A method for recovering uranium, molybdenum and other impurity ions from mine fissure water.
By employing filtration, adsorption, and rinsing processes to treat mine fissure water, the problem of ineffective removal of uranium and molybdenum impurity ions in the water has been solved, achieving 100% recycling of water resources and efficient recovery of uranium and molybdenum.
Patent Information
- Application Number
- CN202611012160.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes cannot effectively treat uranium and molybdenum impurity ions in mine fissure water, making it impossible to achieve 100% water recycling.
The mine fissure water is treated using technologies such as filtration, adsorption, and leaching, including steps such as coarse filtration, fine filtration, ultrafiltration, ion exchange, and precipitation. Anion exchange resin and precipitant are used to remove uranium, molybdenum, and other impurity ions, and uranium and molybdenum metals are recovered through leaching.
It achieves effective recovery of uranium and molybdenum and removal of impurity ions in fissure water. The treated water quality meets the relevant specifications, with uranium ≤2μg/L and molybdenum ≤0.07mg/L. The high removal rate of impurity ions ensures stable equipment operation and reduces production costs.
Smart Images

Figure CN123108326A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrometallurgical technology, specifically relating to a method for recovering uranium, molybdenum and other impurity ions from mine fissure water. Background Technology
[0002] Uranium plays a vital role in the national economy. As a major nuclear power, my country relies heavily on natural uranium, a fundamental raw material for the development and stockpiling of nuclear weapons; its importance is self-evident. Simultaneously, natural uranium is the basic fuel for nuclear power generation, and its reserves and production are essential for ensuring my country's national defense and nuclear power development. Molybdenum also has a wide range of applications, primarily as an additive in the production of low-alloy steel, alloy steel, stainless steel, tool steel, cast iron, superalloys, and molybdenum-based alloys. Molybdenum chemicals are mainly used as lubricants, including pure molybdenum oxide, molybdates, and other lubricants. Furthermore, molybdenum plays an important role in catalysts, pigments, corrosion inhibitors, and reagents. According to statistics from the International Molybdenum Association (IMOA), in 2020, approximately 81% of global molybdenum products were used in the steel industry as furnace feedstocks such as molybdenum oxide or ferromolybdenum, 13% in molybdenum chemicals, and 6% in metal products and other industries. In addition, the demand for molybdenum resources in high-tech and other fields is gradually increasing and developing rapidly. Moreover, molybdenum is also widely used in modern industrial end-user applications.
[0003] A certain mine is being constructed in three phases. In 2022, mining reached the boundary elevation of the first phase open-pit mine. Simultaneously, to ensure the domestic supply of natural uranium, enhance the company's ability to withstand market risks, improve the overall efficiency of state-owned assets, and guarantee the company's high-quality development, the second phase of mine construction needs to be initiated as soon as possible to ensure a smooth continuation of production. According to the predicted mine water inflow, when the open-pit mine reaches a depth of 1480m, the mine water inflow will consist of Quaternary water and bedrock fissure water. After implementing water control measures such as grouting curtains, the maximum water inflow during the second phase of mining is expected to be 104m³. 3 / h, of which the maximum inflow of the Quaternary system is approximately 66m³. 3 / h, the maximum inflow rate from bedrock fissures is approximately 38m³. 3 / h, with an average inflow of approximately 70m³ 3 / h. Bedrock fissure water contains elements such as U, Mo, Ga, and Mg.
[0004] The existing process wastewater is neutralized to a pH of 8.0–8.5 by mixing with calcium carbide slag slurry. After neutralization, the material enters a thickening tank and is filtered using a chamber filter press. The waste residue is transferred to the tailings dam, and the qualified water enters an activated carbon oil removal tower for adsorption and oil removal. The qualified oil-removed water is returned to the system for reuse. The fissure water generated after the second phase of the mining area construction and operation differs significantly in properties from the production wastewater, and the existing production wastewater treatment system cannot handle this fissure water. Analysis of the Quaternary inflow water shows low uranium and molybdenum concentrations. Adhering to the principle of rational water resource utilization, the second phase of the project considers a "clean and polluted water separation" approach for the treatment of mine inflow water, employing different treatment methods for different types of mine inflow water. Specifically, the Quaternary inflow water is intercepted by an open ditch connecting to the shallow Quaternary aquifer in the open-pit mine. After treatment, it is returned to the hydrometallurgical plant for use as production water or directly used for dust suppression on mining roads, reclamation and greening of spoil heaps, and construction water use. Bedrock fissure water contains high levels of impurities such as Ga and Mg, with uranium concentrations ranging from 232.5 to 700 μg / L and molybdenum concentrations from 0.027 to 0.055 g / L. Therefore, it requires treatment before reuse. Hydrometallurgical techniques are the most widely used method for recovering uranium and molybdenum metals due to their wide applicability and high separation and purification efficiency. However, they are less suitable for low-concentration raw materials.
[0005] Therefore, in order to recover uranium and molybdenum metals from fracture water and achieve 100% water recycling, it is urgent to develop a method for recovering uranium, molybdenum and removing other impurity ions from mine fracture water. Summary of the Invention
[0006] The purpose of this invention is to provide a method for recovering uranium, molybdenum and other impurity ions from mine fissure water and removing impurity ions such as calcium and magnesium from the water.
[0007] Technical solution to achieve the purpose of this invention: A method for recovering uranium, molybdenum, and other impurity ions from mine fissure water, the method comprising: Step (1): The mine fissure water is coarsely filtered through a sand filter tank and a self-cleaning filter, and then finely filtered through an activated carbon adsorption tank and a precision filter to obtain pretreated raw water. Step (2): The pretreated raw water is sent to the ultrafiltration system for treatment after being left to stand. The ultrafiltration water is sent to the material separation and treatment system for further purification to obtain concentrated water and purified water. The purified water is returned to the hydrometallurgical plant as boiler feed water. Step (3): After the concentrated water is recycled and enters the ion exchange tower to adsorb uranium and molybdenum in the water, the adsorption tail liquid and saturated resin are obtained. The adsorption tail liquid is returned to the storage tank for temporary storage. Step (4): Add precipitant to the adsorption tail liquid, precipitate and filter to obtain qualified water, and store the filter residue as tail waste. Step (5): Saturated resin is leached with sulfuric acid solution as uranium leaching agent, and uranium leaching solution is obtained by single-tower leaching. The uranium leaching solution is then incorporated into the uranium extraction acid washing solution for reuse. Step (6): The saturated resin after uranium leaching is leached with ammonium solution as molybdenum leaching agent in a single tower to obtain molybdenum leaching solution and lean resin. The molybdenum leaching solution enters the molybdenum back-extraction agent preparation tank. Step (7): The conversion agent is fed into the ion exchange tower to convert the lean resin. The conversion waste liquid is discharged from the bottom of the tower and returned to the eluent preparation tank. The converted resin is reused to adsorb uranium and molybdenum.
[0008] Furthermore, in step (1), the sand filter tank and self-cleaning filter have a filtration accuracy of 50~200μm to remove large particles, silt, organic matter in water, colloidal particles, and microorganisms; the precision filter has an accuracy of 1~10μm to remove fine organic matter and suspended particles in water.
[0009] Furthermore, in step (2), the ultrafiltration system has an accuracy of 0.001~0.1μm to remove colloidal particles; the material separation and processing system is a spiral wound nanofiltration membrane element with an accuracy of 1~5nm, resulting in a purified water conductivity of <100μS / cm and a uranium and molybdenum rejection rate of >99%.
[0010] Furthermore, in step (3), anion exchange resin is used in the ion exchange tower. The anion exchange resin is D314, D231YT, D382 macroporous weak base and strong base anion exchange resin.
[0011] Furthermore, in step (3), the uranium concentration in the adsorption tail liquid is >10 μg / L and the uranium recovery rate is >99% when adsorption is stopped, or the molybdenum concentration in the solution is >0.1 mg / L and the molybdenum recovery rate is >99.9% when adsorption is stopped.
[0012] Furthermore, in step (4), the precipitant is a calcium-based alkaline substance or a carbonate; the calcium-based alkaline substance includes CaO, Ca(OH)2, and carbide slag.
[0013] Further, step (4) includes: adding a calcium-containing alkaline substance to the adsorption tail liquid for primary precipitation, followed by filtration; adding a carbonate solution to the filtered filtrate for secondary precipitation, followed by filtration to obtain qualified water; during the primary precipitation, the pH value is adjusted to 7.5~8.5 using a calcium-containing alkaline substance, the mixture is stirred for 0.5~1h, and a plate and frame filter press is used for the first solid-liquid separation, and the Mg in the filtrate is removed. 2+ Removal rate > 98.3%, Fe 3+ Removal rate > 99%, Al 3+Removal rate > 99.9%; during secondary precipitation, the added carbonate solution concentration is 3wt%~8wt%, and after reacting for 0.5~1h, a second solid-liquid separation is performed using a plate and frame filter press to remove Ca from the water. 2+ When the ion concentration is reduced to ≤3mg / L, the removal rate is >99.5%.
[0014] Furthermore, in step (5), the uranium leaching agent is a 5-20% sulfuric acid solution, and the overall uranium recovery rate is >99%; Furthermore, in step (6), the molybdenum leaching agent is 10-20 wt% ammonia solution + 3-10 wt% ammonium sulfate solution, and the overall molybdenum recovery rate is >99%; Furthermore, in step (7), the transforming agent is a 2-5% sulfuric acid solution, and the transformed resin is washed with qualified water until the pH of the washing effluent is 6-7. The transformed resin is 100% recycled.
[0015] The beneficial technical effects of this invention are as follows: 1. The present invention provides a method for recovering uranium, molybdenum and other impurity ions from mine fissure water. Through concentration, adsorption and leaching, the uranium in the fissure water is ≤2μg / L and the molybdenum is ≤0.07mg / L, which are far below the limits specified in relevant standards. The uranium retention rate in the water is >99.4%, the molybdenum retention rate is >99.6%, and the uranium and molybdenum recovery rate in the fissure water is >99%.
[0016] 2. This invention provides a method for recovering uranium, molybdenum, and other impurity ions from mine fissure water. The method involves deep separation of calcium and magnesium ions in the mine fissure water through adsorption, filtration, and a material separation membrane, followed by precipitation to remove calcium from the fissure water. 2+ Mg 2+ Fe 3 + Al 3+ Isocations, Ca 2+ Concentration ≤3mg / L, removal rate >99.5%; Mg 2+ Concentration ≤1mg / L, removal rate >98.3%; Fe 3+ Trace concentration, removal rate >99%; Al 3+ With a concentration ≤1mg / L and a removal rate >99.9%, impurity ions in the fissure water are effectively removed, while calcium and magnesium scaling is effectively prevented from affecting the reaction equipment and process pipelines, ensuring the heat exchange efficiency of the reaction equipment and avoiding blockage of the process pipelines.
[0017] 3. The present invention provides a method for recovering uranium, molybdenum and other impurity ions from mine fissure water. By treating the mine fissure water, the conductivity of the fissure water is reduced to <100μS / cm, which effectively protects environmental water resources and realizes the rational utilization of water resources. The treated water can be fed into the production steam boiler, which not only ensures the effective recovery of uranium and molybdenum resources, but also further reduces production costs. Attached Figure Description
[0018] Figure 1 The flowchart illustrates a method for recovering uranium, molybdenum, and other impurity ions from mine fissure water, provided by this invention. Detailed Implementation
[0019] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments.
[0020] This invention employs techniques such as filtration concentration, adsorption, and elution to recover low-concentration uranium and molybdenum. For low-concentration U, Mo, and Ca... 2+ Mg 2+ Fe 3+ Al 3+ Isocational impurities were treated by concentration, filtration, neutralization, and deep removal of Ca from carbonates. 2+ The combined method of rinsing and recovery not only recovers uranium and molybdenum metals, but also effectively removes impurity ions and achieves 100% reuse of fracture water. Through a comprehensive comparison of the compatibility, technological maturity, and economic efficiency of existing processes, a method for recovering uranium, molybdenum, and other impurity ions from mine fracture water has been developed.
[0021] This invention uses membrane filtration to isolate valuable metals from fissure water, forming concentrated water containing uranium and molybdenum, and purified water after impurity removal. The treated fissure water (purified water) has uranium ≤2μg / L, molybdenum ≤0.07mg / L, with a uranium removal rejection rate >99.4%, a molybdenum rejection rate >99.6%, and a calcium removal rate >99.6%. 2+ When the ion concentration is reduced to ≤3 mg / L, the retention rate is >98.9%; Mg 2+ Concentration ≤ 1 mg / L, retention rate > 96.7%; Fe 3+ ≤0.1mg / L, retention rate >99.5%, Al 3+ With a concentration ≤1mg / L and a rejection rate >99.9%, this method effectively increases the uranium and molybdenum content in the concentrated water and facilitates its recovery. The purified water can be used as feed water for steam boilers.
[0022] A concentrated aqueous solution rich in uranium and molybdenum is adsorbed using resin and then leached. The uranium and molybdenum in the leaching solution are then incorporated into the original process for extraction and recovery, achieving a uranium and molybdenum recovery rate of >99% in the fissure water. The adsorption tailings are neutralized with alkali (low-cost calcium-containing alkaline substances such as lime, carbide slag, and calcium hydroxide) to remove other impurities from the mine fissure water. Further Ca removal is achieved by applying carbonates to the liquid phase after alkali removal. 2+ It can adsorb Ca in the tail liquid 2+ Mg 2+ Fe 3+ Al 3+ The removal of cationic impurities at a deeper level, compared to traditional one-step neutralization and impurity removal methods, allows for more efficient removal of Ca... 2+ Deep removal of Ca from the recycled water after impurity removal is achieved. 2+ When the ion concentration is reduced to ≤3 mg / L, the removal rate is >99.5%; Mg 2+ Concentration ≤1mg / L, removal rate >98.3%; Fe 3+ Trace concentration, removal rate >99%, Al 3+ With a concentration ≤1 mg / L and a removal rate >99.9%, this method effectively solves the problem of traditional chemical methods being hindered by calcium content. 2+ Incomplete removal leads to the formation of calcium scale during the reuse process, causing blockages in reaction equipment and process pipelines. While ensuring the effective recovery of uranium and molybdenum resources, this method further reduces production costs and achieves 100% reuse of mine fissure water, solving the key problem of mine water that cannot be discharged due to the lack of receiving water bodies.
[0023] Specifically, this invention provides a method for recovering uranium, molybdenum, and other impurity ions from mine fissure water, such as... Figure 1 As shown, the specific steps include: Step (1): The mine fissure water is coarsely filtered through a sand filter tank and a self-cleaning filter, and then finely filtered through an activated carbon adsorption tank and a precision filter to obtain pretreated raw water. In step (1), the mine fissure water first passes through a sand filter tank and a self-cleaning filter with a filtration accuracy of 50~200μm to remove large particles, silt, organic matter, colloidal particles, microorganisms, etc., and then enters a granular activated carbon adsorption tank for filtration to remove fine organic matter and suspended particles in the water. Finally, it enters a precision filter with an accuracy of 1~10μm for filtration to obtain pretreated raw water. Step (2): The pretreated raw water is sent to the ultrafiltration system for treatment after being left to stand. The ultrafiltration water is sent to the material separation and treatment system for further purification to obtain concentrated water and purified water. The purified water is returned to the hydrometallurgical plant as boiler feed water. In step (2), the pretreated raw water is allowed to stand before being fed into an ultrafiltration system with a precision of 0.001~0.1μm to remove colloidal particles. The resulting ultrafiltered water is then further purified using a spiral wound nanofiltration membrane element with a precision of 1~5nm to remove U, Mo, and Ca. 2+ Mg 2+ Fe 3+ Al 3+ Purified water and concentrated water. Purified water conductivity <100 μS / cm, uranium ≤2 μg / L, uranium rejection rate >99.4%, molybdenum ≤0.07 mg / L, molybdenum rejection rate >99.6%, Ca... 2+ ≤3mg / L, retention rate >98.9%; Mg 2+ ≤1 mg / L, retention rate >96.7%; Fe 3+ ≤0.1mg / L, retention rate >99.5%, Al 3+ With a concentration ≤1mg / L and a rejection rate >99.9%, the purified water can be used as boiler water in the production system. Step (3): After the concentrated water is recycled and enters the ion exchange tower to adsorb uranium and molybdenum in the water, the adsorption tail liquid and saturated resin are obtained. The adsorption tail liquid is returned to the storage tank for temporary storage. In step (3), the recovered concentrated water enters a series of two macroporous weak-base and strong-base anion exchange resin towers to adsorb uranium and molybdenum from the water. Adsorption is stopped when the uranium concentration in the adsorption tail liquid is >10 μg / L, the uranium recovery rate is >99%, the molybdenum concentration in the solution is >0.1 mg / L, and the molybdenum recovery rate is >99.9%. The adsorption tail liquid and saturated resin are obtained through adsorption. In specific embodiments, the macroporous weak base and strong base anion exchange resins can be D231YT exchange resin, D314 exchange resin, and D382 exchange resin, respectively.
[0024] Step (4): Add precipitant to the adsorption tail liquid, precipitate and filter to obtain qualified water, and store the filter residue as tail waste. In step (4), the separated adsorption tail liquid is precipitated using calcium-containing alkaline substances. These substances include CaO, Ca(OH)2, and carbide slag. The pH of the material is adjusted to 7.5-8.5 for initial precipitation. After stirring for 0.5-1 hour, a plate and frame filter press is used for the first solid-liquid separation. Mg 2+ Fe 3+ Al 3+ Magnesium hydroxide, iron hydroxide, and aluminum hydroxide precipitates are formed and enter the solid tailings for disposal. Mg in the filtrate 2+ Concentration ≤1mg / L, removal rate >98.3%; Fe 3+ Trace concentration, removal rate >99%, Al 3+Concentration ≤1mg / L, removal rate >99.9%. A 3-8wt% carbonate solution is added to the filtrate, and after a reaction of 0.5-1h, a second solid-liquid separation is performed using a plate and frame filter press. Calcium ions are discarded as calcium carbonate, and the Ca in the water is removed. 2+ When the ion concentration is reduced to ≤3mg / L and the removal rate is >99.5%, qualified water is obtained. The qualified water is reused in the production system, and the filter residue (precipitates such as magnesium hydroxide, iron hydroxide, aluminum hydroxide, and calcium carbonate) is disposed of as waste.
[0025] In a specific implementation, the carbonate can be sodium carbonate or sodium bicarbonate.
[0026] Step (5): Saturated resin is leached with sulfuric acid solution as uranium leaching agent, and uranium leaching solution is obtained by single-tower leaching. The uranium leaching solution is then incorporated into the uranium extraction acid washing solution for reuse. In step (5), 5-20% sulfuric acid solution is used as uranium leaching agent for saturated resin. The amount of uranium leaching agent is about 5-20 times the volume of resin. Single tower leaching is performed. The leaching is stopped when the uranium concentration in the tail liquid is <0.1mg / L, resulting in high-concentration uranium leaching solution and saturated resin. The high-concentration uranium leaching solution is incorporated into the uranium extraction acid washing solution for reuse. The saturated resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 4-5 and the overall uranium recovery rate is >99%, at which point the washing is stopped.
[0027] Step (6): The saturated resin after uranium leaching is leached with ammonium solution as molybdenum leaching agent in a single tower to obtain molybdenum leaching solution and lean resin. The molybdenum leaching solution enters the molybdenum back-extraction agent preparation tank. In step (6), the saturated resin washed with qualified water is further washed with 10-20 wt% ammonia solution + 3-10 wt% ammonium sulfate solution as molybdenum leaching agent. The amount of molybdenum leaching agent is about 10-20 times the volume of the resin. The leaching is carried out in a single tower. The leaching is stopped when the molybdenum concentration in the tail liquid is <0.5 mg / L, resulting in a high-concentration molybdenum leaching solution and lean resin. The high-concentration molybdenum leaching solution is sent to the molybdenum stripping agent preparation tank for reuse as a molybdenum stripping agent. The lean resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 8-10 and the comprehensive molybdenum recovery rate is >99%, at which point the washing is stopped.
[0028] Step (7): The transforming agent is fed into the ion exchange tower to transform the lean resin. The transformation waste liquid is discharged from the bottom of the tower and returned to the eluent preparation tank. The transformed resin is reused to adsorb uranium and molybdenum. In step (7), a 2-5% sulfuric acid solution is prepared and fed into the ion exchange tower to transform the lean resin. The amount of transforming agent used is about 2 to 3 times the volume of the lean resin. The transformation waste liquid is discharged from the bottom of the tower and returned to the eluent preparation tank. After transformation, the resin is washed with the qualified water obtained in step (4) until the pH of the washing effluent is 6 to 7. The transformed resin is reused to adsorb uranium and molybdenum.
[0029] Example 1 Taking the mine fissure water of a primary uranium-molybdenum mine as an example, this invention provides a method for recovering uranium-molybdenum and removing other impurity ions from mine fissure water. This method recovers dissolved uranium-molybdenum resources from the mine fissure water and removes other impurity ions. The treated purified water and qualified water are then incorporated into the circulating water system of the process system. The specific steps are as follows: Step (1): The mine fissure water first passes through a sand filter tank and a self-cleaning filter with a filtration accuracy of 50μm to remove large particles, silt, organic matter, colloidal particles, microorganisms, etc., and then enters a granular activated carbon adsorption tank to remove fine organic matter and suspended particles in the water. Finally, it enters a precision filter with an accuracy of 10μm to obtain pretreated raw water. Step (2): The pretreated raw water is allowed to stand before being fed into a 0.1 μm ultrafiltration system to remove colloidal particles. The resulting ultrafiltration water is then further purified using a 5 nm spiral wound nanofiltration membrane element to remove U, Mo, and Ca. 2+ Mg 2 + Fe 3+ Al 3+ Purified water and concentrated water. Purified water conductivity <100 μS / cm; uranium concentration 1~2 μg / L (uranium rejection rate >99.7%); molybdenum concentration 0.01~0.07 mg / L (molybdenum rejection rate >99.6%); Ca... 2+ 1~3 mg / L, retention rate >99%; Mg 2+ 0.5~1 mg / L, retention rate >97.5%; Fe 3+ 0.01~0.1 mg / L, retention rate >99.6%, Al 3+ With a concentration of 0.1~1mg / L and a rejection rate of >99.9%, the purified water is used as boiler water and enters the production system. Step (3): After the concentrated water is recycled into the D231YT exchange resin exchange tower connected in series with two towers to adsorb uranium and molybdenum in the water, the adsorption time is controlled at 10 min. The adsorption is stopped when the uranium concentration in the adsorption tail liquid reaches 10 μg / L. The uranium recovery rate is >99.5%. At this time, the molybdenum in the solution is about 0.05 mg / L, and the molybdenum recovery rate is >99.9%. The adsorption tail liquid and saturated resin are obtained through adsorption. Step (4): The separated adsorption tail liquid enters the reaction tank, and the pH value of the material is adjusted to 8.0~8.5 using CaO and Ca(OH)2 for preliminary precipitation. After stirring for 1 hour, the first solid-liquid separation is performed using a plate and frame filter press. Mg 2+ Fe 3+ Al 3+ Magnesium hydroxide, iron hydroxide, and aluminum hydroxide precipitates are formed and disposed of as solid waste. Mg in the filtrate... 2+ Concentration 0.05~1 mg / L, removal rate >98.3%; Fe 3+Trace concentration, removal rate >99%, Al 3+ With a concentration of 0.05~0.5 mg / L, the removal rate is >99.9%. A 3 wt% carbonate solution is added to the filtrate, and after reacting for 1 hour, a second solid-liquid separation is performed using a plate and frame filter press. Calcium ions precipitate as calcium carbonate and are discarded. The Ca in the water... 2+ The ion concentration is reduced to 1~3 mg / L, the removal rate is >99.5%, and qualified water is obtained. The qualified water is reused in the production system, and the filter residue (precipitates such as magnesium hydroxide, iron hydroxide, aluminum hydroxide, and calcium carbonate) is disposed of as waste.
[0030] Step (5): Use 18-20 wt% sulfuric acid solution as uranium leaching agent for saturated resin. The amount of uranium leaching agent is about 6-8 times the volume of resin. Leaching is performed on a single tower. The leaching is stopped when the uranium concentration in the tail liquid reaches 0.08 mg / L. High-concentration uranium leaching solution and saturated resin are obtained. The high-concentration uranium leaching solution is incorporated into the uranium extraction acid washing solution for reuse. The saturated resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 4-5 and the overall uranium recovery rate is >99.1%. Then, washing is stopped.
[0031] Step (6): The saturated resin washed with qualified water is further washed with 18-20 wt% ammonia solution + 10 wt% ammonium sulfate as molybdenum leaching agent. The amount of molybdenum leaching agent is about 10-12 times the volume of the resin. The leaching is carried out in a single tower. The leaching is stopped when the molybdenum concentration in the tail liquid reaches 0.2 mg / L. A high-concentration molybdenum leaching solution and lean resin are obtained. The high-concentration molybdenum leaching solution is sent to the molybdenum stripping agent preparation tank for reuse as molybdenum stripping agent. The lean resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 9-10 and the comprehensive molybdenum recovery rate is >99.3%. The washing is then stopped.
[0032] Step (7): Prepare a 2-5% sulfuric acid solution and send it into the ion exchange tower to transform the lean resin. The amount of transforming agent used is about 3 times the volume of the lean resin. The transformed waste liquid is discharged from the bottom of the tower and returned to the eluent preparation tank. After transformation, the resin continues to be washed with the qualified water obtained in step (4) until the pH of the washing water is 6-7. The transformed resin is reused to adsorb uranium and molybdenum. The transforming agent and washing water are used to prepare the molybdenum eluent.
[0033] Example 2 Taking the fissure water of a primary uranium mine as an example, this invention provides a method for recovering uranium, molybdenum, and other impurity ions from fissure water. This method recovers dissolved uranium resources from the fissure water and removes other impurity ions. The treated purified water and qualified water are then incorporated into the circulating water system of the process system. The specific steps are as follows: Step (1): The mine fissure water first passes through a sand filter tank and a self-cleaning filter with a filtration accuracy of 200μm to remove large particles, silt, organic matter, colloidal particles, microorganisms, etc., and then enters a granular activated carbon adsorption tank to remove fine organic matter and suspended particles in the water. Finally, it enters a precision filter with an accuracy of 1μm to obtain pretreated raw water. Step (2): The pretreated raw water is fed into an ultrafiltration system with a precision of 0.001 μm after settling to remove colloidal particles. The resulting ultrafiltration water is then further purified using a spiral wound nanofiltration membrane element with a precision of 1 nm to remove U and Ca. 2+ Mg 2+ Fe 3+ Al 3+ Purified water and concentrated water. Purified water conductivity <100 μS / cm, uranium content 0.05~0.1 μg / L, uranium rejection rate >99.9%, Ca 2+ 1~2 mg / L, retention rate >99%; Mg 2+ 0.05~0.5 mg / L, retention rate >98.7%; Fe 3+ 0.01~0.05 mg / L, retention rate >99.6%, Al 3+ With a concentration of 0.01~0.2 mg / L and a rejection rate of >99.9%, the purified water can be used as boiler water in the production system. Step (3): After the concentrated water is recycled into the D382 exchange resin exchange tower connected in series with two towers to adsorb the uranium metal in the water, the adsorption time is controlled for 20 min. The adsorption is stopped when the uranium concentration in the adsorption tail liquid is >10 μg / L and the uranium recovery rate is >99%. The adsorption tail liquid and saturated resin are obtained through adsorption. Step (4): The separated adsorption tail liquid enters the reaction tank, and the pH value of the material is adjusted to 7.5~8.0 using carbide slag for preliminary sedimentation. After stirring for 1 hour, the first solid-liquid separation is carried out using a plate and frame filter press. Mg 2+ Fe 3+ Al 3+ Magnesium hydroxide, iron hydroxide, and aluminum hydroxide precipitates are formed and disposed of as solid waste. Mg in the filtrate... 2+ Concentration 0.05~0.1 mg / L, removal rate >99%; Fe 3+ 0.01~0.2 mg / L, removal rate >99.7%, Al 3+ Concentration 0.2~1 mg / L, removal rate >99.9%. An 8 wt% carbonate solution is added to the filtrate, and after reacting for 1 hour, a second solid-liquid separation is performed using a plate and frame filter press. Calcium ions are discarded as calcium carbonate, and the Ca in the water is removed. 2+The ion concentration is reduced to 1~2 mg / L, and the removal rate is >99.5%, resulting in qualified water. The qualified water is reused in the production system, while the filter residue (precipitates such as magnesium hydroxide, iron hydroxide, aluminum hydroxide, and calcium carbonate) is disposed of as waste.
[0034] Step (5): Use 5-8 wt% sulfuric acid solution as uranium leaching agent for saturated resin. The amount of uranium leaching agent is about 15-18 times the volume of resin. Leaching is performed on a single tower. The leaching is stopped when the uranium concentration in the tail liquid reaches 0.1 mg / L. High-concentration uranium leaching solution and saturated resin are obtained. The high-concentration uranium leaching solution is incorporated into the uranium extraction acid washing solution for reuse. The saturated resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 4-5 and the overall uranium recovery rate is >99.1%. Then, washing is stopped.
[0035] Step (6): Prepare a 2-5% sulfuric acid solution and send it into the ion exchange tower to transform the saturated resin after washing. The amount of transforming agent used is about twice the volume of the resin. The waste liquid from the transformation is discharged from the bottom of the tower and returned to the rinsing agent preparation tank. The transformed resin continues to be washed with the qualified water obtained in step (4) until the pH of the washing water is 6-7. The transformed resin is reused to adsorb uranium. The transforming agent and washing water are used to prepare uranium rinsing agent.
[0036] Example 3 Taking the mine fissure water of a molybdenum mine as an example, this invention provides a method for recovering uranium, molybdenum, and removing other impurity ions from mine fissure water. This method recovers dissolved molybdenum resources from the fissure water and removes other impurity ions. The treated purified water and qualified water are then incorporated into the circulating water system of the process system. The specific steps are as follows: Step (1): The mine fissure water first passes through a sand filter tank and a self-cleaning filter with a filtration accuracy of 100μm to remove large particles, silt, organic matter, colloidal particles, microorganisms, etc., and then enters a granular activated carbon adsorption tank to remove fine organic matter and suspended particles in the water. Finally, it enters a precision filter with an accuracy of 5μm to obtain pretreated raw water. Step (2): The pretreated raw water is allowed to stand before being fed into a 0.01 μm ultrafiltration system to remove colloidal particles. The resulting ultrafiltration water is then further purified using a 2 nm spiral wound nanofiltration membrane element to remove Mo and Ca. 2+ Mg 2+ Fe 3+ Al 3+ Purified water and concentrated water. Purified water conductivity <100μS / cm, molybdenum 0.01~0.03mg / L, molybdenum retention rate >99.8%, Ca... 2+ 2~3 mg / L, retention rate >99%; Mg 2+ 0.1~0.5 mg / L, retention rate >98%; Fe 3+0.01~0.05 mg / L, retention rate >99.9%, Al 3+ With a concentration of 0.1~0.5mg / L and a rejection rate of >99.9%, the purified water is used as boiler feed water and enters the production system. Step (3): After the concentrated water is recycled into the D314 exchange resin exchange tower connected in series to adsorb the molybdenum metal in the water, the adsorption time is controlled at 15 min. When the molybdenum concentration in the adsorption tail liquid is >0.1 mg / L and the molybdenum recovery rate is >99.9%, the adsorption tail liquid and saturated resin are obtained through adsorption. Step (4): The separated adsorption tail liquid enters the reaction tank, and the pH value of the material is adjusted to 8.2~8.5 using CaO and Ca(OH)2 for preliminary precipitation. After stirring for 1 hour, the first solid-liquid separation is performed using a plate and frame filter press. Mg 2+ Fe 3+ Al 3+ Magnesium hydroxide, iron hydroxide, and aluminum hydroxide precipitates are formed and disposed of as solid waste. Mg in the filtrate... 2+ Concentration 0.01~0.05 mg / L, removal rate >99%; Fe 3+ Trace concentration, removal rate >99%, Al 3+ Concentration 0.05~0.2 mg / L, removal rate >99.9%. A 5 wt% carbonate solution is added to the filtrate, and after a reaction of 0.5 h, a second solid-liquid separation is performed using a plate and frame filter press. Calcium ions precipitate as calcium carbonate and are discarded. The Ca in the water... 2+ The ion concentration is reduced to 1~2 mg / L, and the removal rate is >99.8%, resulting in qualified water. The qualified water is reused in the production system, while the filter residue (precipitates such as magnesium hydroxide, iron hydroxide, aluminum hydroxide, and calcium carbonate) is disposed of as waste.
[0037] Step (5): The saturated resin is further leached with 10-12 wt% ammonia solution + 3-5 wt% ammonium sulfate as molybdenum leaching agent. The amount of molybdenum leaching agent is about 18-20 times the volume of the resin. The leaching is carried out in a single tower. The leaching is stopped when the molybdenum concentration in the tail liquid reaches 0.5 mg / L. A high-concentration molybdenum leaching solution and lean resin are obtained. The high-concentration molybdenum leaching solution is sent to the molybdenum stripping agent preparation tank for reuse as a molybdenum stripping agent. The lean resin is washed with qualified water obtained in step (4) until the pH of the washing effluent is 8-9 and the comprehensive molybdenum recovery rate is >99.1%. The washing is then stopped.
[0038] Step (6): Prepare a 2-5% sulfuric acid solution and send it into the ion exchange tower to transform the lean resin. The amount of transforming agent used is about 3 times the volume of the lean resin. The transformed waste liquid is discharged from the bottom of the tower and returned to the washing agent preparation tank. After transformation, the resin continues to be washed with the qualified water obtained in step (4) until the pH of the washing water is 6~6.5. The transformed resin is reused to adsorb molybdenum. The transforming agent and washing water are used to prepare the molybdenum washing agent.
[0039] The present invention has been described in detail above with reference to the accompanying drawings and embodiments. However, the present invention is not limited to the above embodiments, and various changes can be made within the scope of knowledge possessed by those skilled in the art without departing from the spirit of the present invention. All contents not described in detail in the present invention can be derived from existing technologies.
Claims
1. A method for recovering uranium, molybdenum, and other impurity ions from mine fissure water, characterized in that, The method includes: Step (1): The mine fissure water is coarsely filtered through a sand filter tank and a self-cleaning filter, and then finely filtered through an activated carbon adsorption tank and a precision filter to obtain pretreated raw water. Step (2): The pretreated raw water is sent to the ultrafiltration system for treatment after being left to stand. The ultrafiltration water is sent to the material separation and treatment system for further purification to obtain concentrated water and purified water. The purified water is returned to the hydrometallurgical plant as boiler feed water. Step (3): After the concentrated water is recycled and enters the ion exchange tower to adsorb uranium and molybdenum in the water, the adsorption tail liquid and saturated resin are obtained. The adsorption tail liquid is returned to the storage tank for temporary storage. Step (4): Add precipitant to the adsorption tail liquid, precipitate and filter to obtain qualified water, and store the filter residue as tail waste. Step (5): Saturated resin is leached with sulfuric acid solution as uranium leaching agent, and uranium leaching solution is obtained by single-tower leaching. The uranium leaching solution is then incorporated into the uranium extraction acid washing solution for reuse. Step (6): The saturated resin after uranium leaching is leached with ammonium solution as molybdenum leaching agent in a single tower to obtain molybdenum leaching solution and lean resin. The molybdenum leaching solution enters the molybdenum back-extraction agent preparation tank. Step (7): The conversion agent is fed into the ion exchange tower to convert the lean resin. The conversion waste liquid is discharged from the bottom of the tower and returned to the eluent preparation tank. The converted resin is reused to adsorb uranium and molybdenum.
2. The method for recovering uranium, molybdenum, and other impurity ions from mine fissure water according to claim 1, characterized in that, In step (1), the sand filter tank and self-cleaning filter have a filtration accuracy of 50~200μm, removing large particles, silt, organic matter in water, colloidal particles, and microorganisms; the precision filter has an accuracy of 1~10μm, removing fine organic matter and suspended particles in water.
3. The method for recovering uranium, molybdenum, and other impurity ions from mine fissure water according to claim 1, characterized in that, In step (2), the ultrafiltration system has an accuracy of 0.001~0.1μm to remove colloidal particles; the material separation and processing system is a spiral wound nanofiltration membrane element with an accuracy of 1~5nm, resulting in a purified water conductivity of <100μS / cm and a uranium and molybdenum rejection rate of >99%.
4. The method for recovering uranium, molybdenum, and other impurity ions from mine fissure water according to claim 1, characterized in that, In step (3), anion exchange resin is used in the ion exchange tower. The anion exchange resin is D314, D231YT, or D382 macroporous weak base or strong base anion exchange resin.
5. The method for recovering uranium, molybdenum, and other impurity ions from mine fissure water according to claim 1, characterized in that, In step (3), the uranium concentration in the adsorption tail liquid is >10 μg / L and the uranium recovery rate is >99% when adsorption is stopped, or the molybdenum concentration in the solution is >0.1 mg / L and the molybdenum recovery rate is >99.9% when adsorption is stopped.
6. The method for recovering uranium, molybdenum, and other impurity ions from mine fracture water according to claim 1, characterized in that, In step (4), the precipitant is a calcium-based alkaline substance or carbonate; the calcium-based alkaline substance includes CaO, Ca(OH)2, and carbide slag.
7. The method for recovering uranium, molybdenum, and other impurity ions from mine fracture water according to claim 6, characterized in that, Step (4) includes: adding a calcium-containing alkaline substance to the adsorption tail liquid for primary precipitation, followed by filtration; adding a carbonate solution to the filtered filtrate for secondary precipitation, followed by filtration to obtain qualified water; during the primary precipitation, the pH value is adjusted to 7.5-8.5 using a calcium-containing alkaline substance, and the mixture is stirred for 0.5-1 hour, followed by a first solid-liquid separation using a plate and frame filter press, and the Mg in the filtrate is removed. 2+ Removal rate > 98.3%, Fe 3+ Removal rate > 99%, Al 3+ Removal rate > 99.9%; during secondary precipitation, the added carbonate solution concentration is 3wt%~8wt%, and after reacting for 0.5~1h, a second solid-liquid separation is performed using a plate and frame filter press to remove Ca from the water. 2+ When the ion concentration is reduced to ≤3mg / L, the removal rate is >99.5%.
8. The method for recovering uranium, molybdenum, and other impurity ions from mine fracture water according to claim 1, characterized in that, In step (5), the uranium leaching agent is a 5-20% sulfuric acid solution, and the overall uranium recovery rate is >99%.
9. The method for recovering uranium, molybdenum, and other impurity ions from mine fissure water according to claim 1, characterized in that, In step (6), the molybdenum leaching agent is 10-20 wt% ammonia solution + 3-10 wt% ammonium sulfate solution, and the overall molybdenum recovery rate is >99%.
10. The method for recovering uranium, molybdenum, and other impurity ions from mine fracture water according to claim 1, characterized in that, In step (7), the transforming agent is a 2-5% sulfuric acid solution. The transformed resin is washed with qualified water until the pH of the washing effluent is 6-7. The transformed resin is 100% reusable.