A method for separating and enriching rare earth element components in industrial and mining waste
By combining multi-stage roasting and acid leaching with chelating resin enrichment technology, the problem of separating and enriching rare earth elements in industrial and mining waste has been solved, achieving efficient separation and recycling. This technology is suitable for the resource utilization of wastes such as coal gangue and fly ash.
Patent Information
- Application Number
- CN202611173360.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-04
- Publication Date
- 2026-11-17
AI Technical Summary
How to efficiently separate and enrich rare earth element components in industrial and mining waste, especially to recover high-value metal resources from complex coal gangue and fly ash.
A multi-stage roasting and acid leaching combined with chelating resin enrichment technology is adopted, including first roasting, second roasting and third roasting, followed by acid leaching with acid solution, and then enrichment, elution, co-precipitation and acid dissolution through chelating resin, finally obtaining rare earth element components.
It achieves efficient separation and enrichment of rare earth elements in industrial and mining waste, with high leaching and recovery rates, making it suitable for the resource utilization of large quantities of industrial and mining waste and showing broad application prospects.
Smart Images

Figure CN123108330A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a method for separating and enriching rare earth element components in industrial and mining waste. Background Technology
[0002] Mining, smelting, and power generation are resource- and energy-intensive industries that consume large amounts of natural resources and various energy sources, resulting in a massive amount of solid waste. For example, coal gangue, fly ash, smelting slag, furnace slag, and tailings account for more than 60% of industrial solid waste.
[0003] In recent years, the demand for industrial and mining waste from the infrastructure industry has gradually decreased, leading to an overall decline in the utilization rate of such waste. Therefore, developing new ways to utilize industrial and mining waste resources is of great significance for resource utilization and industrial development.
[0004] To address the aforementioned issues, technicians have attempted to develop new methods. For example, some have used blast furnace slag to prepare microcrystalline glass. Others have proposed using coal gangue to replace coke in phosphate fertilizer production. In addition, how to utilize industrial and mining waste at a high value is a hot topic of interest for those skilled in the art, especially the recovery of high-value metal resources, such as rare earth elements. However, the complex composition of industrial and mining waste means that achieving efficient separation and recovery of rare earth elements remains a challenge for those in the field. Summary of the Invention
[0005] In view of this, the present invention provides a method for separating and enriching rare earth element components in industrial and mining waste. The separation and enrichment method provided by the present invention can effectively enrich rare earth element components in industrial and mining waste.
[0006] This invention provides a method for separating and enriching rare earth element components in industrial and mining waste, comprising the following steps: (1) The industrial and mining waste is roasted in sequence through a first roasting, a second roasting and a third roasting to obtain roasted material; (2) Mix the roasted material and acid solution for acid leaching, and separate the solid and liquid to obtain the acid leaching solution; (3) The acid leaching solution is enriched, eluted, co-precipitated, solid-liquid separated, acid-dissolved and precipitated through chelating resin to obtain rare earth element components.
[0007] Preferably, the industrial and mining waste includes coal gangue and fly ash; the mass ratio of coal gangue to fly ash is 100:25~30; and the particle size of the industrial and mining waste is 50~200 nanometers.
[0008] Preferably, the temperature of the first roasting is 180~210 degrees Celsius, and the time is 1~3 hours.
[0009] Preferably, the second roasting temperature is 450~550 degrees Celsius and the time is 1~3 hours.
[0010] Preferably, the third roasting temperature is 680~750 degrees Celsius and the time is 2~4 hours.
[0011] Preferably, after the third calcination, the resulting product is further subjected to sequential cooling, crushing and pulverizing; the target particle size of the pulverized product is 500~800 nanometers.
[0012] Preferably, the acid solution is a mixture of sulfuric acid, myristic acid and oxalic acid; the concentration of sulfuric acid in the acid solution is 2~4 mol / L; the concentration of myristic acid in the acid solution is 1~3 mol / L; and the concentration of oxalic acid in the acid solution is 0.5~1 mol / L.
[0013] Preferably, the mass ratio of the calcining material to the acid solution is 100:400~700.
[0014] Preferably, the acid leaching temperature is 70-90 degrees Celsius and the time is 2-5 hours.
[0015] Preferably, the acids used for acid dissolution are hydrochloric acid and oxalic acid; the volume ratio of hydrochloric acid to oxalic acid is 100:8~10.
[0016] Compared with the prior art, the present invention has achieved the following beneficial effects: The method for separating and enriching rare earth element components in industrial and mining waste provided by this invention achieves efficient separation and enrichment of rare earth element components in industrial and mining waste through close cooperation between each step and coordinated configuration of parameters in each step. It is suitable for large-volume industrial and mining wastes such as coal gangue, fly ash, steel slag, red mud and various tailings, and has broad application prospects. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of this invention, the accompanying drawings used in the embodiments of this invention or in the prior art are briefly described below. For those skilled in the art, other drawings can be derived from the following drawings without creative effort, and all such drawings are within the protection scope of this invention.
[0018] Figure 1 This is a schematic flowchart of the method for separating and enriching rare earth element components in industrial and mining waste provided by the present invention. Detailed Implementation
[0019] This invention provides a method for separating and enriching rare earth element components in industrial and mining waste, comprising the following steps: (1) The industrial and mining waste is roasted in sequence through a first roasting, a second roasting and a third roasting to obtain roasted material; (2) Mix the roasted material and acid solution for acid leaching, and separate the solid and liquid to obtain the acid leaching solution; (3) The acid leaching solution is enriched, eluted, co-precipitated, solid-liquid separated, acid-dissolved and precipitated through chelating resin to obtain rare earth element components.
[0020] This invention involves sequentially roasting industrial and mining waste through a first roasting, a second roasting, and a third roasting to obtain roasted material. In this invention, the industrial and mining waste may include coal gangue and fly ash; the mass ratio of coal gangue to fly ash may be 100:25~30, specifically 100:26, 100:27, 100:28, or 100:29.
[0021] In this invention, industrial and mining waste can be crushed and pulverized sequentially before use; the target particle size of the industrial and mining waste can be 50~200 nanometers, specifically 100~180 nanometers.
[0022] In this invention, the temperature of the first roasting can be 180~210 degrees Celsius, specifically 185 degrees Celsius, 190 degrees Celsius, 195 degrees Celsius, 200 degrees Celsius or 205 degrees Celsius, and the time can be 1~3 hours, specifically 1.5 hours, 2 hours or 2.5 hours.
[0023] In this invention, the temperature of the second roasting can be 450~550 degrees Celsius, specifically 460 degrees Celsius, 470 degrees Celsius, 480 degrees Celsius, 490 degrees Celsius, 500 degrees Celsius, 510 degrees Celsius, 520 degrees Celsius, 530 degrees Celsius or 540 degrees Celsius, and the time can be 1~3 hours, specifically 2 hours.
[0024] In this invention, the temperature of the third roasting can be 680~750 degrees Celsius, specifically 690 degrees Celsius, 700 degrees Celsius, 710 degrees Celsius, 720 degrees Celsius, 730 degrees Celsius or 740 degrees Celsius, and the time can be 2~4 hours, specifically 3 hours.
[0025] In this invention, the third calcination may further include sequentially cooling, crushing and pulverizing the resulting product; the target particle size of the pulverized product may be 500-800 nanometers, specifically 600 nanometers or 700 nanometers.
[0026] After obtaining the roasted material, the present invention mixes the roasted material with an acid solution for acid leaching, followed by solid-liquid separation to obtain an acid leaching solution. In the present invention, the acid solution can be a mixture of sulfuric acid, myristic acid, and oxalic acid; the concentration of sulfuric acid in the acid solution can be 2~4 mol / L, specifically 3 mol / L; the concentration of myristic acid in the acid solution can be 1~3 mol / L, specifically 2 mol / L; and the concentration of oxalic acid in the acid solution can be 0.5~1 mol / L, specifically 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, or 0.9 mol / L.
[0027] In this invention, the mass ratio of the calcining material to the acid solution can be 100:400~700, specifically 100:500 or 100:600.
[0028] In this invention, the acid leaching temperature can be 70-90 degrees Celsius, specifically 80 degrees Celsius or 85 degrees Celsius, and the time can be 2-5 hours, specifically 3 hours or 4 hours.
[0029] In this invention, solid-liquid separation can be achieved through filtration.
[0030] After obtaining the acid leaching solution, the present invention uses a chelating resin to enrich, elute, co-precipitate, separate solids and liquids, dissolve in acid, and precipitate the solution to obtain rare earth element components. In the present invention, the chelating resin can be an iminodiacetic acid (IDA)-based chelating resin.
[0031] In this invention, the enrichment temperature can be 40-55 degrees Celsius, specifically 45 degrees Celsius or 50 degrees Celsius, the loading speed can be 1-2 times the resin volume / hour, and the column pass method can be bottom in and top out.
[0032] In this invention, the elution reagent can be water; the elution temperature can be 50-55 degrees Celsius, specifically 53 degrees Celsius; the elution rate can be 0.5-1 times the resin volume / hour; and the column pass method can be top-in, bottom-out.
[0033] In this invention, the pH value of coprecipitation can be 5 to 7, specifically 6, and the time can be 0.3 to 3 hours, specifically 0.5 hours, 1 hour, or 2 hours.
[0034] In this invention, solid-liquid separation can be achieved through filtration. This invention obtains a co-precipitated solid through solid-liquid separation.
[0035] In this invention, the acid used for acid dissolution can be hydrochloric acid and oxalic acid; the volume ratio of hydrochloric acid to oxalic acid can be 100:8~10, specifically 100:9; the mass ratio of the coprecipitated solid to the acid used for acid dissolution can be 100:300~500, specifically 100:400.
[0036] In this invention, the precipitation temperature can be 26~35 degrees Celsius, specifically 30 degrees Celsius; the pH value can be 11~12, specifically 11.5; and the precipitation time can be 1~5 hours, specifically 2 hours, 3 hours, or 4 hours.
[0037] In this invention, after precipitation, the process may further include washing the resulting system after solid-liquid separation; the solid-liquid separation may be filtration; and the washing reagent may be distilled water.
[0038] To further illustrate the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings and embodiments.
[0039] Example 1: This embodiment describes the separation and enrichment of rare earth element components in industrial and mining waste. The process flow is as follows: Figure 1 As shown, the specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 185 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0040] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0041] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Afterward, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 1 hour. After filtration, the co-precipitated solid was obtained. The co-precipitated solid was dissolved in a 100:10 mixture of hydrochloric acid and oxalic acid (volume ratio), with a mass ratio of 100:400 between the co-precipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 32°C and pH 12 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0042] Example 2: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 195 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0043] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0044] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Afterward, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 1 hour. After filtration, the co-precipitated solid was obtained. The co-precipitated solid was dissolved in a mixture of hydrochloric acid and oxalic acid at a volume ratio of 100:10, with a mass ratio of 100:400 between the co-precipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 26°C and pH 11 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0045] Example 3: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 180 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0046] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0047] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 0.5 hours. After filtration, the coprecipitated solid was obtained. The coprecipitated solid was dissolved in hydrochloric acid and oxalic acid at a volume ratio of 100:8, with a mass ratio of 100:400 between the coprecipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 35°C and pH 12 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0048] Example 4: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 210 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0049] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0050] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 0.5 hours. After filtration, the coprecipitated solid was obtained. The coprecipitated solid was dissolved in hydrochloric acid and oxalic acid at a volume ratio of 100:8, with a mass ratio of 100:400 between the coprecipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 32°C and pH 12 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0051] Example 5: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 200 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0052] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0053] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 0.3 hours. After filtration, the coprecipitated solid was obtained. The coprecipitated solid was dissolved in a mixture of hydrochloric acid and oxalic acid at a volume ratio of 100:10, with a mass ratio of 100:400 between the coprecipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 32°C and pH 11 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0054] Example 6: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 205 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0055] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0056] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 1 hour. After filtration, the co-precipitated solid was obtained. The co-precipitated solid was dissolved in hydrochloric acid and oxalic acid at a volume ratio of 100:9, with a mass ratio of 100:400 between the co-precipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 27°C and pH 11 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0057] Example 7: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 195 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0058] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0059] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 0.3 hours. After filtration, the coprecipitated solid was obtained. The coprecipitated solid was dissolved in hydrochloric acid and oxalic acid at a volume ratio of 100:9, with a mass ratio of 100:400 between the coprecipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 29°C and pH 12 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0060] Example 8: This embodiment separates and enriches rare earth element components in industrial and mining waste. The specific steps are as follows: (1) The industrial and mining waste (coal gangue and fly ash with a mass ratio of 100:27) is crushed and pulverized to a particle size of 100~180 nanometers. It is first roasted at 200 degrees Celsius for 2 hours, then roasted at 500 degrees Celsius for 2 hours, and then roasted at 715 degrees Celsius for 3 hours. After cooling, it is crushed and pulverized to a particle size of 500~800 nanometers to obtain roasted material.
[0061] (2) Sulfuric acid, myristic acid and oxalic acid were mixed to obtain an acid solution with a sulfuric acid concentration of 3 mol / L, a myristic acid concentration of 2 mol / L and an oxalic acid concentration of 0.7 mol / L. The prepared roasting material and the acid solution were mixed with a mass ratio of 100:600. The mixture was acid-leached at 80 degrees Celsius for 4 hours and then filtered to obtain an acid leaching solution.
[0062] (3) The obtained acid leaching solution was enriched by passing it through an iminodiacetic acid chelating resin at 45°C. The loading rate was 2 times the resin volume / hour, and the column chromatography was bottom-in, top-out. Then, it was eluted with distilled water at 53°C at a rate of 0.5 times the resin volume / hour, using a top-in, bottom-out column chromatography. The pH of the system was adjusted to 6 with sodium carbonate, and co-precipitation was carried out for 0.5 hours. After filtration, the coprecipitated solid was obtained. The coprecipitated solid was dissolved in hydrochloric acid and oxalic acid at a volume ratio of 100:9, with a mass ratio of 100:400 between the coprecipitated solid and the acids (hydrochloric acid and oxalic acid). The precipitation reaction was carried out at 29°C and pH 11 for 3 hours, followed by filtration and washing with distilled water to obtain the rare earth element components.
[0063] Comparative Example 1: The preparation method of this comparative example is the same as that of Example 1, except that the mass ratio of coal gangue to fly ash is 100:50.
[0064] Comparative Example 2: The preparation method of this comparative example is the same as that of Example 1, except that fly ash is replaced with an equal mass of coal gangue.
[0065] Comparative Example 3: The preparation method of this comparative example is the same as that of Example 1, except that: it is directly calcined at 500 degrees Celsius for 2 hours, and then calcined at 715 degrees Celsius for 3 hours, without calcining at 185 degrees Celsius for 2 hours (the first calcination is omitted).
[0066] Comparative Example 4: The preparation method of this comparative example is the same as that of Example 1, except that: it is first calcined at 185 degrees Celsius for 2 hours, then calcined at 715 degrees Celsius for 3 hours, and the second calcination is omitted (the second calcination is omitted).
[0067] Comparative Example 5: The preparation method of this comparative example is the same as that of Example 1, except that: it is first calcined at 185 degrees Celsius for 2 hours, then calcined at 500 degrees Celsius for 2 hours, and calcined at 715 degrees Celsius for 3 hours (the third calcination is omitted).
[0068] Comparative Example 6: The preparation method of this comparative example is the same as that of Example 1, except that myristic acid and oxalic acid are replaced with equimolar amounts of sulfuric acid.
[0069] Comparative Example 7: The preparation method of this comparative example is the same as that of Example 1, except that myristic acid is replaced with an equimolar amount of oxalic acid.
[0070] Comparative Example 8: The preparation method of this comparative example is the same as that of Example 1, except that oxalic acid is replaced with an equimolar amount of myristic acid.
[0071] Comparative Example 9: The preparation method of this comparative example is the same as that of Example 1, except that sulfuric acid and oxalic acid are replaced with equal masses of myristic acid.
[0072] Test Example 1: The recovery effect of rare earth element components in Examples 1-8 and Comparative Examples 1-9 was tested, and the test results are shown in Table 1.
[0073] Table 1. Recovery efficiency of rare earth element components in Examples 1-8 and Comparative Examples 1-9:
[0074] As shown in Table 1, the separation and enrichment method provided by this invention can efficiently separate and enrich rare earth element components in industrial and mining waste, with high leaching and recovery rates. This is attributed to the coordination and parameter control of each step in this invention, especially the multi-stage roasting and the synergistic effect of sulfuric acid, myristic acid, and oxalic acid in the acid solution. The separation and enrichment method provided by this invention has controllable costs and is promising for industrial-scale production.
[0075] The embodiments of the present invention have been described above; however, these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. All other embodiments obtained by those skilled in the art based on the above embodiments of the present invention without inventive effort are within the protection scope of the present invention.
Claims
1. A method for separating and enriching rare earth element components in industrial and mining waste, characterized in that, Includes the following steps: (1) The industrial and mining waste is roasted in sequence through a first roasting, a second roasting and a third roasting to obtain roasted material; (2) Mix the roasted material and acid solution for acid leaching, and separate the solid and liquid to obtain the acid leaching solution; (3) The acid leaching solution is enriched, eluted, co-precipitated, solid-liquid separated, acid-dissolved and precipitated through chelating resin to obtain rare earth element components.
2. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, Industrial and mining waste includes coal gangue and fly ash; the mass ratio of coal gangue to fly ash is 100:25~30; the particle size of industrial and mining waste is 50~200 nanometers.
3. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The first roasting temperature is 180~210 degrees Celsius, and the time is 1~3 hours.
4. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The second roasting temperature is 450~550 degrees Celsius, and the time is 1~3 hours.
5. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The third roasting temperature is 680~750 degrees Celsius, and the time is 2~4 hours.
6. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The third roasting process includes sequentially cooling, crushing, and pulverizing the resulting product; the target particle size for pulverization is 500-800 nanometers.
7. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The acid solution is a mixture of sulfuric acid, myristic acid, and oxalic acid; the concentration of sulfuric acid in the acid solution is 2~4 mol / L; the concentration of myristic acid in the acid solution is 1~3 mol / L; and the concentration of oxalic acid in the acid solution is 0.5~1 mol / L.
8. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The mass ratio of roasting material to acid solution is 100:400~700.
9. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The acid leaching temperature is 70-90 degrees Celsius, and the time is 2-5 hours.
10. The method for separating and enriching rare earth element components in industrial and mining waste according to claim 1, characterized in that, The acids used for acid dissolution are hydrochloric acid and oxalic acid; the volume ratio of hydrochloric acid to oxalic acid is 100:8~10.