High-strength, high-ductility aluminum bronze and its preparation method
By introducing trace amounts of V microalloying and cryogenic treatment into aluminum bronze, combined with adaptive cooling rate control, the problem of traditional aluminum bronze being unable to balance high strength and high plasticity has been solved. A high-strength, high-plasticity aluminum bronze material suitable for extreme working conditions has been prepared, exhibiting excellent wear resistance and corrosion resistance.
Patent Information
- Application Number
- CN202611059264.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-16
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional aluminum bronze materials struggle to balance high strength and high plasticity, and suffer from casting defects such as porosity and air bubbles, resulting in insufficient plasticity and fatigue strength. Existing processes are costly and require large equipment investments, making it difficult to meet the demands of extreme working conditions.
By introducing trace amounts of V microalloying into Cu-Al-Fe alloys and then subjecting them to cryogenic treatment after quenching, high-strength and high-ductility aluminum bronzes were prepared by rationally controlling the V content and cryogenic parameters, combined with an adaptive cooling rate control method to suppress plasticity loss.
Aluminum bronze material with both high strength (≥700MPa) and high plasticity (elongation ≥33%) has been developed, which significantly improves wear resistance and corrosion resistance. It is suitable for extreme working conditions such as aero engines and gas turbines, and its cost is controllable, making it suitable for industrial promotion.
Smart Images

Figure CN123108341A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of copper alloy materials technology, and more specifically, relates to a high-strength, high-ductility aluminum bronze and its preparation method. Background Technology
[0002] Aluminum bronze, due to its high strength, excellent wear resistance, and good corrosion resistance, is widely used in key components of aero engines, gas turbines, water pumps, heavy machinery, and marine engineering equipment. As modern industry moves towards extreme operating conditions such as high speed, high pressure, high temperature, and corrosive media, higher demands are placed on the comprehensive performance of aluminum bronze materials, especially in maintaining high strength while also possessing high plasticity, excellent wear resistance, and corrosion resistance.
[0003] Traditional cast aluminum bronze inevitably suffers from casting defects such as porosity, gas bubbles, and compositional segregation, resulting in insufficient plasticity and fatigue strength. To improve these defects, the industry typically employs forging processes; however, simple forging, without matching alloy composition and heat treatment processes, still struggles to achieve ideal performance. Several aluminum bronzes and their preparation methods have been disclosed in the prior art. Patent CN103882254A discloses a method for producing continuously cast aluminum bronze pipes, using cryolite covering agents for melting. However, this method only involves continuous casting, failing to eliminate defects such as porosity and gas bubbles within the ingot, resulting in low material plasticity and toughness. Patent CN1439734A discloses a copper alloy process route of "casting → homogenization → hot working → solution treatment → aging," but its alloy system is Cu-Ag-Cr, primarily targeting high-conductivity applications. This differs fundamentally from the strengthening mechanism and application requirements of high-wear-resistant aluminum bronze, and the process is not optimized for the high-temperature plasticity characteristics of aluminum bronze. Patent CN110284025A achieved a high strength of 600-850 MPa by adding various microalloying elements such as Ni, Cr, Nb, Ti, and Ce. However, the elongation of the aluminum bronze prepared by this method is only 5-15%, and the Al content is low (4-8%). The microstructure is mainly α phase, which limits the wear resistance. At the same time, this patent uses vacuum melting, which requires large equipment investment and has high production costs, making it unfavorable for industrial promotion. Summary of the Invention
[0004] To address the aforementioned deficiencies or improvement needs of existing technologies, this invention provides a high-strength, high-ductility aluminum bronze and its preparation method. Addressing the problem of traditional aluminum bronze's difficulty in simultaneously achieving high strength and high ductility, as well as insufficient wear resistance and corrosion resistance, this invention introduces trace amounts of v (V) microalloying into a Cu-Al-Fe alloy and incorporates a cryogenic treatment process after quenching and before tempering, enabling v and cryogenic treatment to synergistically strengthen the bronze. By rationally controlling the v content and cryogenic parameters, and establishing a cooling rate control method that adaptively matches the v content with the billet size, the loss of ductility caused by v addition is effectively suppressed. The aluminum bronze prepared by this invention exhibits high tensile strength, good ductility, and excellent wear resistance and corrosion resistance, breaking through the technical bottleneck of traditional aluminum bronze's high strength and low ductility. This invention features a simple process, controllable cost, and is suitable for critical components under extreme operating conditions in aero-engines, gas turbines, heavy machinery, and marine engineering equipment.
[0005] To achieve the above objectives, according to one aspect of the present invention, a method for preparing high-strength, high-ductility aluminum bronze is provided, comprising the following steps: S100: Weigh the furnace charge according to the target proportion. The furnace charge includes electrolytic copper, pure iron, pure aluminum, cryolite, and copper-vanadium master alloy. Add electrolytic copper and pure iron to a melting vessel and melt them. After the pure iron dissolves, add the copper-vanadium master alloy, followed by pure aluminum for alloying. Take samples for spectral analysis to ensure that the Al, Fe, and V contents are within the target range, with fluctuations allowed at ±0.2%. Sprinkle cryolite evenly onto the surface of the melt for refining. After melting, cast the ingot. S200: The obtained ingot is subjected to homogenization annealing, stress-relief annealing, quenching, cryogenic treatment, and tempering in sequence; the cryogenic treatment is performed after quenching and before tempering, with a treatment temperature of -196 ℃ to -150 ℃ and a holding time of 6 hours to 12 hours; the actual cooling rate of the cryogenic treatment is determined according to the following formula:
[0006] Where v is the actual cooling rate, v0 is the reference cooling rate, and k V C is the correction factor for V content. V For the measured V content, D0 is the reference billet diameter, D is the actual billet equivalent diameter, and k D This is the size sensitivity coefficient; S300: The processed billet is heated before forging and then forged. The forging process involves multiple forging passes, followed by air cooling, ultimately yielding high-strength and high-ductility aluminum bronze.
[0007] Preferably, in step S100, the amount of cryolite used is 400 g to 500 g when the alloy ingot is 100 kg.
[0008] Preferably, in step S100, the alloying temperature is 1200 ℃~1250 ℃, and the spectral analysis temperature is 1120 ℃~1180 ℃.
[0009] Preferably, in step S200, the homogenization annealing temperature is 700 ℃~750 ℃, and the time is 5 hours~8 hours.
[0010] Preferably, in step S200, the stress-relief annealing temperature is 400 ℃~500 ℃ and the time is 2 hours~6 hours.
[0011] Preferably, in step S200, the quenching temperature is 850 ℃~950 ℃ and the time is 2 hours~4 hours.
[0012] Preferably, in step S200, the tempering temperature is 450 ℃~500 ℃ and the time is 2 hours~4 hours.
[0013] Preferably, in step S300, the billet is heated to a temperature of 920°C to 950°C before forging, and the holding time is 12 hours to 20 hours.
[0014] Preferably, in step S300, during the forging process, the initial forging temperature is 910 ℃~920 ℃ and the final forging temperature is 850 ℃~860 ℃.
[0015] According to a second aspect of the present invention, a high-strength, high-ductility aluminum bronze is provided, prepared by the method described above, wherein the alloy composition of the high-strength, high-ductility aluminum bronze is as follows by mass percentage: Al 8.5%-11.0%, Fe 2.0%-4.0%, V 0.10%-0.20%, with the balance being Cu and unavoidable impurities.
[0016] In summary, compared with the prior art, the above-described technical solutions conceived by this invention can achieve the following beneficial effects: 1. This invention, through the synergistic effect of V-microalloying and cryogenic treatment, achieves high strength (≥700MPa) while maintaining high plasticity (elongation ≥33%), successfully overcoming the technical contradiction of traditional aluminum bronze: "high strength equals low plasticity, and good plasticity equals insufficient strength." Traditional aluminum bronze either lacks sufficient strength to meet load-bearing requirements or has low plasticity to withstand impact loads. This invention, however, combines high strength with good plastic deformation capacity, simultaneously meeting the application requirements of both high load-bearing capacity and high toughness. Its comprehensive mechanical properties are significantly superior to those of traditional materials.
[0017] 2. This invention significantly improves the surface hardness and wear resistance of the alloy through the formation of the hard phase in V and the densification brought about by cryogenic treatment. The wear rate is significantly reduced compared to traditional aluminum bronze, effectively extending the service life of bearings, bushings, gears, and other components under friction conditions. Simultaneously, the corrosion rate of this invention is much lower than that of traditional materials, the pitting potential shifts significantly to a positive value, the passivation film is more stable, and the resistance to localized corrosion is stronger. In highly corrosive environments such as marine engineering, shipbuilding, and seawater pumps and valves, it can maintain a longer effective service life, significantly reducing the risk of failure and maintenance costs caused by wear and corrosion.
[0018] 3. This invention employs atmospheric pressure melting combined with cryolite refining, eliminating the need for vacuum equipment. Its investment and operating costs are significantly lower than vacuum melting processes, facilitating large-scale industrial application. Furthermore, the adaptive cooling method for cryogenic treatment proposed in this invention automatically adjusts process parameters based on compositional fluctuations and billet size variations across different batches. This maximizes processing efficiency while preventing cracking, overcoming the shortcomings of traditional fixed-parameter processes such as narrow process windows and low yields. It exhibits excellent process stability and scalable production prospects, providing a stable and scalable material and process foundation for the preparation of critical components under extreme operating conditions, such as those for aero-engines, gas turbines, heavy machinery, and marine engineering equipment. Attached Figure Description
[0019] Figure 1 This is a process flow diagram of high-strength, high-ductility aluminum bronze according to an embodiment of the present invention; Figure 2 This is a schematic diagram illustrating the effect of V content on the tensile strength of aluminum bronze in an embodiment of the present invention; Figure 3 This is a schematic diagram illustrating the effect of V content on the elongation of aluminum bronze in an embodiment of the present invention. Figure 4 This is a finished product image of a precision mold made from high-strength, high-ductility aluminum bronze according to an embodiment of the present invention. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.
[0021] This invention provides a high-strength, high-ductility aluminum bronze and its preparation method. The alloy composition of the high-strength, high-ductility aluminum bronze has the following mass percentages: Al 8.5%-11.0%, Fe 2.0%-4.0%, V 0.10%-0.20%, with the balance being Cu and unavoidable impurities. The method includes the following steps: S100: Based on the preparation of 100 kg alloy ingots, weigh the furnace charge according to the target proportions. The furnace charge includes electrolytic copper, pure iron, pure aluminum, cryolite, and copper-vanadium master alloy (CuV10, V content 10 wt%). Add electrolytic copper and pure iron to a melting vessel and heat to 1220-1250 ℃ to melt. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to 1160 ℃, add pure aluminum, and then heat to 1200-1250 ℃ for alloying. Take samples at 1120-1180 ℃ for pre-furnace spectral analysis to ensure that the Al, Fe, and V contents are within the target range, with an allowable fluctuation of ±0.2%. After confirming the composition is qualified, evenly sprinkle 400 g-500 g of cryolite onto the surface of the melt for refining, and allow it to stand to remove slag. Adjust the melt temperature to 1150 ℃, pour it into a preheated mold at a pouring temperature of 1100-1180 ℃, and air cool to obtain an ingot; S200: The obtained ingot is processed sequentially as follows: (1) Homogenize and anneal at 700-750 ℃, hold for 5-8 hours, and then furnace cool to below 300 ℃; (2) Stress-reducing annealing at 400-500 ℃, holding for 2-6 hours, and then cooling with the furnace; (3) Quench at 850-950 ℃, hold for 2-4 hours, then water quench; (4) Cryogenic treatment: Performed after quenching and before tempering, with a treatment temperature of -196 ℃ to -150 ℃ and a holding time of 6-12 hours; the cooling rate v of the cryogenic treatment is determined according to the following formula:
[0022] Where v is the actual cooling rate, v0 is the reference cooling rate, and k V C is the correction factor for V content. V The measured V content (wt%) is given, D0 is the reference billet diameter, D is the actual billet equivalent diameter, and k is the value of k. D The equivalent diameter D is determined based on the principle of volume equivalence. For non-cylindrical blanks, D = (6V / π)^(1 / 3), where V is the actual volume of the blank. v0 = 1℃ / min, D0 = 100mm, k V =2.5, k D =0.3. k V The value of k is based on a comprehensive fit between the theoretical model and experimental data on the effect of V content on the thermal conductivity of the alloy. When the V content deviates from the benchmark value by 0.15%, the critical cooling rate needs to be adjusted accordingly. V =2.5 is the correction factor determined by linear regression analysis of the critical cooling rate data of multiple samples with different V contents; k DThe value of k is based on the physical law of the influence of billet size on thermal stress in heat transfer. The larger the equivalent diameter of the billet, the more significant the temperature gradient between the surface and the core, and the lower the required cooling rate. D =0.3 is the size sensitivity coefficient determined after heat transfer theory calculation and experimental verification; S300: The heat-treated billet is heated to 920-950 ℃, held for 12-20 hours, and then forged in multiple passes. The initial forging temperature is 910-920 ℃, the final forging temperature is 850-860 ℃, and the forging passes are 3-5 times. After forging, it is air-cooled to finally obtain high-strength and high-ductility aluminum bronze.
[0023] Adding trace amounts of vanadium (V) to aluminum bronze can significantly improve the alloy's strength, but it also leads to decreased hot working plasticity and an increased risk of forging cracks. To resolve the technical contradiction of achieving both high strength and high plasticity, this invention introduces cryogenic treatment into the heat treatment process. Experiments have shown that after cryogenic treatment, the tensile strength of V-containing aluminum bronze increased from 695 MPa to 723 MPa, while the elongation remained above 34%, essentially equivalent to that of untreated V-containing aluminum bronze (35.0%), effectively suppressing the plasticity loss caused by V addition.
[0024] Furthermore, during cryogenic treatment, it was found that when the billet is rapidly cooled from the quenching temperature to -196 ℃ to -150 ℃, a significant temperature gradient is generated between the surface and the core of the billet, which in turn causes thermal stress. When the cooling rate is too fast, the thermal stress exceeds the tensile strength of the material, which can lead to microcracks in the billet, and in severe cases, even cracking. When the cooling rate is too slow, although cracking can be avoided, the processing cycle will be prolonged, production efficiency will be reduced, and costs will be increased. Through a large number of experiments, it has been found that the V content and billet size are the key factors affecting the magnitude of thermal stress. A fixed cooling rate cannot be used, but should be adaptively adjusted according to the measured V content and billet size. Based on this, the present invention proposes an adaptive cooling rate calculation formula as shown in equation (1). In the formula, v0 is the baseline cooling rate (the optimal value when V=0.15% and D=100 mm), k V k is the V content correction factor (reflecting the degree of influence of V content changes on the cooling rate). D This is a size sensitivity coefficient used to adjust the cooling rate inversely based on the deviation between the measured V content and the benchmark value (0.15%) (reducing the rate when the V content is too high and increasing the rate when the V content is too low). Using this formula, the optimal cooling rate can be calculated in real time based on the actual V content and billet size, maximizing processing efficiency while avoiding cracking.
[0025] In the following examples, v0 = 1℃ / min and k are all taken as... V =2.5, k D =0.3, D0=100mm are used as examples for illustration.
[0026] The following detailed description of the solution described in this application will be provided in conjunction with specific embodiments. Example 1
[0027] (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 9.5%, Fe 2.5%, V 0.10%, with the balance being Cu and unavoidable impurities.
[0028] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Heat to 1220 ℃ to fully melt and alloy them. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to approximately 1160 ℃, quickly add the pure aluminum block, and then heat to 1200 ℃, stirring thoroughly to ensure uniform alloying. Take a concave sample at 1120 ℃ and perform pre-furnace spectral analysis to measure C. V =0.10%. Sprinkle 400 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload from the furnace.
[0029] (3) Preheat the ingot mold, and pour the melt at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1100 ℃. After pouring, allow the ingot to cool naturally to room temperature in the air, resulting in a billet with dimensions of approximately 410 mm × 180 mm × 205 mm. According to the principle of volume equivalence, D = (6V / π). 1 / 3 The equivalent diameter D is calculated to be 150 mm.
[0030] (4) The obtained ingot is homogenized and annealed, and the furnace temperature is raised to 700 ℃ and held for 5 hours. Then the furnace is cooled to below 300 ℃ before being taken out of the furnace.
[0031] (5) Stress-relief annealing is performed on the ingot by heating to 400 ℃, holding for 2 hours, and then cooling in the furnace. Finally, quenching and aging are performed by heating to 850 ℃, holding for 2 hours, and then water quenching.
[0032] (6) The water-quenched billet is subjected to cryogenic treatment. The equivalent diameter D of the billet is 150 mm. The cooling rate of the cryogenic treatment is calculated according to the following formula:
[0033] The calculated cooling rate was 1.00 ℃ / min. The water-quenched billet was cooled to -150 ℃ at a cooling rate of 1.00 ℃ / min, held at that temperature for 6 hours, and then slowly warmed back to room temperature at a heating rate of 0.5 ℃ / min. Finally, it was tempered at 450 ℃ for 2 hours.
[0034] (7) Before forging, heat the treated billet to 920 ℃ and hold it for 12 hours. The initial forging temperature is 910 ℃, then it is pressed three times, and the final forging temperature is 850 ℃. After forging, it is air-cooled and tested. Example 2
[0035] (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 9.8%, Fe 2.6%, V 0.12%, with the balance being Cu and unavoidable impurities.
[0036] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Heat to 1220 °C to fully melt and alloy them. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to approximately 1160 °C, and quickly add the pure aluminum block while immersing it in the molten copper to prevent oxidation. Then heat to 1210 °C and stir thoroughly to ensure uniform alloying. Take a concave sample at 1140 °C and perform pre-furnace spectral analysis to measure C. V =0.12%. Sprinkle 420 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload from the furnace.
[0037] (3) Preheat the ingot mold and pour the molten material at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1120 ℃. After pouring, allow the ingot to cool naturally to room temperature in the air.
[0038] (4) The obtained ingot is homogenized and annealed, and the furnace temperature is raised to 720 °C and held for 6 hours. Then the furnace is cooled to below 300 °C before being taken out of the furnace.
[0039] (5) Stress-relief annealing is performed on the ingot by heating to 430 ℃, holding for 3 hours, and then cooling in the furnace. Finally, quenching and aging are performed by heating to 880 ℃, holding for 2 hours, and then water quenching.
[0040] (6) The water-quenched billet is subjected to deep cryogenic treatment. The equivalent diameter D of the billet is 150 mm. According to formula (1), v = 0.95 ℃ / min is calculated. The billet is cooled to -160 ℃ at a cooling rate of 0.95 ℃ / min and held for 7 hours. Then, it is slowly warmed back to room temperature at a heating rate of 1 ℃ / min and then tempered at 460 ℃ for 3 hours.
[0041] (7) Before forging, heat the treated billet to 935 ℃ and hold it for 14 hours. The initial forging temperature is 910 ℃, then it is pressed three times, and the final forging temperature is 855 ℃. After forging, it is air-cooled and tested. Example 3
[0042] (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 10.1%, Fe 2.8%, V 0.14%, with the balance being Cu and unavoidable impurities.
[0043] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Heat to 1220 ℃ to fully melt and alloy them. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to approximately 1160 ℃, and quickly add the pure aluminum block immersed in the copper liquid to prevent oxidation. Then heat to 1225 ℃ and stir thoroughly to ensure uniform alloying. Take a concave sample at 1160 ℃ and perform pre-furnace spectral analysis to measure C. V =0.14%. Sprinkle 440 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload from the furnace.
[0044] (3) Preheat the ingot mold, and pour the molten material at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1140 ℃. After pouring, allow the ingot to cool naturally to room temperature in the air.
[0045] (4) The obtained ingot is homogenized and annealed, heated to 730 °C in the furnace, held for 7 hours, and then cooled to below 300 °C before being taken out of the furnace.
[0046] (5) Stress-relief annealing is performed on the ingot by heating to 480 ℃, holding for 4 hours, and then cooling in the furnace. Finally, quenching and aging are performed by heating to 900 ℃, holding for 3 hours, and then water quenching.
[0047] (6) The billet after water quenching is subjected to deep cryogenic treatment. The equivalent diameter D of the billet is 150 mm. According to formula (1), v = 0.91 ℃ / min is calculated. The billet is cooled to -170 ℃ at a cooling rate of 0.91 ℃ / min and held for 9 hours. Then, it is slowly warmed back to room temperature at a heating rate of 1.5 ℃ / min and then tempered at 470 ℃ for 2 hours.
[0048] (7) Before forging, heat the treated billet to 940 ℃ and hold it for 16 hours. The initial forging temperature is 920 ℃, then it is pressed four times, and the final forging temperature is 855 ℃. After forging, it is air-cooled and tested. Example 4
[0049] (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 10.4%, Fe 2.9%, V 0.18%, with the balance being Cu and unavoidable impurities.
[0050] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Heat to 1220 ℃ to fully melt and alloy them. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to approximately 1160 ℃, and quickly add the pure aluminum block immersed in the copper liquid to prevent oxidation. Then heat to 1235 ℃ and stir thoroughly to ensure uniform alloying. Take a concave sample at 1180 ℃ and perform pre-furnace spectral analysis to measure C. V =0.18%. Sprinkle 480 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let it stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload the furnace.
[0051] (3) Preheat the ingot mold, and pour the melt at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1160 ℃. After pouring, allow the ingot to cool naturally to room temperature in the air.
[0052] (4) The obtained ingot is homogenized and annealed, heated to 740 ℃ in the furnace, held for 8 hours, and then cooled to below 300 ℃ before being taken out of the furnace.
[0053] (5) Stress-relief annealing is performed on the ingot by heating to 500 ℃, holding for 5 hours, and then cooling in the furnace. Finally, quenching and aging are performed by heating to 920 ℃, holding for 3 hours, and then water quenching.
[0054] (6) The water-quenched billet is subjected to deep cryogenic treatment. The equivalent diameter D of the billet is 150 mm. According to formula (1), v = 0.82 ℃ / min is calculated. The billet is cooled to -180 ℃ at a cooling rate of 0.82 ℃ / min and held for 10 hours. Then, it is slowly warmed back to room temperature at a heating rate of 2 ℃ / min and then tempered at 480 ℃ for 4 hours.
[0055] (7) Before forging, heat the treated billet to 950 ℃ and hold it for 18 hours. The initial forging temperature is 915 ℃, then it is pressed four times, and the final forging temperature is 860 ℃. After forging, it is air-cooled and tested. Example 5
[0056] (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 11%, Fe 3.0%, V 0.20%, with the balance being Cu and unavoidable impurities.
[0057] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Heat to 1220 °C to fully melt and alloy them. After the pure iron is completely dissolved, add the copper-vanadium master alloy. Reduce the melt temperature to approximately 1160 °C, and quickly add the pure aluminum block while immersing it in the molten copper to prevent oxidation. Then heat to 1250 °C and stir thoroughly to ensure uniform alloying. Take a concave sample at 1180 °C and perform pre-furnace spectral analysis to measure C. V=0.20%. Sprinkle 500 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let it stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload the furnace.
[0058] (3) Preheat the ingot mold, and pour the melt at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1180 ℃. After pouring, allow the ingot to cool naturally to room temperature in the air.
[0059] (4) The obtained ingot is homogenized and annealed, heated to 750 °C in the furnace, held for 8 hours, and then cooled to below 300 °C before being taken out of the furnace.
[0060] (5) Stress-relief annealing is performed on the ingot by heating to 500 ℃, holding for 6 hours, and then cooling in the furnace. Finally, quenching and aging are performed by heating to 950 ℃, holding for 4 hours, and then water quenching.
[0061] (6) The water-quenched billet is subjected to deep cryogenic treatment. The equivalent diameter D of the billet is 150 mm. According to formula (1), v = 0.77 ℃ / min is calculated. The billet is cooled to -196 ℃ at a cooling rate of 0.77 ℃ / min and held for 12 hours. Then, it is slowly warmed back to room temperature at a heating rate of 2 ℃ / min and then tempered at 500 ℃ for 4 hours.
[0062] (7) Before forging, heat the treated billet to 950 ℃ and hold it for 20 hours. The initial forging temperature is 920 ℃, then it is pressed five times, and the final forging temperature is 860 ℃. After forging, it is air-cooled and tested.
[0063] Comparative Example 1 This comparative example is based on the preparation of a 100 kg alloy ingot, with the raw materials formulated according to the target composition of Al 10%, Fe 2.5%, V 0.05%, and the balance Cu. The remaining processes are the same as in Example 1.
[0064] Comparative Example 2 This comparative example is based on the preparation of a 100 kg alloy ingot, with the raw materials formulated according to the target composition of Al 10%, Fe 2.5%, V 0.25%, and the balance Cu. The remaining processes are the same as in Example 1.
[0065] Comparative Example 3 This comparative example uses the preparation of a 100 kg alloy ingot as a baseline, with the raw materials formulated according to the target composition of Al 10%, Fe 2.5%, V 0.15%, and the balance Cu. The melting, casting, homogenization annealing, stress-relief annealing, and quenching steps are the same as in Example 4. The difference lies in the cryogenic treatment: the water-quenched billet is cooled to -120 °C at a cooling rate of 0.93 °C / min, held at that temperature for 8 hours, then slowly warmed back to room temperature at a heating rate of 0.89 °C / min, and subsequently tempered at 450 °C for 3 hours. The remaining forging steps are the same as in Example 4.
[0066] Comparative Example 4 (1) Based on the preparation of 100 kg alloy ingot, the ingredients are prepared according to the target composition of Al 10%, Fe 2.5%, with the balance being Cu and unavoidable impurities.
[0067] (2) First, add all the electrolytic copper and pure iron into the induction furnace. Raise the temperature to 1220 ℃ to fully melt and alloy the copper. After the pure iron has completely melted, lower the melt temperature to about 1160 ℃ and quickly add the pure aluminum block while immersing it in the copper liquid to prevent oxidation. Then raise the temperature to 1225 ℃ and stir thoroughly to ensure uniform alloying. Take a concave sample at 1150 ℃ and perform pre-furnace spectral analysis to confirm that the Al and Fe contents are within the target range. Sprinkle 450 g of pure cryolite evenly onto the surface of the melt, stir thoroughly, let it stand to remove slag, adjust the melt temperature to 1150 ℃, and prepare to unload the furnace.
[0068] (3) Preheat the ingot mold, and pour the melt at 1150 ℃ into the mold quickly and steadily at a pouring temperature of 1140 ℃. After pouring, air cool the ingot to room temperature.
[0069] (4) The obtained ingot is homogenized and annealed, heated to 725 ℃ and held for 6 hours, and then cooled to below 300 ℃ before being taken out of the furnace.
[0070] (5) The ingot is subjected to stress-relief annealing, held at 450 ℃ for 3 hours, and then cooled in the furnace. Finally, it is subjected to quenching and aging, heated to 850 ℃ and held for 2 hours, and then water quenched.
[0071] (6) During tempering, the billet is held at 450 ℃ for 3 hours. Before forging, the treated billet is heated to 935 ℃ and held for 16 hours. The initial forging temperature is 920 ℃, and three pressing forgings are performed. The final forging temperature is 855 ℃, and the billet is air-cooled after forging.
[0072] Comparative Example 5 The raw material ratios for this comparative example are the same as those for Example 4: based on the preparation of 100 kg alloy ingots, Al 10.4%, Fe 2.9%, V 0.18%, with the balance being Cu.
[0073] The steps of smelting, casting, homogenizing annealing, stress-relieving annealing, quenching, tempering, and forging are exactly the same as in Example 4. The difference is that in the billet processing, deep cryogenic treatment is not performed after quenching, and tempering is performed directly.
[0074] Comparative Example 6 The raw material ratios for this comparative example are the same as those for Comparative Example 4: based on the preparation of 100 kg alloy ingots, Al 10%, Fe 2.5%, and the balance Cu.
[0075] The melting, casting, homogenization annealing, stress-relief annealing, and quenching steps are the same as those in Comparative Example 4. The difference is that a cryogenic treatment step is added after quenching in the billet processing: the water-quenched billet is cooled to -196 ℃ at a cooling rate of 1.22 ℃ / min, held at that temperature for 8 hours, and then slowly warmed back to room temperature at a heating rate of 1 ℃ / min. The subsequent tempering and forging steps are the same as those in Comparative Example 4.
[0076] Performance testing The aluminum bronze forgings prepared in Examples 1-5 and Comparative Examples 1-6 were subjected to mechanical property tests, wear resistance tests, and corrosion resistance tests. The corrosion resistance test employed a salt spray test, conducted according to ASTM B117 standard using a neutral salt spray method. The test conditions were: 5% NaCl solution, test chamber temperature 35 ℃, and continuous spraying for 120 hours. The test results are shown in Tables 1, 2, and 3. Figure 2 and Figure 3 Line graphs showing the effect of different V contents on the tensile strength and elongation of aluminum bronze forgings.
[0077] Table 1 Mechanical performance test results
[0078] From Table 1, Figure 2 and Figure 3 It can be seen that the effect of V content on the mechanical properties of aluminum bronze forgings exhibits a clear critical characteristic. As the V content increases from 0.10% to 0.18%, the tensile strength and yield strength of the alloy continue to rise, while the elongation decreases slightly but remains at a high level. When the V content further increases to 0.20%, the tensile strength and yield strength begin to decrease, and the elongation decreases more significantly. This indicates that there is an optimal range for V content; excessively high V content can actually impair the plasticity and strength of the alloy. Furthermore, when V addition is combined with cryogenic treatment, the strength is further improved, while the elongation remains at a high level. This demonstrates that V and cryogenic treatment produce a synergistic strengthening effect, and the combined effect is better than using them individually. In particular, the comprehensive mechanical properties of Example 4 are significantly better than those of the comparative examples. This shows that the present invention successfully achieves a synergistic improvement in both high strength and high plasticity through the organic combination of V microalloying and cryogenic treatment.
[0079] Table 2 Abrasion resistance test results
[0080] As shown in Table 2, the wear rate continuously decreases with increasing hardness, indicating that the present invention effectively improves the hardness of the alloy through V microalloying and cryogenic treatment, thereby significantly improving wear resistance. As the V content increases from 0.10% to 0.18%, hardness and wear resistance continue to improve; when the V content reaches 0.20%, hardness and wear resistance slightly decrease but remain at a relatively high level. There is an optimal range for V content. When the V content is too low (Comparative Example 1), hardness and wear resistance are significantly insufficient; when the V content is too high (Comparative Example 2), the improvement in wear resistance tends to saturate or even slightly decreases. Comparing the material performance data of the two alone reveals that the combined effect of V and cryogenic treatment is better than the simple sum of their individual effects, indicating a synergistic effect in improving hardness and wear resistance.
[0081] This demonstrates that the present invention, through the organic combination of V micro-alloying and cryogenic treatment, significantly improves the hardness and wear resistance of aluminum bronze, thus meeting the application requirements under high wear conditions.
[0082] Table 3 Corrosion resistance test results
[0083] Table 3 shows that the V content has a significant impact on corrosion resistance: as the V content increases from 0.10% to 0.18%, the corrosion current density continuously decreases while the pitting potential continuously increases. Performance slightly declines when the V content reaches 0.20%, indicating that appropriate V addition can improve corrosion resistance and that there is an optimal range. Cryogenic treatment also improves corrosion resistance; regardless of whether V is added, the corrosion current density decreases and the pitting potential increases after cryogenic treatment. More importantly, the combined corrosion resistance of the two is superior to that of either material alone, consistent with the variation patterns of mechanical properties and wear resistance. This demonstrates that the present invention significantly improves the corrosion resistance of aluminum bronze through the organic combination of V microalloying and cryogenic treatment.
[0084] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing high-strength, high-ductility aluminum bronze, characterized in that, Includes the following steps: S100: Weigh the furnace charge according to the target proportion. The furnace charge includes electrolytic copper, pure iron, pure aluminum, cryolite, and copper-vanadium master alloy. Add electrolytic copper and pure iron to a melting vessel and melt them. After the pure iron dissolves, add the copper-vanadium master alloy, followed by pure aluminum for alloying. Take samples for spectral analysis to ensure that the Al, Fe, and V contents are within the target range, with fluctuations allowed at ±0.2%. Sprinkle cryolite evenly onto the surface of the melt for refining. After melting, cast the ingot. S200: The obtained ingot is subjected to homogenization annealing, stress-relief annealing, quenching, cryogenic treatment, and tempering in sequence; the cryogenic treatment is performed after quenching and before tempering, with a treatment temperature of -196 ℃ to -150 ℃ and a holding time of 6 hours to 12 hours; the actual cooling rate of the cryogenic treatment is determined according to the following formula: Where v is the actual cooling rate, v0 is the reference cooling rate, and k V C is the correction factor for V content. V For the measured V content, D0 is the reference billet diameter, D is the actual billet equivalent diameter, and k D This is the size sensitivity coefficient; S300: The processed billet is heated before forging and then forged. The forging process involves multiple forging passes, followed by air cooling, ultimately yielding high-strength and high-ductility aluminum bronze.
2. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 1, characterized in that, In step S100, the amount of cryolite used is 400 g to 500 g when the alloy ingot is 100 kg.
3. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 2, characterized in that, In step S100, the alloying temperature is 1200 ℃~1250 ℃, and the spectral analysis temperature is 1120 ℃~1180 ℃.
4. A method for preparing high-strength, high-ductility aluminum bronze according to any one of claims 1-3, characterized in that, In step S200, the homogenization annealing temperature is 700 ℃~750 ℃, and the time is 5 hours~8 hours.
5. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 4, characterized in that, In step S200, the stress-relief annealing temperature is 400 ℃~500 ℃, and the time is 2 hours~6 hours.
6. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 5, characterized in that, In step S200, the quenching temperature is 850 ℃~950 ℃, and the time is 2 hours~4 hours.
7. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 6, characterized in that, In step S200, the tempering temperature is 450 ℃~500 ℃, and the time is 2 hours~4 hours.
8. A method for preparing high-strength, high-ductility aluminum bronze according to any one of claims 1-3, characterized in that, In step S300, the billet is heated to 920 ℃~950 ℃ before forging, and the holding time is 12 hours~20 hours.
9. The method for preparing a high-strength, high-ductility aluminum bronze according to claim 8, characterized in that, In step S300, during the forging process, the initial forging temperature is 910 ℃~920 ℃, and the final forging temperature is 850 ℃~860 ℃.
10. A high-strength, high-ductility aluminum bronze, characterized in that, The high-strength, high-ductility aluminum bronze is prepared by the method described in any one of claims 1-9, wherein the alloy composition by mass percentage is: Al 8.5%-11.0%, Fe 2.0%-4.0%, V 0.10%-0.20%, with the balance being Cu and unavoidable impurities.
Citation Information
Patent Citations
Aluminium bronze continuously-cast tube with both high strength and high ductility, and production method thereof
CN103882254A
Aluminum bronze material and preparation method thereof
CN110284025A
Acid bronze alloy and manufacturing method for high strength and thermal conductivity forging therewith
CN1439734A