A method for quenching and tempering heat treatment of large ball valve castings for pumped storage power stations
By using alternating water-air quenching and infrared temperature control, the problems of uneven cooling and cracking in large valve castings were solved, achieving uniform internal and external properties and high strength in the castings, thus meeting the technical requirements of pumped storage power stations.
Patent Information
- Application Number
- CN202611273057.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, large valve castings are prone to cracking during quenching, oil quenching causes contamination, and cooling is uneven, making it difficult to meet high-performance requirements.
The water-air alternating quenching method is adopted. By calculating the cooling time of each stage and controlling the temperature in real time with infrared temperature measurement, the uniformity and safety of cooling are ensured. This includes setting the time for the first water cooling, the first air cooling, the second water cooling, the second air cooling, and the third water cooling. Combined with tempering treatment, this ensures that the internal and external properties of the casting are uniform.
It achieves improved cooling uniformity and strength of large valve castings, avoids cracking risk, meets high performance requirements, has an internal and external hardness difference of less than 10 HBW, and exhibits excellent mechanical properties.
Smart Images

Figure CN123108262A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal heat treatment technology, and in particular to a method for quenching and tempering heat treatment of large ball valve castings for pumped storage power stations. Background Technology
[0002] In pumped storage power stations, ball valves are currently the preferred inlet valve type for large and medium-sized, high-head units. Their core castings mainly include the valve body and the valve valve itself. The valve body is the outer shell that bears all the water pressure, while the valve valve is a rotating ball with a through-hole, which is the core component for performing opening and closing actions. Valve castings are typically manufactured using casting methods, and their size is enormous, belonging to large or even super-large castings, with a single piece weighing tens or even hundreds of tons.
[0003] With the rapid development of pumped storage power station construction in my country, the demand for high-performance valve castings is increasing, and the requirements for their mechanical performance indicators are constantly rising. Currently, for valve castings with lower technical requirements, normalizing and tempering heat treatment is sufficient to meet performance requirements. To meet higher performance indicators, some companies have tried quenching oil cooling and tempering, but this method is only suitable for small valve castings with smaller dimensions and lower tonnage. For large valve castings with dimensions of 4m×3m×2m or more and a tempering weight of 50t or more, there are problems such as insufficient quenching oil tank size, excessively high oil temperature which can easily cause fires and oil fume pollution. Other companies have proposed a forced-air spray cooling method, but the spray only acts on the outer surface of the casting and cannot cool the inner cavity, resulting in uneven performance between the inside and outside of the casting. Some companies have also tried water quenching, but due to the complex structure of large valve castings, the risk of cracking during the water cooling process is extremely high.
[0004] Therefore, there is an urgent need for a heat treatment method for large valve castings that can balance cooling capacity, uniformity, and crack prevention. Summary of the Invention
[0005] Based on the above analysis, the present invention aims to provide a tempering heat treatment method for large ball valve castings used in pumped storage power stations, in order to solve at least one of the following problems in the prior art: water quenching easily causes cracking, oil quenching causes pollution and has poor heat storage capacity, spray cooling is uneven and the performance of forced draft normalizing is substandard.
[0006] On one hand, embodiments of the present invention provide a method for quenching and tempering heat treatment of large ball valve castings for pumped storage power stations, comprising the following steps: Step 1: Place the valve casting to be quenched into the heat treatment furnace; Step 2: Heat the valve casting to the austenitizing temperature and hold it at that temperature; Step 3: The austenitized valve casting is hoisted into a quenching water tank for alternating water and air quenching. The alternating water and air quenching includes sequential water cooling, air cooling, water cooling, air cooling and water cooling. The process parameters for the water-air alternating quenching are determined based on the maximum wall thickness δ of the valve casting: The first water cooling time t1 = [δ / 100 × (0.8 min ~ 1.2 min)] rounded down; The first air-cooling time t2 = (2~3) × t1; The second water cooling time t3 = [0.6 × t1 + (3 - t2 / t1) × 0.1 × t1] (rounded down); The second air cooling time t4 = (1~2) × t2; The third water cooling time t5 = [0.6 × t3 + (2 - t4 / t2) × 0.1 × t3] (rounded down); Step 4: Temper the quenched valve casting.
[0007] Furthermore, in step 3, the hoisting time is controlled within 7 minutes.
[0008] Furthermore, in step 3, infrared thermography is used to monitor the surface temperature of the valve casting in real time during the air cooling process. If the surface temperature exceeds the preset tempering temperature T, the air cooling is immediately terminated and the next water cooling is performed.
[0009] Furthermore, during the first air cooling process, if the surface temperature exceeds the tempering temperature T within time t2, a second water cooling is immediately performed; during the second air cooling process, if the surface temperature exceeds T-100℃ within time t4, a third water cooling is immediately performed.
[0010] Furthermore, step 3 also includes a third air cooling: air cooling the valve casting to a surface temperature of 250℃~300℃. If the temperature rises above 400℃ during the air cooling process, add a 1~2 minute water cooling before continuing air cooling.
[0011] Furthermore, in step 2, the heating adopts a stepped heating method: first, it is heated to 400℃~450℃ at a rate of ≤50℃ / h and held for 4~8 hours, and then heated to 860℃~910℃ at a rate of ≤80℃ / h.
[0012] Furthermore, the heat preservation time t at 860℃~910℃ 保 =[δ / 100×(2h~3h)] (rounded down).
[0013] Furthermore, in step 4, the tempering treatment includes: holding the valve casting at 250℃~300℃ for 3~6 hours, then raising the temperature to the tempering temperature T at a rate of ≤50℃ / h, and holding it at the tempering temperature T for a holding time t. 回 =[δ / 100×(3h~4h)] rounded down, then furnace cooled.
[0014] Furthermore, the valve casting is made of ASTM A148 Gr80-50 material, the maximum wall thickness δ of the valve casting is 730mm~910mm, and the weight of a single piece is 50t~70t.
[0015] The valve casting, after heat treatment, has a yield strength ≥350MPa, tensile strength ≥550MPa, elongation after fracture ≥18%, reduction of area ≥30%, and impact KV2 ≥27J at 0℃.
[0016] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1) This invention calculates the water-cooling / air-cooling time for each stage based on the maximum wall thickness δ (first water-cooling time t1 = [δ / 100 × (0.8 min ~ 1.2 min)] rounded down, first air-cooling time t2 = (2 ~ 3) × t1, second water-cooling time t3 = [0.6 × t1 + (3 - t2 / t1) × 0.1 × t1] rounded down, second air-cooling time t4 = (1 ~ 2) × t2, third water-cooling time t5 = [0.6 × t3 + (2 - t4 / t2) × 0.1 × t3] rounded down), ensuring that the cooling times of each stage are matched. After treatment with this method, valve castings with a wall thickness of 730 mm ~ 910 mm and a weight of 50 t ~ 70 t achieve a yield strength of 393 MPa ~ 432 MPa (≥350 MPa required) and a tensile strength of 577 MPa ~ 603 MPa (≥550 MPa required), without any quenching cracks.
[0017] 2) This invention incorporates air cooling between water cooling and air cooling, with the water cooling and air cooling times of each stage progressively decreasing, causing the surface temperature of the casting to decrease gradually, releasing stress step by step, and avoiding the risk of cracking when water cooling reaches its limit.
[0018] 3) This invention uses infrared thermography to monitor the surface temperature of the casting in real time during the air cooling process, and uses the tempering temperature T and T-100℃ as overheat judgment thresholds to control the timing of water immersion. When the air cooling temperature rises above the threshold, water immersion is immediately used to cool down, preventing the temperature rise from exceeding the tempering temperature and causing performance degradation, while also avoiding excessive stress due to overcooling.
[0019] 4) The valve casting treated by the method of the present invention has uniform cooling inside and out, and the average hardness difference between the outer surface and the inner cavity can be controlled within 10 HBW. In contrast, the average hardness difference between the inside and outside of the casting using the spray cooling method is greater than 20 HBW, which solves the problem that the spray cooling method for large valve castings can only cool the outer surface, resulting in uneven internal and external performance.
[0020] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0021] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0022] Figure 1 This is a graph showing the change of water / air cooling temperature over time during the quenching process of the valve casting of the present invention. Figure 2 This is a schematic diagram of the structure of the valve casting of the present invention. Detailed Implementation
[0023] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0024] The valve casting is the core component in the ball valve of the pumped storage power station that performs the opening and closing action. It is usually made of ASTM A148 Gr80-50 high-strength low-alloy cast steel. The main body is spherical, with cylindrical support journals extending symmetrically outward on both sides of the sphere. A through hole for medium flow is opened in the middle of the sphere. The maximum wall thickness of the casting is δ, which is 700mm~1000mm, and the weight of a single piece is 50t~70t.
[0025] Due to the large wall thickness, the cooling rates of the surface and core differ significantly during quenching. If the cooling rate is too slow, the required strength and toughness cannot be achieved; if the cooling rate is too fast, the excessive temperature difference between the surface and core leads to cracking. To address these issues, this invention proposes a solution.
[0026] A specific embodiment of the present invention discloses a water-air conditioning heat treatment method for large ball valve castings used in pumped storage power stations, such as... Figure 1 and Figure 2 As shown, the method includes the following steps: Step 1: Place the valve casting to be quenched into the heat treatment furnace; Step 2: Heat the valve casting to the austenitizing temperature and hold it at that temperature; Step 3: The austenitized valve casting is hoisted into a quenching water tank for water-air alternating quenching. The water-air alternating quenching includes a first water cooling, a first air cooling, a second water cooling, a second air cooling, and a third water cooling in sequence. The process parameters of the water-air alternating quenching are determined according to the maximum wall thickness δ of the valve casting. Step 4: Temper the quenched valve casting.
[0027] The method for determining the water cooling time and air cooling time for each stage in step 3 is as follows: Let the maximum wall thickness of the valve casting be δ (unit: mm). The calculation of each time segment is based on δ / 100. The initial water cooling time for each 100 mm wall thickness is 0.8 min to 1.2 min (e.g., 0.8 min, 0.9 min, 1.0 min, 1.1 min, 1.2 min).
[0028] The first water cooling time t1 = [δ / 100 × (0.8 min ~ 1.2 min)] rounded down to the nearest minute; The first air cooling time t2 = (2~3) × t1, in minutes. During the air cooling, infrared thermometry is used to monitor the surface temperature of the workpiece in real time. If the surface temperature of the workpiece exceeds the tempering temperature T within t2, the air cooling is immediately terminated and the second water cooling is performed. Otherwise, the air cooling continues until time t2. The second water cooling time t3 = [0.6 × t1 + (3 - t2 / t1) × 0.1 × t1] rounded down to the nearest minute; The second air cooling time t4 = (1~2) × t2, in minutes. During the air cooling period, infrared thermometry is used to monitor the surface temperature of the workpiece in real time. If the surface temperature of the workpiece exceeds T-100℃ within t4, the air cooling is immediately terminated and the third water cooling is performed. Otherwise, the air cooling continues until time t4. The third water cooling time t5 = [0.6 × t3 + (2 - t4 / t2) × 0.1 × t3] rounded down to the nearest minute.
[0029] Compared with existing technologies, the method provided in this embodiment uses alternating water and air quenching, which ensures cooling capacity while avoiding the cracking risk of water quenching. The water cooling stage rapidly cools the surface of the casting, ensuring sufficient cooling speed for the surface layer to form the desired microstructure. The air cooling stage transfers heat from the inside of the casting to the surface, causing the surface to warm up and releasing the thermal stress between the surface and the core, preventing cracking. Through multiple alternating water and air cooling stages, the casting temperature gradually decreases, with each water cooling depth decreasing progressively, ultimately achieving a uniform temperature throughout the casting. This ensures sufficient cooling speed for the core while avoiding quenching cracks caused by excessive temperature differences.
[0030] It should be noted that schemes employing alternating water-air quenching and adjusting cooling time using formulas, such as adjusting water temperature to modify quenching time, are merely compensations for external environmental factors based on existing processes. This invention, however, determines the initial value based on the workpiece's maximum wall thickness δ and recursively calculates subsequent time segments using proportional relationships. This allows the cooling intensity of each segment to adaptively match the wall thickness, avoiding the extreme risks of insufficient cooling rate due to excessively short water cooling time or stress cracking due to excessively long water cooling time, which are common when relying on empirical values. Simultaneously, during the quenching process, infrared thermography dynamically controls the timing of water immersion, promptly supplementing water cooling when the air cooling temperature exceeds a threshold, preventing excessively high temperatures from damaging performance.
[0031] Furthermore, in step 3, the hoisting time should be controlled within 7 minutes. Excessive hoisting time will cause the surface temperature of the casting to drop below the austenite transformation temperature, affecting the quenching effect. Controlling the time to within 7 minutes ensures that the surface is in an austenitic state upon immersion in water.
[0032] Furthermore, in step 3, infrared thermography is used to monitor the surface temperature of the valve casting in real time during the air cooling process. If the surface temperature exceeds the preset tempering temperature T, the air cooling is immediately terminated and the next water cooling is performed.
[0033] Air cooling allows heat to transfer from the inside of the casting to the outside. However, when the surface temperature exceeds the tempering temperature T, it means the overall temperature of the casting is still too high. If air cooling continues at this point, the prolonged high temperature may cause the supercooled austenite to undergo a non-martensitic transformation, or cause the already formed martensite structure to soften during tempering, ultimately resulting in insufficient strength. By setting T as the over-temperature threshold, the casting is immediately immersed in water for cooling when the surface temperature exceeds T, ensuring that the casting temperature is always controlled below the tempering temperature, thus preventing high-temperature tempering of the quenched structure.
[0034] Furthermore, during the first air cooling process, if the surface temperature exceeds the tempering temperature T within time t2, a second water cooling is immediately performed; during the second air cooling process, if the surface temperature exceeds T-100℃ within time t4, a third water cooling is immediately performed.
[0035] Since the overall temperature of the casting is lower after the second water cooling than after the first, the peak temperature rise is also lower. Therefore, the over-temperature threshold for the second air cooling is set to T-100℃. If the temperature rise during the second air cooling exceeds T-100℃, it indicates that the casting still has excessive heat storage, requiring additional heat removal during the third water cooling. These two different temperature thresholds enable graded control of the casting temperature, ensuring precise timing of water immersion for each cooling cycle.
[0036] Furthermore, step 3 also includes a third air cooling: air cooling the valve casting to a surface temperature of 250℃~300℃ (e.g., 250℃, 260℃, 265℃, 275℃, 280℃, 290℃, 300℃). If the temperature rises above 400℃ during the air cooling process, add a water cooling for 1~2 minutes (e.g., 1min, 1.1min, 1.25min, 1.5min, 1.7min, 1.85min, 2min) before continuing air cooling.
[0037] The peak temperature of the casting after the third water cooling and subsequent air cooling should not exceed 400℃ (e.g., 180℃, 230℃, 270℃, 310℃, 345℃, 370℃, 400℃). If this value is exceeded, it indicates that the total cooling capacity of the first three water cooling cycles is insufficient. Adding 1-2 minutes of supplementary water cooling can further reduce the temperature without causing excessive temperature differences. Another consideration for setting 400℃ is that the martensitic transformation is basically completed within the range of 200℃ to 400℃. Controlling the temperature return below 400℃ can prevent the transformed martensite structure from softening due to high-temperature tempering, thereby ensuring that the yield strength and tensile strength meet the requirements.
[0038] Further, in step 2, the heating adopts a stepped temperature increase: first, heating is carried out at a rate of ≤50℃ / h (e.g., 5℃ / h, 15℃ / h, 22℃ / h, 30℃ / h, 38℃ / h, 45℃ / h, 50℃ / h) to 400℃~450℃ (e.g., 400℃, 408℃, 416℃, 425℃, 433℃, 442℃, 450℃) and then holding at that temperature for 4h~8h (e.g., 4h, ...). 4.7h, 5.3h, 6h, 6.6h, 7.2h, 8h), then heat to 860℃~910℃ (e.g. 860℃, 868℃, 876℃, 885℃, 892℃, 901℃, 910℃) at a rate ≤80℃ / h (e.g., 10℃ / h, 25℃ / h, 38℃ / h, 50℃ / h, 62℃ / h, 70℃ / h, 80℃ / h) and hold at that temperature for a holding time t. 保 =[δ / 100×(2h~3h)] (rounded down).
[0039] It should be noted that during the heating process of large castings, the surface and core layers heat up at different rates. Excessive heating can generate significant thermal stress, leading to deformation or even cracking. The first stage involves a slow heating rate of ≤50℃ / h to 400℃~450℃ and a prolonged holding period to homogenize the temperature across the casting cross-section and to initially release casting and processing stresses. The second stage involves heating at ≤80℃ / h to the austenitizing temperature. At this point, the casting is in a temperature range with good plasticity, reducing the risk of thermal stress. The austenitizing temperature of 860℃~910℃ ensures complete dissolution of carbides and homogenization of austenite. The holding time is calculated based on the wall thickness to ensure that the core layer also completes its microstructure transformation.
[0040] Further, in step 4, the tempering treatment includes: holding the valve casting at 250℃~300℃ (e.g., 250℃, 258℃, 265℃, 272℃, 280℃, 289℃, 300℃) for 3h~6h (e.g., 3h, 3.5h, 4h, 4.6h, 5h, 5.4h, 6h), then heating it to the tempering temperature T at a heating rate ≤50℃ / h (e.g., 8℃ / h, 16℃ / h, 24℃ / h, 32℃ / h, 40℃ / h, 45℃ / h, 50℃ / h), and holding it at the tempering temperature T for a holding time t. 回 =[δ / 100×(3h~4h)] rounded down, then furnace cooled.
[0041] After quenching, the casting contains significant internal stress. Tempering is used to eliminate this stress and adjust its mechanical properties. Holding the casting at 250℃~300℃ before tempering allows for initial stress release, preventing stress buildup and cracking during the heating process. A slow heating rate of ≤50℃ / h ensures uniform temperature distribution throughout the casting. The holding time is calculated based on the wall thickness to ensure the core reaches the tempering temperature. After furnace cooling to 250℃~300℃, the casting is removed from the furnace and air-cooled to prevent excessively rapid surface cooling and the generation of new thermal stresses upon removal from the furnace at high temperatures.
[0042] The heat treatment method of this invention, through the synergistic cooperation of the above steps, achieves the effect of no cracking during the quenching process of large valve castings and uniform internal and external properties (with a stable internal and external hardness difference ≤10HBW). The valve castings heat-treated by this method have a yield strength of 393MPa~432MPa, tensile strength of 577MPa~603MPa, elongation after fracture of 23.0%~25.0%, reduction of area of 69%~72%, and an impact KV2 of 31~89J at 0℃. All mechanical properties meet the technical requirements for ball valve castings in pumped storage power stations (yield strength ≥350MPa, tensile strength ≥550MPa, elongation after fracture ≥18%, reduction of area ≥30%, impact KV2 ≥27J at 0℃).
[0043] The present invention will be described in more detail below through specific embodiments. These embodiments are merely descriptions of the best implementation of the invention and do not limit the scope of the invention in any way.
[0044] Example 1 In this embodiment, the valve casting has external dimensions of 5.1m × 3.5m × 2.6m, a weight of 60.8t, a maximum wall thickness of 820mm, and is made of ASTM A148 Gr80-50 material. The mechanical property requirement is a yield strength R. p0.2 ≥350MPa, tensile strength R m ≥550MPa, elongation after fracture A≥18%, reduction of area Z≥30%, impact KV2 at 0℃≥27J.
[0045] The quenching and tempering heat treatment method for the valve casting in this embodiment includes the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0046] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 5 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 870℃ and holds for 20 hours.
[0047] Step 3: Hoist the casting to the quenching water tank. After 4 minutes of hoisting, the workpiece is fully immersed in the water; perform alternating water-air-water quenching. First water-air cooling: The first water cooling time t1 is 7 minutes. After water cooling, the valve casting is lifted out for air cooling. The first air cooling time t2 is 20 minutes. During air cooling, infrared temperature measurement is used for additional control. Within 20 minutes of air cooling, the highest infrared temperature of the workpiece is 547℃, which does not exceed the process tempering temperature of 590℃. Second water-cooling: Immerse the workpiece in water. The second water-cooling time t3 is 4 minutes. After water cooling, lift the valve casting out for air cooling. The second air cooling time t4 is 30 minutes. Infrared temperature measurement is also performed during air cooling. After 30 minutes of air cooling, the highest infrared temperature of the workpiece is 433℃, which is 157℃ lower than the process tempering temperature. Third water-cooling: Immerse the workpiece in water for a third water-cooling time t5 of 3 minutes. After water cooling, remove the valve casting for air cooling. The highest temperature reached during air cooling is 372℃, which does not exceed 400℃. Continue air cooling according to process requirements. Once the valve casting has cooled to 280℃, load it into the furnace for tempering.
[0048] Step 4, Tempering: Hold at 280℃ for 5 hours, then raise the temperature to the tempering temperature of 590℃ and hold for 30 hours before furnace cooling.
[0049] After tempering, the valve casting was tested for performance. The yield strength Rp0.2 was 402 MPa, the tensile strength Rm was 577 MPa, the elongation after fracture A was 25.0%, the reduction of area Z was 72%, and the impact KV2 at 0℃ was 51 J, 76 J, and 89 J. The mechanical properties were qualified.
[0050] Example 2 The valve casting in this embodiment has external dimensions of 5.6m × 3.9 × 2.9m, a weight of 66.5t, a maximum wall thickness of 910mm, and is made of ASTM A148 Gr80-50 material. Its mechanical performance requirements are the same as those in Embodiment 1.
[0051] The quenching and tempering heat treatment method for the valve casting in this embodiment includes the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0052] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 7 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 880℃ and holds for 20 hours.
[0053] Step 3: Hoist the casting to the quenching water tank. After 5 minutes of hoisting, the workpiece is fully immersed in the water; perform alternating water-air-water quenching. First water-air cooling: The first water cooling time t1 is 9 minutes. After water cooling, the valve casting is lifted out for air cooling. The first air cooling time t2 is 25 minutes. During air cooling, infrared temperature measurement is used for additional control. Within 25 minutes of air cooling, the highest infrared temperature of the workpiece is 530℃, which does not exceed the process tempering temperature of 570℃. Second water-cooling: The workpiece is re-immersed in water. The second water-cooling time t3 is 5 minutes. After water cooling, the valve casting is lifted out for air cooling. The second air cooling time t4 is 40 minutes. Infrared temperature measurement is also performed during air cooling. After 40 minutes of air cooling, the highest infrared temperature of the workpiece is 450℃, which is 120℃ lower than the process tempering temperature. Third water-cooling: Immerse the workpiece in water for a third water-cooling time t5 of 3 minutes. After water cooling, remove the valve casting for air cooling. The highest temperature reached during air cooling is 385℃, which does not exceed 400℃. Continue air cooling according to process requirements. Once the valve casting has cooled to 300℃, load it into the furnace for tempering.
[0054] Step 4, Tempering: Hold at 280℃ for 6 hours, then raise the temperature to the tempering temperature of 570℃ and hold for 30 hours before furnace cooling.
[0055] Performance testing of valve castings after tempering and removal from the furnace, yield strength R p0.2The tensile strength is 432 MPa, and the tensile strength R is... m The strength is 603 MPa, the elongation after fracture (A) is 23.5%, the reduction of area (Z) is 70%, and the impact strength (KV2) at 0℃ is 47 J, 31 J, and 37 J, respectively. The mechanical properties are qualified.
[0056] Example 3 The valve casting in this embodiment has external dimensions of 4.8m × 3.2 × 2.3m, a weight of 51.8t, a maximum wall thickness of 730mm, and is made of ASTM A148 Gr80-50. Its mechanical performance requirements are the same as those in Embodiment 1.
[0057] The quenching and tempering heat treatment method for the valve casting in this embodiment includes the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0058] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 5 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 870℃ and holds for 16 hours.
[0059] Step 3: Hoist the casting to the quenching water tank. After 4 minutes of hoisting, the workpiece is fully immersed in the water; perform alternating water-air-water quenching. First water-air cooling: The first water cooling time t1 is 6 minutes. After water cooling, the valve casting is lifted out for air cooling. The first air cooling time t2 is 15 minutes. During air cooling, infrared temperature measurement is used for additional control. Within 15 minutes of air cooling, the highest infrared temperature of the workpiece is 527℃, which does not exceed the process tempering temperature of 570℃. Second water-cooling: Immerse the workpiece in water. The second water-cooling time t3 is 3 minutes. After water cooling, lift the valve casting out for air cooling. The second air cooling time t4 is 30 minutes. Infrared temperature measurement is also performed during air cooling. After 30 minutes of air cooling, the highest infrared temperature of the workpiece is 457℃, which is 113℃ lower than the process tempering temperature. Third water-cooling: Immerse the workpiece in water for a third water-cooling time t5 of 2 minutes. After water cooling, remove the valve casting for air cooling. The highest temperature reached during air cooling is 387℃, which does not exceed 400℃. Continue air cooling according to process requirements. Once the valve casting has cooled to 280℃, load it into the furnace for tempering.
[0060] Step 4, Tempering: Hold at 280℃ for 4 hours, then raise the temperature to the tempering temperature of 570℃ and hold for 24 hours before furnace cooling.
[0061] Performance testing of valve castings after tempering and removal from the furnace, yield strength R p0.2 The tensile strength is 393 MPa, and the tensile strength R is...m The strength is 582 MPa, the elongation after fracture (A) is 23.0%, the reduction of area (Z) is 69%, and the impact strength (KV2) at 0℃ is 54 J, 43 J, and 42 J, respectively. The mechanical properties are qualified.
[0062] Comparative Example 1 This comparative example gate is identical to the gate in Example 1, meaning its structure, materials, and mechanical performance requirements are all the same. The difference from Example 1 is: The tempering heat treatment method for valve castings is by forced air, including the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0063] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 6 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 900℃ and holds for 16 hours.
[0064] Step 3, Blowing air after exiting the furnace: Pull the casting out of the heat treatment furnace and blow air with a powerful blower until the surface temperature of the workpiece is ≤200℃; Step 4, Tempering: After loading the furnace for tempering, hold at 280℃ for 6 hours, then raise the temperature to the tempering temperature of 570℃ and hold for 32 hours before furnace cooling. Performance testing of valve castings after tempering and removal from the furnace, yield strength R p0.2 The tensile strength is 321 MPa, and the tensile strength R is... m The strength and toughness tests were all unqualified, with an elongation at break (A) of 31.0%, a reduction of area (Z) of 69%, and impact strength (KV2) of 23J, 33J, and 24J at 0℃.
[0065] Comparative Example 2 The comparative example valve is the same as the valve in Example 1, and will not be described again here. The difference from Example 1 is: The heat treatment method for valve castings is suspended spraying, which includes the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0066] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 6 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 880℃ and holds for 16 hours.
[0067] Step 3, Lowering and Spraying: Lower the casting and spray it for 1.5 hours, then use a forced-air cooling system to cool the workpiece surface to ≤200℃.
[0068] Step 4, Tempering: After loading the furnace for tempering, hold at 280℃ for 6 hours, then raise the temperature to the tempering temperature of 550℃ and hold for 24 hours before furnace cooling.
[0069] Performance testing of valve castings after tempering and removal from the furnace, yield strength R p0.2 The tensile strength is 345 MPa, and the tensile strength R is... m The strength was 560 MPa, the elongation after fracture (A) was 27.0%, the reduction of area (Z) was 66%, and the impact strength (KV2) at 0℃ was 56 J, 39 J, and 58 J, respectively. The yield strength test was unqualified.
[0070] Comparative Example 3 The comparative example valve is the same as the valve in Example 1, and will not be described again here. The difference from Example 1 is: The heat treatment method for valve castings is water cooling, which includes the following steps: Step 1: Place the valve casting to be quenched near the center of the heat treatment furnace. Use wedges to fill the gap between the workpiece and the shims to reduce deformation during the heat treatment process.
[0071] Step 2, Quenching: Heat the valve casting at a heating rate of ≤50℃ / h, hold at 430℃ for 6 hours, then continue heating at a heating rate of ≤80℃ / h until it reaches 880℃ and holds for 16 hours.
[0072] Step 3, hoisting: Hoist the casting to the quenching water tank. After 4 minutes of hoisting, the workpiece is completely immersed in the water.
[0073] Step 4, water quenching: After cooling the workpiece in water for 40 minutes, lift it out. 10 minutes after lifting it out, measure the surface temperature of the workpiece, which is 166℃.
[0074] Step 5, Tempering: After loading the furnace for tempering, hold at 280℃ for 6 hours, then raise the temperature to the tempering temperature of 570℃ and hold for 24 hours before furnace cooling. Performance testing of valve castings after tempering and removal from the furnace, yield strength R p0.2 The tensile strength is 432 MPa, and the tensile strength R is... m The strength of the valve casting is 600 MPa, the elongation after fracture (A) is 26.5%, the reduction of area (Z) is 69%, and the impact strength (KV2) at 0℃ is 84 J, 87 J, and 51 J. The valve casting passed the inspection. However, after the valve casting was taken out of the furnace, a quenching crack was found on the inner circular wall below the riser. It needs to be repaired by welding in the later stage, which will affect the production cycle and increase the cost.
[0075] Comparative Example 4 The comparative example valve is the same as the valve in Example 1, and will not be described again here. The difference from Example 1 is: Step 3: When using alternating water and air quenching, the water cooling / air cooling time is not calculated according to the formula of this invention, but is determined based on experience (first water cooling 5 min, first air cooling 20 min, second water cooling 6 min, second air cooling to ≤300℃), and the remaining steps are the same as in Example 1.
[0076] Mechanical property test results of the valve casting, yield strength R p0.2 The tensile strength is 342 MPa, and the tensile strength R is... m The strength is 558 MPa, the elongation after fracture (A) is 29.0%, the reduction of area (Z) is 71%, and the impact strength (KV2) at 0℃ is 43 J, 51 J, and 47 J. The yield strength test is unqualified (the requirement is ≥350 MPa).
[0077] Comparative Example 5 The comparative example valve is the same as the valve in Example 1, and will not be described again here. The difference from Example 1 is: Step 3: When using alternating water and air quenching, the water cooling / air cooling time is not calculated according to the formula of this invention, but is determined based on experience (first water cooling 12min, first air cooling 15min, second water cooling 6min, second air cooling to ≤300℃), and the remaining steps are the same as in Example 1.
[0078] Mechanical property test results of the valve casting, yield strength R p0.2 The tensile strength is 405 MPa, and the tensile strength R is... m The strength of the valve casting was 578 MPa, the elongation after fracture (A) was 28.0%, the reduction of area (Z) was 72%, and the impact strength (KV2) at 0℃ was 72 J, 76 J, and 80 J. The valve casting passed the inspection. However, after the valve was taken out of the furnace, a vertical quenching crack was found on the circular inner wall of the valve cavity. It needs to be repaired by welding in the later stage, which will affect the production cycle and increase the cost.
[0079] Characterization results analysis: The hardness test results of the embodiments and comparative examples are shown in Table 2; to facilitate the comparison and analysis of the processing effects of each embodiment and comparative example, the mechanical properties of each embodiment and comparative example are summarized in Table 1.
[0080] Table 1 Performance test results of valve castings in the examples and comparative examples
[0081] Note: The three values in the "0℃ Impact Energy KV2" column of Table 1 are the results of a single test of three parallel impact specimens prepared from the same test location of the casting.
[0082] Table 2. Hardness test results of valves in the examples and comparative examples
[0083] Note: The “average difference between inner and outer surfaces” in Table 2 is the absolute value of the difference between the average hardness measurement values at three locations on the outer surface and the average hardness measurement values at three locations on the inner cavity. The calculation result is rounded to one decimal place.
[0084] As shown in Tables 1 and 2, the yield strength of Examples 1-3 is 393 MPa~432 MPa, tensile strength is 577 MPa~603 MPa, elongation after fracture is 23.0%~25.0%, reduction of area is 69%~72%, and impact KV2 at 0℃ is 31~89 J, all meeting the standard requirements (e.g., ball valve cast steel standard T / CFA 020101223-2021) and without any cracking. The difference between internal and external hardness is consistently ≤10 HBW. In contrast, although the hardness differences of some Comparative Examples 1-5 are smaller, they all suffer from insufficient strength, low plasticity, or unqualified impact resistance, and some even crack directly during quenching, failing to meet all the indicators. This indicates that the present invention achieves effective control of internal and external cooling uniformity while ensuring no cracking and meeting all performance standards.
[0085] In summary, the method of this invention successfully ensures that the mechanical properties of large valve castings meet the requirements, and no quenching cracks occur; the hardness difference between the inside and outside of the casting is small, and the cooling uniformity is better than that of existing solutions. It solves the problems of easy cracking during water quenching, pollution and poor heat storage capacity during oil quenching, uneven spray cooling, and substandard performance of forced draft normalizing in existing technologies for large valve castings.
[0086] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for heat treatment of large ball valve castings for pumped storage power stations, characterized in that, Includes the following steps: Step 1: Place the valve casting to be quenched into the heat treatment furnace; Step 2: Heat the valve casting to the austenitizing temperature and hold it at that temperature; Step 3: The austenitized valve casting is hoisted into a quenching water tank for alternating water and air quenching. The alternating water and air quenching includes sequential water cooling, air cooling, water cooling, air cooling and water cooling. The process parameters for the water-air alternating quenching are determined based on the maximum wall thickness δ of the valve casting: The first water cooling time t1 = [δ / 100 × (0.8 min ~ 1.2 min)] rounded down; The first air-cooling time t2 = (2~3) × t1; The second water cooling time t3 = [0.6 × t1 + (3 - t2 / t1) × 0.1 × t1] (rounded down); The second air cooling time t4 = (1~2) × t2; The time for the third water cooling is t5 = [0.6 × t3 + (2 - t4 / t2) × 0.1 × t3] (rounded down). Step 4: Temper the quenched valve casting.
2. The quenching and tempering heat treatment method according to claim 1, characterized in that, In step 3, the hoisting time is controlled within 7 minutes.
3. The quenching and tempering heat treatment method according to claim 1, characterized in that, In step 3, infrared thermography is used to monitor the surface temperature of the valve casting in real time during the air cooling process. If the surface temperature exceeds the preset tempering temperature T, the air cooling is immediately terminated and the next water cooling is performed.
4. The quenching and tempering heat treatment method according to claim 3, characterized in that, If the surface temperature exceeds the tempering temperature T within time t2 during the first air cooling process, a second water cooling is immediately performed; if the surface temperature exceeds T-100℃ within time t4 during the second air cooling process, a third water cooling is immediately performed.
5. The quenching and tempering heat treatment method according to claim 1, characterized in that, Step 3 also includes a third air cooling: air cool the valve casting to a surface temperature of 250℃~300℃. If the temperature rises above 400℃ during the air cooling process, add a 1~2 minute water cooling before continuing the air cooling.
6. The quenching and tempering heat treatment method according to claim 1, characterized in that, In step 2, the heating adopts a stepped heating method: first, heat to 400℃~450℃ at a rate of ≤50℃ / h and hold for 4~8 hours, then heat to 860℃~910℃ at a rate of ≤80℃ / h.
7. The quenching and tempering heat treatment method according to claim 6, characterized in that, The heat preservation time t at 860℃~910℃ 保 =[δ / 100×(2h~3h)] (rounded down).
8. The quenching and tempering heat treatment method according to claim 1, characterized in that, In step 4, the tempering treatment includes: holding the valve casting at 250℃~300℃ for 3~6 hours, then raising the temperature to the tempering temperature T at a rate of ≤50℃ / h, and holding it at the tempering temperature T for a holding time t. 回 =[δ / 100×(3h~4h)] rounded down, then furnace cooled.
9. The quenching and tempering heat treatment method according to claim 1, characterized in that, The valve casting is made of ASTM A148 Gr80-50 material, the maximum wall thickness δ of the valve casting is 730mm~910mm, and the weight of a single piece is 50t~70t.
10. A large ball valve casting for a pumped storage power station, manufactured using the quenching and tempering heat treatment method described in any one of claims 1-9, characterized in that... The valve casting has a yield strength ≥350MPa, tensile strength ≥550MPa, elongation after fracture ≥18%, reduction of area ≥30%, and impact KV2 ≥27J at 0℃.