Determination of Tungsten Trioxide in Carbonate

By using high-aluminum crucibles and specific compounds to treat in the detection of tungsten trioxide in carbonate, the occurrence of amorphous precipitation is avoided, and the problems of differences in analysis results and repeated detection costs are solved, achieving high accuracy and low cost detection effects .

CN118362550BActive Publication Date: 2024-11-15云南省有色地质局地质勘查院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410462113.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-15
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

The prior art causes differences and errors in the analysis results in the detection of tungsten trioxide in carbonate due to the generation of amorphous precipitation, which increases the analysis cost of repeated detection.

Method used

Sample treatment was performed using a high-aluminum crucible, ammonium chloride and sodium peroxide were added to control the high-temperature melting process, followed by compounds such as ammonium chloride, potassium thiocyanate, hydrochloric acid, sodium hypophosphite, aluminum trichloride and titanium trichloride. Precipitation and dilution are carried out, and the tungsten trioxide content is determined by colorimetric method or inductively coupled plasma emission spectroscopy to avoid the formation of amorphous precipitation.

Benefits of technology

It improves the accuracy of the measurement results, reduces the cost of repeated testing caused by errors, and meets the precision and accuracy requirements of "Geological and Mineral Laboratory Test Quality Management Specifications" DZ/T0130.3-2006.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 6709E7CDD1456
    Figure 6709E7CDD1456
  • Figure BDA0004796127900000031
    Figure BDA0004796127900000031
  • Figure BDA0004796127900000051
    Figure BDA0004796127900000051
Patent Text Reader

Abstract

The present invention discloses a method for determining tungsten trioxide in carbonate, and the method comprises the following steps: (1) weighing a sample and pre-treating the sample by high-temperature melting; (2) adding ammonium chloride to a high-aluminum crucible containing the molten cooled sample, leaching with hot water, boiling to remove hydrogen peroxide, cooling and settling to obtain a test solution; (3) filtering the test solution, adding potassium thiocyanate solution, hydrochloric acid, sodium hypophosphite solution, aluminum trichloride solution, and titanium trichloride solution, and settling to obtain a tungsten colorimetric test solution; (4) preparing tungsten trioxide standard solutions of different concentrations; (5) drawing a standard working curve; (6) checking the amount of tungsten trioxide in the sample according to the working curve, and calculating the analysis result. The present invention adopts the method of adding ammonium chloride before leaching to effectively inhibit the formation of amorphous colloidal precipitation of calcium carbonate, effectively avoiding the amorphous colloidal precipitation adsorbing tungstate ions in the solution to cause the analysis result to be low or wrong, thereby improving the accuracy of the measurement result and reducing the analysis cost caused by repeated detection due to the wrong result.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tungsten trioxide detection, and in particular to a method for determining tungsten trioxide in carbonate. Background Art

[0002] Calcium carbonate exists in six forms, including three anhydrous crystalline phases: calcite, aragonite and vaterite; two hydrated crystalline phases: calcium carbonate hexahydrate and calcium carbonate monohydrate, as well as amorphous calcium carbonate (ACC). Precipitation can be roughly divided into two categories according to its shape: crystalline precipitation and amorphous precipitation. The specific type of precipitation depends mainly on the nature of the precipitation itself and the precipitation conditions. During the precipitation formation process, the ions in the solution combine with each other at a relatively high speed to form small crystal nuclei. This action speed is called the aggregation speed. At the same time, the electrostatic attraction makes the ions arrange in a certain order in the crystal lattice. This action speed is called the orientation speed. When the aggregation speed is greater than the orientation speed, the ions quickly gather to form crystal nuclei, but they do not have time to arrange in a certain order in the crystal lattice, so an amorphous precipitation is obtained. On the contrary, when the aggregation speed is less than the orientation speed, the speed at which ions aggregate into crystal nuclei is slow, so the number of crystal nuclei is small, and the number of ions in the corresponding solution is large. At this time, there are enough ions arranged in a certain order in the crystal lattice to make the crystal grow, and a crystalline precipitate is obtained. It can be seen that different precipitation conditions will result in different shapes of precipitates.

[0003] Since many laboratories compared the analysis results of tungsten trioxide in carbonates, there were obvious differences and even wrong results. The fundamental reason was that amorphous precipitation of calcium carbonate was produced during the hot water leaching process after sodium peroxide alkali melting. There are two types of calcium carbonate precipitation: crystalline precipitation and amorphous precipitation. The crystalline precipitation has little adsorption of tungstate ions in the solution. The amorphous precipitation has a disordered internal arrangement and loose structure during the formation process, which makes it very easy to adsorb tungstate ions in the solution. Therefore, avoiding amorphous colloidal precipitation during hot water leaching can ensure accurate analysis results. Through related field searches, for the detection of tungsten trioxide in carbonates, it was only found that Dong Wei and others from the Guangdong Provincial Geological Experimental Testing Center published a paper entitled "Research on Pretreatment Methods of Tungsten in Carbonate Ores" to study the smelting method of tungsten in carbonate ores. This method did not use the national standard high-aluminum crucible sodium peroxide melting sample, but instead used a nickel crucible sodium hydroxide melting sample. In actual work, customers usually require the use of the national standard melting sample method, but the precipitation morphology has an impact on tungsten trioxide. Therefore, how to use the national standard method to determine the tungsten trioxide content, avoid the formation of amorphous precipitation, and reduce the analysis cost caused by repeated testing due to erroneous results is an urgent problem to be solved. Summary of the invention

[0004] The main purpose of the present invention is to propose a method for determining tungsten trioxide in carbonate, aiming to provide a national standard method for determining the content of tungsten trioxide in carbonate by melting sample, effectively avoiding the generation of amorphous precipitation, and reducing the analysis cost caused by repeated detection due to erroneous results.

[0005] To achieve the above object, the present invention provides a method for determining tungsten trioxide in carbonate, comprising the following steps:

[0006] (1) Weigh the sample into a high-aluminum crucible. If the arsenic content is high, add ammonium chloride to mix well. Place the sample in a high-temperature furnace at 300°C to 400°C and burn it. After cooling, add sodium peroxide. Stir well and add sodium peroxide again to cover the sample. Then place the sample in a high-temperature furnace that has been preheated to 630°C to 670°C. Heat it to 680°C to 720°C and keep it for 5 to 7 minutes until the melt is just fully melted. Take out the high-aluminum crucible and cool it.

[0007] (2) Place a high-aluminum crucible in a beaker, add ammonium chloride to the high-aluminum crucible, add 70-100 mL of warm water to the beaker, immediately cover the high-aluminum crucible with a watch glass, add 5-6 drops of anhydrous ethanol and formaldehyde solution from the mouth of the beaker, place the beaker on a high-temperature electric hot plate or a small electric furnace and boil for 3-5 minutes, remove it, wash the watch glass and high-aluminum crucible with distilled water, cool it, and make up to volume in a 100 mL or 250 mL volumetric flask with distilled water, mix well, and obtain a test solution;

[0008] (3) Dry filter the test solution and take the filtrate into a volumetric flask. If the filtrate is less than 20 mL, add 2% sodium hydroxide solution to make up, add potassium thiocyanate solution and shake well, immediately add hydrochloric acid and shake well, cool in ice water or running water bath, add sodium hypophosphite solution and aluminum chloride solution in turn, shake well, then add titanium chloride solution, shake well, dilute with water to the scale, shake well, and obtain tungsten test solution. At the same time, make a blank sample and process it at the same time as the sample;

[0009] (4) Take 0.00mL, 0.25mL, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 4.00mL, and 5.00mL of tungsten trioxide standard solution respectively and place them in a 50mL volumetric flask (aluminum chloride should be added to eliminate interference when the fluorine content is high), add sodium hydroxide solution to 20mL, add potassium thiocyanate solution and shake well, immediately add hydrochloric acid and shake well, place in ice water or running water bath to cool, add sodium hypophosphite solution and aluminum chloride solution in turn, shake well, then add titanium chloride solution, shake well, dilute with water to the scale, shake well, and obtain tungsten trioxide standard solutions of different concentrations;

[0010] (5) Select a suitable cuvette, use the blank as a reference, measure the absorbance of different concentrations of tungsten trioxide standard solution at 420nm, perform a blank test together, subtract the absorbance of the blank test, and draw a working curve with the amount of tungsten trioxide as the horizontal axis and the absorbance as the vertical axis, or dilute the tungsten trioxide standard solution 10 times and measure the emission intensity of tungsten at 207.91nm on an inductively coupled plasma emission spectrometer, and draw a standard working curve with the emission intensity of tungsten at 207.91nm as the vertical axis and the amount of tungsten trioxide as the horizontal axis;

[0011] (6) measuring the absorbance of the tungsten test solution at 420 nm, and finding the content of tungsten trioxide in the sample according to the working curve, or measuring the emission intensity of tungsten at 207.91 nm on an inductively coupled plasma emission spectrometer, and finding the content of tungsten trioxide in the sample according to the working curve.

[0012] Optionally, in step (1), the mass of the sample is 0.1500-0.5000 g, the amount of sodium peroxide added is 4 g, and the amount of sodium peroxide added again is 1 g.

[0013] Optionally, in step (2), the amount of ammonium chloride added is 1 to 2 g.

[0014] Optionally, in step (3), the dry filtration uses quantitative filter paper, and the volume of the filtrate is 5.00 to 20.00 mL.

[0015] Optionally, in step (3), the mass concentration of the potassium thiocyanate solution is 50%.

[0016] Optionally, in step (3), the density of the hydrochloric acid is 1.19 g / mL.

[0017] Optionally, in step (3), the density of the sodium hypophosphite solution is 100 g / L.

[0018] Optionally, in step (3), the density of the aluminum chloride solution is 500 g / L.

[0019] Optionally, in step (3), the density of the titanium trichloride solution is 15 g / L.

[0020] Optionally, in step (6), the calculation analysis result adopts the following calculation formula:

[0021]

[0022] Where:

[0023] m1: the amount of tungsten trioxide found on the working curve, in micrograms (μg);

[0024] V0: total volume of the test solution, in milliliters (mL);

[0025] V1: the volume of the test solution taken, in milliliters (mL);

[0026] m0: is the mass of the sample, in grams (g).

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] In the technical solution provided by the present invention, ammonium chloride is added in advance before immersion to effectively inhibit the formation of amorphous colloidal precipitation of calcium carbonate, effectively avoiding the amorphous colloidal precipitation from adsorbing tungstate ions in the solution and causing low or erroneous analysis results, thereby improving the accuracy of the measurement results and reducing the analysis costs caused by repeated testing due to erroneous results. DETAILED DESCRIPTION

[0029] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.

[0030] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0031] Example 1 Determination of tungsten trioxide in carbonate

[0032] (1) Weigh 0.5000 g of sample into a high-aluminum crucible, add 4 g of sodium peroxide, stir evenly, add 1 g of sodium peroxide again to cover the sample, and then place it in a high-temperature furnace preheated to 650°C, heat it to 700°C and keep it for 5 min until the melt is just fully melted, take out the high-aluminum crucible, and cool it;

[0033] (2) Place a high-aluminum crucible in a beaker, add 2 g of ammonium chloride to the high-aluminum crucible, add 100 mL of warm water to the beaker, immediately cover the high-aluminum crucible with a watch glass, add 5 drops of anhydrous ethanol and formaldehyde solution from the mouth of the beaker, place the beaker on a high-temperature electric hot plate or a small electric furnace and boil for 5 minutes, remove it, wash the watch glass and the high-aluminum crucible with distilled water, cool it, make up to volume in a 100 mL volumetric flask with distilled water, mix well, and obtain a test solution;

[0034] (3) Dry filter the test solution, take 5.00 mL of the filtrate into a 50 mL volumetric flask, add 2% sodium hydroxide solution to make up to 20 mL, add 2 mL of 50% potassium thiocyanate solution and shake well, immediately add 20 mL of hydrochloric acid with a density of 1.19 g / mL and shake well, cool in ice water or running water bath, add 1 mL of sodium hypophosphite solution with a density of 100 g / L and 1 mL of aluminum chloride solution with a density of 500 g / L in sequence, shake well, then add 1.5 mL of titanium chloride solution with a density of 15 g / L, shake well, dilute to the scale with water, shake well, obtain tungsten test solution, and prepare blank sample at the same time, which is processed at the same time as the sample;

[0035] (4) Take 0.00mL, 0.25mL, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 4.00mL, and 5.00mL of tungsten trioxide standard solution and place them in a 50mL volumetric flask. Add 2% sodium hydroxide solution to make up to 20mL, add 2mL of 50% potassium thiocyanate solution and shake well, immediately add 20mL of hydrochloric acid with a density of 1.19g / mL and shake well, place in ice water or running water bath to cool, add 1mL of sodium hypophosphite solution with a density of 100g / L and 1mL of aluminum chloride solution with a density of 500g / L in turn, shake well, then add 1.5mL of titanium chloride solution with a density of 15g / L, shake well, dilute to the scale with water, and shake well to obtain tungsten trioxide standard solutions of different concentrations;

[0036] (5) Select a suitable cuvette, use the blank as a reference, measure the absorbance of different concentrations of tungsten trioxide standard solution at 420nm, perform a blank test together, subtract the absorbance of the blank test, and draw a working curve with the amount of tungsten trioxide as the horizontal axis and the absorbance as the vertical axis, or dilute the tungsten trioxide standard solution 10 times and measure the emission intensity of tungsten at 207.91nm on an inductively coupled plasma emission spectrometer, and draw a standard working curve with the emission intensity of tungsten at 207.91nm as the vertical axis and the amount of tungsten trioxide as the horizontal axis;

[0037] (6) Measure the absorbance of the tungsten test solution at 420 nm, and find out the amount of tungsten trioxide in the sample according to the working curve, or measure the emission intensity of tungsten at 207.91 nm of the tungsten test solution on an inductively coupled plasma emission spectrometer, and find out the amount of tungsten trioxide in the sample according to the working curve, and calculate the analysis result.

[0038] Test methods and results

[0039] (1) Precision

[0040] The samples Dht21-421 and Dht21-517 were measured 12 times in parallel by spectrophotometry and inductively coupled plasma emission spectrometry using the method of the present invention. From the results in Table 1, it can be seen that the relative standard deviations of the test results of the two samples measured by different methods are less than 5%, which meets the "Quality Management Standard for Laboratory Testing of Geological and Mineral Resources" DZ / T0130.3-2006.

[0041] Table 1 Precision results of the test method

[0042]

[0043]

[0044] (2) Accuracy

[0045] For samples Dht21-421 and Dht21-517, spike recovery was adopted. WO3 standard solution was added in advance during hot water immersion, and the samples were measured 12 times in parallel under the same conditions. It can be seen from the results in Table 2 that the recovery rate range of the two measured samples meets the requirement of 95%-105%.

[0046] Table 2 Accuracy results of the test method

[0047]

[0048]

[0049] (3) Blank comparison and result comparison

[0050] Table 3 Blank comparison table of different analysis methods

[0051]

[0052] Table 4 Conventional pretreatment of high aluminum crucible and iron crucible

[0053]

[0054]

[0055] The samples selected in the above test, Dht21-406, Dht21-421, Dht21-431, Dht21-453, Dht21-464, and Dht21-475, are all calcites with a calcium oxide content of more than 50%. The maximum and minimum values ​​are calculated using the results of ammonium chloride leaching as theoretical values. It can be seen from Table 4 above that when ammonium chloride is not added, the measured values ​​of tungsten trioxide in the high-aluminum crucible smelt and carbonate both show erroneous results, showing negative errors. When the iron crucible smelts, the test results of low-content tungsten trioxide are biased high. Since the blank of the iron crucible is relatively high and the blank values ​​of different iron crucibles vary greatly, it is difficult to unify when deducting the blank of the iron crucible. It is not recommended to use iron crucible melting sample for low content tungsten trioxide determination. Three samples with more than 0.2% were selected, two of which were within the error range, and one was beyond the error range, showing a negative error. For samples with high content, using iron crucible melting sample can avoid the adsorption of amorphous precipitation on tungstate to a certain extent, but there will still be some low analysis results. The analysis results of different content sections and different test methods of adding ammonium chloride in advance are relatively stable. The blank value of high aluminum crucible melting sample is also relatively stable and far below the detection limit of the method.

[0056] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A method for determining tungsten trioxide in carbonate, characterized in that: The following steps are involved: (1) Weigh the sample into a high-aluminum crucible, add sodium peroxide, stir evenly, and then add sodium peroxide again to cover the sample. Then place it in a high-temperature furnace that has been preheated to 630-670°C, heat it to 680-720°C and keep it for 5-7 min until the melt is just fully melted. Then take out the high-aluminum crucible and cool it. (2) Place the high-alumina crucible in a beaker, add ammonium chloride to the high-alumina crucible, add 70-100 mL of warm water to the beaker, immediately cover the high-alumina crucible with a watch glass, add 5-6 drops of anhydrous ethanol and formaldehyde solution from the mouth of the beaker, place the beaker on a high-temperature electric hot plate or a small electric stove and boil for 3-5 minutes, remove it, wash the watch glass and high-alumina crucible with distilled water, cool it down, make up to volume in a 100 mL or 250 mL volumetric flask with distilled water, mix well, and obtain the test solution; (3) Dry filter the test solution and put the filtrate into a volumetric flask. If the filtrate is less than 20 mL, add 2% sodium hydroxide solution to make up the volume. Add potassium thiocyanate solution and shake well. Immediately add hydrochloric acid and shake well. Cool in ice water or running water bath. Add sodium hypophosphite solution and aluminum chloride solution in turn and shake well. Then add titanium chloride solution and shake well. Dilute with water to the mark and shake well to obtain tungsten test solution. At the same time, prepare a blank sample and process it at the same time as the sample. (4) Take 0.00 mL, 0.25 mL, 0.50 mL, 1.00 mL, 2.00 mL, 3.00 mL, 4.00 mL, and 5.00 mL of tungsten trioxide standard solution and place them in a 50 mL volumetric flask. Add sodium hydroxide solution to make up to 20 mL. Add potassium thiocyanate solution and shake well. Immediately add hydrochloric acid and shake well. Cool in ice water or running water bath. Add sodium hypophosphite solution and aluminum chloride solution in turn. Shake well. Add titanium chloride solution and shake well. Dilute to the mark with water and shake well to obtain tungsten trioxide standard solutions of different concentrations. (5) Select a suitable cuvette, use the blank as a reference, measure the absorbance of different concentrations of tungsten trioxide standard solution at 420nm, perform a blank test together, subtract the absorbance of the blank test, and draw a working curve with the amount of tungsten trioxide as the horizontal axis and the absorbance as the vertical axis, or dilute the tungsten trioxide standard solution 10 times and measure the emission intensity of tungsten at 207.91nm on an inductively coupled plasma emission spectrometer, and draw a standard working curve with the emission intensity of tungsten at 207.91nm as the vertical axis and the amount of tungsten trioxide as the horizontal axis; (6) measuring the absorbance of the tungsten test solution at 420 nm, and finding out the amount of tungsten trioxide in the sample according to the working curve, or measuring the emission intensity of tungsten at 207.91 nm on an inductively coupled plasma emission spectrometer, and finding out the amount of tungsten trioxide in the sample according to the working curve, and calculating the analysis results; In step (1), the mass of the sample is 0.1500-0.5000 g, the amount of sodium peroxide added is 4 g, and the amount of sodium peroxide added again is 1 g; In step (2), the amount of ammonium chloride added is 1 to 2 g.

2. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the dry filtration uses quantitative filter paper, and the volume of the filtrate is 5.00 to 20.00 mL.

3. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the mass concentration of the potassium thiocyanate solution is 50%.

4. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the density of the hydrochloric acid is 1.19 g / mL.

5. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the density of the sodium hypophosphite solution is 100 g / L.

6. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the density of the aluminum chloride solution is 500 g / L.

7. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (3), the density of the titanium trichloride solution is 15 g / L.

8. The method for determining tungsten trioxide in carbonate according to claim 1, characterized in that: In step (6), the calculation analysis results are calculated using the following formula: Where: m1: the amount of tungsten trioxide found on the working curve, in micrograms (μg); V0: total volume of the test solution, in milliliters (mL); V1: volume of test solution, in milliliters (mL); m0: mass of sample, in grams (g).