A method for preparing wide rare earth magnesium alloy plates

By employing a method for preparing wide-width rare-earth magnesium alloy plates, combining semi-continuous casting, homogenization treatment, multi-directional forging, and wide-width rolling, the problems of uneven deformation and cracking in magnesium alloys have been solved, enabling high-precision and high-performance production of large-size plates suitable for aerospace and new energy vehicles.

CN123108375APending Publication Date: 2026-11-17SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611596167.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing magnesium alloys have limited room temperature slip systems, asymmetric tensile and compressive yields, and insufficient absolute strength and forming stability, resulting in uneven deformation, edge cracking, plate instability, and difficulty in controlling dimensional accuracy of large-size high rare earth magnesium alloy billets.

Method used

A method for preparing wide plates of rare earth magnesium alloy was adopted, including semi-continuous casting, homogenization treatment, multi-directional forging, wide rolling and aging treatment. Through alloy composition optimization and process synergy, combined with parameter optimization such as inter-pass heat preservation and step deformation, wide plates with a width ≥2000mm and a thickness of 20~50mm were prepared.

Benefits of technology

It effectively solves the problems of uneven deformation, edge cracking and dimensional accuracy of large billets, reduces stress accumulation and scrap rate during forging and rolling, and improves the plasticity and mechanical properties of the alloy to meet the performance requirements of aerospace and new energy vehicle scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108375A_ABST
    Figure CN123108375A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing wide-width rare-earth magnesium alloy plates. The process involves sequential semi-continuous casting, homogenization and hot water quenching, multi-directional forging, gradient heating, wide-width rolling, hot straightening and quenching, and isothermal aging. The resulting plates have a width of 2000-2300 mm and a thickness of 25-40 mm. This method reduces energy consumption and raw material loss, decreases scrap rate during deformation, eliminates component segregation, and releases residual stress. These three steps synergistically minimize the risk of cracking during deformation. Simultaneously, the high solid solubility of Gd and Y elements promotes non-basal plane slip activation, enhancing the alloy's plasticity during high-temperature deformation. The isothermal aging temperature and time allow for flexible control of the size and distribution density of nano-precipitates, enabling customized material mechanical properties and achieving excellent mechanical performance. Furthermore, it maintains the inherent lightweight advantages of magnesium alloys, possesses good corrosion resistance and high-temperature stability, and meets the performance application requirements of various scenarios such as aerospace and new energy vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials processing technology, and specifically relates to a method for preparing wide rare earth magnesium alloy plates. Background Technology

[0002] Magnesium alloys, due to their low density, high specific strength, good vibration damping properties, and recyclability, have broad application prospects in the automotive industry, 3C products, aerospace, and rail transportation. In recent years, the application ratio of wrought magnesium alloys has gradually increased, but their commercialization level still lags behind that of wrought aluminum alloys. This is mainly due to the limited room-temperature slip system, asymmetric tensile and compressive yielding, and insufficient absolute strength and forming stability of magnesium alloys. Alloy composition and hot deformation process parameters are key factors determining the microstructure and properties of magnesium alloys.

[0003] In Mg-Re-Zn alloys, appropriate alloy composition and solidification, homogenization, and hot deformation regimes can form long-period stacked ordered phases (LPSO phases) and rare-earth-enriched second phases. Different morphologies of the second phases influence dynamic recrystallization, dislocation movement, and local deformation coordination; therefore, it is necessary to synergistically control the second phase state, grain structure, and hot working path.

[0004] In related technologies, the main methods for plastic processing of magnesium alloys include forging, rolling, and extrusion. Extrusion can produce high-performance bars or profiles, but the transverse dimensions of the product are limited by the extrusion cylinder and die. Unidirectional forging is prone to causing a single strain path and non-uniform shape, and large-size high-rare-earth magnesium alloys are also prone to cracking due to temperature drop and strain concentration. Although unidirectional rolling can produce large-size plates, it is prone to producing strong texture, edge cracking, warping, and non-uniform structure between the center and the edge. Summary of the Invention

[0005] In view of this, the present invention aims to provide a method for preparing wide rare earth magnesium alloy plates by combining alloy composition with multi-stage deformation process. The method solves the problems of uneven deformation, edge cracking, plate shape instability and difficulty in controlling dimensional accuracy of large-size high rare earth magnesium alloy billets by semi-continuous casting, homogenization, multi-directional forging, wide rolling and aging treatment.

[0006] This invention provides a method for preparing wide-width rare-earth magnesium alloy plates. The rare-earth magnesium alloy comprises, by mass percentage, 8.5%~9.2% Gd, 3.5%~4.2% Y, 1.0%~1.6% Zn, and 0.2%~0.3% Zr, with the balance being Mg and unavoidable impurities. The preparation method includes semi-continuous casting, homogenization treatment and hot water quenching, multi-directional forging, three-stage gradient heating before rolling, wide-width rolling, hot straightening and quenching, and isothermal aging treatment to obtain plates with a width of 2000~2300 mm.

[0007] Furthermore, the pouring temperature of the semi-continuous casting is 725~740℃, the casting speed is 90~105 mm / min, and the equivalent cooling rate at the solidification front is 5.5~7℃ / s.

[0008] Furthermore, the homogenization temperature is 505~525℃, the holding time is 18~21 h, and the selected temperature is at least 10℃ lower than the initial melting temperature of the alloy determined by differential scanning calorimetry or equivalent methods; after homogenization, it is placed in hot water at 80~100℃ for quenching, and the quenching medium is kept from boiling violently.

[0009] Furthermore, the initial forging temperature for multi-directional forging is 425~440℃, with a holding time of 28~32 min before initial forging; the first pass reduction rate is 8%~10%, and the subsequent single pass reduction rate is 8%~14%. After completing each directional group (transverse then longitudinal), the temperature is replenished at 420~440℃ for 20 min. During the forging process, light pressing and shaping, thickness direction pressing, flipping and elongation, 90° rotation and cross pressing, zone widening, and small pressing and shaping are performed sequentially, with a total thickness direction deformation of 55%-64%.

[0010] Furthermore, the forging billet is heated in three stages before rolling: first, it is held at 250~260℃ for 4 hours, then heated to 350~360℃ for 4~5 hours, and then heated to 420~440℃ for 4 hours.

[0011] Furthermore, the wide-width rolling process sequentially employs transverse rolling for initial rolling, longitudinal rolling and transverse widening, and longitudinal final rolling.

[0012] Furthermore, the rolling speed of the transverse rolling is 0.20~0.35 m / s, and the first pass reduction rate is 5%~7%; the longitudinal rolling and transverse widening involve rotating the slab 90° for 4 passes of longitudinal rolling, reducing the thickness, and then rotating it 90° again for 5 passes of transverse widening rolling, further reducing the thickness and increasing the width; the reduction rate of the intermediate passes is 7%~16%; after every 3~4 passes, the slab is reheated in a furnace at 400~440℃ for 30~60 min; the longitudinal final rolling involves 6 passes of final rolling finishing along the longitudinal direction, reducing the thickness from approximately 60 mm to 35 mm, with a final rolling pass reduction rate of 6%~12%, a total rolling reduction rate of 81%~87%, and a total of 17~20 passes; the final rolling temperature is not lower than 350℃.

[0013] Furthermore, hot straightening and quenching are performed immediately after longitudinal final rolling. The quenching medium is water, the quenching temperature is 100℃, and the final cooling is air cooling.

[0014] The beneficial effects of the technical solution provided by the embodiments of the present invention are as follows: The present invention uses rare earth magnesium alloys of Mg, Gd, Y, Zn and Zr as the base raw materials to prepare wide plates: a multi-process synergy of semi-continuous casting to prepare ingots, homogenization treatment, forging, rolling and isothermal aging, combined with parameter optimization such as heat preservation between passes and step deformation, through alloy composition optimization and process synergy, reduces stress accumulation and bending instability of samples during forging and rolling, slowly deforms to refine grains and enhances the strengthening effect of aging nano-precipitates; effectively solves the technical problems of uneven deformation of large-size billets, edge cracking and difficulty in controlling dimensional accuracy, and prepares wide plates with a width ≥2000mm and a thickness of 20~50mm. Semi-continuous casting replaces traditional vacuum melting casting, simplifying the ingot preparation process, reducing energy consumption and raw material loss, and producing large-sized round ingots, allowing the ingot specifications to be compatible with subsequent multi-directional forging and wide-width rolling. By optimizing the pass parameters and holding regime of multi-directional forging and rolling, the strain path of the billet is changed, allowing the center, edges, and corners to participate in deformation sequentially. This facilitates the crushing and redistribution of coarse second phases and improves the uniformity of forging deformation, reducing the scrap rate during deformation. Homogenization treatment constrained by the initial melting temperature reduces dendritic segregation in the as-cast state, and hot water quenching maintains the microstructure required for subsequent hot deformation. Homogenization treatment eliminates compositional segregation, forging pretreatment releases residual stress, and holding between rolling passes alleviates stress accumulation. These three steps work together to minimize the risk of cracking during deformation. At the same time, the high solid solubility of Gd and Y elements promotes the activation of non-basal plane slip, improving the plasticity of the alloy during high-temperature deformation. By adjusting the isothermal aging temperature and time, the size and distribution density of nano-precipitates can be flexibly controlled, achieving customization of the material's mechanical properties. Three-stage gradient heating, cross-rolling, and inter-pass heating work together to control the temperature difference and deformation distribution inside and outside the thick plate; hot straightening after final rolling is used to improve the plate shape. The preparation method of this invention achieves customized material mechanical properties; at the same time, it maintains the inherent lightweight advantages of magnesium alloys, possesses good corrosion resistance and high-temperature stability, and meets the performance application requirements of different scenarios such as aerospace and new energy vehicles. Attached Figure Description

[0015] Figure 1 This is a schematic diagram of the process for preparing wide rare earth magnesium alloy plates according to an embodiment of the present invention, where Φ represents the diameter and L represents the length;

[0016] Figure 2 This is a schematic diagram of multi-directional forging according to an embodiment of the present invention;

[0017] Figure 3 This is a schematic diagram of the wide-width rolling route according to an embodiment of the present invention;

[0018] Figure 4 These are microstructure diagrams of the wide-width plates prepared by the methods in Examples 2-5 of this invention;

[0019] Figure 5 A physical image of the wide sheet material prepared by the method of this embodiment of the invention;

[0020] Figure 6 The mechanical property curves of the wide-width plates prepared by the methods in Examples 2 to 5 of this invention are shown.

[0021] Among them, 101 is semi-continuous casting, 102 is homogenization treatment and hot water quenching, 103 is multi-directional forging, 104 is three-stage gradient heating before rolling, 105 is wide-width rolling, 106 is hot straightening and quenching, 107 isothermal aging, 201 is the initial billet, 202 is the billet after the first pass of pressing or upsetting, 203 is the billet after being rotated 90° and reoriented, 204 is the billet after the second pass of drawing or widening, 205 is the upper and lower anvils, 206 is the pressing direction, 207 is the billet rotation direction, 301 is the horizontal rolling opening, 302 is the first 90° rotation, 303 is the longitudinal rolling, 304 is the second 90° rotation, 305 is the transverse widening, 306 is the longitudinal final rolling and hot straightening, 307 is the slab, 308 is the roll, 309 is the rolling direction, and 310 is the hot straightening roll. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, further explanation is provided below in conjunction with the accompanying drawings and embodiments.

[0023] In this embodiment of the invention, unless otherwise specified, alloy composition refers to mass percentages; the total rolling reduction is calculated as (thickness before rolling - thickness after rolling) / thickness before rolling × 100%. Heating and reheating temperatures are furnace temperature settings, and the final rolling temperature is the temperature measured on the middle surface of the plate after the last pass. The equivalent cooling rate at the solidification front is calculated according to the temperature-time curve of the solidification zone calibrated by the equipment; the lower limit of the rolling process temperature is 350℃. Room temperature tensile properties are obtained from the engineering stress-strain curve: the 0.2% specified plastic elongation strength is determined using the offset method, the tensile strength is taken as the peak engineering stress, and the fracture engineering strain is taken as the engineering strain at the fracture point. Flatness error is recorded as the maximum gap over a 1 m reference length. The final length of the plate is determined by the actual measurement results after trimming and length setting, and is not considered a limiting parameter of this invention.

[0024] Example 1

[0025] See attached document Figure 1This invention provides a method for preparing wide-width rare-earth magnesium alloy plates. The rare-earth magnesium alloy comprises, by mass percentage, 8.5%~9.2% Gd, 3.5%~4.2% Y, 1.0%~1.6% Zn, and 0.2%~0.3% Zr, with the balance being Mg and unavoidable impurities. The preparation method includes semi-continuous casting 101, homogenization and hot water quenching 102, multi-directional forging 103, three-stage gradient heating before rolling 104, wide-width rolling 105, hot straightening and quenching 106, and isothermal aging 107, to obtain plates with a width of 2000~2300 mm. This invention controls the alloy composition, reversing deformation path, pass reduction rate, and temperature compensation regime as interrelated process conditions to prepare plates with a width of 2000~2300 mm.

[0026] See attached document Figure 1 This invention provides a method for preparing wide rare earth magnesium alloy plates, specifically including the following steps:

[0027] (1) Batching and smelting: Weigh out industrial pure Mg, Mg-Gd master alloy, Mg-Y master alloy, pure Zn and Mg-Zr master alloy according to the nominal alloy composition of Gd 8.5%-9.2%, Y 3.5%-4.2%, Zn 1.0%-1.6%, Zr 0.2%-0.3% and balance Mg; remove oil, scale and moisture before feeding, and preheat the furnace body, trough and filter device;

[0028] Mg is melted under a protective atmosphere, and Mg-Gd, Mg-Y and Mg-Zr master alloys are added in sequence. After they are fully melted, Zn is added. After stirring, refining, settling, slag removal and filtration, the mixture is fed into a semi-continuous casting tank. The alloy also contains unavoidable impurities.

[0029] (2) Semi-continuous casting 101: The pouring temperature of the semi-continuous casting trough is controlled at 725~740℃, the casting speed is controlled at 90~105 mm / min, and the equivalent cooling rate at the solidification front is controlled at 5.5~7℃ / s to obtain a circular cross-section ingot with a diameter of 450~520 mm and a length of 2400~2600 mm; the liquid level is kept stable during the casting process to avoid gas entrapment and slag inclusions in the melt; after the ingot cools, the unstable sections at the head and tail are removed. The semi-continuous casting parameters are determined according to the thermal process calibration results of the casting equipment. After the unstable sections at the head and tail are removed, the ingot is rolled, chamfered, and non-destructive tested, it enters the homogenization process.

[0030] (3) Homogenization and hot water quenching 102: The circular cross-section ingot is machined to remove about 5 mm of surface layer, and chamfering and non-destructive testing are completed; then the circular cross-section ingot is heated in the furnace to 505~525℃ and held for 18~21 h, and the homogenization temperature is at least 10℃ lower than the initial melting temperature of the alloy determined by differential scanning calorimetry or equivalent method; after the holding period, it is transferred to hot water at about 80~100℃ for quenching to obtain a homogenized initial ingot 201. After cooling, the surface is inspected to confirm that there are no macroscopic quenching cracks.

[0031] (4) Multi-directional forging 103: The homogenized initial billet 201 is heated to 425~440℃ and held for 28~32min. In the first pass, the billet is lightly pressed along the first direction with a reduction rate of 8%~10%. Then, the billet is flipped and the remaining surfaces are alternately pressed to gradually transform the circular cross section into a near-rectangular cross section with stable anvil contact. The reduction rate of subsequent single passes is controlled at 8%~14%. The thickness direction is pressed, flipped and elongated, rotated 90° and cross-pressed, and widened in sections are performed in sequence. After each direction group (transverse and then longitudinal) is completed, the temperature is replenished at 420~440℃ for 20min. After multiple upsetting, elongation and widening, the billet is shaped with a small reduction to obtain a forging billet with a thickness of 190~210 mm and a total deformation in the thickness direction of 55%~64%. The forging is trimmed, polished and non-destructive tested after forging.

[0032] See attached document Figure 2 Specifically, the homogenized initial billet 201 is placed between the upper anvil and the lower anvil 205, with an initial forging temperature of 425~440℃ and a holding temperature of 28~32 min before initial forging. In the first pass, the initial billet 201 is lightly pressed or upset along the pressing direction 206 at a reduction rate of 8%~10%, resulting in a billet 202 after the first pass of pressing or upset, gradually transforming the circular cross-section into a near-rectangular cross-section with stable anvil surface contact. Subsequently, the billet is rotated 90° along the billet rotation direction 207, resulting in a billet 203 after being rotated 90° and reoriented. Then, the billet 203 after being rotated 90° and reoriented is drawn or widened along the pressing direction 206 at a reduction rate of 8%~14%, resulting in a billet 204 after the second pass of drawing or widening. Subsequently, the above "rotate 90° - press down" cycle is repeated to complete the pressing down in the thickness direction, flipping and elongating, cross pressing down and partitioning widening in sequence. After each direction group (transverse and then longitudinal) is completed, it is heated at 420~440℃ for 20 min. After multiple upsetting, elongation and widening, it is shaped with a small pressing down to obtain a forging billet with a thickness of 190~210 mm and a total deformation in the thickness direction of 55%~64%.

[0033] (5) Pre-rolling three-stage gradient heating 104: The forging billet is first kept at 250~260℃ for 4 h, then heated to 350~360℃ for 4~5 h, and then heated to 420~440℃ for 4 h to carry out three-stage gradient heating so that the core of the forging billet reaches the rolling temperature; after the heat preservation is completed, it is quickly sent into the rolling mill to reduce the temperature drop during transfer.

[0034] (6) Wide-width rolling 105: This includes, in sequence, transverse rolling 301 to establish bite and initial width expansion, longitudinal rolling 303 and transverse widening 305 and longitudinal final rolling;

[0035] See attached document Figure 3 Specifically, the process begins with the horizontal rolling initialization stage 301, where the forged billet is fed into the rolling mill as slab 307. Rolls 308 apply pressure to the slab 307 along the rolling direction 309 at a rolling speed of 0.20–0.35 m / s. The initial reduction rate is 5%–7%, and four passes of reciprocating rolling are performed horizontally, reducing the thickness of the slab 307 from approximately 200 mm to approximately 150 mm, establishing stable bite and forming initial width. After each pass, the entry end, edges, and corners are inspected. After horizontal rolling initialization 301, a first 90° rotation 302 is performed, rotating the slab 307 90° around its thickness direction, changing the rolling direction from horizontal to longitudinal. Subsequently, the longitudinal rolling stage 303 begins, where four passes of rolling are performed longitudinally. Rollers 308 continue to apply pressure along the rolling direction 309, reducing the thickness of the slab 307 from approximately 150 mm to approximately 100 mm. After longitudinal rolling is completed, a second 90° rotation (304) is performed, rotating the slab 307 90° again around the thickness direction to return to the transverse rolling orientation. Then, the transverse widening stage (305) is entered, and five passes of widening rolling are performed in the transverse direction to reduce the thickness of the slab 307 from about 100 mm to about 60 mm, and gradually increase the width of the plate to close to the target width. The reduction rate of the intermediate passes is 7%~16%. After every 3~4 passes or when the surface temperature of the slab 307 is close to the lower limit of the process, it is reheated in the furnace at 400~440℃ for 30~60 min. After the transverse widening is completed, the plate enters the longitudinal final rolling and hot straightening stage 306. The slab 307 is rotated to the longitudinal orientation and finished with 6 passes of final rolling along the longitudinal direction, reducing the thickness from about 60 mm to 35 mm. The final rolling pass reduction rate is 6%~12%, the total rolling reduction rate is 81%~87%, the total number of passes is 17~20, and the final rolling temperature is not lower than 350℃. Immediately after final rolling, the plate is hot straightened by hot straightening rolls 310 to make the plate straight in the width and length directions.

[0036] (7) Hot straightening and quenching 106: Hot straightening and quenching immediately after final rolling. The quenching medium is water and the quenching temperature is 100℃. After quenching, air cooling is used for final cooling.

[0037] (8) Isothermal aging 107: The quenched plate is kept at 195℃ for 38 h, and then air-cooled after being taken out of the furnace. The edge cutting, length setting, surface inspection and non-destructive testing are completed to obtain a wide plate with a width ≥2000mm and a thickness of 20~50mm.

[0038] The wide-width plates prepared by the method of this invention were subjected to uniaxial tensile testing at room temperature. The yield strength (Rp0.2) was determined using the 0.2% offset method. The yield strength obtained was 301.7~345.2 MPa, the tensile strength was 383.5~411.0 MPa, and the fracture engineering strain was 10.1%~18.6%. The flatness error was no greater than 3.0 mm / m.

[0039] Example 2

[0040] This invention provides a method for preparing wide rare earth magnesium alloy plates, specifically including the following steps:

[0041] (1) Batching and smelting: Weigh out industrial pure Mg, Mg-Gd master alloy, Mg-Y master alloy, pure Zn and Mg-Zr master alloy according to the nominal composition of the alloy: Gd 8.5%, Y 3.5%, Zn 1.0%, Zr 0.2%, with the balance Mg and smelt.

[0042] (2) Semi-continuous casting: The pouring temperature of the semi-continuous casting trough is controlled at 725℃, the casting speed is controlled at 90mm / min, and the equivalent cooling rate at the solidification front is controlled at 5.5℃ / s to obtain a circular cross-section ingot with a diameter of Φ 450 mm × 2400 mm.

[0043] (3) Homogenization treatment and hot water quenching: The round ingot is heated to 505℃ in the furnace and held for 18 h, and this temperature is at least 10℃ lower than the measured initial melting temperature; after the holding period, it is transferred to hot water at about 85℃ for quenching to obtain a homogenized ingot.

[0044] (4) Multi-directional forging: The homogenized billet is initially heated to 425°C and held for 30 min; the first pass is lightly pressed along the first direction with a reduction rate of 8%, and then the billet is flipped over and the remaining surfaces are alternately pressed down, so that the circular cross section is gradually transformed into a near-rectangular cross section with stable anvil contact; the reduction rate of subsequent single passes is controlled at 8%~12%, and the thickness direction is pressed down, flipped and elongated, rotated 90° and cross-pressed down and widened in sections are carried out in sequence; after each direction group (transverse and longitudinal) is completed, it is heated at 420°C for 20 min; after multiple upsetting, elongation and widening, it is shaped with a small reduction to obtain a forging billet of about 200 mm × 820 mm × 2250 mm;

[0045] (5) Three-stage gradient heating before rolling: The forging billet is first kept at 250℃ for 4 h, then heated to 350℃ for 4 h, and then heated to 420℃ for 4 h to carry out three-stage gradient heating;

[0046] (6) Wide-width rolling: The rolling speed of the horizontal rolling billet is 0.20 m / s, and the first pass reduction rate is 5%; the reduction rate of the intermediate passes of longitudinal rolling and transverse widening is 7%~14%; after every 3~4 passes or when the temperature is close to the lower limit of the process, it is reheated in the furnace at 410~430℃ for 30~60 min; the reduction rate of the final longitudinal rolling pass is 6%-10%, the total rolling reduction rate is 82.5%, and the total number of passes is 19.

[0047] (7) Hot straightening and quenching: Hot straightening and quenching immediately after final rolling, the quenching medium is water, the quenching temperature is 100℃, and air cooling is used for final cooling after quenching.

[0048] (8) Isothermal aging: The quenched plate is held at 195℃ for 38 h, then air-cooled after being taken out of the furnace. Edge trimming, length setting, surface inspection and non-destructive testing are completed to obtain a wide plate with a width of 2000 mm and a thickness of 35 mm. The rest is the same as in Example 1.

[0049] The wide sheet material prepared in this embodiment of the invention was subjected to uniaxial tensile testing at room temperature. The yield strength (Rp0.2) was determined using the 0.2% offset method. The yield strength was 325.3 MPa, the tensile strength was 396.4 MPa, and the fracture engineering strain was 10.4%. The flatness error was no greater than 3.0 mm / m.

[0050] Example 3

[0051] The nominal composition of the alloy in this embodiment is 9.0% Gd, 4.0% Y, 1.5% Zn, and 0.3% Zr, with the balance being Mg and unavoidable impurities.

[0052] (1) Batching and smelting: Weigh the raw materials according to the nominal composition above, melt Mg under a protective atmosphere, and add Mg-Gd, Mg-Y, Mg-Zr master alloy and Zn in sequence. After the raw materials are completely melted, stir, refine and let stand, remove the slag and let the melt enter the semi-continuous casting stream through the filter device.

[0053] (2) Semi-continuous casting: The pouring temperature was controlled at 735℃, the casting speed was controlled at 100 mm / min, and the equivalent cooling rate at the solidification front was controlled at 6.5℃ / s to obtain a Φ (diameter) 500 mm × 2500 mm round ingot. After removing the unstable sections at the beginning and end of the ingot, about 6 mm of the surface layer was removed by turning, and chamfering and non-destructive testing were completed; any shallow defects were inspected again after local grinding.

[0054] (3) Homogenization and hot water quenching: The ingot is heated to 520℃ in the furnace and held for 20 h. The homogenization temperature is at least 10℃ lower than the initial melting temperature of the alloy determined by differential scanning calorimetry or equivalent method, so as to reduce the segregation in the as-cast state. After the holding period, it is quickly transferred to hot water at 80-100℃ for quenching. After cooling, it is taken out and the surface is inspected to confirm that no macroscopic quenching cracks are present.

[0055] (4) Initial forging preheating and light pressing shaping: Heat the billet to 435℃ and hold for 30 min. Press down in the first direction with a reduction rate of 9% in the first pass, then turn the billet over and alternately lightly press the remaining surfaces to gradually transform the circular cross section into a near rectangular cross section and form a stable anvil contact.

[0056] (5) Multi-directional forging: The reduction rate of subsequent passes is controlled at 8%-14%. First, the billet is pressed down along the thickness direction and then drawn up along the length direction. Then, the billet is rotated 90° for cross-pressing and widening. After each directional group (transverse to longitudinal) is completed, it is heated at 430℃ for 20 min. After multiple upsetting, drawing and sectional widening, the billet is shaped with a smaller reduction to obtain a forging billet of about 200 mm × 1000 mm × 2450 mm. After forging, the burrs and surface folds are removed, and non-destructive testing is performed.

[0057] (6) Three-stage gradient heating before rolling: The forging billet is held at 260℃ for 4 hours to alleviate the thermal stress during the heating process, then heated to 360℃ and held for 4 hours to reduce the temperature difference between the core and the surface, and then heated to 430℃ and held for 4 hours to make the forging billet meet the rolling conditions as a whole. After exiting the furnace, it is quickly sent into the rolling mill to reduce the temperature drop during transfer.

[0058] (7) Horizontal rolling: The rolling speed is 0.30 m / s and the first pass reduction rate is 6%. In the first stage, four reciprocating rolling passes are carried out in the transverse direction to reduce the thickness of the forging billet from about 200 mm to about 150 mm; the focus is on establishing stable bite and initial width expansion, and after each pass, the entry end, edge and corner are checked for cracks.

[0059] (8) Longitudinal rolling and transverse widening: Rotate the slab 90° and perform 4 passes of longitudinal rolling, reducing the thickness from about 150 mm to about 100 mm; rotate it 90° again and perform 5 passes of transverse widening rolling, reducing the thickness from about 100 mm to about 60 mm, and gradually bringing the slab width close to 2200 mm; control the reduction rate of intermediate passes to 8%-15%; after every 3-4 passes or when the slab surface temperature is close to the lower limit of the process, reheat it in the furnace at 420-440℃ for 30-60 min.

[0060] (9) Longitudinal final rolling, hot straightening and quenching: Six final rolling passes are performed along the longitudinal direction to reduce the thickness from about 60 mm to 30 mm. The reduction rate of the final rolling pass is controlled at 8%-12%, and the total rolling reduction rate is 85%. The final rolling temperature is not lower than 350℃. After rolling, hot straightening is performed immediately to make the plate straight in the width and length directions. Then, quenching is performed. The quenching medium is water, the quenching temperature is 100℃, and the plate is finally cooled by air cooling after quenching.

[0061] (10) Isothermal aging: The quenched plate is held at 200℃ for 40 h, then air-cooled after being taken out of the furnace, and the edges are cut and the length is fixed to obtain a plate with a width of 2200 mm and a thickness of 30 mm. The rest is the same as in Example 1.

[0062] The sheet material prepared by the method of this embodiment of the invention was subjected to uniaxial tensile testing at room temperature. The yield strength (Rp0.2) was determined by the 0.2% offset method. The yield strength was 345.2 MPa, the tensile strength was 411.0 MPa, the fracture engineering strain was 10.1%, and the flatness error was 2.2 mm / m.

[0063] Example 4

[0064] This invention provides a method for preparing wide rare earth magnesium alloy plates, specifically including the following steps:

[0065] (1) Batching and smelting: Weigh out industrial pure Mg, Mg-Gd master alloy, Mg-Y master alloy, pure Zn and Mg-Zr master alloy according to the nominal composition of the alloy: Gd 8.5%, Y 3.5%, Zn 1.0%, Zr 0.2%, with the balance Mg;

[0066] (2) Semi-continuous casting: The pouring temperature is controlled at 740℃, the casting speed is controlled at 105 mm / min, and the equivalent cooling rate at the solidification front is controlled at 7℃ / s. A circular cross-section ingot with a diameter of 520 mm × 2400 mm is produced by semi-continuous casting.

[0067] (3) Homogenization treatment and hot water quenching: The circular cross-section ingot is heated to 525°C in the furnace and held for 21 h. After the holding period, it is transferred to hot water at about 90°C for quenching to obtain a homogenized ingot.

[0068] (4) Multi-directional forging: The billet is initially heated to 440℃ and held for 28 min. The first pass is lightly pressed and shaped with a reduction rate of 10%. Then, the thickness direction is pressed down, flipped and elongated, and then widened laterally after rotating 90° with a single pass reduction rate of 9%~14%. After each direction group is completed, it is reheated in the furnace at 430~440℃ for 20 min. The multi-directional upsetting and widening cycle is repeated to ensure that the center and edge of the billet are fully involved in the deformation. Finally, the thickness and shape are corrected with a small reduction to obtain a forging billet of about 190mm×1100mm×2400mm.

[0069] (5) Three-stage gradient heating before rolling: The forging billet is first held at 260℃ for 4 h, then heated to 360℃ for 5 h, and then heated to 440℃ for 4 h.

[0070] (6) Wide-width rolling: The rolling speed of the transverse rolling billet is 0.35 m / s, the first pass reduction rate is 7%, and four reciprocating rollings are performed in the transverse direction to reduce the thickness from about 190 mm to about 140 mm, forming the initial width; longitudinal rolling and further transverse widening: the billet is rotated 90° and four longitudinal rollings are performed to reduce the thickness from about 140 mm to about 90 mm; then rotated 90° again and five transverse rollings are performed to reduce the thickness from about 90 mm to about 55 mm, while the width of the plate gradually reaches 2300 mm. The intermediate pass reduction rate is controlled at 9%~16%. After every 3~4 passes or when the slab temperature is close to the lower limit of the process, the slab is reheated at 420~440℃ for 30~60 minutes. Seven final rolling passes are performed along the longitudinal direction to reduce the thickness from about 55 mm to 25 mm. The final rolling pass reduction rate is 8%~12%, and the total rolling reduction rate is about 86.8%. If cracks appear at the edge, rolling is suspended, the edges are trimmed, and the temperature is replenished before the final rolling is completed with a small reduction pass.

[0071] (7) Hot straightening and quenching longitudinal final rolling and shape control: The final rolling temperature shall not be lower than 350℃; hot straightening and quenching shall be performed immediately after final rolling, the quenching medium shall be water, the quenching temperature shall be 100℃, and the final cooling shall be air-cooled after quenching.

[0072] (8) Isothermal aging: The quenched plate was kept at 210℃ for 45 h, and after being taken out of the furnace, it was air cooled, trimmed, and cut to length to obtain a plate with a width of 2300 mm and a thickness of 25 mm. The rest is the same as in Example 1.

[0073] The wide sheet prepared in this embodiment of the invention was subjected to uniaxial tensile testing at room temperature. The yield strength (Rp0.2) was determined using the 0.2% offset method. The yield strength was 301.7 MPa, the tensile strength was 384.3 MPa, the fracture engineering strain was 18.6%, and the flatness error was 2.5 mm / m.

[0074] Example 5

[0075] This invention provides a method for preparing wide rare earth magnesium alloy plates, specifically including the following steps:

[0076] (1) Batching and smelting: Weigh out industrial pure Mg, master alloy and Zn according to the nominal composition of the alloy as Gd 8.8%, Y 3.8%, Zn 1.3% and Zr 0.3%, with the balance being Mg and unavoidable impurities, and smelt them;

[0077] (2) Semi-continuous casting: The pouring temperature is controlled at 730℃, the casting speed is controlled at 90 mm / min, and the equivalent cooling rate at the solidification front is controlled at 6℃ / s. A circular cross-section ingot with a diameter of Φ480 mm×2600 mm is produced by semi-continuous casting.

[0078] (3) Homogenization and hot water quenching: The round ingot is heated to 515℃ and held for 19 h, and then transferred to hot water at about 90℃ for quenching to obtain a homogenized ingot blank.

[0079] (3) Multi-directional forging: The billet is heated to 430℃ and held for 32 min. The first pass reduction rate is 8%. The subsequent single pass reduction rate is controlled at 8%~12%. Upsetting, turning and elongation, 90° rotation and cross pressing, elongation again and widening in sections are completed in sequence. After each direction group (transverse and then longitudinal) is completed, it is reheated in the furnace at 420~430℃ for 20 min. Finally, it is shaped with a small reduction to obtain a forging billet of about 210 mm×895 mm×2500 mm.

[0080] (4) Three-stage gradient heating before rolling: The billet is first kept at 250℃ for 4 hours, then heated to 360℃ for 4 hours, and then heated to 425℃ for 4 hours to make the temperature inside and outside of the billet uniform before it is sent for rolling.

[0081] (5) Wide-width rolling: The rolling speed of the transverse rolling is 0.25 m / s, the first pass reduction rate is 5%, and four reciprocating rollings are performed in the transverse direction to reduce the thickness of the forging billet from about 210 mm to about 160 mm, to establish a stable bite and gradually widen the billet with a low reduction rate; Longitudinal rolling and transverse widening: The billet is rotated 90° and four longitudinal rollings are performed to reduce the thickness from about 160 mm to about 110 mm; it is rotated 90° again and four transverse widening rollings are performed to reduce the thickness from about 110 mm to about 70 mm, and the width of the plate gradually reaches 2100 mm, with a reduction rate of 7%-14% in the intermediate passes; the billet temperature is measured every 3-4 consecutive rollings; when the temperature is close to the lower limit of the process or cracks appear at the edge, it is reheated in the furnace at 400-435℃ for 30-60 min; Longitudinal final rolling is performed in five longitudinal finishing passes to reduce the thickness from about 70 mm to 40 mm. mm, the final rolling pass reduction rate is controlled at 7%-12%, and the total rolling reduction rate is approximately 81.0%;

[0082] (7) Hot straightening and quenching: Hot straightening and quenching are performed immediately after final rolling. The quenching medium is water and the quenching temperature is 100℃. After quenching, the final cooling is done by air cooling.

[0083] (8) Isothermal aging: The quenched plate was kept at 190℃ for 42 h, and then air-cooled after being taken out of the furnace. The edges were cut, the length was measured and the surface was inspected to obtain a plate with a width of 2100 mm and a thickness of 40 mm. The rest is the same as in Example 1.

[0084] The wide sheet material prepared in this embodiment of the invention was subjected to uniaxial tensile testing at room temperature. The yield strength (Rp0.2) was determined using the 0.2% offset method. The yield strength was 307.0 MPa, the tensile strength was 383.5 MPa, the fracture engineering strain was 16.1%, and the flatness error was 2.0 mm / m.

[0085] See attached document Figure 4 The microstructure shown in the figure is the longitudinal metallographic structure along the rolling direction of the wide-width plates prepared in Examples 2-5 of this invention. The sampling location is the central region of the plate, and the observation surface is parallel to the rolling direction. Figure 4 It can be seen that the matrix structure of the plate in the embodiments of the present invention all exhibits a strip-shaped streamline morphology extending along the rolling direction. The grains are significantly elongated under the action of hot deformation with a large reduction rate. The rare earth enriched second phase particles are distributed in discontinuous chain or band shape along the rolling direction. No macroscopic cracks, pores and coarse undeformed areas were observed, indicating that after homogenization treatment, multi-directional forging and cross-rolling, the dendritic segregation in the cast state is effectively eliminated and the deformation structure has good uniformity.

[0086] Comparing Figures 4(a) to (d), it can be seen that Example 2 [ Figure 4 The microstructure of [a] exhibits a distinct streamlined shape along the rolling direction, with the second phase mainly distributed in strip-like or discontinuous granular forms. Its quantity and density are at a moderate level, resulting in good microstructure uniformity and thus a relatively balanced strength and plasticity. Example 3 [ Figure 4 [b] Due to the highest content of Gd, Y, and Zn, the matrix contains the most and finest second-phase particles. Combined with isothermal aging at 200℃ for 40h, the dispersion strengthening effect of the precipitated phase is significant, resulting in the highest yield strength and tensile strength. Example 4 [ Figure 4 The middle (c) has the highest total rolling reduction (approximately 86.8%), the highest degree of grain refinement, and the finest flow lines. However, due to the high aging temperature (210°C), the precipitates are somewhat coarsened, resulting in slightly lower strength but the highest fracture engineering strain (18.6%). Example 5 Figure 4The middle (d) section exhibits the largest finished product thickness, the smallest total reduction (approximately 81.0%), relatively wide strip spacing, moderate deformation, good plasticity retention, and optimal flatness. These microstructural characteristics are consistent with the mechanical property results listed in Table 1, verifying the effectiveness of this invention in achieving a balance between strength and plasticity in the sheet material through synergistic control of composition and process.

[0087] The results of the room temperature uniaxial tensile test of the wide plates prepared in Examples 2 to 5 of the present invention are compared, as shown in Table 1.

[0088] Table 1. Room temperature uniaxial tensile test results (Rp0.2) of wide-width plates prepared in Examples 2-5

[0089] Example Board width / mm Plate thickness / mm Yield strength / MPa Tensile strength / MPa Fracture engineering strain / % Flatness error / (mm / m) two 2000 35 325.3 396.4 10.4 ≤3.0 three 2200 30 345.2 411.0 10.1 2.2 Four 2300 25 301.7 384.3 18.6 2.5 five 2100 40 307.0 383.5 16.1 2.0

[0090] See attached document Figure 5 The wide sheet material prepared in this embodiment of the invention has a width greater than 2000 mm and a thickness of 25 mm.

[0091] See attached document Figure 6 Sampling was performed on the wide plates prepared by the methods in Examples 2 to 5 of this invention. The sampling location was uniformly the area of ​​the plate center parallel to the rolling direction, with a gauge length of 20 mm. Six parallel samples were used for each data set to test the room temperature mechanical properties of the wide plates.

[0092] From Table 1 and Appendix Figure 6 It can be seen that the preparation method of the present invention can obtain rare earth magnesium alloy plates with excellent mechanical properties, a width of 2000~2300 mm and a thickness of 25~40 mm, within the actual composition and process window covered by the preparation method of the present invention.

[0093] The above embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art can make equivalent adjustments to the heating rate, holding time, number of reversals, and number of passes based on ingot specifications, furnace capacity, and rolling mill capacity without departing from the concept of the present invention; all such equivalent adjustments should fall within the scope defined by the claims of the present invention.

Claims

1. A method for preparing wide-width rare-earth magnesium alloy plates, characterized in that, The rare earth magnesium alloy comprises, by mass percentage, 8.5%-9.2% Gd, 3.5%-4.2% Y, 1.0%-1.6% Zn, and 0.2%-0.3% Zr, with the balance being Mg and unavoidable impurities; the preparation method sequentially includes semi-continuous casting, homogenization treatment and hot water quenching, multi-directional forging, three-stage gradient heating before rolling, wide-width rolling, hot straightening and quenching, and isothermal aging treatment.

2. The method of producing a rare earth magnesium alloy wide plate according to claim 1, characterized by, Includes the following steps: (1) Semi-continuous casting: The pouring temperature of the semi-continuous casting trough is controlled at 725~740℃, the casting speed is controlled at 90~105 mm / min, and the equivalent cooling rate at the solidification front is controlled at 5.5~7℃ / s to obtain a round cross-section ingot. (2) Homogenization treatment and hot water quenching: The circular cross-section ingot is heated to 505~525℃ in the furnace and held for 18~21 h. After the holding period, it is transferred to hot water at about 80~100℃ for quenching to obtain a homogenized initial ingot blank. (3) Multi-directional forging: The initial forging temperature of the homogenized initial billet is 425~440℃, and the initial forging is held for 28~32 min. The first pass reduction rate is 8%~10%, and the subsequent single pass reduction rate is 8%~14%. Light pressing, thickness direction pressing, flipping and elongation, 90° rotation cross pressing, partition widening and small pressing shaping are performed in sequence. After each direction group is completed, the temperature is replenished at 420~440℃ for 20 min to obtain a forging billet with a thickness of 190~210 mm and a total thickness direction deformation of 55%~64%. (4) Three-stage gradient heating before rolling: The forging billet is first kept at 250~260℃ for 4 h, then heated to 350~360℃ for 4~5 h, and then heated to 420~440℃ for 4 h, and the three-stage gradient heating is carried out. (5) Wide-width rolling: This includes, in sequence, transverse rolling to establish bite and initial width expansion, longitudinal rolling and transverse widening, and longitudinal final rolling; (6) Hot straightening and quenching: Hot straightening and quenching are performed immediately after final rolling. The quenching medium is water and the quenching temperature is 100℃. After quenching, air cooling is used for final cooling. (7) Isothermal aging: After air cooling, the quenched plate is kept at 195℃ for 38 hours, and after being taken out of the furnace, it is air cooled. The edge cutting, length setting, surface inspection and non-destructive testing are completed to obtain a wide plate with a width ≥2000mm and a thickness of 20~50mm.

3. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, It also includes batching and smelting. Before semi-continuous casting, industrial pure Mg, Mg-Gd master alloy, Mg-Y master alloy, pure Zn and Mg-Zr master alloy are weighed according to the nominal alloy composition of Gd 8.5%-9.2%, Y 3.5%-4.2%, Zn 1.0%-1.6%, Zr 0.2%-0.3% and balance Mg. Mg is melted under a protective atmosphere, and Mg-Gd, Mg-Y and Mg-Zr master alloys are added in sequence. After they are fully melted, Zn is added. After stirring, refining, settling, slag removal and filtration, it enters the semi-continuous casting tank.

4. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, Before homogenization and hot water quenching, the circular cross-section ingot is pretreated by turning to remove about 5 mm of the surface layer, and then chamfering and non-destructive testing are completed.

5. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, In wide-width rolling, the rolling speed of the transverse rolling blank is 0.20~0.35 m / s, the first pass reduction rate is 5%~7%, and four reciprocating rolling passes are carried out in the transverse direction to reduce the thickness of the forging blank, establish a stable bite, and form the initial width.

6. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, Longitudinal rolling and transverse widening in wide-width rolling: The slab is rotated 90° for 4 passes of longitudinal rolling to reduce the thickness. Then, it is rotated 90° again for 5 passes of transverse widening rolling to further reduce the thickness and increase the width. The reduction rate of the intermediate passes is 7%~16%. After every 3~4 passes, the slab is reheated in the furnace at 400~440℃ for 30~60 minutes.

7. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, In wide-width rolling, the longitudinal final rolling is carried out in 6 passes to reduce the thickness from about 60 mm to 35 mm. The final rolling reduction rate is 6%~12%, the total rolling reduction rate is 81%~87%, and the total number of passes is 17~20. The final rolling temperature is not lower than 350℃.

8. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, The flatness error of the prepared wide-width plates is no greater than 3.0 mm / m.

9. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, The prepared wide-width plates shall have a plastic elongation strength of not less than 300 MPa, a tensile strength of not less than 380 MPa, and a fracture strain of not less than 10.0% at room temperature with a 0.2% specified value.

10. The method of producing a rare earth magnesium alloy wide plate according to claim 1 or 2, characterized by, The preparation method described herein produces wide rare earth magnesium alloy plates. The plate composition, by mass percentage, includes 8.5%~9.2% Gd, 3.5%~4.2% Y, 1.0%~1.6% Zn, and 0.2%~0.3% Zr, with the balance being Mg and unavoidable impurities. The width is 2000~2300 mm, the thickness is 25~40 mm, and the 0.2% specified plastic elongation strength is not less than 300 MPa, tensile strength is not less than 380 MPa, fracture strain is not less than 10.0%, and flatness error is not greater than 3.0 mm / m.