A lithium extraction method
By utilizing the contact between solvent vapor and solid powder in a supergravity reactor, a lithium chloride solution is selectively formed and separated, solving the problem of low lithium extraction efficiency from low-grade lithium resources in existing technologies. This achieves high-purity and high-recovery lithium extraction, while reducing energy consumption and pollution.
Patent Information
- Application Number
- CN202611297207.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium extraction technologies suffer from problems such as low lithium recovery rate, low purity, high energy consumption, high pollution, or lengthy processes when dealing with low-grade lithium resources. In particular, it is difficult to achieve efficient purification when processing resources such as lithium clay, lithium ore, high magnesium-to-lithium ratio brine, and lithium extraction slag with a lithium content of less than 0.5 wt%.
The supergravity reactor technology is used to bring solvent vapor into contact with the solid powder to be purified under the action of supergravity where centrifugal force is greater than gravity. Taking advantage of the critical deliquescence humidity difference between lithium chloride and alkali metal/alkaline earth metal halide salts in the solvent, a lithium chloride solution is selectively formed and separated in time to avoid the dissolution of impurities, and no additional processing is required afterward.
This method enables the efficient and low-cost extraction of high-purity lithium chloride solutions from complex matrices, simplifying the process, improving lithium recovery rate and purity, and reducing energy consumption and pollution.
Smart Images

Figure CN123108318A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of purification technology, and more specifically, to a method for lithium extraction. Background Technology
[0002] With the explosive growth of the new energy industry, lithium's strategic importance as "white oil" is becoming increasingly prominent. Global lithium demand is projected to triple by 2030, while current production capacity is far from sufficient. Currently, the mainstream industrial lithium extraction technologies mainly include traditional acid leaching precipitation and solvent extraction. However, these technologies exhibit significant limitations when dealing with low-grade lithium resources (such as lithium clay with a lithium content below 0.5 wt%, high magnesium-to-lithium ratio brines, and lithium extraction slag), resulting in low lithium recovery rates, low purity, high energy consumption, significant pollution, or lengthy processes. Summary of the Invention
[0003] To address the aforementioned shortcomings, this application provides a lithium extraction method to achieve efficient purification of lithium resources from complex matrices.
[0004] This application is implemented as follows: In a first aspect, an example of this application provides a lithium extraction method, comprising: Solvent vapor is conveyed to a centrifugal reactor and brought into contact with the solid powder to be purified. The solid powder absorbs the solvent vapor and deliquesces to form a lithium chloride solution. Simultaneously, the centrifugal reactor separates the lithium chloride solution from the undeliquesced solid powder, collecting the lithium chloride solution. The solvent vapor includes at least one of water vapor and polar small-molecule solvent vapors, and the solid powder to be purified contains lithium ions and chloride ions.
[0005] In the above process, the solid powder to be purified and solvent vapor are introduced into a hypergravity reactor. Under the action of hypergravity where the centrifugal force is greater than the gravity force, the solvent (at least one of water and polar small molecule solvent) comes into full contact with the solid powder containing chloride ions and lithium ions in the gas phase. Due to the difference in critical deliquescence humidity between lithium chloride and other alkali metal / alkaline earth metal halide salts (such as halides of Na, K, Mg, and Ca) in the above solvent, the solid powder to be purified absorbs the solvent vapor and can deliquesce to form a lithium chloride solution (it can be understood that the solute in the lithium chloride solution is lithium chloride, and the solvent is at least one of water and polar small molecule solvent). Meanwhile, under the influence of supergravity, the deliquescent lithium chloride solution can be separated from the non-deliquescent solid powder in a timely manner. This not only avoids the lithium chloride solution from accumulating on the surface of the non-deliquescent solid powder for a long time, thus improving the problem of excessive dissolution of other impurities (such as the aforementioned alkali metal / alkaline earth metal halide salts) in the solid powder due to localized excessive solvent, but also eliminates the need for subsequent post-processing such as extraction and washing of the separated lithium chloride solution. This allows for the efficient collection of a purified solution with a high lithium ion concentration, and the lithium ion purification yield and purity are both high.
[0006] In conjunction with the first aspect, in an optional embodiment of this application, the solvent vapor includes water vapor, wherein the relative humidity of the water vapor is 11% ≤ RH ≤ 33%.
[0007] In the above process, water vapor with suitable relative humidity and the solid powder to be purified containing chloride and lithium ions are transported to a hypergravity reactor. Under the action of hypergravity, where centrifugal force is greater than gravity, water in the gas phase (water vapor) comes into full contact with the solid powder containing chloride and lithium ions. Due to the difference in critical deliquescence humidity between lithium chloride and other alkali metal / alkaline earth metal halides (such as halides of Na, K, Mg, and Ca) in water vapor, when the relative humidity (RH) of water vapor is ≥11%, the solid powder to be purified can selectively deliquesce lithium chloride to form a lithium chloride solution by absorbing water vapor; when the relative humidity (RH) of water vapor is ≤33%, alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca do not deliquesce, thus enabling the selective and timely separation of the lithium chloride aqueous solution from the non-deliquescing solid powder under the action of hypergravity. Promptly separating the lithium chloride aqueous solution from the non-hygroscopic solid powder can prevent excessive accumulation of lithium chloride aqueous solution on the surface of the non-hygroscopic solid powder. If alkali metal / alkaline earth metal halide salts are in contact with the lithium chloride aqueous solution for an extended period, it will accelerate the dissolution of the alkali metal / alkaline earth metal, thereby reducing the purity of lithium ions in the purification solution.
[0008] In conjunction with the first aspect, in an optional embodiment of this application, the number of carbon atoms of the polar small molecule solvent in the polar small molecule solvent vapor does not exceed 4; and / or, the polarity index P' of the polar small molecule solvent in the polar small molecule solvent vapor satisfies: 3.5≤P'≤5.5.
[0009] In the above-described process, the use of the aforementioned polar small-molecule solvent allows for the selective deliquescence of lithium chloride to form a lithium chloride solution, while alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca remain largely deliquescent. Furthermore, the polar small-molecule solvent vapor has no relative humidity requirement; selective separation of lithium chloride and obtaining a high-purity lithium chloride solution can be achieved regardless of whether low or high humidity is used. Higher relative humidity of the polar small-molecule solvent vapor indicates a higher concentration of the polar small-molecule solvent in the gas system, which is more conducive to the selective dissolution of lithium ions.
[0010] In conjunction with the first aspect, in optional embodiments of this application, the polar small molecule solvent includes at least one of methanol, ethanol, and isopropanol. Alternatively, the polar small molecule solvent includes a first solvent and a second solvent, the first solvent including acetone, and the second solvent including at least one of methanol, ethanol, and isopropanol; the volume ratio of the first solvent vapor to the second solvent vapor in the solvent vapor is (3:1) to (1:3).
[0011] In the above process, the solubility of alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca in the aforementioned polar small-molecule solvents is much lower than that of lithium chloride. Therefore, the polar small-molecule solvent vapor and the solid powder to be purified containing chloride and lithium ions are transported to a hypergravity reactor. Under the influence of hypergravity, where centrifugal force is greater than gravity, the polar small-molecule solvent in the gas phase comes into full contact with the solid powder to be purified. The solid powder absorbs the polar small-molecule solvent in the solvent vapor, selectively causing lithium chloride to deliquesce and form a lithium chloride solution. Then, under the influence of hypergravity, the lithium chloride solution can be selectively separated from the non-deliquescent solid powder in a timely manner. Timely separation of the lithium chloride solution from the non-deliquescent solid powder avoids the gradual accumulation of excessive lithium chloride solution on the surface of the non-deliquescent solid powder. If the alkali metal / alkaline earth metal halides are in contact with the lithium chloride solution for a prolonged period, there is a problem of localized solvent excess, which accelerates the dissolution of the alkali metal / alkaline earth metal and thus reduces the purity of lithium ions in the purification solution.
[0012] In addition, even though the solubility of alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca in methanol, ethanol, and isopropanol is much lower than that of lithium chloride, directly immersing the solid powder to be purified in the aforementioned polar small-molecule solvents to separate lithium ions from the aforementioned alkali metal / alkaline earth metal ions requires the addition of large amounts of organic solvents. Furthermore, current industrial equipment suffers from limited mass transfer and poor mixing, making it virtually impossible to avoid localized over-concentration from a microscopic perspective (for example, due to poor mixing, a large number of chloride ions may surround nickel in the system, leading to [NiCl4]). 2 When complex ions are formed and coordinate with organic cations, they are easily soluble in organic solvents, thus making it impossible to achieve efficient selective leaching. Impurity ions are easily carried into the liquid phase along with lithium chloride, making them difficult to separate. As a result, the purity of the lithium-containing solution product will be greatly reduced.
[0013] In conjunction with the first aspect, in an optional embodiment of this application, the solvent vapor includes polar small molecule solvent vapor, and the relative humidity of the polar small molecule solvent vapor is 0% < RH ≤ 100%.
[0014] In the above-described process, when the polar small-molecule solvent vapor is contacted with the solid powder to be purified for deliquescence lithium extraction, the polar small-molecule solvent vapor exhibits better selectivity and has no relative humidity requirement. Under the influence of a hypergravity field, regardless of whether low or high humidity is used, selective separation of lithium chloride can be achieved, yielding a high-purity lithium chloride solution. Higher relative humidity of the polar small-molecule solvent vapor indicates a higher concentration of the polar small-molecule solvent in the gas system, which is more conducive to the selective dissolution of lithium ions.
[0015] In conjunction with the first aspect, in an optional embodiment of this application, the solvent vapor includes water vapor and polar small molecule solvent vapor; in the solvent vapor, the volume ratio of water vapor to polar small molecule solvent vapor is (8:1) to (1:9).
[0016] In the above process, water vapor and polar small molecule solvent vapor are mixed to form solvent vapor, which can improve the leaching efficiency of lithium ions while taking into account the purity of lithium ions.
[0017] In conjunction with the first aspect, in an optional embodiment of this application, the molar ratio of lithium ions to chloride ions in the solid powder to be purified is 1:(1.2~2).
[0018] In the above process, controlling the molar ratio of lithium ions to chloride ions in the solid powder to be purified to 1:(1.2~2) can avoid a low lithium ion yield due to insufficient chloride ion content, while also preventing the dissolution of other impurity ions due to excessive chloride ion content, which would affect purity. For example, when the chloride content is too high, chloride ions are more likely to cause local overconcentration. Some transition metals easily form coordination relationships with chloride to form coordination anions. After combining with organic cations, according to the principle of "like dissolves like," these salts are usually easily soluble in ethanol and other organic solvents, thus entering the liquid phase along with lithium ions, leading to a decrease in the purity of the lithium product.
[0019] In conjunction with the first aspect, in optional embodiments of this application, the solvent vapor further includes a carrier gas, which includes at least one of nitrogen, argon, helium, neon, krypton, xenon, and air.
[0020] In the above process, using at least one of nitrogen, argon, helium, neon, krypton, xenon and air as the carrier gas in the solvent vapor can not only dilute the solvent in the solvent vapor, which helps the solid powder to be purified to selectively deliquesce and separate lithium chloride, but also avoid the carrier gas from reacting with lithium ions, reduce side reactions and improve yield.
[0021] In some embodiments, the solvent vapor includes polar small molecule solvent vapor, and the carrier gas is at least one of nitrogen, argon, helium, neon, krypton, and xenon.
[0022] In the above technical solutions, when only organic solvents are used, the presence of carbon dioxide in the air easily leads to side reactions, causing lithium carbonate crystals to precipitate in the lithium solution, thus reducing the lithium dissolution efficiency and yield. Therefore, at least one of nitrogen, argon, helium, neon, krypton, and xenon is selected as the carrier gas. When water vapor is used as the solvent vapor, air can be used as the carrier gas. In air, due to the presence of carbon dioxide, as the gas flow rate increases, lithium carbonate is less likely to form, or the formed lithium carbonate is converted into lithium bicarbonate, which is highly soluble in water, thus having a relatively small impact on the lithium yield.
[0023] In conjunction with the first aspect, in optional embodiments of this application, the solid powder to be purified includes at least one of lithium clay ore, spodumene ore, salt lake brine crystallization powder, dried powder of waste battery acid leaching solution, and acid leaching residue from lithium ore extraction lines.
[0024] In the above-mentioned implementation process, the lithium extraction method according to this application can not only extract lithium from lithium ores with low lithium grade such as lithium clay ore and spodumene ore, but also from brines with high magnesium-to-lithium ratio such as salt lake brine crystal powder. It can also be applied to lithium extraction from waste batteries and slag from lithium extraction production lines, and has a wide range of applications.
[0025] In conjunction with the first aspect, in an optional embodiment of this application, the particle size of the solid powder to be purified does not exceed 100 μm.
[0026] In conjunction with the first aspect, in an optional embodiment of this application, the solid powder to be purified includes an ion-intercalated layered compound, and the particle size of the solid powder to be purified is 1 μm to 50 μm.
[0027] In the above process, before purifying the solid material to be purified, the solid material is first ball-milled or crushed to form powder with a particle size of no more than 100μm. Under the action of a supergravity field, the gas-solid mass transfer effect between the solid powder to be purified and the solvent gas phase can be accelerated, thereby improving the purification efficiency and yield and reducing the production cost.
[0028] In addition, when the substance to be purified is an ion-intercalated layered compound, controlling the particle size of the solid powder to be purified to be 1μm~50μm, combined with the aforementioned effect of the hypergravity field, can prevent particle agglomeration, ensure the gas-solid mass transfer effect between the solid powder to be purified and the solvent vapor, improve purification efficiency and yield, and reduce the production cost caused by excessive crushing.
[0029] In conjunction with the first aspect, in an optional embodiment of this application, the volume ratio of the solid powder to solvent vapor to be purified is 1:(5~10).
[0030] In the above process, when supplying solvent vapor to the supergravity reactor, controlling the volume ratio of the solid powder to be purified to the solvent vapor to be 1:(5~10) can improve the yield while reducing the production cost.
[0031] In conjunction with the first aspect, in an optional embodiment of this application, the lithium content in the solid powder to be purified is less than 0.1 wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 4 hours.
[0032] Alternatively, the lithium content in the solid powder to be purified is 0.1wt%~0.5wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 1 hour.
[0033] Alternatively, the lithium content in the solid powder to be purified is greater than 0.5 wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 30 min.
[0034] In the above process, when the lithium content in the solid powder to be purified is less than 0.1 wt%, the reactivity is low. By appropriately extending the residence time of the solid powder to be purified to more than 4 hours, the yield can be improved. Further controlling the residence time to not exceed 6 hours can avoid the increase in production costs caused by excessive residence time.
[0035] When the lithium content in the solid powder to be purified is 0.1wt%~0.5wt%, adjusting the residence time of the solid powder to be purified in the supergravity reactor with solvent vapor to more than 1 hour can improve the yield. Further controlling the residence time to not exceed 2 hours can avoid the increase in production cost caused by excessive residence time.
[0036] When the lithium content in the solid powder to be purified is greater than 0.5 wt%, adjusting the residence time of the solid powder in contact with the solvent vapor in the supergravity reactor to more than 30 minutes can improve the yield. Further controlling the residence time to not exceed 1 hour can avoid the increase in production costs caused by excessive residence time.
[0037] In conjunction with the first aspect, the centrifugal force of the hypergravity reactor is no less than 10G.
[0038] And / or, the solvent vapor is delivered to the hypergravity reactor to maintain the pressure in the hypergravity reactor at 0.5 MPa to 0.55 MPa.
[0039] In the above implementation process, the centrifugal force of the supergravity reactor is controlled to be no less than 10G, and can be selected as 10G~50G. This can not only promote the gas-solid mass transfer between the solid powder to be purified and the solvent vapor, but also separate the lithium chloride solution formed by deliquescence in a timely manner, thereby improving the lithium extraction yield and efficiency.
[0040] Furthermore, by transporting solvent vapor to the hypergravity reactor and maintaining the pressure in the hypergravity reactor at 0.5MPa~0.55MPa, the lithium extraction efficiency can be accelerated while meeting the humidity requirements for separating lithium chloride. Attached Figure Description
[0041] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0042] Figure 1 A flow chart of lithium extraction process provided as an example in this application. Detailed Implementation
[0043] The embodiments of this application will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of this application. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0044] Currently, the mainstream lithium extraction technologies in industry mainly include acid leaching precipitation and solvent extraction. However, these technologies exhibit significant limitations when dealing with low-grade lithium resources (such as lithium clay and other lithium ores with a lithium content of less than 0.5 wt%, high magnesium-to-lithium ratio brines, and lithium extraction slag).
[0045] For example, clay-type lithium ore powder, sulfate, concentrated sulfuric acid, and water are mixed and roasted (at a holding temperature of 480℃~750℃) to obtain roasted clinker and roasting flue gas. The roasted clinker is then leached with water to obtain a lithium leachate. However, this technology uses concentrated sulfuric acid for roasting, which poses significant safety risks and has stringent environmental safety requirements. Furthermore, the high energy consumption of roasting leads to high operating costs and poor economic viability. For lithium extraction from low-grade lithium ore, the revenue often fails to cover the costs.
[0046] For example, lithium extraction slag can be processed through pulping, grinding, leaching, pulp conditioning, flotation, magnetic separation, gravity separation, and weak magnetic separation to achieve comprehensive utilization of lithium resources. However, the lithium recovery rate is usually no more than 65%, and the process is relatively complicated.
[0047] For example, after mechanical activation pretreatment of low-grade lepidolite, it is calcined in stages with the addition of two auxiliary agents (sodium sulfate and calcium fluoride), followed by selective leaching with sodium carbonate solution, and then deep purification through adsorption using a 5μm filter membrane and chelating resin. However, this technology requires the use of fluorine-containing substances for calcination, which poses environmental risks and has high energy consumption; in addition, an extra impurity removal process is required after leaching.
[0048] In addition, high-purity lithium ion extraction is often difficult to achieve in systems containing large amounts of coexisting ions such as magnesium, sodium, and potassium, especially when the Mg / Li mass ratio in the raw material is greater than 10:1, at which point the separation coefficient drops sharply. For transition metals such as Fe, Co, and Ni in leachate from spent batteries, traditional methods also require multi-stage precipitation for impurity removal, which is cumbersome. Heating, evaporation, and multi-stage extraction consume large amounts of electrical and thermal energy, resulting in high production costs and limiting the development and utilization of low-grade resources. Furthermore, these methods require the extensive use of acids, alkalis, and organic solvents, generating difficult-to-treat industrial waste and wastewater, which does not meet the requirements of green and sustainable development.
[0049] Based on this, please refer to Figure 1 This application provides a lithium extraction method, including: The solid powder to be purified and solvent vapor are transported to a high-gravity reactor, where the solid powder absorbs the solvent vapor and deliquesces to form a lithium chloride solution. Simultaneously, the high-gravity reactor separates the lithium chloride solution from the undeliquesced solid powder, collecting the lithium chloride solution. The solvent vapor includes at least one of water vapor and polar small-molecule solvent vapors, and the solid powder to be purified contains lithium ions and chloride ions.
[0050] In this application, "deliquescence" refers to the phenomenon in which certain solid substances absorb solvent (such as at least one of polar small molecule solvents such as water and methanol) from solvent vapor and gradually dissolve in the absorbed solvent, eventually forming a solution.
[0051] In this application, "hypergravity" refers to centrifugal force generated by high-speed rotation, where the centrifugal force is greater than gravity. The hypergravity reactor is a conventional hypergravity reactor, typically featuring a rotating drum capable of generating extremely large centrifugal forces, with through-holes in the drum wall to allow gas-liquid flow. It is understood that, in this application, depending on the particle size of the solid powder to be purified, a hypergravity reactor with through-hole diameters smaller than the particle size of the solid powder to be purified needs to be selected.
[0052] The solid powder to be purified and solvent vapor are introduced into a hypergravity reactor. Under the influence of hypergravity, where centrifugal force exceeds gravity, the solvent (at least one of water and a polar small-molecule solvent) contacts the solid powder containing chloride and lithium ions in the gas phase. Due to the difference in critical deliquescence humidity between lithium chloride and other alkali metal / alkaline earth metal halides (e.g., halides of Na, K, Mg, and Ca) in the solvent, the solid powder absorbs the solvent vapor and deliquesces to form a lithium chloride solution (understandably, the solute in the lithium chloride solution is lithium chloride, and the solvent is at least one of water and a polar small-molecule solvent). Furthermore, through gas-solid mass transfer, the amount of solvent in contact with the solid per unit time is relatively small, which can improve the problem of localized excess solvent on the surface of the solid powder, reduce the probability of impurity dissolution, and ultimately obtain a lithium-containing solution with high lithium content and low impurity content. Although a large amount of solvent vapor needs to be introduced, the solvent vapor can be circulated through a gas path, which can reduce costs.
[0053] Simultaneously, under the influence of gravity, the deliquescent lithium chloride solution can be promptly separated from the non-deliquescent solid powder, preventing the lithium chloride solution from accumulating on the surface of the non-deliquescent solid powder for extended periods. This mitigates the problem of excessive solvent localization leading to the dissolution of other impurities in the solid powder (such as the aforementioned alkali metal / alkaline earth metal halides) into the lithium chloride solution. Subsequently, the obtained lithium chloride solution can be directly purified into high-purity lithium chloride crystals through simple fractionation (the solvent obtained from fractionation can also be reused), or lithium carbonate can be precipitated directly by passing carbon dioxide through it (the filtrate can be reused). The solvent is essentially unaffected, serving only as a transport carrier, which significantly reduces process costs.
[0054] If the solid powder to be purified is directly mixed with a liquid solvent and lithium is extracted based on the difference in solubility, the solubility difference between lithium chloride and alkali metal / alkaline earth metal halides in the liquid solvent is small. Furthermore, transition metals easily form anionic ligands with chloride ions, which combine with organic cations to form organic complexes and thus dissolve in organic solvents. This results in poor purification effect and low purity and concentration of lithium ions in the purified solution. Further purification is required through subsequent concentration, precipitation, filtration, or washing, which is a cumbersome process.
[0055] If the solid material to be purified is simply crushed and placed in a conventional stirred tank or reaction vessel, relying on the natural convection of solvent vapor results in a limited gas-solid contact area, long reaction time, low purification efficiency, and low yield. Moreover, the lithium chloride solution formed by deliquescence cannot be discharged from the surface of the undeliquescent solid powder in a timely manner. The lithium chloride solution accumulates on the surface of the undeliquescent solid powder for a long time, which leads to excessive dissolution of other impurities in the solid powder (such as the aforementioned alkali metal / alkaline earth metal halide salts) in the lithium chloride solution, thereby reducing the purity of the lithium extraction solution.
[0056] In addition, the supergravity reactor of this application can not only serve as a reactor for the solid powder to be purified and the solvent vapor, but also as a stirrer to rotate the solid powder to be purified, thereby improving the contact effect between the solid powder to be purified and the solvent vapor. Furthermore, it can serve as a gas-liquid-solid three-phase separator, which can further reduce production costs.
[0057] In this application, "solvent vapor includes at least one of water vapor and polar small molecule solvent vapor" means that the solvent vapor contains water vapor or polar small molecule solvent vapor, or both water vapor and polar small molecule solvent vapor. In some cases, the solvent vapor may also contain a carrier gas, such as at least one of nitrogen, argon, helium, neon, krypton, xenon, and air.
[0058] In some embodiments, based on the difference in critical deliquescence humidity between lithium chloride and other alkali metal / alkaline earth metal halides (e.g., halides of Na, K, Mg, and Ca) in a specific solvent vapor, the humidity can be adjusted to selectively deliquesce lithium chloride while other alkali metal / alkaline earth metal halides remain almost non-deliquescent, thereby forming a high-purity lithium chloride solution. Under the influence of gravity, the lithium chloride solution is promptly discharged and separated from the non-deliquescent solid powder, preventing the lithium chloride solution from accumulating on the surface of the non-deliquescent solid powder for a long time, which would lead to other impurities and solvents in the solid powder to be purified, thus further improving the purity.
[0059] In some embodiments, the solvent vapor includes water vapor, wherein the relative humidity of the water vapor is 11% ≤ RH ≤ 33%.
[0060] The relative humidity of water vapor refers to the percentage of the actual partial pressure of water vapor in the solvent vapor compared to the saturated water vapor pressure at the same temperature.
[0061] When the relative humidity (RH) of water vapor is ≥11%, the solid powder to be purified absorbs water vapor, selectively causing lithium chloride to deliquesce and form a lithium chloride solution. Furthermore, when the relative humidity (RH) is ≤33%, alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca are essentially non-deliquescent, allowing for selective and timely separation of the lithium chloride aqueous solution from the non-deliquescent solid powder under the influence of gravity. Timely separation of the lithium chloride aqueous solution from the non-deliquescent solid powder prevents excessive accumulation of lithium chloride aqueous solution on the surface of the non-deliquescent solid powder. If alkali metal / alkaline earth metal halides are in prolonged contact with the lithium chloride aqueous solution, it will accelerate the dissolution of the alkali metal / alkaline earth metal, thus reducing the purity of lithium ions in the purification solution. If the relative humidity of water vapor is greater than 33%, alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca will gradually dissolve, resulting in lower lithium ion purity in the lithium chloride solution.
[0062] As an example, the solvent vapor is water vapor, and the relative humidity RH of the water vapor can be one of 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, or 33%, or any value between two of them.
[0063] As an example, the solvent vapor includes water vapor, with a relative humidity (RH) of 25% to 33%. Higher relative humidity indicates a higher concentration of water in the system. Using water vapor with higher relative humidity can suppress the deliquescence of alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca, while further improving the leaching efficiency of lithium ions.
[0064] Furthermore, this application does not limit how the solvent vapor with the above-mentioned relative humidity is obtained. In some embodiments, water can be heated to form water vapor, and the water vapor can be mixed with the carrier gas to form water vapor with a certain relative humidity.
[0065] Alternatively, in other embodiments, since the air humidity above a saturated solution of a specific salt in a confined space stabilizes at a fixed value, a carrier gas can be passed through the saturated salt solution to obtain solvent vapor with a certain humidity. For example, humid air can be controlled by passing air through a saturated solution to obtain water vapor with a certain water content. For example, the solution may be a salt solution of lithium chloride, calcium bromide, lithium iodide, potassium acetate, potassium fluoride, magnesium chloride, sodium iodide, potassium carbonate, magnesium nitrate, sodium bromide, cobalt chloride, potassium iodide, strontium chloride, sodium nitrate, sodium chloride, ammonium chloride, potassium bromide, ammonium sulfate, potassium chloride, strontium nitrate, potassium nitrate, potassium sulfate, or potassium chromate. For example, when preparing water vapor with a relative humidity of approximately 20%, sufficient potassium acetate solid can be placed in a sealable container, a small amount of distilled water can be added, and the mixture can be stirred continuously until a paste-like mixture with undissolved solids remaining at the bottom of the cup is formed, ensuring that the solution is saturated and the air humidity above the saturated solution stabilizes at around 20%.
[0066] Alternatively, the dry carrier gas and the saturated vapor of the solvent can be mixed, and the solvent vapor can be adjusted to the desired relative humidity.
[0067] Alternatively, a commercial humidity generator can be used to prepare solvent vapor with the appropriate humidity as needed.
[0068] In some embodiments, the number of carbon atoms of the polar small molecule solvent in the polar small molecule solvent vapor does not exceed 4. And / or, the polarity index P' of the polar small molecule solvent in the polar small molecule solvent vapor satisfies: 3.5 ≤ P' ≤ 5.5.
[0069] Using the aforementioned polar small-molecule solvents, lithium chloride can be selectively deliquesced to form a lithium chloride solution, while alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca are essentially non-deliquescing. Furthermore, the vapors of these polar small-molecule solvents have no relative humidity requirement; selective separation of lithium chloride can be achieved regardless of whether low or high humidity is used, yielding a high-purity lithium chloride solution. Higher relative humidity of the polar small-molecule solvent vapor indicates a higher concentration of the solvent in the gas system, which is more conducive to the selective dissolution of lithium ions.
[0070] As examples, the number of carbon atoms in a polar small molecule solvent can be 1, 2, 3, or 4. For example, methanol (CH3OH) is an example of a solvent with 1 carbon atom. Ethanol (C2H5OH) is an example of a solvent with 2 carbon atoms. Propanol (C3H7OH) is an example of a solvent with 3 carbon atoms. Butanol is an example of a solvent with 4 carbon atoms.
[0071] A higher polarity index (P') indicates stronger polarity. The polarity index (P') of polar small molecule solvents can be obtained from reference materials. Selecting organic small molecule solvents with a polarity index of 3.5 ≤ P' ≤ 5.5 provides suitable polarity, enabling the deliquescence of lithium chloride while reducing the probability of deliquescence of alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca. This, in turn, improves product purity and lithium ion leaching rate.
[0072] As an example, the polarity index P' of a polar small molecule solvent vapor can be one of 3.5, 4.0, 4.5, 5.0 or 5.5, or any value between two of them.
[0073] In some embodiments, the polar small molecule solvent includes at least one of methanol, ethanol, and isopropanol.
[0074] The polarity index P' of methanol (CH3OH) is approximately 5.1. The polarity index P' of ethanol (C2H5OH) is approximately 5.2. The polarity index P' of isopropanol (CH3-CH(OH)-CH3) is approximately 3.9~4.3.
[0075] In addition, even though the solubility of alkali metal / alkaline earth metal halides such as Na, K, Mg, and Ca in the above-mentioned polar small molecule solvents is much lower than that of lithium chloride, if the solid powder to be purified is directly immersed in the above-mentioned polar small molecule solvent liquid to separate lithium ions and the above-mentioned alkali metal / alkaline earth metal ions, a large amount of organic solvent will be required, and the purity of the purified lithium liquid will also be low.
[0076] In some embodiments, the polar small molecule solvent includes a first solvent and a second solvent. The first solvent includes acetone, and the second solvent includes at least one of methanol, ethanol, and isopropanol. When extracting lithium from brines with a high magnesium-to-lithium ratio, such as salt lake brine crystals, using a mixture of the first and second solvents provides better separation of lithium chloride and magnesium chloride compared to using only the second solvent. This results in a lower magnesium ion content in the collected lithium chloride solution, thereby improving the purity of the extracted lithium product.
[0077] In some embodiments, the volume ratio of the first solvent vapor to the second solvent vapor in the solvent vapor is (3:1) to (1:3). As an example, the volume ratio of the first solvent vapor to the second solvent vapor is one of 3:1, 2:1, 1:1, 1:2 or 1:3, or a value between any two.
[0078] The relative humidity of the aforementioned polar small molecule solvent vapor can be controlled by referring to the aforementioned method for controlling the relative humidity of water vapor, and this application does not impose any restrictions.
[0079] In some embodiments, the solvent vapor includes polar small molecule solvent vapor, and the relative humidity of the polar small molecule solvent vapor is 0% < RH ≤ 100%. The relative humidity of the polar small molecule solvent vapor can also be referred to as the polar small molecule solvent vapor saturation (the partial pressure of the organic small molecule solvent vapor in the current atmosphere / the saturated vapor pressure of the liquid organic small molecule solvent at the same temperature).
[0080] When lithium is extracted by contacting the above-mentioned polar small molecule solvent vapor with the solid powder to be purified through deliquescence, the above-mentioned polar small molecule solvent vapor has better selectivity and no relative humidity requirement. Under the action of hypergravity, regardless of whether low or high humidity is used, selective separation of lithium chloride can be achieved to obtain a high-purity lithium chloride solution.
[0081] As an example, the relative humidity RH of polar small molecule solvent vapor can be one of 0.01%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 100%, or any value between two of them.
[0082] Furthermore, in some embodiments, the relative humidity of the polar small molecule solvent vapor is 40%≤RH≤95%.
[0083] Furthermore, in some embodiments, the relative humidity of the polar small molecule solvent vapor is 60% ≤ RH ≤ 90%.
[0084] Adjusting the relative humidity of the polar small molecule solvent vapor to 40%≤RH≤95%, or optionally 60%≤RH≤90%, combined with the aforementioned hypergravity field, can improve purification yield while reducing production costs. If the relative humidity of the polar small molecule solvent vapor is too high, even if the solid powder to be purified can have sufficient contact with the solvent vapor under hypergravity, the vapor easily condenses into droplets and rapidly separates into solid and liquid under hypergravity. This results in insufficient utilization of the solvent and a decrease in the lithium concentration in the lithium extraction solution, increasing production costs. If the relative humidity of the polar small molecule solvent is too low, while the solid powder to be purified can have sufficient contact with the solvent vapor under hypergravity, the relatively low content of the polar small molecule solvent vapor means that some of the solid powder cannot efficiently adsorb sufficient polar small molecule solvent vapor, leading to lower purification efficiency and lower yield.
[0085] In some embodiments, the solvent vapor includes water vapor and polar small molecule solvent vapor; the volume ratio of water vapor to polar small molecule solvent vapor in the solvent vapor is 8:1 to 1:9.
[0086] In the above process, mixing water vapor and polar small-molecule solvent vapor to form solvent vapor can improve the leaching efficiency of lithium ions while maintaining lithium ion purity. In this case, the relative humidity of the solvent vapor is not limited and can be controlled by calculating the relative humidity and volume ratio of the water vapor and the polar small-molecule solvent vapor.
[0087] As an example, in solvent vapor, the volume ratio of water vapor to polar small molecule solvent vapor can be one of 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8 or 1:9, or any value between two of them.
[0088] In some embodiments, the solvent vapor also includes a carrier gas. This application does not limit the specific type of carrier gas; further, in some embodiments, the carrier gas includes at least one selected from air, nitrogen, argon, helium, neon, krypton, and xenon.
[0089] Furthermore, in some embodiments, the carrier gas includes at least one of air, nitrogen, argon, and helium.
[0090] Using at least one of air, nitrogen, argon, helium, neon, krypton, and xenon as a carrier gas in the solvent vapor can not only dilute the solvent vapor and help the solid powder to be purified to selectively deliquesce and separate lithium chloride, but also avoid the carrier gas from reacting with lithium ions, reduce side reactions, and improve the yield.
[0091] In some embodiments, the solvent vapor is a polar small-molecule solvent vapor, and the carrier gas is at least one selected from nitrogen, argon, helium, neon, krypton, and xenon. When only an organic solvent is used, the presence of carbon dioxide in the air easily leads to side reactions, causing lithium carbonate crystals to precipitate in the lithium solution, thereby reducing the lithium dissolution efficiency and yield. Therefore, at least one of nitrogen, argon, helium, neon, krypton, and xenon is selected as the carrier gas. However, when water vapor is used as the solvent vapor, air can be used as the carrier gas. In air, due to the presence of carbon dioxide, as the gas flow rate increases, lithium carbonate is less likely to be formed, or the formed lithium carbonate is converted into lithium bicarbonate, which is highly soluble in water, and has little impact on the lithium yield.
[0092] Furthermore, this application does not limit the specific type of solid raw material. In some embodiments, the solid powder to be purified includes at least one of lithium clay ore, spodumene ore, salt lake brine crystallization powder, dried powder of waste battery acid leaching solution, and acid leaching residue from lithium ore extraction lines.
[0093] The lithium extraction method of this application can be used not only to extract lithium from lithium ores with low lithium grade, such as lithium clay ore and spodumene ore, but also to extract lithium from brines with high magnesium-to-lithium ratios, such as salt lake brine crystal powder. It can also be applied to the extraction of lithium from waste batteries and slag from lithium extraction production lines, making it widely applicable.
[0094] In conjunction with the first aspect, in an optional embodiment of this application, the molar ratio of lithium ions to chloride ions in the solid powder to be purified is 1:(1.2~2).
[0095] In the above process, controlling the molar ratio of lithium ions to chloride ions in the solid powder to be purified to 1:(1.2~2) can avoid a low lithium ion yield due to insufficient chloride ion content, while also preventing the dissolution of other impurity ions due to excessive chloride ion content, which would affect purity. For example, when the chloride content is too high, chloride ions are more likely to cause local overconcentration. Some transition metals easily form coordination relationships with chloride to form coordination anions. After combining with organic cations, according to the principle of "like dissolves like," these salts are usually easily soluble in ethanol and other organic solvents, thus entering the liquid phase along with lithium ions, leading to a decrease in the purity of the lithium product.
[0096] As an example, in the solid powder to be purified, the molar ratio of lithium ions to chloride ions is one of 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2.0, or any value between the two.
[0097] As an example, in the solid powder to be purified, the molar ratio of lithium ions to chloride ions is 1:(1.2~1.5); or, in the solid powder to be purified, the molar ratio of lithium ions to chloride ions is 1:(1.5~2.0).
[0098] Furthermore, when the chloride ion content in the raw material to be purified is low, the raw material and the chloride can be mixed and ground together during the preparation of the solid powder to be purified. For example, the chloride can be ammonium chloride. For example, the chloride can be sodium chloride or potassium chloride.
[0099] For example, when the raw material to be purified is lithium montmorillonite clay ore, ammonium chloride can be added to the lithium clay ore at a molar ratio of Li:Cl=1:1.5, and then jaw crushing and ball milling can be performed.
[0100] Furthermore, in order to improve lithium extraction efficiency and yield, in some embodiments, the particle size of the solid powder to be purified can be controlled to not exceed 100 μm.
[0101] Before purifying the solid materials to be purified, the solid materials are first ball-milled or crushed to form powder with a particle size of no more than 100μm. Under the action of a supergravity field, the gas-solid mass transfer effect between the solid powder to be purified and the solvent gas phase can be accelerated, thereby improving the purification efficiency and yield and reducing the production cost.
[0102] As an example, the particle size of the solid powder to be purified can be controlled to be one of 1μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, or 100μm, or any value between two of these. The particle size of the solid powder to be purified mentioned above is the maximum particle size of the solid powder to be purified.
[0103] As an example, in order to obtain a solid powder of suitable particle size for purification, the raw material to be purified and the optional chloride can be put into a crusher for crushing, then ball milled, and finally sieved to collect the sieve material.
[0104] Furthermore, the solid powder to be purified includes ion-intercalated layered compounds, and the particle size of the solid powder to be purified is 1μm~50μm.
[0105] When the substance to be purified is an ion-intercalated layered compound, controlling the particle size of the solid powder to be purified to be 1μm~50μm, combined with the aforementioned effect of the hypergravity field, can prevent particle agglomeration, ensure the gas-solid mass transfer effect between the solid powder to be purified and the solvent gas phase, improve purification efficiency and yield, and reduce the production cost caused by excessive crushing.
[0106] As an example, in lithium montmorillonite clay ore, lithium ions are embedded in the layered aluminosilicate lattice of montmorillonite (interlayer domain). If the particle size is too small, the powder is prone to agglomeration under electrostatic action.
[0107] As an example, when recycling used ternary lithium batteries, the precursor of the ternary cathode material is a cationic layered compound. When extracting lithium from the solid waste of such production lines, the particle size of the solid powder to be purified should not be too small.
[0108] As an example, to facilitate obtaining a solid powder of suitable particle size for purification, the powder can be filtered multiple times, and the intermediate filter material can be collected. For instance, first, the powder can be passed through a 50μm sieve, and the undersize material can be collected. Then, it can be passed through a 1μm sieve, and the oversize material can be collected to obtain a solid powder of particle size ranging from 1μm to 50μm for purification.
[0109] Furthermore, when lithium extraction from salt lake brine is required, the brine can be pretreated first: ammonium chloride is added at a molar ratio of Li:Cl = 1:(1.2~2). Due to the high viscosity of the brine, a small amount of dispersant (sodium polyacrylate, 0.1%) is added for dilution and modification. Subsequently, the liquid is atomized into tiny crystals with an average particle size of 50μm by spray drying (orifice diameter 0.5mm), and then filtered.
[0110] Furthermore, during lithium extraction, the solvent vapor can be transported to the high-gravity reactor to contact the solid powder to be purified, with a volume ratio of solid powder to solvent vapor of 1:(5~10). Controlling the volume ratio of solid powder to solvent vapor to 1:5~10 can improve the yield while reducing production costs.
[0111] As an example, the volume ratio of the solid powder to the solvent vapor to be purified is one of 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, or any value between two of them.
[0112] Furthermore, in some embodiments, when the lithium content in the solid powder to be purified is less than 0.1 wt%, the residence time of the solid powder to be purified in the hypergravity reactor is not less than 4 hours, and can be selected as 4 hours to 6 hours.
[0113] When the lithium content in the solid powder to be purified is less than 0.1 wt%, the reactivity is low. By appropriately extending the residence time of the solid powder to be purified to more than 4 hours, the yield can be improved. Further controlling the residence time to not exceed 6 hours can avoid the increase in production costs caused by excessive residence time.
[0114] As an example, when the lithium content in the solid powder to be purified is less than 0.1 wt%, the residence time can be one of 4 h, 5 h, or 6 h, or any value in between. When the particle size of the solid powder to be purified is small, the residence time can be appropriately reduced within the above range.
[0115] In some embodiments, the lithium content in the solid powder to be purified is 0.1wt%~0.5wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 1h, and can be selected as 1h~2h.
[0116] When the lithium content in the solid powder to be purified is 0.1wt%~0.5wt%, adjusting the residence time of the solid powder to be purified in the supergravity reactor with solvent vapor to more than 1 hour can improve the yield. Further controlling the residence time to not exceed 2 hours can avoid the increase in production cost caused by excessive residence time.
[0117] In some embodiments, the lithium content in the solid powder to be purified is greater than 0.5 wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 30 min, and can be selected as 30 min to 1 h.
[0118] When the lithium content in the solid powder to be purified is greater than 0.5 wt%, adjusting the residence time of the solid powder in contact with the solvent vapor in the supergravity reactor to more than 30 minutes can improve the yield. Further controlling the residence time to not exceed 1 hour can avoid the increase in production costs caused by excessive residence time.
[0119] In some embodiments, the centrifugal force of the centrifugal reactor is not less than 10G, and can be selected from 10G to 50G. Controlling the centrifugal force of the centrifugal reactor to be not less than 10G, and can be selected from 10G to 50G, not only promotes the gas-solid mass transfer between the solid powder to be purified and the solvent vapor, but also enables timely separation of the lithium chloride solution formed by deliquescence, thereby improving the lithium extraction yield and efficiency. It can be understood that centrifugal force = mass × squared angular velocity × radius.
[0120] As an example, the centrifugal force of the hypergravity reactor can be one of 10G, 20G, 30G, 40G, or 50G, or any value in between.
[0121] In some embodiments, solvent vapor is supplied to the hypergravity reactor, maintaining the reactor pressure at 0.5 MPa to 0.55 MPa. Supplying solvent vapor to the hypergravity reactor while maintaining the reactor pressure at 0.5 MPa to 0.55 MPa can accelerate lithium extraction efficiency while meeting the humidity requirements for lithium chloride separation.
[0122] As an example, the gas pressure of the hypergravity reactor can be one of 0.5 MPa, 0.51 MPa, 0.52 MPa, 0.53 MPa, 0.54 MPa or 0.55 MPa, or any value in between.
[0123] Furthermore, in order to obtain further lithium-extracted products, the lithium extraction method also includes post-processing steps: Using a fractional distillation process, the solvent in the lithium chloride solution (which can be understood as the solute in the lithium chloride solution being lithium chloride, and the solvent being at least one of the above-mentioned water and polar small molecule solvents) can be reused by distillation regeneration (to prepare solvent vapor again). During the evaporation process, lithium chloride crystals are precipitated to obtain lithium chloride crystal products.
[0124] Alternatively, when the solvent in the lithium chloride solution is an organic solvent, pure carbon dioxide gas can be directly introduced into the lithium chloride solution to precipitate lithium carbonate crystals. After solid-liquid separation, the solvent can be reused.
[0125] Alternatively, when the solvent in the lithium chloride solution is water, pure carbon dioxide gas can be directly introduced into the lithium chloride solution and heated to above 80°C to avoid the formation of lithium bicarbonate, which would reduce the lithium precipitation yield. After solid-liquid separation, the solvent can be reused to precipitate lithium carbonate crystals.
[0126] The lithium extraction method of this application will be further described in detail below with reference to the embodiments.
[0127] Example 1 This embodiment provides a lithium extraction method, including: (1) Preparation of solid powder to be purified Raw material characteristics: Lithium-containing montmorillonite clay ore from a certain region in Jiangxi Province was selected. This type of raw material exhibits a unique lithium occurrence state, with lithium ions embedded in the layered aluminosilicate lattice of montmorillonite (interlayer domains), accompanied by gangue minerals such as kaolinite. Its Li content is approximately 0.2 wt%, with a high aluminum-to-silicon ratio. Traditional acid leaching methods easily lead to the dissolution of large amounts of aluminum and silicon, causing severe colloid formation and making solid-liquid separation extremely difficult.
[0128] Lithium clay ore was subjected to jaw crushing and ball milling. During ball milling, ammonium chloride was added at a molar ratio of Li:Cl = 1:1.5. After ball milling, the material was sieved to obtain undersize material with a particle size not exceeding 20 μm. The oversize material was then ball-milled again. The undersize material was subsequently dried at 110°C to remove surface free water.
[0129] (2) Lithium extraction The solid powder to be purified obtained in step (1) is fed into a high-gravity reactor and isopropanol vapor is introduced (the carrier gas is air, and the relative humidity of the isopropanol vapor is 20%). The volume ratio of the solid powder to isopropanol vapor is 1:5. The centrifugal force is set to 40G, the reaction temperature is 25℃, the pressure in the reaction chamber is maintained at 0.52MPa, and the residence time is 1.5h.
[0130] After lithium extraction, the lithium chloride solution is discharged from the outlet of the centrifugal reactor. Carbon dioxide is then introduced into the lithium chloride solution to adjust the temperature to 85°C, resulting in solid-liquid separation to obtain lithium carbonate. The solvent is then recovered.
[0131] Elemental content was determined using inductively coupled plasma optical emission spectrometry (ICP-OES).
[0132] Experimental results show that the lithium leaching rate reached 88.7% (leaching rate is the mass of lithium ions in the lithium chloride solution / the mass of lithium ions in the solid powder to be purified), and the content of aluminum and iron impurities in the lithium chloride solution was less than 0.01%. The purity of the lithium product reached 99.1% (lithium product purity = lithium content detected in the lithium product / theoretical lithium content in the lithium product).
[0133] Example 2 This embodiment provides a lithium extraction method, including: (1) Preparation of solid powder to be purified Raw material characteristics: The residue is acid leaching residue (hereinafter referred to as lithium extraction residue) from a spodumene mine's sulfuric acid lithium extraction production line. This waste residue is a terminal product of traditional processes and is usually treated as solid waste and disposed of through stockpiling. Analysis shows that the waste residue still contains 0.1wt%~0.2wt% Li, mainly in the form of unreacted spodumene phase or adsorbed lithium. The waste residue has a complex composition, containing a large amount of calcium sulfate, undecomposed aluminosilicates, and a small amount of residual acid, with a weakly acidic pH (approximately 4.5).
[0134] The lithium extraction slag is dried and sieved to remove large particles of impurities. Considering the potential presence of trace amounts of free acid in the slag, a small amount of alkaline solution (such as sodium carbonate solution) is sprayed onto the slag for neutralization and conditioning to adjust the pH to 6.5-7.0, thus preventing equipment corrosion and optimizing the reaction environment. The slag is then ball-milled, and the resulting material is sieved to obtain undersize particles with a diameter not exceeding 50 μm. The oversize material is then ball-milled again. The undersize material is subsequently dried at 110°C to remove surface free water.
[0135] (2) Lithium extraction The solid powder to be purified obtained in step (1) is fed into a supergravity reactor and isopropanol vapor is introduced (the carrier gas is air, and the relative humidity of the isopropanol vapor is 30%). The volume ratio of the solid powder to isopropanol vapor is 1:10. The centrifugal force is set to 40G, the reaction temperature is 25℃, the pressure in the reaction chamber is maintained at 0.53MPa, and the residence time is 1.0h.
[0136] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0137] Experimental results show that the lithium leaching rate reached 85.3%, and the lithium product purity reached 98.9%. This embodiment not only demonstrates the adaptability of the lithium extraction method provided in this embodiment to low-grade and difficult-to-process raw materials, but also opens up a green circular economy path of "turning waste into treasure".
[0138] Example 3 This embodiment provides a lithium extraction method, including: (1) Preparation of solid powder to be purified Raw material characteristics: Low-grade spodumene concentrate from the Sichuan Jiajika mining area was selected, with a lithium content of 0.4 wt% and a large amount of associated magnesium, iron, and aluminum silicates. The Mg / Li mass ratio was approximately 12:1.
[0139] The ore was subjected to jaw crushing and ball milling. During ball milling, ammonium chloride was added at a molar ratio of Li:Cl = 1:2. After ball milling, the ore was sieved to obtain undersize material with a particle size not exceeding 5 μm. The oversize material was then ball milled again. The undersize material was subsequently dried at 110°C to remove surface free water.
[0140] (2) Lithium extraction The solid powder to be purified obtained in step (1) is sent into a supergravity reactor and ethanol vapor is introduced (the carrier gas is nitrogen and the relative humidity of the ethanol vapor is 20%). The volume ratio of the solid powder to the ethanol vapor is 1:7. The centrifugal force is set to 50G, the reaction temperature is 25℃, the pressure in the reaction chamber is maintained at 0.55MPa, and the residence time is 1.0h.
[0141] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0142] Experimental results show that the leaching rate of lithium reached 93.1%, and the leaching rate of magnesium was less than 0.008%, achieving efficient magnesium-lithium separation, with the lithium product purity reaching 98.4%.
[0143] Example 4 This embodiment provides a method for lithium extraction from high magnesium-to-lithium ratio salt lake brine crystallization, including: (1) Preparation of solid powder to be purified Raw material characteristics: The original brine from the Qarhan Salt Lake in Qinghai Province, after preliminary sun-drying and concentration, Li + The concentration is 0.3 g / L, Mg 2+ The concentration is as high as 30 g / L (Mg / Li≈100:1), and it also contains a large amount of Na. + K + B 3+ Plasma.
[0144] Sodium chloride was first added at a molar ratio of Li:Cl = 1:2. Due to the high viscosity of the brine, a small amount of dispersant (sodium polyacrylate, 0.1 wt.%) was added for dilution and modification. Subsequently, the liquid was atomized into tiny crystals with an average particle size of 50 μm by spray drying (orifice diameter 0.5 mm).
[0145] (2) Lithium extraction The solid powder to be purified obtained in step (1) is sent into a supergravity reactor and water vapor is introduced (the carrier gas is air and the relative humidity of the water vapor is 18%). The volume ratio of the solid powder to water vapor is 1:7. The centrifugal force is set to 10G, the reaction temperature is 25℃, the pressure in the reaction chamber is maintained at 0.55MPa, and the residence time is 30min.
[0146] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0147] Experimental results showed that the lithium leaching rate reached 90.5%, and the lithium product purity reached 99.0%. This demonstrates the applicability of the method in extremely high magnesium environments.
[0148] Example 5 This embodiment provides a method for lithium extraction from the acid leaching solution of waste lithium iron phosphate batteries, including: (1) Preparation of solid powder to be purified Raw material characteristics: Extracted from the hydrochloric acid leaching solution of black powder from dismantled retired new energy vehicle batteries. This solution contains Li. + Fe 2+ PO4 3- and a small amount of Co 2+ Ni 2+ It has a pH of approximately 2.0, a complex composition, and contains many interfering ions.
[0149] The pH of the hydrochloric acid leaching solution was adjusted to 4.0-5.0 to hydrolyze and precipitate most of the iron ions. The precipitate was removed by filtration, leaving lithium ions in the solution. The purified liquid was then spray-dried, granulated, and passed through 50μm and 10μm sieves to produce a solid powder with a particle size of 10μm-50μm for purification.
[0150] (2) Lithium extraction The solid powder to be purified obtained in step (1) is sent into a supergravity reactor and ethanol vapor is introduced (the carrier gas is air and the relative humidity of the ethanol vapor is 15%). The volume ratio of the solid powder to be purified to the ethanol vapor is 1:9. The centrifugal force is set to 40G, the reaction temperature is 25℃, the pressure in the reaction chamber is maintained at 0.55MPa, and the residence time is 1.0h.
[0151] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0152] Experimental results show that the lithium recovery rate reached 91.8%, the magnesium leaching rate was less than 0.008%, achieving efficient magnesium-lithium separation. The lithium product purity reached 99.3%, and no obvious transition metal impurities such as iron, cobalt, and nickel were detected, indicating that this method is suitable for the recycling of complex electronic waste.
[0153] Example 6 This embodiment provides a lithium extraction method, which differs from Embodiment 3 in that: In step (2), the solvent vapor contains acetone vapor and ethanol vapor, the carrier gas is nitrogen, the relative humidity of the ethanol vapor is 20%, and the volume ratio of acetone to ethanol is 1:1.
[0154] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0155] Experimental results show that the leaching rate of lithium reached 94.1%, and the leaching rate of magnesium was less than 0.003%, achieving efficient magnesium-lithium separation, with the lithium product purity reaching 99.6%.
[0156] Example 7 This embodiment provides a lithium extraction method, which differs from Embodiment 3 in that: In step (2), butanol vapor is introduced (the carrier gas is nitrogen, and the relative humidity of the butanol vapor is 20%).
[0157] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0158] Experimental results showed that the lithium leaching rate reached 86.1%, the magnesium leaching rate was less than 0.09%, and the lithium product purity reached 98.6%.
[0159] Example 8 This embodiment provides a lithium extraction method, which differs from Embodiment 3 in that: In step (1), ammonium chloride is added during ball milling at a molar ratio of Li:Cl = 1:2.5.
[0160] After lithium extraction is completed, the lithium chloride solution is discharged from the outlet of the high gravity reactor, and the lithium leaching rate and lithium product purity are tested according to the method in Example 1.
[0161] The experimental results showed that the lithium leaching rate reached 93.5%, the magnesium leaching rate was about 0.8%, and the lithium product purity reached 88.6%.
[0162] Example 9 This embodiment provides a lithium extraction method, which differs from Embodiment 4 in that: In step (2), the solvent vapor includes water vapor and isopropanol vapor, with a volume ratio of water vapor to isopropanol vapor of 8:1 and a relative humidity of 18% for the water vapor.
[0163] Experimental results showed that the lithium leaching rate reached 92.4% and the lithium product purity reached 99.3%.
[0164] Example 10 This embodiment provides a lithium extraction method, which differs from Embodiment 4 in that: In step (2), the solvent vapor includes water vapor and isopropanol vapor, with a volume ratio of water vapor to isopropanol vapor of 1:9 and a relative humidity of 18% for the water vapor.
[0165] Experimental results showed that the lithium leaching rate reached 91.1% and the lithium product purity reached 99.6%.
[0166] Example 11 This embodiment provides a lithium extraction method, which differs from Embodiment 4 in that: In step (2), the relative humidity of the water vapor is 11%.
[0167] Experimental results showed that the lithium leaching rate reached 98.6% and the lithium product purity reached 99.3%.
[0168] Example 12 This embodiment provides a lithium extraction method, which differs from Embodiment 4 in that: In step (2), the relative humidity of the water vapor is 33%.
[0169] Experimental results showed that the lithium leaching rate reached 91.8% and the lithium product purity reached 98.6%.
[0170] Comparative Example 1 This comparative example provides a lithium extraction method, including: (1) Raw material characteristics: Lithium montmorillonite clay ore from a certain place in Jiangxi Province (same as in Example 1).
[0171] (2) Pretreatment: The lithium clay is ground to ensure that the mass percentage of clay-type lithium ore powder with a particle size ≤0.074mm is ≥65%.
[0172] (3) Calcination: Clay lithium ore powder, sodium sulfate, concentrated sulfuric acid and water are mixed and calcined to obtain calcined clinker and calcination flue gas respectively; the mass ratio of clay lithium ore powder: sodium sulfate: sulfuric acid is 1:0.25:0.6; the calcination temperature is 500℃.
[0173] (4) Leaching: The leaching raw material is added to the reaction tank. The calcined material and the water used for leaching are leached in water at a mass ratio of 1:3 to obtain lithium leaching solution.
[0174] Because the lithium leaching solution prepared in Comparative Example 1 was highly acidic, sodium carbonate was added to the resulting lithium chloride solution. The amount added was twice the amount needed to completely convert lithium ions into lithium carbonate, and the pH was 9. A lithium precipitation reaction was then carried out for 4 hours at a temperature of 90°C and a stirring speed of 400 r / min. After the reaction was completed, the solution was filtered to obtain a solid, which was lithium salt (unpurified lithium carbonate). This solid was washed four times with hot water and dried to obtain the lithium carbonate product. The hot water temperature was 80°C, and the liquid-to-solid ratio during washing was 4:1.
[0175] Experimental results showed that the lithium leaching rate reached 90.1% and the lithium product purity reached 17%.
[0176] Comparative Example 2 This comparative example provides a lithium extraction method, including: (1) Raw material characteristics: Low-grade spodumene concentrate from the Sichuan Jiajika mining area was selected, with a lithium content of 0.4wt% and a large amount of magnesium, iron and aluminum silicates as associated with it. The Mg / Li mass ratio is about 12:1.
[0177] (2) Pretreatment: Water is added to slag of spodumene smelting and stirred to make a slurry with a solid-liquid ratio of 1:1. The slurry is classified by hydrocyclone. The coarse slurry with a particle size of 45μm or larger is fed into a ball mill for grinding. Ceramic media is used for grinding. The fineness is 92% -45μm. The finely ground slurry is combined with the fine slurry with a particle size of less than 45μm from the hydrocyclone classification as leaching raw material.
[0178] (3) Leaching: The leaching raw material is added to a conventional stirred reactor or reaction tank, and concentrated acid is added to adjust the pH to 1.0. The mixture is heated to 80°C and stirred for 2 hours. After leaching, a centrifuge is used to separate the solid and liquid components to obtain leaching residue and lithium-poor leaching solution A. The leaching residue is washed to obtain lithium-poor leaching solution B. Lithium-poor leaching solution A and lithium-poor leaching solution B are combined and returned to the stirred pulping process for cyclic leaching. The lithium-rich solution obtained after cyclic leaching twice is returned to the lithium precipitation section of the lithium carbonate plant to continue the production of lithium carbonate products.
[0179] The lithium leaching rate and lithium product purity were determined according to the method in Example 1.
[0180] Test results: The lithium leaching rate reached 66.7%, and the lithium product purity was 59%.
[0181] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for lithium extraction, characterized in that, include: Solvent vapor is transported to a high-gravity reactor and brought into contact with the solid powder to be purified, so that the solid powder absorbs the solvent vapor and deliquesces to form a lithium chloride solution. Simultaneously, the supergravity reactor performs solid-liquid separation between the lithium chloride solution and the non-hygroscopic solid powder, and collects the lithium chloride solution; wherein, the solvent vapor includes at least one of water vapor and polar small molecule solvent vapor, and the solid powder to be purified contains lithium ions and chloride ions.
2. The lithium extraction method according to claim 1, characterized in that, The solvent vapor includes water vapor, and the relative humidity of the water vapor is 11% ≤ RH ≤ 33%.
3. The lithium extraction method according to claim 1, characterized in that, The number of carbon atoms in the polar small molecule solvent vapor does not exceed 4; and / or, the polarity index P' of the polar small molecule solvent vapor satisfies: 3.5≤P'≤5.
5.
4. The lithium extraction method according to claim 3, characterized in that, The polar small molecule solvent includes at least one of methanol, ethanol, and isopropanol; Alternatively, the polar small molecule solvent includes a first solvent and a second solvent, the first solvent including acetone, and the second solvent including at least one of methanol, ethanol and isopropanol; the volume ratio of the first solvent vapor to the second solvent vapor in the solvent vapor is (3:1) to (1:3).
5. The lithium extraction method according to claim 3, characterized in that, The solvent vapor includes the polar small molecule solvent vapor, and the relative humidity of the polar small molecule solvent vapor is 0% < RH ≤ 100%.
6. The lithium extraction method according to claim 3, characterized in that, The solvent vapor includes water vapor and polar small molecule solvent vapor; the volume ratio of water vapor to polar small molecule solvent vapor in the solvent vapor is (8:1) to (1:9).
7. The lithium extraction method according to any one of claims 1 to 6, characterized in that, In the solid powder to be purified, the molar ratio of lithium ions to chloride ions is 1:(1.2~2).
8. The lithium extraction method according to any one of claims 1 to 6, characterized in that, The solvent vapor also includes a carrier gas, which includes at least one of nitrogen, argon, helium, neon, krypton, xenon, and air.
9. The lithium extraction method according to claim 8, characterized in that, The solvent vapor includes the polar small molecule solvent vapor, and the carrier gas includes at least one of nitrogen, argon, helium, neon, krypton, and xenon.
10. The lithium extraction method according to any one of claims 1 to 6, characterized in that, The solid powder to be purified includes at least one of lithium clay ore, spodumene ore, salt lake brine crystallization powder, dried powder of waste battery acid leaching solution, and acid leaching residue from lithium extraction lines.
11. The lithium extraction method according to claim 1, characterized in that, The particle size of the solid powder to be purified does not exceed 100 μm; And / or, the solid powder to be purified includes an ion-intercalated layered compound, and the particle size of the solid powder to be purified is 1 μm to 50 μm.
12. The lithium extraction method according to claim 1, characterized in that, The volume ratio of the solid powder to the solvent vapor is 1:(5~10).
13. The lithium extraction method according to claim 1 or 12, characterized in that, The lithium content in the solid powder to be purified is less than 0.1 wt%, and the residence time of the solid powder to be purified in the supergravity reactor is not less than 4 hours. Alternatively, the lithium content in the solid powder to be purified is 0.1wt%~0.5wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 1 hour; Alternatively, the lithium content in the solid powder to be purified is greater than 0.5 wt%, and the residence time of the solid powder to be purified in the hypergravity reactor is not less than 30 min.
14. The lithium extraction method according to claim 12, characterized in that, The centrifugal force of the hypergravity reactor is not less than 10G; And / or, the solvent vapor is delivered to the hypergravity reactor to maintain the pressure of the hypergravity reactor at 0.5 MPa to 0.55 MPa.