Selective Recovery Method of Vanadium-Tungsten Active Metals from Waste Catalysts

By combining microscopic manipulation with a robotic arm and a synchronous oxidation-reduction pulsed electric field with a targeted coordination extractant, the problem of uncontrollable concentration caused by the simultaneous dissolution of vanadium and tungsten was solved, achieving efficient and selective recovery and purity improvement of vanadium and tungsten active metals.

CN123108324APending Publication Date: 2026-11-17WUYI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611033755.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing wet recovery processes, the simultaneous leaching of vanadium and tungsten leads to uncontrollable ion concentration ratios, insufficient coordination selectivity of vanadium and tungsten, and a lack of differentiated control capabilities at the single particle scale during the leaching process. This results in cross-contamination of tungsten with the vanadium back-extraction solution and low vanadium and tungsten recovery rates.

Method used

A single-particle pendant sample is generated using a robotic arm micro-manipulation platform. A synchronous oxidation-reduction pulsed electric field is applied, combined with a targeted coordination extractant, to achieve selective recovery of vanadium and tungsten. The specific steps include single-particle positioning and gripping, pendant clamping, electrochemical leaching, targeted coordination extraction, and ion exchange adsorption, constructing a precise micro-reaction environment to control the dissolution behavior of vanadium and tungsten.

Benefits of technology

This method achieves efficient and selective recovery of vanadium-tungsten active metals, ensuring a stable vanadium-tungsten dissolution ratio, reducing cross-contamination, and improving the recovery rate and purity of vanadium-tungsten.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108324A_ABST
    Figure CN123108324A_ABST
Patent Text Reader

Abstract

This invention provides a method for the selective recovery of vanadium and tungsten active metals from spent catalysts, belonging to the field of spent catalyst resource recovery technology. The method includes: performing single-particle positioning, grasping, and droplet clamping operations on spent catalyst particles using a robotic arm micro-manipulation platform to generate single-particle droplet samples; applying a synchronous oxidation-reduction pulsed electric field to the single-particle droplet samples to generate a mixed leachate containing vanadium ions and tungstate ions; injecting a targeted coordination extractant into the mixed leachate, whereby the targeted coordination extractant selectively complexes vanadium ions to generate a vanadium-loaded extract phase and a raffinate containing tungstate ions; performing a back-extraction operation on the vanadium-loaded extract phase to generate a vanadium-containing back-extraction solution, and performing an ion exchange adsorption operation on the raffinate to generate a tungsten-containing eluent. This method achieves highly selective recovery of vanadium and tungsten from spent catalysts through precise micro-scale manipulation and electrochemical-extraction synergistic separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of waste catalyst resource recovery technology, and in particular to a method for selectively recovering vanadium-tungsten active metals from waste catalysts. Background Technology

[0002] The recovery of vanadium-tungsten active metals from spent catalysts mainly employs hydrometallurgical processes. Vanadium and tungsten are dissolved together through acid or alkaline leaching, followed by separation and purification of the mixed solution. Acid leaching uses sulfuric acid or hydrochloric acid to convert vanadium pentoxide and tungsten trioxide into soluble salts, obtaining a mixed leachate containing vanadium and tungsten. Alkaline leaching utilizes sodium hydroxide or sodium carbonate solution, allowing vanadium and tungsten to enter the liquid phase together as sodium vanadate and sodium tungstate. After obtaining the mixed leachate, vanadium and tungsten are separated using solvent extraction or ion exchange. Solvent extraction commonly uses amine extractants, adjusting the solution pH to preferentially allow vanadium to enter the organic phase, while tungsten remains in the aqueous phase. Ion exchange utilizes the difference in affinity of resins for different ions to achieve gradient desorption.

[0003] Existing acid or alkaline leaching techniques for treating spent catalyst particles lack spatial selectivity, resulting in the simultaneous dissolution of vanadium and tungsten from the particle surface. This leads to the coexistence of the two metal ions in the leachate with uncontrollable concentration ratios. When adjusting pH for extraction and separation, the hydrolytic characteristics of vanadium and tungsten are similar, easily leading to co-extraction or co-precipitation. Under low pH conditions, the coordination selectivity of the extractant for vanadium is insufficient to completely exclude the interference of tungstate ions, and some tungsten is entrained into the organic phase as a heteropolyacid, affecting the purity of vanadium in the back-extraction solution. When treating tungsten-containing leaching residue with ion exchange, residual vanadium ions compete for resin active sites, reducing the adsorption capacity and recovery rate of tungsten. Furthermore, conventional stirred leaching methods struggle to precisely control the mechanical forces acting on the particles, making it impossible to implement differentiated electric field-driven leaching strategies at the single-particle scale. This lack of synchronized regulation of the redox dissolution processes of vanadium and tungsten limits the possibility of controlling the metal ion ratio from the dissolution source. Summary of the Invention

[0004] The purpose of this invention is to provide a method for selectively recovering vanadium-tungsten active metals from waste catalysts, which solves the problems of uncontrollable ion concentration ratio and insufficient coordination selectivity of vanadium-tungsten caused by the simultaneous dissolution of vanadium and tungsten in existing wet recovery processes, avoids cross-contamination of vanadium back-extraction solution by tungsten, and improves the ability to differentiate and control the dissolution behavior of vanadium and tungsten at the single particle scale.

[0005] To achieve the above objectives, the present invention provides the following technical solution: The present invention provides a method for selectively recovering vanadium-tungsten active metals from waste catalysts, which achieves efficient and selective recovery of vanadium-tungsten active metals through the synergistic effect of single-particle microscale manipulation, precise electrochemical leaching, targeted coordination separation, and selective enrichment.

[0006] In this invention, a robotic arm micro-manipulation platform performs single-particle positioning, grasping, and droplet clamping operations on waste catalyst particles to generate single-particle droplet samples. As a preferred embodiment, a vision-guided system identifies the particle size distribution and surface morphology features of the waste catalyst particles, generating particle identification coordinate data. The piezoelectrically driven micro-grippers in the robotic arm micro-manipulation platform are driven to move along the particle identification coordinate data to a first grasping position, grasping the target particle with a first clamping force. This first clamping force is dynamically adjusted according to the particle size data of the target particle through a force feedback control loop, thereby avoiding damage to the particle's microstructure due to excessive clamping force or particle slippage due to insufficient clamping force. The grasped target particle is then immersed in a micro-droplet generation chamber containing deionized water. The piezoelectrically driven micro-grippers are controlled to squeeze the target particle with a second clamping force greater than the first clamping force, causing the micro-droplets adhering to the particle surface to detach and encapsulate the target particle, generating a single-particle droplet sample. The method of generating this pendant drop sample enables the construction of a precisely defined microreaction environment at the single-particle scale, providing a foundation for subsequent highly selective and highly uniform electrochemical leaching.

[0007] In this invention, a synchronous oxidation-reduction pulsed electric field is applied to the single-particle suspended drop sample to generate a mixed leachate containing vanadium ions and tungstate ions. As a preferred embodiment of this invention, the single-particle suspended drop sample is transferred to an electrochemical leaching microreactor chamber, which integrates a first electrode array at the bottom and a second electrode array at the top. An anodic oxidation pulsed voltage waveform is applied to the first electrode array, the amplitude of which is determined based on the vanadium pentoxide content transition parameters in the single-particle suspended drop sample. This waveform is used to generate localized oxidation micro-regions at the interface between the suspended drop sample and the first electrode array, converting vanadium pentoxide into soluble vanadium oxide cations. Simultaneously, a cathodic reduction pulsed voltage waveform is applied to the second electrode array, the duty cycle of which is set based on the tungsten trioxide content distribution data in the single-particle suspended drop sample. This pulsed voltage waveform is used to generate localized reduction micro-regions at the interface between the suspended drop sample and the second electrode array, reducing tungsten trioxide to soluble tungstate ions. By simultaneously applying pulsed electric fields of two polarities, the synergistic oxidative leaching of vanadium and the reductive leaching of tungsten can be achieved within the same pendant drop micro-region system, maintaining a stable concentration ratio of vanadium ions to tungstate ions in the mixed leaching solution. Preferably, the first and second electrode arrays are platinum electrodes or glassy carbon electrodes, and their surfaces are coated with a nanoporous titanium dioxide film to enhance the charge transfer efficiency at the contact interface, significantly improving the leaching reaction rate and reducing energy consumption.

[0008] In this invention, a targeted coordination extractant is injected into the mixed leachate. This targeted coordination extractant selectively complexes vanadium ions to generate a vanadium-loaded extract phase and a raffinate containing tungstate ions. As a preferred embodiment of this invention, the mixed leachate is introduced into the first inlet channel of a microfluidic extraction chip, and the targeted coordination extractant is introduced into the second inlet channel. This targeted coordination extractant is a compound solution of trioctylamine and N1923 extractant, with a volume ratio of trioctylamine to N1923 extractant of 3:1 to 5:1. The pH of the mixed leachate is adjusted to a first preset pH range, preferably 2.0 to 2.8, so that vanadium ions are released as VO2+. + The form exists and enhances the coordination selectivity of the targeted coordination extractant for vanadium ions. Before adjusting the pH, as a further preferred method, a portion of the mixed leachate is introduced into an online pH monitoring sensor to obtain real-time pH data. Based on the deviation between this real-time data and a first preset pH range, dilute hydrochloric acid or dilute sodium hydroxide solution is injected into the mixed leachate via a micro-injection pump as a pH adjuster. Once the real-time pH data stabilizes within the preset range, the extractant injection operation is then performed, thereby ensuring that the extraction process is always under optimal acidity conditions. The microchannel structure within the microfluidic extraction chip mixes the mixed leachate and the targeted coordination extractant to form a laminar flow interface. At this interface, trioctylamine and N1923 extractant form a cationic extraction group through a protonation reaction. This cationic extraction group reacts with VO2... + An ion association reaction occurs, generating an extract phase loaded with vanadium; while the raffinate containing tungstate ions is retained in the aqueous phase due to electrostatic repulsion, thus achieving highly selective separation of vanadium and tungsten in one step.

[0009] In this invention, the vanadium-loaded extractant phase is back-extracted to generate a vanadium-containing back-extracting solution. In a preferred embodiment, the vanadium-loaded extractant phase is transferred to a back-extraction microreactor, preferably a microreactor with a helical channel having a semi-circular cross-section. A sodium carbonate back-extraction solution with a concentration of 0.5 mol / L to 1.2 mol / L is injected into the back-extraction microreactor, and the temperature inside the reactor is controlled to a first preset temperature range, preferably 40°C to 60°C. Within this temperature range, the N1923 extractant in the targeted coordination extractant undergoes a deprotonation reaction, releasing vanadium ions into the sodium carbonate back-extraction solution, generating a vanadium-containing back-extraction solution. The targeted coordination extractant is then regenerated to its initial state and can be recycled. The sodium carbonate back-extraction solution and the vanadium-loaded extractant phase flow in parallel within the helical channel. The length of the helical channel is determined based on the mass transfer time of vanadium ions diffusing from the extractant phase to the back-extraction solution phase. This structural design enhances the contact mixing and mass transfer between the two phases, achieving efficient back-extraction of vanadium ions and regeneration of the extractant within a very short channel length.

[0010] Simultaneously, the raffinate is subjected to ion exchange adsorption to generate a tungsten-containing eluent. In a preferred embodiment, the raffinate is passed through an ion exchange adsorption column at a first flow rate. The column is packed with a quaternary ammonium salt-type anion exchange resin, which selectively adsorbs tungstate ions from the raffinate to generate a tungsten-loaded resin phase. The effluent is a purified solution in which vanadium impurities have been substantially removed. An ammonia eluent with a concentration of 3 mol / L to 6 mol / L is injected into the tungsten-loaded resin phase. Upon contact with the tungsten-loaded resin phase, the ammonia eluent desorbs tungstate ions, generating a high-purity tungsten-containing eluent.

[0011] Furthermore, the present invention also includes subsequent productization steps. The generated vanadium-containing back-extraction solution is treated and introduced into a first crystallization vessel. Ammonium chloride precipitant is added; the amount of ammonium chloride added is determined by stoichiometry based on the vanadium ion concentration in the vanadium-containing back-extraction solution, generating ammonium metavanadate precipitate. The generated tungsten-containing eluent is treated and introduced into a second crystallization vessel. Evaporation and crystallization parameters are controlled, specifically including evaporation temperature and evaporation rate. The evaporation temperature is maintained by a heating power adjustment loop based on dynamic monitoring data of the tungsten-containing eluent volume, causing tungsten in the tungsten-containing eluent to crystallize and precipitate as ammonium paratungstate, ultimately obtaining high-value-added vanadium and tungsten end products.

[0012] The technical effects and advantages provided by the present invention in the above technical solution are as follows: A robotic arm micro-manipulation platform performs single-particle positioning, grasping, and droplet clamping operations to generate single-particle suspended droplet samples, confining the leaching reaction of waste catalyst to a micro-droplet adhering to the surface of a single particle. A piezoelectrically driven micro-gripper grasps the target particle with a first clamping force dynamically adjusted by a force feedback control loop, and then applies a larger second clamping force to compress the particle, causing deionized water to encapsulate it and form a droplet. This operation transforms the dissolution space of vanadium and tungsten from a traditional batch reactor to a micro-region of liquid film on the surface of a single particle, ensuring that the leaching reaction occurs only at the contact interface between the target particle and the micro-droplet. This spatially eliminates the ion concentration fluctuations caused by uneven vanadium and tungsten dissolution rates when multiple particles coexist. The single-particle suspended droplet sample, as an independent reaction unit, has a fixed vanadium and tungsten oxide content. When an electric field is subsequently applied, waveform parameters can be set according to the particle's compositional characteristics, thus establishing a feedforward adjustment basis for the concentration ratio of vanadium ions to tungstate ions at the dissolution source.

[0013] By applying a synchronous oxidation-reduction pulsed electric field to a single-particle suspended drop sample, localized oxidation and reduction microregions are simultaneously generated within the electrochemical leaching microreactor. The amplitude of the anodic oxidation pulsed voltage waveform is determined based on the vanadium pentoxide content transition parameters, converting vanadium pentoxide into soluble vanadium-oxygen cations at the contact interface. The duty cycle of the cathodic reduction pulsed voltage waveform is set based on tungsten trioxide content distribution data, reducing tungsten trioxide to tungstate ions at the contact interface. The synchronous application of pulsed electric fields at both the anode and cathode allows the oxidation and dissolution of vanadium and the reduction and dissolution of tungsten to occur in parallel over time. Unlike alternating or stepwise leaching methods, the synchronous electric field drives the generation of both metal ions within a single suspended drop sample. The vanadium and tungstate ions in the mixed leachate achieve a predetermined concentration ratio from the initial generation stage, providing a feed solution with a defined ion ratio for subsequent extraction and separation, thus reducing the degradation of extraction selectivity caused by concentration mismatch from the source. Attached Figure Description

[0014] Figure 1 This is a flowchart of a method for selectively recovering vanadium-tungsten active metals from spent catalysts; Figure 2 This is a flowchart of synchronous pulse voltage electrochemical leaching based on the component content parameters of a single-particle hanging drop sample; Figure 3 This is a schematic diagram of the vanadium back-extraction microfluidic system. Detailed Implementation

[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0016] It should be noted that although functional modules are divided in the device schematic diagram and a logical order is shown in the flowchart, in some cases, the steps shown or described may be performed in a different order than the module division in the device or the order in the flowchart. The terms "first," "second," etc., in the specification, claims, and the following drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.

[0017] In this embodiment of the invention, the terms "furthermore," "exemplarily," or "optionally" are used as examples, illustrations, or descriptions and should not be construed as being more preferred or advantageous than other embodiments or designs. The use of the terms "furthermore," "exemplarily," or "optionally" is intended to present the relevant concepts in a specific manner.

[0018] See Figure 1This invention provides a method for selectively recovering vanadium-tungsten active metals from spent catalysts, comprising the following steps: performing single-particle positioning, grasping, and droplet clamping operations on spent catalyst particles using a robotic arm micro-manipulation platform to generate single-particle droplet samples; and applying simultaneous oxidation to the single-particle droplet samples. A pulsed electric field is reduced to generate a mixed leachate containing vanadium ions and tungstate ions. A targeted coordination extractant is injected into the mixed leachate, which selectively complexes the vanadium ions to generate a vanadium-loaded extract phase and a raffinate containing tungstate ions. The vanadium-loaded extract phase is back-extracted to generate a vanadium-containing back-extractant, and the raffinate is subjected to ion exchange adsorption to generate a tungsten-containing eluent.

[0019] Example 1: In its implementation, the vision-guided system first performs a global optical scan of the spent catalyst particles mounted on the stage to acquire backscattered light intensity distribution data and surface height undulation data. The system's built-in multi-core heterogeneous processor receives the backscattered light intensity distribution data and calls the particle contour extraction model to generate a single-particle contour binary image of the spent catalyst particles. The particle contour extraction model consists of a cascaded first convolutional processing layer, a second convolutional processing layer, a hollow space pyramid pooling layer, and an edge sharpening output layer. The first convolutional processing layer uses a 3×3 depth-separable convolutional kernel, the second convolutional processing layer uses a 5×5 depth-separable convolutional kernel, the hollow space pyramid pooling layer has three parallel branches with expansion rates of 1, 3, and 5, respectively, and the edge sharpening output layer uses the Laplacian operator to enhance the boundaries of the multi-scale fusion features before outputting the single-particle contour binary image. Each closed connected region in the single-particle contour binary image of the spent catalyst particles corresponds to the two-dimensional projection of at least one spent catalyst particle. The vision-guided system calculates the Freret diameter distribution for each closed connected region to obtain the particle size distribution of the spent catalyst particles. The visual guidance system performs Gaussian regression on the surface height undulation data to construct a continuous height field characterizing the surface geometry of the spent catalyst particles. It also calculates the average Gaussian curvature and average mean curvature of the continuous height field to generate the surface morphology features of the spent catalyst particles.

[0020] After obtaining the particle size distribution and surface morphology features, the vision-guided system sorts the Ferrette diameter distribution in ascending order and performs radial and tangential distortion correction on the centroid coordinates of each closed connected domain, generating particle identification coordinate data with the piezoelectrically driven micro-gripper end coordinate system as the reference frame. The particle identification coordinate data includes the axial coordinates of the s-th waste catalyst particle in the piezoelectrically driven micro-gripper end coordinate system. radial coordinates and height coordinates The vision guidance system encapsulates particle recognition coordinate data into real-time data packets, which are then pushed to the multi-axis motion control card of the robotic arm's micro-manipulation platform via a high-speed serial peripheral interface bus using hardware interrupts.

[0021] The multi-axis motion control card in the robotic arm's micro-manipulation platform parses real-time data packets and extracts axial coordinates. radial coordinates and height coordinates The multi-axis motion control card runs an interpolation algorithm based on trapezoidal velocity profiles, synchronously generating pulse width modulation (PWM) signal sequences in the axial, radial, and height directions. These three PWM signal sequences sequentially drive the axial, radial, and height piezoelectric linear motors, causing the piezoelectrically driven micro-gripper tip to move from its initial homing position along a linear trajectory to the first gripping position. At the first gripping position, the vertical distance between the piezoelectrically driven micro-gripper tip and the highest point on the surface of the spent catalyst particle is determined by the height coordinates. The offset is determined together with the preset offset at the end of the piezoelectric-driven micro gripper.

[0022] After the piezoelectrically driven micro-gripper reaches the first gripping position, the multi-axis motion control card activates the force feedback control loop. The force feedback control loop consists of a semiconductor strain gauge, signal conditioning circuitry, and proportional control circuitry attached to the base of the piezoelectrically driven micro-gripper's fingertips. integral The differential controller consists of a semiconductor strain gauge that measures the bending strain generated by the fingertip during the grasping motion, and a signal conditioning circuit that converts the bending strain into a voltage feedback signal. integral The differential controller generates a pulse width modulation duty cycle adjustment based on the deviation between the voltage feedback signal and the force setpoint. The first clamping force setpoint of the force feedback control loop is determined based on the particle size data of the waste catalyst particles. The force feedback control loop dynamically adjusts the pulse width modulation duty cycle corresponding to the semiconductor strain gauge to stabilize the clamping force applied to the target particles by the piezoelectric driven micro-gripper at the first clamping force setpoint.

[0023] The first clamping force setting value is obtained by: the multi-axis motion control card reading the Freret diameter value corresponding to the target particle in the Freret diameter distribution of the waste catalyst particles, and substituting it into the clamping force calculation model.

[0024] in, This is the initial clamping force setting, in micronewtons. The value represents the Freette diameter of the target particle, in micrometers. For particle material correlation constants, This represents the particle size dependence index. The particle material correlation constant. The value is 0.38, which is the particle size dependence index. The value is 1.72, which is the particle material correlation constant. and particle size dependence index The value is based on the force obtained from uniaxial compression experiments on spent catalyst particles. The displacement curve was determined by nonlinear least squares fitting. When taking the measured Freret diameter value, The calculated value is the first clamping force setting value. The piezoelectrically driven micro-gripper grasps the target particle with the first clamping force and maintains the grasping state.

[0025] After grasping, the multi-axis motion control card drives the piezoelectric micro-gripper to move the target particle out of the waste catalyst particle group along a preset lifting trajectory. Subsequently, the multi-axis motion control card drives the piezoelectric micro-gripper to translate in three-dimensional space to directly above the microdroplet generation chamber, and controls the piezoelectric micro-gripper to descend vertically, completely immersing the target particle in the deionized water contained within the microdroplet generation chamber. The deionized water in the microdroplet generation chamber has a volume of 800 microliters and a resistivity of 18.2 megohm-cm.

[0026] After the target particles are immersed in deionized water, the force feedback control circuit of the piezoelectrically driven micro-gripper switches the clamping force setting from a first clamping force setting to a second clamping force setting. The second clamping force setting is 1.6 times the first clamping force setting. In specific implementation, if the first clamping force setting is... Then the second clamping force setting value .Proportion integral The differential controller adjusts the pulse width modulation duty cycle, gradually increasing the pressure applied to the target particle by the piezoelectric-driven micro-gripper to the second clamping force setting value. During this pressure increase, the deionized water film adhering to the target particle surface due to immersion migrates outwards under pressure and converges around the particle to form a closed liquid film. When the pressure reaches the second clamping force setting value, the microdroplets adhering to the target particle surface completely detach from the original surface and re-encapsulate the entire particle, generating a single-particle suspended drop sample consisting of the target particle and the deionized water film surrounding it. The vision-guided system performs lateral imaging of the single-particle suspended drop sample and calculates the average thickness of the deionized water film. When the average thickness of the deionized water film is within the range of 15 to 25 micrometers, the single-particle suspended drop sample is considered to have been successfully generated. The robotic arm micro-manipulation platform transfers the single-particle suspended drop sample to the temporary storage area of ​​the microdroplet generation chamber, awaiting further processing.

[0027] Example 2: In specific implementation, please refer to Figure 2The transfer of single-particle suspended droplet samples from the temporary storage area of ​​the microdroplet generation chamber to the electrochemical leaching microreactor chamber is performed by a robotic arm micro-manipulation platform. A piezoelectrically driven micro-gripper maintains the gripping state of the deionized aqueous film on the outer layer of the single-particle suspended droplet sample. A multi-axis motion control card loads a preset transfer trajectory, driving the piezoelectrically driven micro-gripper to deliver the single-particle suspended droplet sample into the inlet of the electrochemical leaching microreactor chamber along a linear path. The electrochemical leaching microreactor chamber is a cuboid cavity. The inner surface of the bottom plate of the cavity is integrated with a first electrode array via magnetron sputtering, and the inner surface of the top plate is integrated with a second electrode array via magnetron sputtering. The first electrode array consists of 48 disk-shaped platinum electrode units, each 100 micrometers in diameter, arranged in 6 rows × 8 columns with equal spacing. The center-to-center distance between adjacent disk-shaped platinum electrode units is 400 micrometers. The second electrode array consists of 48 disk-shaped platinum electrode units, each 100 micrometers in diameter, arranged in 6 rows × 8 columns at equal intervals. Each disk-shaped platinum electrode unit in the second electrode array is directly opposite the corresponding disk-shaped platinum electrode unit in the first electrode array. Both the surfaces of the first and second electrode arrays are coated with a nanoporous titanium dioxide film. The nanoporous titanium dioxide film is coated by growing a 1.2-micrometer-thick titanium dioxide nanotube array layer on the surface of the platinum electrode units using anodizing. The titanium dioxide nanotube array layer is then annealed at 450 degrees Celsius in air for 2 hours, transforming it into anatase-phase nanoporous titanium dioxide film. The pore size distribution of the nanoporous titanium dioxide film ranges from 20 nanometers to 40 nanometers, and the porosity of the nanoporous titanium dioxide film is 58%.

[0028] After a single-particle suspended droplet sample enters the electrochemical leaching microreactor, it settles under the combined influence of gravity and the surface tension of the deionized water film. The lower surface of the deionized water film of the single-particle suspended droplet sample forms a first contact interface with the surface of the nanoporous titanium dioxide film of the multiple disk-shaped platinum electrode units in the first electrode array. A micro-displacement lifting mechanism at the top of the electrochemical leaching microreactor drives the second electrode array to descend vertically until the surface of the nanoporous titanium dioxide film of the multiple disk-shaped platinum electrode units in the second electrode array forms a second contact interface with the upper surface of the deionized water film of the single-particle suspended droplet sample. The displacement resolution of the micro-displacement lifting mechanism is 50 nanometers.

[0029] After the first and second contact interfaces are formed, the multi-channel electrochemical workstation starts the synchronous pulse voltage output mode. The first output channel of the multi-channel electrochemical workstation is electrically connected to 16 disk-shaped platinum electrode units in the first electrode array that are within the projection coverage area of ​​the single-particle suspended drop sample, and the second output channel is electrically connected to 16 disk-shaped platinum electrode units in the second electrode array that are within the projection coverage area of ​​the single-particle suspended drop sample.

[0030] Before applying the anodic oxidation pulse voltage waveform to the first electrode array, the content transition parameters of vanadium pentoxide in the single-particle suspended drop sample are obtained. The content transition parameters are obtained as follows: in-situ laser-induced breakdown spectroscopy analysis is performed on the single-particle suspended drop sample. The characteristic emission line intensity of vanadium at a wavelength of 440.85 nm is collected. Using the characteristic emission line intensity against the blank background of the deionized water film as a reference baseline, the relative difference ratio between the characteristic emission line intensity of vanadium and the characteristic emission line intensity of the reference baseline is calculated. This relative difference ratio is then compared and interpolated with a preset vanadium pentoxide content calibration curve to obtain the mass fraction of vanadium pentoxide in the dry basis of the single-particle suspended drop sample. Multiplying this mass fraction by the dry basis mass of the single-particle suspended drop sample yields the content transition parameters. The content transition parameters characterize the absolute mass of vanadium pentoxide in the single-particle suspended drop sample.

[0031] The amplitude of the anodizing pulse voltage waveform is determined based on the content transition parameters. The calculation method for the amplitude of the anodizing pulse voltage waveform is as follows:

[0032] in, This represents the amplitude of the anodizing pulse voltage waveform, in volts. This is the content transition parameter, in nanograms. The base oxidation voltage is set to 1.2 volts. Oxidation voltage The mass proportion factor is set at 0.45 volts per nanogram. The basic oxidation voltage... The value of 1.2 volts corresponds to the standard electrode potential for the oxidation-dissolution reaction of vanadium pentoxide in a buffer solution with a pH of 2.5, and is the oxidation voltage. mass ratio coefficient The value of 0.45 volts per nanogram was obtained by performing linear regression on the relationship between peak potential shift and loading after linear scanning voltammetry on single-particle pendant drop samples with different vanadium pentoxide loadings. The multi-channel electrochemical workstation will then use the content transition parameter... Substituting the values ​​into the formula for calculating the amplitude of the anodizing pulse voltage waveform, we obtain the amplitude of the anodizing pulse voltage waveform. The frequency of the anodizing pulse voltage waveform is 100 Hz, and the duty cycle of the anodizing pulse voltage waveform is 35%.

[0033] A multi-channel electrochemical workstation applies anodizing pulse voltage waveform to 16 disk-shaped platinum electrode units within the projection coverage area of ​​the single-particle suspended drop sample in the first electrode array via the first output channel. During the high-level period of the anodizing pulse voltage waveform, strongly oxidizing hydroxyl radicals are generated on the surface of the nanoporous titanium dioxide film at the first contact interface, forming localized oxidation microregions. These localized oxidation microregions act on the vanadium pentoxide crystal phase in the single-particle suspended drop sample. The vanadium-oxygen bonds in the vanadium pentoxide lattice break under the attack of hydroxyl radicals, and vanadium pentoxide is converted into soluble vanadium-oxygen cations. The soluble vanadium-oxygen cations are converted into VO2+. + The vanadium pentoxide crystals on the surface of the single-particle suspended drop sample dissolve and enter the deionized aqueous film, forming a diffusion layer containing vanadium oxygen cations in the deionized aqueous film.

[0034] Synchronously with the application of the anodic oxidation pulse voltage waveform, the second output channel of the multi-channel electrochemical workstation applies the cathodic reduction pulse voltage waveform to the second electrode array. The duty cycle of the cathodic reduction pulse voltage waveform is set based on the tungsten trioxide content distribution data in the single-particle suspended drop sample. The tungsten trioxide content distribution data is obtained as follows: 30 particles are randomly selected from the same batch of spent catalyst particles as the single-particle suspended drop sample. Microscopic X-ray fluorescence spectroscopy is performed on each of the 30 particles to construct a spatial distribution map of the tungsten trioxide mass fraction within each particle. The statistical average of the spatial distribution maps of the tungsten trioxide mass fraction of the 30 particles is calculated to obtain the tungsten trioxide content distribution data. The tungsten trioxide content distribution data is a two-dimensional matrix, where the first... Line 1 Column elements Represents coordinates in normalized space The average mass fraction of tungsten trioxide. The duty cycle of the cathode reduction pulse voltage waveform is set to... The median value of the matrix is ​​multiplied by 100. A multi-channel electrochemical workstation reads the median value of the two-dimensional matrix containing tungsten trioxide content distribution data. Multiplying the median value by 100 yields the duty cycle percentage of the cathodic reduction pulse voltage waveform. The amplitude of the cathodic reduction pulse voltage waveform is 2.8 volts, and its frequency is 100 Hz.

[0035] A multi-channel electrochemical workstation applies a cathode reduction pulse voltage waveform to 16 disk-shaped platinum electrode units within the projection coverage area of ​​the single-particle suspended drop sample in the second electrode array via a second output channel. During the high level of the cathode reduction pulse voltage waveform, electrons are injected into the surface of the nanoporous titanium dioxide film at the second contact interface, forming a localized reduction microregion. This localized reduction microregion acts on the tungsten trioxide crystal phase in the single-particle suspended drop sample, where hexavalent tungsten in the tungsten trioxide lattice gains electrons and is reduced, converting tungsten trioxide into soluble tungstate ions. The soluble tungstate ions are converted into WO4²⁻.- The form dissolves from the tungsten trioxide grains on the surface of the single-particle suspended drop sample and enters the deionized aqueous film, forming a diffusion layer containing tungstate ions in the deionized aqueous film.

[0036] A multi-channel electrochemical workstation synchronously applies anodic oxidation pulse voltage waveforms and cathodic reduction pulse voltage waveforms within the same clock cycle. Vanadium oxide cations dissolved from the first contact interface and tungstate ions dissolved from the second contact interface simultaneously exist in the deionized water membrane. The amplitude of the anodic oxidation pulse voltage... The duty cycles of the cathode reduction pulse voltage and the vanadium pentoxide tungsten trioxide tungsten oxide tungsten oxide tungsten oxide tungsten oxide tungstate ... + Concentration and WO4² - The concentration ratio ranges from 1.8:1 to 2.2:1.

[0037] Example 3: In practice, the outlet of the electrochemical leaching microreactor is connected to the common port of a three-way switching valve via a quartz capillary tube with an inner diameter of 100 micrometers. The first branch port of the three-way switching valve is connected to the inlet of the online pH monitoring sensor, and the second branch port is connected to the first inlet channel of the microfluidic extraction chip. The outlet of the online pH monitoring sensor is connected to a waste collection bottle via another quartz capillary tube. Initially, the common port of the three-way switching valve is connected to the first branch port, and the mixed leachate enters the flow cell of the online pH monitoring sensor at a flow rate of 10 microliters per minute under nitrogen back pressure.

[0038] The online pH monitoring sensor is an ion-sensitive field-effect transistor type pH microsensor. The sensitive area of ​​the online pH monitoring sensor is 0.5 square millimeters, and the response time is less than 3 seconds. The output of the online pH monitoring sensor is connected in sequence to an instrumentation amplifier and a 16-bit analog-to-digital converter (ADC). The ADC converts the amplified voltage signal into a digital signal. The embedded microcontroller reads the digital signal through a serial peripheral interface and calculates the real-time pH data of the mixed leachate. The embedded microcontroller internally stores the lower limit (2.0) and upper limit (2.8) of a first preset pH range, as well as the target pH value. The value is 2.4.

[0039] The embedded microcontroller compares real-time pH data with a first preset pH range. When the real-time pH data is less than 2.0 or greater than 2.8, the embedded microcontroller initiates the pH adjustment procedure. The embedded microcontroller then adjusts the pH based on the real-time pH data and the target pH value. The deviation is calculated based on the single injection volume of the pH adjuster, using the following method:

[0040] in, The volume of the pH adjuster injected at one time, in liters; The data is dimensionless and represents real-time pH data of the mixed leachate acquired by an online pH monitoring sensor. For the set target pH value, The value is 2.4; This refers to the total volume of the mixed leachate. The value is 1.2 × 10 -6 Lift; This refers to the buffer capacity parameter of the mixed leachate, expressed in moles per liter per pH. The value is 1.8 × 10 - ³ moles per liter per pH; This is the equivalent concentration of the pH adjuster, expressed in moles per liter. The value is 1.8 × 10 - The method for determining ³ moles per liter per pH is as follows: 10 samples are randomly taken from the mixed leachate generated from the same batch of spent catalyst particles, and the pH of each sample of the mixed leachate is determined. Acid-base titrations were performed within the range of 2.0 to 2.8. The change in pH of the mixed leachate was recorded for every 0.1 μmol of hydrogen or hydroxide ions added. The amount of hydrogen or hydroxide ions required to change the pH by 1 unit per unit volume of the mixed leachate was calculated. The arithmetic mean of the results from 10 samples was taken as the final value. The value of . When Greater than At that time, the embedded microcontroller specified the pH adjuster as a dilute hydrochloric acid solution, and the concentration of the dilute hydrochloric acid solution was... It is 0.1 moles per liter; when Less than At that time, the embedded microcontroller specified a dilute sodium hydroxide solution as the pH adjuster, and the concentration of the dilute sodium hydroxide solution was... It is 0.1 moles per liter.

[0041] The embedded microcontroller will calculate The value is converted into a pulse count, which drives the stepper motor of the micro-injection pump via a control circuit. The micro-injection pump has a syringe volume of 100 microliters and a single-step feed rate of 0.05 microliters. The micro-injection pump can deliver a volume of 100 microliters within 15 seconds. The pH adjuster is injected into the mixed leachate through the second branch port of the three-way switching valve at the junction with the mixed leachate pipeline. After the pH adjuster is injected, the mixed leachate flows through a serpentine mixing pipe containing a 0.5 mm diameter PTFE magnetic stir bar. Under the action of an external rotating magnetic field, the magnetic stir bar stirs at 300 rpm for 5 seconds to ensure that the pH adjuster and the mixed leachate are evenly mixed. The evenly mixed mixed leachate then re-enters the flow cell of the online pH monitoring sensor. The embedded microcontroller acquires new real-time pH data and repeats the pH comparison and pH adjuster injection operations until the real-time pH data stabilizes within the range of 2.0 to 2.8.

[0042] Once the real-time pH data stabilizes within the first preset pH range, the embedded microcontroller shuts down the nitrogen back pressure drive system and switches the common port of the three-way switching valve to be connected to the second branch port. The pH-adjusted mixed leachate is then introduced into the first inlet channel of the microfluidic extraction chip. The microfluidic extraction chip is fabricated by bonding a polydimethylsiloxane sheet to a borosilicate glass cover sheet via oxygen plasma. The chip's interior is etched with a first inlet channel, a second inlet channel, a Y-shaped converging microchannel, a spiral mixing microchannel, and a phase separation triangle. Both the first and second inlet channels have a cross-sectional width of 100 micrometers and a depth of 80 micrometers. The Y-shaped converging microchannel has an included angle of 60 degrees, and the spiral mixing microchannel consists of 12 turns of an Archimedean spiral, with a total length of 50 millimeters.

[0043] The targeted coordination extractant is a compound solution of trioctylamine and N1923 extractant, with a volume ratio of 4:1. The targeted coordination extractant is prepared as follows: 80 mL of trioctylamine and 20 mL of N1923 extractant are added to a separatory funnel, followed by 100 mL of sulfonated kerosene as a diluent. The mixture is shaken and mixed at a constant temperature of 25°C for 30 minutes. After standing and phase separation, the upper organic phase is collected as the targeted coordination extractant. The targeted coordination extractant is then filled into the syringe of a second micro-injection pump, which introduces the targeted coordination extractant into the second inlet channel of the microfluidic extraction chip at a flow rate of 10 μL / min, the same as the mixed leachate.

[0044] The mixed leachate and the targeted coordination extractant converge at the junction of the Y-shaped converging microchannel, forming a parallel laminar flow. Due to the Reynolds number being less than 1 within the microchannel, viscous forces dominate, resulting in a clear and stable laminar contact interface between the two phases. At the laminar contact interface, trioctylamine molecules in the targeted coordination extractant undergo a protonation reaction under acidic conditions, with the nitrogen atom of the trioctylamine molecule combining with hydrogen ions to form a trioctylammonium cation; the nitrogen atom of the N1923 extractant molecule combines with hydrogen ions to form an alkylammonium cation. The trioctylammonium cation and the alkylammonium cation together constitute the cationic extraction group. Vanadium ions in the mixed leachate mainly exist as VO2 in the pH range of 2.0 to 2.8. + It exists in form, VO2 + At the laminar interface, vanadium-containing extractable groups form electrically neutral ion-pair complexes through electrostatic attraction and ion association. These complexes then migrate across the interface from the aqueous phase to the organic phase, forming the vanadium-loaded extractable phase. The tungstate ions (WO4²) in the mixed leachate... - Because of its negative charge, the tungstate ions are electrostatically repelled by the cationic extraction groups, preventing them from undergoing ion association reactions. They remain on the aqueous side of the mixed leachate, forming a raffinate containing tungstate ions.

[0045] The vanadium-loaded extractant and the raffinate containing tungstate ions flow through a spiral mixing microchannel. Under the influence of centrifugal force and secondary flow, the contact area between the two phases is continuously renewed, and the extraction rate of vanadium ions gradually increases. A phase separation triangle is connected at the outlet of the spiral mixing microchannel. The inner wall of the upper branch of the phase separation triangle is locally modified with octadecyltrichlorosilane to make it hydrophobic, while the inner wall of the lower branch remains hydrophilic. The vanadium-loaded extractant enters the upper branch due to the hydrophobic effect and is collected in the vanadium-loaded extractant receiving bottle; the raffinate containing tungstate ions enters the lower branch due to the hydrophilic effect and is collected in the raffinate receiving bottle, thus completing the separation of the vanadium-loaded extractant and the raffinate containing tungstate ions.

[0046] Example 4: In specific implementation, please refer to Figure 3 The transfer of the vanadium-loaded extractant phase from the vanadium-loaded extractant phase receiving bottle of the microfluidic extraction chip to the back-extraction microreactor is achieved through a first high-precision syringe pump. The syringe of the first high-precision syringe pump is connected to the outlet of the vanadium-loaded extractant phase receiving bottle via a PTFE connecting tube. The first high-precision syringe pump draws all the vanadium-loaded extractant phase into the syringe chamber in aspiration mode. After aspiration is complete, it switches to injection mode, and the syringe outlet is connected to the first sample inlet channel of the back-extraction microreactor via another PTFE connecting tube. The flow rate of the first high-precision syringe pump is set to 8 μL per minute.

[0047] The sodium carbonate back-extraction solution was prepared as follows: 10.60 g of anhydrous sodium carbonate solid was weighed into a volumetric flask, dissolved in deionized water, and brought to a final volume of 100 mL to obtain a sodium carbonate back-extraction solution stock solution with a concentration of 1.0 mol / L. The stock solution was then filtered through a 0.22 μm pore size polyethersulfone membrane to remove insoluble matter and transferred to a storage bottle. The sodium carbonate back-extraction solution was loaded into the syringe of a second high-precision syringe pump. The outlet of the second high-precision syringe pump was connected to the second injection channel of the back-extraction microreactor via a polytetrafluoroethylene connecting tube. The flow rate of the second high-precision syringe pump was set to 8 μL / min.

[0048] The back-extraction microreactor is a microreactor with a helical channel. It is fabricated by bonding an upper borosilicate glass cover plate and a lower polydimethylsiloxane sheet via oxygen plasma. The helical channel is etched onto the upper surface of the polydimethylsiloxane sheet, and its cross-section is semi-circular with a radius of... The pitch is 200 micrometers, the total number of turns in the helical channel is 18, the initial pitch is 1.2 mm, the final pitch is 0.8 mm, and the pitch decreases linearly from the beginning to the end. The total length of the centerline of the helical channel is... The first and second injection channels correspond to two independent inlet channels located at the innermost ring of the spiral channel. These channels merge at the starting point of the spiral channel, maintaining a semi-circular cross-section after merging. The sodium carbonate back-extraction solution and the vanadium-loaded extraction phase flow in parallel at the starting point of the spiral channel. Due to the viscous forces dominating the flow behavior of the vanadium-loaded extraction phase and the sodium carbonate back-extraction solution at the microchannel scale, the two phases maintain a stable parallel laminar flow state within the spiral channel. The vanadium-loaded extraction phase flows closer to the inner wall of the spiral channel, while the sodium carbonate back-extraction solution flows closer to the outer wall, forming a curved liquid-liquid interface between the two phases.

[0049] Total length of the centerline of the spiral channel The total length of the centerline of the spiral channel was determined based on the mass transfer time of vanadium ions diffusing from the vanadium-loaded extraction phase to the sodium carbonate back-extraction solution. The calculation formula is:

[0050] in, This represents the total length of the centerline of the spiral channel, in meters. The average linear velocity, expressed in meters per second, represents the parallel flow of the sodium carbonate back-extraction solution and the vanadium-loaded extraction phase within the spiral channel. Values meters per second, The value is determined as follows: sodium carbonate back-extraction liquid phase flow rate Phase flow rate of the vanadium-loaded extraction phase Sum of the sum divided by the area of ​​the semi-circular cross-section of the spiral channel , and Both are 8 microliters per minute, totaling cubic meters per second equal , It is 200 micrometers, calculated as follows for square meters, total two-phase volumetric flow rate for cubic meters per second Meters per second, after considering the secondary flow deceleration factor of 0.52 introduced by the helical bending effect, the result is... final value meters per second; The characteristic mass transfer time, expressed in seconds, is required for vanadium ions to diffuse from the vanadium-loaded extraction phase across the two-phase interface into the sodium carbonate back-extraction liquid phase. The value is 62 seconds. The values ​​are determined by measuring the total mass transfer coefficient of vanadium ions between the sodium carbonate back-extraction solution and the vanadium-loaded extract phase using the membrane cell method within a temperature range of 40°C to 60°C. The total mass transfer coefficient of vanadium ions at 50°C is also measured. for meters per second, equivalent thickness of the vanadium-loaded extraction phase liquid film within the spiral channel It is 200 micrometers. Seconds, rounded down The value is 62 seconds. and Substituting the numerical value into the formula for calculating the total length of the centerline of the spiral channel, we obtain... The total length of the centerline of the spiral channel is designed to be 274 millimeters.

[0051] The back-extraction microreactor is embedded in a temperature-controlled metal block, which contains a Peltier semiconductor heating and cooling element and a platinum resistance temperature sensor. The platinum resistance temperature sensor collects the current temperature of the back-extraction microreactor and feeds it back to the temperature controller. The temperature controller adjusts the direction and magnitude of the driving current of the Peltier semiconductor heating and cooling element based on the deviation of the current temperature from a first preset temperature range. The first preset temperature range is 40°C to 60°C, and the target temperature of the temperature controller is set to 50°C. At 50°C, the sodium carbonate back-extraction solution and the vanadium-loaded extraction phase flow in a spiral channel and undergo a back-extraction reaction. In the vanadium-loaded extraction phase, the N1923 extractant molecules targeting the coordination extractant undergo a deprotonation reaction in the alkaline environment provided by the sodium carbonate back-extraction solution. The N1923 extractant molecule originally exists as a protonated cation in the vanadium-loaded extraction phase and forms an ion-pair complex with the vanadate anion. When hydroxide ions from the sodium carbonate back-extraction solution cross the liquid-liquid interface into the vanadium-loaded extraction phase, the ammonium binding sites of the N1923 extractant molecule lose protons and transform into a neutral free amine molecule. The ion-pair complex between the N1923 extractant molecule and the vanadate anion disintegrates, and the vanadate ions are released as VO4³⁺. - The vanadium-containing back-extraction solution is released into the sodium carbonate back-extraction solution, generating a vanadium-containing back-extraction solution. Under conditions greater than pH 10, the trioctylamine molecules in the targeted coordination extractant also undergo deprotonation, reverting from a trioctylammonium cation to a neutral trioctylamine molecule. The ion-pair complex between the trioctylamine molecule and the vanadate anion disintegrates, and the remaining vanadium ions are completely released. The N1923 extractant molecules after the release of vanadium ions and the trioctylamine molecules together constitute the regenerated targeted coordination extractant, which returns to its initial neutral state. The vanadium-containing back-extraction solution and the regenerated targeted coordination extractant are separated by density difference in a Y-type phase separator connected at the spiral channel outlet. The vanadium-containing back-extraction solution flows into the lower branch collection bottle, while the regenerated targeted coordination extractant flows into the upper branch recovery bottle.

[0052] Example 5: In practice, the raffinate containing tungstate ions is taken from the raffinate receiving bottle of the microfluidic extraction chip and delivered to the inlet of the ion exchange adsorption column via a 1.0 mm inner diameter polytetrafluoroethylene (PTFE) flexible tube through a first peristaltic pump. The speed of the first peristaltic pump is adjusted to allow the raffinate to pass through the ion exchange adsorption column at a first flow rate, which is set to 3.0 mL per minute. The first flow rate is set based on the ratio between the bed volume of the ion exchange adsorption column and the target contact time of 15 minutes. The actual measured bed volume is 45 mL.

[0053] The ion exchange adsorption column consists of a jacketed glass chromatography column with an inner diameter of 26 mm and a length of 300 mm. The bottom of the column is fitted with a porous polyethylene sieve plate with a pore size of 20 μm. The column is packed with quaternary ammonium salt anion exchange resin to a height of 85 mm, corresponding to a bed volume of 45 mL for the wetted volume of the resin. The quaternary ammonium salt anion exchange resin is a chloride-form strong base anion exchange resin with a macroporous styrene-divinylbenzene copolymer framework. The exchange capacity of the quaternary ammonium salt anion exchange resin is 3.8 mmol / g, and the particle size range is 0.315 mm to 1.25 mm. Before packing, the quaternary ammonium salt anion exchange resin was soaked in deionized water for 24 hours. Then, the column was pre-washed with a sodium chloride solution with a concentration of 1.0 mol / L at a flow rate of 2.0 mL / min for 6 bed volumes. Finally, the column was washed with deionized water until the silver nitrate test of the effluent showed no turbidity.

[0054] The raffinate enters the ion exchange adsorption column from the top at a first flow rate. Under the combined action of gravity and pump drive, the raffinate flows downwards through the quaternary ammonium salt anion exchange resin bed. The raffinate contains tungstate ions (WO4²⁻). - The tungsten exists as polytungstate anions at pH 2.0 to 2.8. These anions undergo an ion exchange reaction with the quaternary ammonium groups on the quaternary ammonium salt anion exchange resin, replacing chloride ions. The polytungstate anions are selectively adsorbed and immobilized on the active sites of the quaternary ammonium groups, forming a tungsten-loaded resin phase. Trace amounts of vanadium-containing cations that may remain in the raffinate do not react with the quaternary ammonium salt anion exchange resin due to their positive charge. These vanadium-containing cations flow out of the ion exchange adsorption column with the effluent, which is collected as a purified solution to remove vanadium impurities. After all the raffinate has passed through the ion exchange adsorption column, the first peristaltic pump stops, and the tungsten-loaded resin phase is rinsed with deionized water at a flow rate of 3.0 mL / min for two bed volumes to remove residual raffinate trapped between the quaternary ammonium salt anion exchange resin particles.

[0055] After rinsing, the second peristaltic pump is activated, delivering the ammonia eluent from the eluent storage tank through a 1.0 mm inner diameter PTFE hose to the upper inlet of the ion exchange adsorption column. The flow rate of the second peristaltic pump is set to 1.5 mL per minute. The concentration of the ammonia eluent is 4.5 mol / L. The ammonia eluent is prepared as follows: measure 302 mL of concentrated ammonia solution with a concentration of 25% to 28%, dilute with deionized water, and bring the volume to 1000 mL. Ammonia eluent enters the quaternary ammonium salt anion exchange resin bed from top to bottom. Hydroxide ions in the ammonia eluent exchange with polytungstate anions on the tungsten-loaded resin phase, causing hydroxide ions to replace polytungstate anions and bind to the quaternary ammonium group sites of the quaternary ammonium salt anion exchange resin. The polytungstate anions desorb from the quaternary ammonium salt anion exchange resin framework and are released into the liquid phase. In the alkaline ammonia environment, the polytungstate anions depolymerize into tungstate ions (WO4²). - Tungstate ions flow with the ammonia eluent to the outlet of the ion exchange adsorption column, and the liquid flowing out of the outlet is collected as tungsten-containing eluent in an eluent collection bottle. When the continuously injected volume of ammonia eluent reaches 5 bed volumes, the second peristaltic pump stops operating, and the total volume of tungsten-containing eluent collected is 225 ml.

[0056] The vanadium-containing back-extraction solution is transferred from the lower branch collection bottle of the back-extraction microreactor to the feed line of the first crystallization vessel. The first crystallization vessel has a volume of 500 ml, and its jacket is filled with circulating, temperature-controlled water at 25 degrees Celsius, controlled by a first temperature-controlled circulation tank. After the vanadium-containing back-extraction solution enters the first crystallization vessel, the first mechanical agitator begins stirring at a speed of 150 rpm.

[0057] Ammonium chloride precipitant, which is analytical grade ammonium chloride solid powder, is added to the first crystallization vessel. The amount of ammonium chloride precipitant added is determined by stoichiometry based on the vanadium ion concentration in the vanadium-containing back-extraction solution. The calculation method is as follows:

[0058] in, This refers to the amount of ammonium chloride precipitant added, expressed in grams. This represents the molar concentration of vanadium ions in the vanadium-containing back-extraction solution, expressed in moles per liter. The value was obtained by inductively coupled plasma atomic emission spectrometry and recorded as 0.042 mol / L. The volume of the vanadium-containing back-extraction solution is expressed in liters. The actual volume is 0.185 liters; This represents the stoichiometric coefficient of ammonium chloride consumed per mole of vanadium ions in the ammonium metavanadate precipitation reaction. The value is set to 1 because the stoichiometric ratio of ammonium ions to vanadium atoms in ammonium metavanadate NH4VO3 is 1:1. The molar mass of ammonium chloride is expressed in grams per mole. The value is 53.49 grams per mole; This is the yield coefficient for the precipitation process, dimensionless. The value is 0.92. The value was determined by taking the arithmetic mean of the ratio of the actual mass of ammonium metavanadate obtained to the theoretically calculated mass in three parallel precipitation experiments conducted on waste catalyst particles from the same source under the same conditions, which was 0.92. , , , and Substitute the numerical value into the formula for calculating the amount of ammonium chloride precipitant to be added. Calculations yielded The concentration was 0.452 g. Using an analytical balance, 0.452 g of ammonium chloride solid powder was added to the first crystallization vessel in three equal portions, 5 minutes apart, while stirring. After the ammonium chloride precipitant was completely added, stirring continued for 30 minutes, resulting in the formation of a white ammonium metavanadate precipitate in the vanadium-containing back-extraction solution. After stopping stirring, the mixture was allowed to stand for 2 hours. The ammonium metavanadate precipitate and supernatant were separated by vacuum filtration using a 0.45-micron pore size polyvinylidene fluoride filter membrane. The ammonium metavanadate precipitate was washed three times with a small amount of deionized water at 4 degrees Celsius and dried in a 105-degree Celsius forced-air drying oven for 4 hours to obtain the solid ammonium metavanadate product.

[0059] The tungsten-containing eluent is transferred from the eluent collection bottle to the feed line of the second crystallizer. The second crystallizer has a volume of 500 ml and its jacket is filled with heat transfer oil, which is heated by an electric heating rod and circulated by a circulation pump. The input power of the electric heating rod is controlled by a heating power regulating circuit. The second crystallizer is equipped with a second mechanical agitator, whose rotation speed is set to 80 rpm. The second crystallizer is connected to a condenser and a distillate collection bottle, and the cooling water temperature of the condenser is set to 5 degrees Celsius.

[0060] The evaporation and crystallization parameters of the second crystallization vessel are controlled to cause tungsten in the tungsten-containing eluent to crystallize and precipitate as ammonium paratungstate. These parameters include evaporation temperature and evaporation rate. The evaporation temperature is maintained by a heating power regulation loop based on dynamic monitoring data of the tungsten-containing eluent volume. The initial volume of the tungsten-containing eluent is 225 ml. An ultrasonic level sensor is attached to the bottom of the outer wall of the second crystallization vessel. This sensor emits ultrasonic pulses at a frequency of 200 kHz to the surface of the tungsten-containing eluent at 0.5-second intervals and receives the echoes. The signal processing unit within the ultrasonic level sensor calculates the current liquid level height based on the time difference between the ultrasonic pulse emission and echo reception. The liquid level height is multiplied by the cross-sectional area of ​​the second crystallization vessel to obtain the dynamic volume data of the tungsten-containing eluent. The heating power regulation loop reads the dynamic volume data output by the ultrasonic level sensor. The heating power regulation loop consists of a proportional-integral controller. The setpoint of the proportional-integral controller is the target evaporation temperature curve, which specifies that when the dynamic volume data of the tungsten-containing eluent... When the volume of the heat transfer oil is greater than or equal to 70% of the initial volume, the target temperature is 65 degrees Celsius; when the dynamic volume data of the tungsten-containing eluent... When the volume of the heat transfer oil is less than 70% and greater than or equal to 40% of the initial volume, the target temperature is 75 degrees Celsius; (The last part, "when the dynamic volume data of the tungsten-containing eluent...", appears to be unrelated and likely refers to a different topic.) When the volume is less than 40% of the initial volume, the target temperature of the heat transfer oil is 82 degrees Celsius. A thermocouple in the heating power regulation circuit is inserted into the heat transfer oil to measure its temperature in real time. The proportional-integral controller calculates the required input power adjustment for the electric heating rod based on the deviation between the real-time heat transfer oil temperature and the target evaporation temperature. This drives a solid-state relay to adjust the on / off duty cycle of the electric heating rod, maintaining the heat transfer oil temperature at the target evaporation temperature corresponding to the current dynamic volume data of the tungsten-containing eluent. The evaporation rate is indirectly controlled by the evaporation temperature. At 65 degrees Celsius, the evaporation rate is approximately 0.8 ml / min; at 75 degrees Celsius, it is approximately 1.3 ml / min; and at 82 degrees Celsius, it is approximately 1.8 ml / min.

[0061] During the evaporation and crystallization process, water in the tungsten-containing eluent continuously evaporates, and the concentration of tungstate ions gradually increases. The pH of the solution is maintained in the range of 8.5 to 9.0 under the influence of free ammonia introduced by the ammonia eluent. Tungstate ions polymerize under alkaline concentration conditions and combine with ammonium ions to form ammonium paratungstate crystals. When the dynamic volume of the tungsten-containing eluent drops to 15% of the initial volume, i.e., 33.75 mL, the heating power adjustment circuit stops the electric heating rod, and the liquid in the second crystallization vessel cools naturally to 25 degrees Celsius. During the cooling process, a large amount of white ammonium paratungstate crystals precipitate. The cooled liquid is vacuum filtered through a polyvinylidene fluoride filter membrane with a pore size of 0.45 micrometers. The ammonium paratungstate crystals are washed twice with a small amount of deionized water at 4 degrees Celsius and dried in a vacuum drying oven at 60 degrees Celsius for 6 hours to obtain solid ammonium paratungstate product.

[0062] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for selectively recovering vanadium-tungsten active metal from spent catalysts, characterized in that, Includes the following steps: Based on the robotic arm micro-manipulation platform, single-particle positioning, grasping and droplet clamping operations are performed on waste catalyst particles to generate single-particle droplet samples. A synchronous oxidation-reduction pulsed electric field is applied to the single-particle suspended drop sample to generate a mixed leachate containing vanadium ions and tungstate ions; A targeted coordination extractant is injected into the mixed leachate, the targeted coordination extractant selectively complexing the vanadium ions to generate an extract phase loaded with vanadium and a raffinate containing tungstate ions. The vanadium-loaded extract phase is subjected to back-extraction to generate a vanadium-containing back-extraction solution, and the raffinate is subjected to ion exchange adsorption to generate a tungsten-containing eluent.

2. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, The method involves using a robotic arm micro-manipulation platform to perform single-particle positioning, grasping, and droplet holding operations on spent catalyst particles to generate single-particle droplet samples, including: The particle size distribution and surface morphology features of the spent catalyst particles are identified by a visual guidance system, generating particle identification coordinate data. The piezoelectric driven micro-gripper in the micro-manipulation platform of the robotic arm moves along the particle identification coordinate data to the first grasping position. The piezoelectric driven micro-gripper grasps the target particle with a first clamping force. The first clamping force is dynamically adjusted according to the particle size data of the target particle through a force feedback control loop. The grasped target particle is immersed in a microdroplet generation chamber containing deionized water. The piezoelectrically driven micro-gripper is controlled to squeeze the target particle with a second clamping force, causing the microdroplets adhering to the surface of the target particle to detach and encapsulate the target particle, generating the single-particle suspended droplet sample. The second clamping force is greater than the first clamping force.

3. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, The process of applying a synchronous oxidation-reduction pulsed electric field to the single-particle suspended drop sample to generate a mixed leachate containing vanadium ions and tungstate ions includes: The single-particle suspended drop sample is transferred into an electrochemical leaching microreaction chamber, wherein a first electrode array is integrated at the bottom and a second electrode array is integrated at the top. An anodic oxidation pulse voltage waveform is applied to the first electrode array. The amplitude of the anodic oxidation pulse voltage waveform is determined according to the content transition parameters of vanadium pentoxide in the single-particle suspended drop sample. The anodic oxidation pulse voltage waveform is used to generate local oxidation micro-regions at the contact interface between the single-particle suspended drop sample and the first electrode array, converting vanadium pentoxide into soluble vanadium oxy cations. A cathodic reduction pulse voltage waveform is applied to the second electrode array. The duty cycle of the cathodic reduction pulse voltage waveform is set according to the content distribution data of tungsten trioxide in the single-particle suspended drop sample. The cathodic reduction pulse voltage waveform is used to generate a local reduction micro-region at the contact interface between the single-particle suspended drop sample and the second electrode array, thereby reducing tungsten trioxide to soluble tungstate ions. The anodic oxidation pulse voltage waveform and the cathodic reduction pulse voltage waveform are applied simultaneously to maintain the concentration ratio of vanadium ions to tungstate ions in the mixed leachate.

4. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, The step of injecting a targeted coordination extractant into the mixed leachate, wherein the targeted coordination extractant selectively complexes the vanadium ions to generate a vanadium-loaded extract phase and a raffinate containing tungstate ions, comprises: The mixed leachate is introduced into the first inlet channel of the microfluidic extraction chip, and the targeted coordination extractant is introduced into the second inlet channel of the microfluidic extraction chip. The targeted coordination extractant is a compound solution of trioctylamine and N1923 extractant, and the volume ratio of trioctylamine to N1923 extractant in the compound solution is 3:1 to 5:

1. The pH of the mixed leachate is adjusted to a first preset pH range, which is 2.0 to 2.8, so that the vanadium ions are expressed as VO2+. + The form exists and enhances the coordination selectivity of the targeted coordination extractant for the vanadium ions; The microchannel structure within the microfluidic extraction chip mixes the mixed leachate with the targeted coordination extractant to form a laminar flow interface. At this interface, trioctylamine in the targeted coordination extractant reacts with N1923 extractant via a protonation reaction to form a cationic extraction group. This cationic extraction group reacts with VO2... + An ion association reaction occurs, generating the vanadium-loaded extract phase. The raffinate containing tungstate ions is retained in the mixed leachate due to electrostatic repulsion.

5. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, The step of back-extracting the vanadium-loaded extraction phase to generate a vanadium-containing back-extraction solution includes: The vanadium-loaded extract phase is transferred to a back-extraction microreactor, and a sodium carbonate back-extraction solution with a concentration of 0.5 mol / L to 1.2 mol / L is injected into the back-extraction microreactor. The temperature inside the back-extraction microreactor is controlled to a first preset temperature range, which is 40°C to 60°C. Under the first preset temperature range, the N1923 extractant in the targeted coordination extractant undergoes a deprotonation reaction, releasing the vanadium ions into the sodium carbonate back-extraction solution to generate the vanadium-containing back-extraction solution. The targeted coordination extractant is then regenerated to its initial state.

6. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, The step of performing ion exchange adsorption on the raffinate to generate a tungsten-containing eluent includes: The raffinate is passed through an ion exchange adsorption column at a first flow rate. The ion exchange adsorption column is filled with a quaternary ammonium salt anion exchange resin. The quaternary ammonium salt anion exchange resin selectively adsorbs the tungstate ions in the raffinate to generate a tungsten-loaded resin phase. The effluent is a purified liquid containing vanadium impurities removed. An ammonia eluent with a concentration of 3 mol / L to 6 mol / L is injected into the tungsten-loaded resin phase. After contacting the tungsten-loaded resin phase, the ammonia eluent desorbs the tungstate ions to generate the tungsten-containing eluent.

7. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 1, characterized in that, After performing back-extraction on the vanadium-loaded extract phase to generate a vanadium-containing back-extraction solution, and performing ion exchange adsorption on the raffinate to generate a tungsten-containing eluent, the process further includes: The vanadium-containing back-extraction solution is introduced into the first crystallization vessel, and ammonium chloride precipitant is added to the first crystallization vessel. The amount of ammonium chloride precipitant added is determined by stoichiometry based on the vanadium ion concentration in the vanadium-containing back-extraction solution to generate ammonium metavanadate precipitate. The tungsten-containing eluent is introduced into a second crystallization vessel, and the evaporation and crystallization parameters of the second crystallization vessel are controlled to cause the tungsten in the tungsten-containing eluent to crystallize and precipitate in the form of ammonium paratungstate. The evaporation and crystallization parameters include evaporation temperature and evaporation rate. The evaporation temperature is maintained by a heating power adjustment loop based on dynamic monitoring data of the volume of the tungsten-containing eluent.

8. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 4, characterized in that, Before adjusting the pH value of the mixed leachate to the first preset pH range, the method further includes: A portion of the mixed leachate was introduced into an online pH monitoring sensor to obtain real-time pH data of the mixed leachate; Based on the deviation between the real-time pH data and the first preset pH range, a pH adjuster, which is a dilute hydrochloric acid solution or a dilute sodium hydroxide solution, is injected into the mixed leachate via a micro-injection pump. After the real-time pH data stabilizes within the first preset pH range, the injection operation of the targeted coordination extractant is performed.

9. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 3, characterized in that, The first electrode array and the second electrode array are platinum electrodes or glassy carbon electrodes. The surfaces of the first electrode array and the second electrode array are coated with a nanoporous titanium dioxide film, which is used to enhance the charge transfer efficiency at the contact interface.

10. The method for selectively recovering vanadium-tungsten active metal from spent catalysts according to claim 5, characterized in that, The back-extraction microreactor is a microreactor with a spiral channel. The cross-section of the spiral channel is semi-circular. The sodium carbonate back-extraction solution and the vanadium-loaded extraction phase flow in parallel within the spiral channel. The length of the spiral channel is determined based on the mass transfer time of vanadium ions diffusing from the extraction phase to the back-extraction solution phase.