding temperature is 480~550℃.

[0051] The chemical composition of the refined steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the remainder being iron and other unavoidable impurities.

[0052] The thickness of thin-gauge hot-rolled steel with a strength of 355MPa is ≤4mm.

[0053] In some embodiments, the slab is heated to 1170~1210°C and subjected to rough rolling and finish rolling in sequence.

[0054] In some embodiments, the finishing rolling temperature is 810~845℃.

[0055] In some embodiments, the winding temperature is 480~520°C.

[0056] In some embodiments, the winding temperature is 480~516°C.

[0057] In some embodiments, the chemical composition of the refined steel, by mass fraction, includes: C 0.18~0.20%, Si 0.10~0.18%, Mn 0.30~0.40%, Als 0.018~0.030%, Ti 0.013~0.019%, P≤0.020%, S≤0.010%, N≤0.0045%, with the remainder being iron and other unavoidable impurities.

[0058] In some embodiments, the chemical composition of the refined steel, by mass fraction, includes: C 0.185~0.195%, Si 0.103~0.160%, Mn 0.35~0.40%, Als 0.0186~0.022%, Ti 0.0135~0.0185%, P≤0.020%, S≤0.010%, N≤0.0045%, with the remainder being iron and other unavoidable impurities.

[0059] The aforementioned method for controlling transverse wrinkles on the surface of 355 MPa strength-grade thin-gauge hot-rolled steel achieves effective suppression of transverse wrinkles and a significant reduction in production cycle through synergistic regulation of composition and process. Specifically, RH vacuum denitrification treatment strictly controls the N content in the steel to ≤0.0055%, and adds Ti for microalloying. Ti preferentially combines with N to form fine and stable TiN, effectively reducing the N content dissolved in ferrite and the formation of coarse TiN precipitates at grain boundaries. This reduces the pinning effect of Cotillard atmospheres formed by C and N interstitial atoms on dislocations, thereby shortening the yield plateau length YPE in the tensile curve and reducing the risk of transverse wrinkles during stamping. Through KR desulfurization, converter smelting, argon station slag washing, and washing with tapping lime and high-alumina pre-melted slag, along with controlling slag basicity and the Mn / S ratio of molten steel, the cleanliness of the molten steel is effectively improved, reducing the number and size of inclusions and minimizing transverse wrinkle defects induced by stress concentration around inclusions. By controlling the center segregation and porosity of the slab to ≤C1.5, the uniformity and density of the internal structure of the slab are significantly improved, thus enhancing the surface quality of thin-gauge hot-rolled steel. Furthermore, this invention utilizes vacuum denitrification to control the yield plateau length of the material at low temperatures during the finishing rolling and coiling steps.

[0060] In some embodiments, the vacuum degree of the RH vacuum denitrification treatment is 100~133Pa, and after circulating for 6~8 minutes, Ti is added and circulated for 2~3 minutes. After breaking the vacuum, the mixture is gently blown and stirred for 8~12 minutes to obtain the refined molten steel.

[0061] The nitrogen content in the refined steel is ≤0.0050%.

[0062] The Ti / N mass ratio in the refined steel is ≥2.8.

[0063] In some embodiments, the vacuum degree of the RH vacuum denitrification process is 105~125 Pa.

[0064] In some embodiments, the vacuum degree of the RH vacuum denitrification process is 110~123 Pa.

[0065] In some embodiments, the nitrogen content in the refined steel is ≤0.0045%.

[0066] In some embodiments, the steel preparation steps include: performing KR desulfurization on the molten iron, then smelting it in a converter, and finally washing the slag in an argon station to obtain the molten steel.

[0067] The iron-to-metal ratio is ≥75%.

[0068] The slag basicity (CaO / SiO2) after steelmaking in the converter is 4-7.

[0069] The mass ratio of Mn / S in the molten steel is ≥30.

[0070] In some embodiments, the molten iron ratio is 75-85%.

[0071] In some embodiments, the slag basicity (CaO / SiO2) after steelmaking in the converter is 5.0 to 6.5.

[0072] In some embodiments, the slag basicity CaO / SiO2 after steelmaking in the converter is 5.2~6.0.

[0073] In some embodiments, the Mn / S mass ratio in the molten steel is 30-45.

[0074] In some embodiments, the Mn / S mass ratio in the molten steel is 35-45.

[0075] In some embodiments, the sulfur content in the molten iron after KR desulfurization is ≤0.005%.

[0076] Before tapping, add 1.5~3.0 kg / t of lime to the ladle. 50~75 seconds before tapping is complete, add 1.5~3.5 kg / t of lime and high-alumina pre-melted slag.

[0077] The composition of the lime, by mass fraction, includes: CaO≥90%, SiO2≤5%, MgO 4~8%, moisture≤0.5%, with the balance being unavoidable impurities.

[0078] The composition of the high-alumina pre-melted slag, by mass fraction, includes: Al2O3 20~30%, CaO 50~60%, SiO2 ≤15%, MgO 4~8%, with the balance being unavoidable impurities.

[0079] In some embodiments, 1.6~2.3 kg / t of lime is added to the ladle before tapping, and 1.8~3.0 kg / t of lime and high-alumina pre-melted slag are added 60~75 seconds before tapping is completed.

[0080] In some embodiments, the casting superheat of the continuous casting is 10~25°C.

[0081] The continuous casting employs dynamic light reduction, with a reduction amount of 4~6mm.

[0082] The casting speed is 4.0~4.5m / min.

[0083] In some embodiments, the casting superheat of the continuous casting is 15~25°C.

[0084] In some embodiments, the casting superheat of the continuous casting is 17~21°C.

[0085] In some embodiments, the continuous casting employs dynamic light reduction, with a reduction amount of 4.5~5mm.

[0086] In some embodiments, the casting speed of the continuous casting is 4.2~4.5 m / min.

[0087] In some embodiments, the furnace exit temperature of the slab after heating is 1170~1220℃.

[0088] The feed temperature of the roughing mill is ≤980℃.

[0089] The inlet temperature of the finishing mill is 830~870℃.

[0090] In some embodiments, the furnace exit temperature of the slab after heating is 1170~1210℃.

[0091] In some embodiments, the feed temperature of the roughing mill is 970~980°C.

[0092] In some embodiments, the inlet temperature of the finishing mill is 850~860°C.

[0093] In some embodiments, the ultra-fast cooling rate is 20~30℃ / s.

[0094] The laminar flow cooling rate is 10~15℃ / s.

[0095] In some embodiments, the ultra-fast cooling rate is 20~25℃ / s.

[0096] In some embodiments, the ultra-fast cooling rate is 22~24℃ / s.

[0097] In some embodiments, the laminar cooling rate is 12~14°C / s.

[0098] In some embodiments, the thickness of the 355MPa strength grade thin-gauge hot-rolled steel is 1.5~4mm.

[0099] The steel coil is naturally cooled to an uncoiling temperature of ≤50℃.

[0100] In some embodiments, the thickness of the 355MPa strength grade thin-gauge hot-rolled steel is 2.0~3.5mm.

[0101] The control method of this invention is simple and easy to operate, requiring no additional post-processing steps such as offline annealing, surface grinding, or repeated leveling. The process flow is concise, significantly shortening the production cycle of thin-gauge hot-rolled steel and improving production line efficiency and yield. This control method is particularly suitable for the production of thin-gauge 355 MPa grade hot-rolled steel with a thickness ≤4mm. The resulting products meet usage requirements in terms of surface quality and have a good aesthetic appearance, demonstrating promising prospects for industrial application.

[0102] This invention provides a 355MPa strength grade thin-gauge hot-rolled steel, which is prepared according to the above-mentioned method for controlling the transverse wrinkles on the surface of the 355MPa strength grade thin-gauge hot-rolled steel.

[0103] In some embodiments, the chemical composition of the 355MPa strength grade thin-gauge hot-rolled steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the balance being Fe and unavoidable impurities.

[0104] The yield strength of the 355MPa strength grade thin-gauge hot-rolled steel is 380~450MPa.

[0105] The tensile strength of the 355MPa strength grade thin-gauge hot-rolled steel is 500~580MPa.

[0106] The elongation of the 355MPa strength grade thin-gauge hot-rolled steel is ≥22%.

[0107] The yield plateau length of the 355MPa strength grade thin-gauge hot-rolled steel is ≤3.5mm, and the surface is free of transverse creases.

[0108] In some embodiments, the yield strength of the 355MPa strength grade thin-gauge hot-rolled steel is 390~430MPa.

[0109] In some embodiments, the yield strength of the 355MPa strength grade thin-gauge hot-rolled steel is 396~415MPa.

[0110] In some embodiments, the tensile strength of the 355MPa strength grade thin-gauge hot-rolled steel is 510~560MPa.

[0111] In some embodiments, the tensile strength of the 355MPa strength grade thin-gauge hot-rolled steel is 524~542MPa.

[0112] In some embodiments, the elongation of the 355MPa strength grade thin-gauge hot-rolled steel is 22-30%.

[0113] In some embodiments, the elongation of the 355MPa strength grade thin-gauge hot-rolled steel is 25-30%.

[0114] In some embodiments, the elongation of the 355MPa strength grade thin-gauge hot-rolled steel is 27-30%.

[0115] In some embodiments, the yield plateau length of the 355MPa strength grade thin-gauge hot-rolled steel is 1.5~3.5mm.

[0116] In some embodiments, the yield plateau length of the 355MPa strength grade thin-gauge hot-rolled steel is 1.8~2.9mm.

[0117] To further illustrate the present invention, the following examples are provided: Example 1 A method for controlling transverse wrinkles on the surface of 2.5mm thick, 355MPa strength grade hot-rolled steel, comprising the following steps: S1: The molten iron undergoes KR desulfurization treatment, with an iron-to-water ratio of 83%. The sulfur content in the desulfurized molten iron is 0.002%. It is then smelted in a converter at a temperature of 1350℃. A top-and-bottom blown converter is used for smelting, and slag-retaining tapping is employed. The slag discharge from the converter is 3.5 kg / t. Before tapping, 2.0 kg / t of lime is added to the ladle. 60 seconds before tapping, 3.0 kg / t of lime and high-alumina pre-melted slag are added. During tapping, C, Si, and Mn alloying is performed. The alloy content of elements other than Ti is adjusted to over 80% of the target content before tapping from the argon station. The slag basicity of the molten steel after tapping is 5.5, and the Mn / S mass ratio in the molten steel is 43. After stirring for 10 minutes, molten steel is obtained. The molten steel undergoes RH vacuum denitrification treatment at a vacuum degree of 110 Pa. After 7.5 minutes of circulation, Ti is added, followed by 2.5 minutes of circulation. After breaking the vacuum, soft blowing and stirring for 9 minutes yields refined molten steel. The chemical composition of the refined molten steel, by mass fraction, is: C 0.185%, Si 0.113%, Mn 0.35%, P 0.0112%, S 0.008%, Al 0.0186%, N 0.0045%, Ti 0.0135%, with the balance being iron and unavoidable impurities.

[0118] S2: Refined molten steel is continuously cast at a superheat of 20°C. The casting speed is 4.2 m / min, and a dynamic light reduction of 4.5 mm is used to obtain a slab. The center segregation and center porosity of the slab are both C1.0.

[0119] S3: The slab is heated to 1170℃, and after exiting the furnace, it undergoes rough rolling and finish rolling. The entry temperature for rough rolling is 970℃, the entry temperature for finish rolling is 850℃, and the final rolling temperature for finish rolling is 845℃. Then, it undergoes ultra-rapid cooling and laminar flow cooling respectively, with an ultra-rapid cooling rate of 24℃ / s and a laminar flow cooling rate of 12℃ / s. Finally, it is coiled at a temperature of 516℃ to obtain a steel coil. The steel coil is then naturally cooled to an uncoiling temperature of 30℃ to obtain a 2.5mm thick, 355MPa strength grade thin-gauge hot-rolled steel. See [link to relevant documentation]. Figure 1 .

[0120] Tests showed that the 355MPa strength grade thin-gauge hot-rolled steel prepared in Example 1 had a yield strength of 410MPa, a tensile strength of 534MPa, an elongation of 27%, and a yield plateau length of 2.9mm; the surface had no transverse creases.

[0121] Example 2 A method for controlling transverse wrinkles on the surface of 2.5mm thick, 355MPa strength grade hot-rolled steel, comprising the following steps: S1: Molten iron undergoes KR desulfurization treatment, with an iron-to-water ratio of 85%. The sulfur content in the desulfurized molten iron is 0.002%. It is then smelted in a converter at a temperature of 1380℃. A top-and-bottom blown converter is used for smelting and tapping, employing slag-blocking and slag-retaining tapping techniques, controlling the slag discharge at 3.0 kg / t. Before tapping, 2.3 kg / t of lime is added to the ladle, and 2.8 kg / t of lime and high-alumina pre-melted slag are added 60 seconds before tapping is complete. During tapping, C, Si, and Mn alloying is performed. The alloy content of elements other than Ti is adjusted to over 80% of the target content before tapping from the argon station. The slag basicity after tapping the molten steel is 6.0, and the Mn / S mass ratio in the molten steel is 37. The mixture is stirred for 10 minutes to obtain the final molten steel. Molten steel was subjected to RH vacuum denitrification treatment at a vacuum degree of 113 Pa. After 7.5 min of circulation, Ti was added for 2.5 min of microalloying. After breaking the vacuum, the mixture was gently blown and stirred for 10 min to obtain refined molten steel. The chemical composition of the refined molten steel, by mass fraction, was: C 0.195%, Si 0.103%, Mn 0.40%, P 0.0132%, S 0.009%, Al 0.0196%, N 0.0042%, Ti 0.0185%, with the balance being iron and unavoidable impurities.

[0122] S2: Refined molten steel is continuously cast at a superheat of 18°C. The casting speed is 4.4 m / min, and a dynamic light reduction of 4.5 mm is used to obtain a slab. The center segregation and center porosity of the slab are both C1.5.

[0123] S3: The slab is heated to 1170℃, and after exiting the furnace, it is subjected to rough rolling and finish rolling respectively. The entry temperature of rough rolling is 970℃, the entry temperature of finish rolling is 850℃, and the finishing rolling temperature is 815℃. Then, it is subjected to ultra-rapid cooling and laminar flow cooling respectively. The ultra-rapid cooling rate is 22℃ / s, and the laminar flow cooling rate is 13℃ / s. Finally, it is coiled at a temperature of 486℃ to obtain a steel coil. The steel coil is naturally cooled to an uncoiling temperature of 25℃ to obtain a 2.5mm thick, 355MPa strength grade thin-gauge hot-rolled steel.

[0124] Tests showed that the 355MPa strength grade thin-gauge hot-rolled steel obtained in Example 2 had a yield strength of 396MPa, a tensile strength of 524MPa, an elongation of 30%, and a yield plateau length of 1.8mm; the surface had no transverse creases.

[0125] Example 3 A method for controlling transverse wrinkles on the surface of 2.0mm thick, 355MPa strength grade hot-rolled steel, comprising the following steps: The molten iron was subjected to KR desulfurization treatment with a molten iron ratio of 75% and a sulfur content of 0.002% after desulfurization. It was then smelted in a converter at a temperature of 1380℃. Steelmaking was carried out using a top-and-bottom blown converter, employing slag-blocking and slag-retaining tapping techniques. The slag amount was controlled at 3.2 kg / t. Before tapping, 1.6 kg / t of lime was added to the ladle, and 1.8 kg / t of lime and high-alumina pre-melted slag were added 70 seconds before tapping. During tapping, alloying with elements such as C, Si, and Mn was performed. The alloy content of elements other than Ti was adjusted to over 80% of the target content before tapping from the argon station. The slag basicity after tapping the molten steel was 5.6, and the Mn / S mass ratio in the molten steel was 36. After stirring for 10 minutes, molten steel was obtained. The molten steel underwent RH vacuum denitrification treatment at a vacuum degree of 113 Pa. After 7 minutes of circulation, Ti was added and circulated for 2.2 minutes. Following vacuum breaking, soft blowing and stirring were performed for 9.7 minutes to obtain refined molten steel. The chemical composition of the refined molten steel, by mass fraction, was: C 0.19%, Si 0.160%, Mn 0.36%, Al 0.5%. 0.021%, Ti 0.016%, P 0.020%, S 0.010%, N 0.0038%, balance is iron and unavoidable impurities.

[0126] S2: Refined molten steel is continuously cast at a superheat of 21°C. The casting speed is 4.5 m / min, and a dynamic light reduction of 5 mm is used to obtain a slab. The center segregation and center porosity of the slab are both C1.5.

[0127] S3: The slab is heated to 1210℃, and after exiting the furnace, it is subjected to rough rolling and finish rolling. The entry temperature of rough rolling is 970℃, the entry temperature of finish rolling is 850℃, and the final rolling temperature of finish rolling is 810℃. Then, it is subjected to ultra-rapid cooling and laminar flow cooling respectively. The ultra-rapid cooling rate is 22℃ / s, and the laminar flow cooling rate is 12℃ / s. Finally, it is coiled at a temperature of 490℃ to obtain a steel coil. The steel coil is naturally cooled to an uncoiling temperature of 30℃ to obtain a 2.0mm thick, 355MPa strength grade thin-gauge hot-rolled steel.

[0128] Tests showed that the yield strength of the 355MPa strength grade thin-gauge hot-rolled steel prepared in Example 3 was 405MPa, the tensile strength was 531MPa, and the elongation was 29%; the surface had no transverse creases.

[0129] Example 4 A method for controlling transverse wrinkles on the surface of 3.5mm thick, 355MPa strength grade thin-gauge hot-rolled steel, comprising the following steps: S1: Molten iron undergoes KR desulfurization treatment, with an iron-to-water ratio of 80%. The sulfur content in the desulfurized molten iron is 0.002%. It is then smelted in a converter at a temperature of 1380℃. A top-and-bottom blown converter is used for smelting and tapping, employing slag-blocking and slag-retaining tapping techniques, controlling the slag discharge to 3.2 kg / t. Before tapping, 2.0 kg / t of lime is added to the ladle. 75 seconds before tapping, another 2.0 kg / t of lime and high-alumina pre-melted slag are added. During tapping, C, Si, and Mn alloying is performed. The alloy content of elements other than Ti is adjusted to over 80% of the target content before tapping from the argon station. The slag basicity after tapping is 5.2, and the Mn / S mass ratio in the molten steel is 44. The mixture is stirred for 10 minutes to obtain the final molten steel. Molten steel was subjected to RH vacuum denitrification treatment at a vacuum degree of 123 Pa. After 6 min of circulation, Ti was added and circulated for 2 min. After breaking the vacuum, the mixture was gently blown and stirred for 9.7 min to obtain refined molten steel. The chemical composition of the refined molten steel, by mass fraction, was: C 0.185%, Si 0.12%, Mn 0.35%, Als 0.022%, Ti 0.016%, P 0.016%, S 0.008%, N 0.0037%, with the balance being iron and unavoidable impurities.

[0130] S2: Refined molten steel is continuously cast at a superheat of 17°C. The casting speed is 4.3 m / min, and a dynamic light reduction of 5 mm is used to obtain a slab. The center segregation and center porosity of the slab are both C1.5.

[0131] S3: The slab is heated to 1200℃, and after exiting the furnace, it is subjected to rough rolling and finish rolling respectively. The entry temperature of rough rolling is 970℃, the entry temperature of finish rolling is 860℃, and the finishing rolling temperature is 810℃. Then, it is subjected to ultra-rapid cooling and laminar flow cooling respectively. The ultra-rapid cooling rate is 23℃ / s, and the laminar flow cooling rate is 14℃ / s. Finally, it is coiled at a temperature of 480℃ to obtain a steel coil. The steel coil is naturally cooled to an uncoiling temperature of 30℃ to obtain a 3.5mm thick, 355MPa strength grade thin-gauge hot-rolled steel.

[0132] Tests showed that the yield strength of the 355MPa strength grade thin-gauge hot-rolled steel prepared in Example 4 was 415MPa, the tensile strength was 542MPa, and the elongation was 28%; the surface had no transverse creases.

[0133] Comparative Example 1 A method for controlling transverse wrinkles on the surface of hot-rolled steel with a thickness of 2.5 mm, comprising the following steps: S1: The molten iron undergoes KR desulfurization treatment, resulting in an S content of 0.002% in the converter, a converter temperature of 1350℃, and an iron-to-stain ratio of 78%. A top-and-bottom blown converter is used for initial refining, producing a C content of 0.08% in the tapped steel, using a slag-blocking and slag-retaining tapping operation. LF refining with white slag is employed, achieving a slag basicity of 5.2. After adjusting the steel composition appropriately, calcium treatment is performed to modify inclusions, resulting in a Ca content of 0.0015%. The mixture is stirred for 10 minutes and then poured at a suitable temperature. The resulting molten steel has the following chemical composition by mass fraction: C 0.185%, Si 0.113%, Mn 0.45%, P 0.0152%, S 0.008%, Als 0.0226%, Ti 0.0335%, N 0.0065%, with the balance being iron and unavoidable impurities.

[0134] S2: The time from molten steel leaving the LF station to continuous casting is 25 minutes. The superheat during casting is 15℃, the casting speed is 1.15m / min, and the dynamic light reduction at the end of solidification is 4.5mm, resulting in a 230mm thick slab. The slab has a center segregation and center porosity grade of C1.0, with no defects such as central cracks or triangular cracks. The slab is placed in the heating furnace 15 hours after casting.

[0135] S3: After heating the slab, descaling, rough rolling, finish rolling, and coiling are performed. The furnace exit temperature is 1175℃, and the finish rolling temperature is 885℃. After finish rolling, ultra-rapid cooling and laminar flow cooling are carried out, and the coiling temperature is 626℃, resulting in hot-rolled steel with a thickness of 2.5mm. See [link / reference]. Figure 2 .

[0136] Tests showed that the hot-rolled steel prepared in Comparative Example 1 had a yield strength of 421 MPa, a tensile strength of 552 MPa, an elongation of 26.5%, and a yield plateau length of 3.8 mm; the surface had obvious transverse creases, with a transverse crease occurrence rate of 80%.

[0137] Comparative Example 2 Compared to Example 1, the N content in the molten steel and the parameters of RH vacuum denitrification were changed.

[0138] In Comparative Example 2, the nitrogen content in the molten steel was 0.0070%, the vacuum degree of RH vacuum denitrification was 235 Pa, and the cycle was 5 min. The denitrification was not sufficient, resulting in poor denitrification effect. The nitrogen content after refining was 0.0070%. Other steps were the same as in Example 1.

[0139] Tests showed that the hot-rolled steel prepared in Comparative Example 2 had a yield strength of 378 MPa, a tensile strength of 496 MPa, an elongation of 28%, and obvious transverse creases on the surface, with a transverse crease occurrence rate of 75%.

[0140] Comparative Example 3 Compared to Example 1, the continuous casting process was changed.

[0141] In Comparative Example 3, without dynamic light pressing, the slab exhibited center segregation of grade C3.0 and center porosity of grade 2.0. Other steps were the same as in Example 1.

[0142] Tests showed that the hot-rolled steel prepared in Comparative Example 3 had a yield strength of 390 MPa, a tensile strength of 520 MPa, and an elongation of 22.5%. However, the poor internal quality of the slab resulted in the presence of banded structures of more than 2.5 mm in the hot-rolled steel, and transverse creases appeared on the material surface, with a transverse crease occurrence rate of 80%.

[0143] Comparative Example 4 Compared to Example 1, the winding temperature was changed.

[0144] In Comparative Example 4, the winding temperature was 630°C. Other steps were the same as in Example 1.

[0145] Tests showed that the hot-rolled steel prepared in Comparative Example 4 had a yield strength of 320 MPa, a tensile strength of 455 MPa, and an elongation of 30%. Due to the excessively high coiling temperature, the mechanical properties of the hot-rolled steel were unqualified.

[0146] The aforementioned method for controlling transverse wrinkles on the surface of 355 MPa strength-grade thin-gauge hot-rolled steel achieves effective suppression of transverse wrinkles and a significant reduction in production cycle through synergistic regulation of composition and process. Specifically, RH vacuum denitrification treatment strictly controls the N content in the steel to ≤0.0055%, and adds Ti for microalloying. Ti preferentially combines with N to form fine and stable TiN, effectively reducing the N content dissolved in ferrite and the formation of coarse TiN precipitates at grain boundaries. This reduces the pinning effect of Cotillard atmospheres formed by C and N interstitial atoms on dislocations, thereby shortening the yield plateau length YPE in the tensile curve and reducing the risk of transverse wrinkles during stamping. Through KR desulfurization, converter smelting, argon station slag washing, and washing with tapping lime and high-alumina pre-melted slag, along with controlling slag basicity and Mn / S ratio, the cleanliness of the molten steel is effectively improved, reducing the number and size of inclusions and minimizing transverse wrinkle defects induced by stress concentration around inclusions. By controlling the center segregation and porosity of the slab to ≤C1.5, the uniformity and density of the internal structure of the slab are significantly improved, thus enhancing the surface quality of thin-gauge hot-rolled steel. Furthermore, this invention employs vacuum denitrification within a vacuum range of 100~133Pa, and controls the length of the yield plateau of the material at low temperatures during the finishing rolling and coiling steps.

[0147] The control method of this invention is simple and easy to operate, requiring no additional post-processing steps such as offline annealing, surface grinding, or repeated leveling. The process flow is concise, significantly shortening the production cycle of thin-gauge hot-rolled steel and improving production line efficiency and yield. This control method is particularly suitable for the production of thin-gauge 355 MPa grade hot-rolled steel with a thickness ≤4.0 mm. The resulting products have surface quality that meets usage requirements, good appearance, and promising prospects for industrial application.

[0148] The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for controlling transverse wrinkles on the surface of thin-gauge hot-rolled steel with a strength of 355MPa, characterized in that, Includes the following steps: S1: The molten steel is subjected to RH vacuum denitrification treatment and Ti is added for microalloying to obtain refined molten steel; S2: The refined molten steel is continuously cast to obtain a slab, wherein the center segregation and center porosity of the slab are both ≤C1.5; S3: The slab is heated to 1150~1230℃, and then roughed and finished rolled in sequence. Then it is cooled by ultra-fast cooling and laminar flow cooling respectively. Finally, it is coiled to obtain a steel coil. The finishing rolling temperature is 810~850℃; The winding temperature is 480~550℃; The chemical composition of the refined steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the remainder being iron and other unavoidable impurities; The thickness of thin-gauge hot-rolled steel with a strength of 355MPa is ≤4mm.

2. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The vacuum degree of the RH vacuum denitrification treatment is 100~133Pa. After circulating for 6~8 minutes, Ti is added and circulated for 2~3 minutes. After breaking the vacuum, the mixture is gently blown and stirred for 8~12 minutes to obtain the refined molten steel. The nitrogen content in the refined steel is ≤0.0050%; The Ti / N mass ratio in the refined steel is ≥2.

8.

3. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The steel preparation steps include: after KR desulfurization, the molten iron is smelted in a converter, and then slag washed in an argon station to obtain the molten steel. The iron content is ≥75%; The basicity of the slag after steelmaking in the converter is 4~7 (CaO / SiO2). The mass ratio of Mn / S in the molten steel is ≥30.

4. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 3, characterized in that, The sulfur content in the molten iron after KR desulfurization is ≤0.005%; Before tapping, add 1.5~3.0 kg / t of lime to the ladle. 50~75 seconds before tapping is completed, add 1.5~3.5 kg / t of lime and high-alumina pre-melted slag. The composition of the lime, by mass fraction, includes: CaO≥90%, SiO2≤5%, MgO 4~8%, moisture≤0.5%, with the remainder being unavoidable impurities; The composition of the high-alumina pre-melted slag, by mass fraction, includes: Al2O3 20~30%, CaO 50~60%, SiO2≤15%, MgO 4~8%, with the balance being unavoidable impurities.

5. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The casting superheat of the continuous casting is 10~25℃; The continuous casting adopts dynamic light reduction, with a light reduction amount of 4~6mm; The casting speed is 4.0~4.5m / min.

6. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The furnace exit temperature of the slab after heating is 1170~1220℃; The feed temperature of the roughing mill is ≤980℃; The inlet temperature of the finishing mill is 830~870℃.

7. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The ultra-fast cooling rate is 20~30℃ / s; The laminar flow cooling rate is 10~15℃ / s.

8. The method for controlling surface transverse wrinkles of 355MPa strength grade thin-gauge hot-rolled steel according to claim 1, characterized in that, The thickness of the 355MPa strength grade thin-gauge hot-rolled steel is 1.5~4mm; The steel coil is naturally cooled to an uncoiling temperature of ≤50℃.

9. A thin-gauge hot-rolled steel with a strength of 355 MPa, characterized in that, The surface transverse wrinkles of the 355MPa strength grade thin-gauge hot-rolled steel are prepared according to any one of claims 1 to 8.

10. The 355MPa strength grade thin-gauge hot-rolled steel according to claim 9, characterized in that, The chemical composition of the 355MPa strength grade thin-gauge hot-rolled steel, by mass fraction, includes: C 0.17~0.21%, Si 0.10~0.20%, Mn 0.20~0.50%, Als 0.018~0.050%, Ti 0.01~0.02%, P≤0.025%, S≤0.010%, N≤0.0055%, with the balance being Fe and unavoidable impurities; The yield strength of the 355MPa strength grade thin-gauge hot-rolled steel is 380~450MPa; The tensile strength of the 355MPa strength grade thin-gauge hot-rolled steel is 500~580MPa; The elongation of the 355MPa strength grade thin-gauge hot-rolled steel is ≥22%; The yield plateau length of the 355MPa strength grade thin-gauge hot-rolled steel is ≤3.5mm, and the surface is free of transverse creases.