High-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloys and their preparation methods
By using alloying element doping and a special annealing process, a high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy was prepared, which solved the problems of poor plasticity, low hardness, and insufficient wear resistance of existing VCoNi-based medium-entropy alloys, and achieved a simultaneous improvement in strength, plasticity, and wear resistance.
Patent Information
- Application Number
- CN202611510362.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing VCoNi-based medium-entropy alloys have insufficient plastic deformation capacity, poor hardness and wear resistance, severe segregation in the as-cast alloy structure, weak comprehensive mechanical properties, and lack of precise microstructure control methods in engineering applications.
High-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloys, including VCoNi, (VCoNi)94AlxTiy, and V18Co42Ni40, were prepared by alloying element doping and special annealing processes. Vacuum arc melting, magnetic stirring, and annealing were used to ensure uniform element diffusion and microstructure homogenization.
It significantly improves the plasticity and hardness of the alloy, enhances wear resistance, and achieves an optimized balance between strength and plasticity. The tensile strength and elongation of the cast alloy are significantly improved, the hardness is increased by more than 30%, and the wear resistance is significantly enhanced.
Smart Images

Figure CN123108388A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy materials technology, and in particular to a high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy and its preparation method. Background Technology
[0002] VCoNi medium-entropy alloys are a novel class of metallic materials with a face-centered cubic (FCC) single-phase structure, attracting widespread attention in recent years. Studies have shown that equiatomic VCoNi medium-entropy alloys exhibit high tensile strength and good thermal stability at room temperature. Their strengthening mechanism is mainly attributed to the synergistic contribution of solid solution strengthening, grain refinement strengthening, and high-density annealing twins. By controlling thermomechanical processing techniques, κ phases or nanoscale precipitates can be further introduced, enabling the alloy strength to exceed the GPa level. Currently, VCoNi medium-entropy alloys are considered among the strongest medium-entropy alloys with an FCC structure, showing promising application prospects in the field of structural materials.
[0003] Despite the excellent room-temperature strength of VCoNi matrix alloys, they still suffer from the following significant drawbacks in practical engineering applications: Insufficient plastic deformation capacity: Pure VCoNi is a uniform equiaxed fine-grained single-phase FCC structure, lacking a multi-scale grain-coordinated deformation mechanism. During tensile testing, dislocations easily accumulate in large quantities at grain boundaries, leading to undispersed local stress concentrations and premature microcrack initiation at grain boundaries. The elongation after fracture in the as-cast state is only 19.5%, making it difficult to meet the requirements of plastic forming processes such as stamping and bending. Poor hardness and wear resistance: The lattice distortion of a single VCoNi matrix is limited, resulting in low dislocation slip resistance and a Vickers hardness of only 257.6 HV. Under frictional shear loads, the surface layer is prone to large-scale plastic flow, producing large-area blocky fatigue spalling, failing to form a uniform and stable friction lubrication layer, and exhibiting poor wear resistance. Non-atomic V... 18 Co 42 Ni 40 As-cast alloys have extremely poor properties: As-cast V 18 Co 42 Ni 40 The alloy exhibits a coarse dendritic structure with severe elemental segregation. Brittle segregated phases are enriched between the dendrites. Its tensile strength is only 370 MPa, elongation is 12%, and hardness is only 234.3 HV. Its strength, plasticity, and hardness are all low, making it unsuitable for engineering applications.
[0004] Existing VCoNi alloys rely solely on a single, uniform equiaxed FCC solid solution structure, lacking precise microstructure control methods: they do not construct multi-scale mixed-crystal structures through alloy element doping, nor do they have a dedicated homogenization annealing process for segregated dendritic alloys, thus failing to simultaneously achieve synergistic improvements in strength, plasticity, and wear resistance. Summary of the Invention
[0005] The purpose of this invention is to provide a high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy and its preparation method, addressing the shortcomings of existing VCoNi-based medium-entropy alloys, such as poor plasticity, low hardness, and insufficient wear resistance. 18 Co 42 Ni 40 The problem of severe segregation and weak comprehensive mechanical properties in as-cast alloys is addressed by simultaneously developing a complete smelting and heat treatment process. This process improves the alloy's plasticity, hardness, and wear resistance while maintaining the single-phase FCC crystal structure. The process is simple and easy to scale up for production.
[0006] To achieve the above objectives, this invention provides a high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy, comprising Co, Ni, V, Al, and Ti metal particles with a purity of not less than 99.9 wt%, and chemical formulas VCoNi and (VCoNi). 94 Al x Ti y V 18 Co 42 Ni 40 The value of x ranges from 2 to 4, and the value of y ranges from 2 to 4.
[0007] Preferably, VCoNi contains 30.22 wt% V, 34.96 wt% Co, and 34.82 wt% Ni.
[0008] Preferably, x takes the value of 3, y takes the value of 3, and (VCoNi) 94 Al3Ti3 contains 29.03 wt% V, 33.58 wt% Co, 33.45 wt% Ni, 1.47 wt% Al, and 2.47 wt% Ti.
[0009] Preferred, V 18 Co 42 Ni 40 It contains 16.05 wt% V, 43.14 wt% Co, and 40.81 wt% Ni.
[0010] This invention also provides a method for preparing a high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy, comprising the following steps: Step 1: Mix the metal particles, sand them with sandpaper to remove the oxide layer on the surface of the metal particles, weigh them, place them in an ultrasonic cleaner, ultrasonically clean them with anhydrous ethanol for 30 minutes, and air dry them naturally in the air to eliminate surface oxidation pollution. Step 2: Place the metal granule raw material into a vacuum electric arc furnace for melting, and evacuate to a vacuum level of 3.2 × 10⁻⁶. -3 ~3.5×10 -3 Pa, fill the furnace with 99.99wt% high-purity argon gas to a pressure of -0.04 to -0.08 MPa to isolate it from air and prevent oxidation; Step 3: The alloy is repeatedly melted no less than 5 times. During the 2nd and 4th melting, magnetic stirring is turned on for 30 seconds to promote uniform diffusion of elements and eliminate micro-component segregation. Step 4: After melting, allow the alloy to cool naturally in the furnace or perform heat treatment. For heat treatment, place the melted alloy in a vacuum furnace, maintaining a vacuum level of 6.6 × 10⁻⁶. -3 ~6.7×10 -3 Pa is used to prevent oxidation. The temperature is increased to the annealing temperature of 800-900℃ at a heating rate of 3-7℃ / min, held for 20-35min, and then cooled in the furnace at a rate of 3℃ / min to eliminate residual stress.
[0011] Preferably, in step 4, the heat treatment heating rate is 5℃ / min, the annealing temperature is 850℃, and the holding time is 30min.
[0012] The advantages and beneficial effects of the present invention using the above-mentioned high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy and its preparation method are as follows: 1. The alloy of this invention exhibits significantly improved plasticity and strength (VCoNi) 94 The Al3Ti3 alloy exhibits a room temperature elongation after fracture of 28.5%, which is 46% higher than that of the VCoNi matrix (19.5%). Simultaneously, its tensile strength is 735 MPa, achieving an optimized balance between strength and plasticity, which is beneficial for plastic forming.
[0013] 2. The present invention uses 850℃ annealing V 18 Co 42 Ni 40 The medium-entropy alloy has a yield strength of 550 MPa, a tensile strength of 850 MPa, and an elongation after fracture of 18%. At this point, V... 18 Co 42 Ni 40 The medium-entropy alloy exhibits a significant improvement in both strength and plasticity, with tensile strength increasing by approximately 130% and elongation by 50% compared to the as-cast alloy.
[0014] 3. The present invention significantly improves hardness and wear resistance (VCoNi). 94 The microhardness of the Al3Ti3 alloy increased from 257.6 HV to 334.9 HV compared to the VCoNi matrix, representing a 30% increase. Friction and wear cross-sectional morphology showed that the modified alloy exhibited significantly reduced wear spalling pits, a more uniform distribution of the plastic rheological layer, and superior wear resistance compared to the VCoNi matrix.
[0015] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0016] Figure 1Flowchart for the preparation of high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloys; Figure 2 These are metallographic micrographs of the VCoNi alloy before and after room temperature quasi-static tensile testing of the present invention; where A represents before tensile testing and B represents after tensile testing. Figure 3 This invention (VCoNi) 94 Metallographic micrographs of Al3Ti3 alloy before and after quasi-static tensile testing at room temperature; where A represents before tensile testing and B represents after tensile testing. Figure 4 V before and after heat treatment at 850℃ in this invention 18 Co 42 Ni 40 Metallographic images of the microstructure of a medium-entropy alloy, where A is an image before heat treatment, B is a tensile image before heat treatment, C is an image after heat treatment, and D is a tensile image after heat treatment. Figure 5 The XRD diffraction pattern of the VCoNi-based medium-entropy alloy of this invention; Figure 6 The present invention relates to VCoNi and (VCoNi) 94 Room temperature stretched micro-region XRD diffraction pattern of Al3Ti3; Figure 7 The stress-strain curves for the VCoNi-based alloy at room temperature in this invention are shown. Figure 8 This is a bar chart showing the average Vickers hardness of the VCoNi-based alloy of this invention. Figure 9 The present invention relates to VCoNi and (VCoNi) 94 Metallographic morphology of Al3Ti3 alloy under tribological wear, where A represents VCoNi and B represents (VCoNi). 94 Al3Ti3; Figure 10 The present invention relates to VCoNi and (VCoNi) 94 Tribology and wear curves of Al3Ti3 alloy. Detailed Implementation
[0017] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments.
[0018] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.
[0019] The following examples are not intended to limit the invention, but are only for illustration. Unless otherwise specified, the experimental methods used in the following examples are generally performed under conventional conditions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0020] Example 1 A high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy, comprising Co, Ni, V, Al, and Ti metal particles with a purity of not less than 99.9 wt%, with the chemical formulas VCoNi and (VCoNi). 94 Al x Ti y V 18 Co 42 Ni 40 The values of x and y range from 2 to 4. The range of x and y refers to the range of atomic percentages.
[0021] Select Co, Ni, V, Al, and Ti metal particles with a purity of not less than 99.9 wt%. Prepare the mixture (VCoNi) according to the atomic percentages in Table 1. 94 Al3Ti3, VCoNi and V 18 Co 42 Ni 40 Alloy. Each ingot has a total mass of 100g.
[0022] Table 1. Element ratios in the optimal alloy (g)
[0023] (VCoNi) 94 The method for preparing Al3Ti3 alloy includes the following steps: (1) Raw material pretreatment Select V, Co, Ni, Al, and Ti metal particles with a purity ≥99.9wt%; sandpaper is used to remove the oxide scale on the surface of the particles, and the particles are weighed precisely according to the formula; they are placed in a KQ2200DA ultrasonic cleaner and ultrasonically cleaned with anhydrous ethanol for 30 minutes, and then air-dried naturally to eliminate surface oxidation contamination.
[0024] (2) Vacuum arc melting casting of ingots ① Place the dried metal raw material into a DHL-500 vacuum arc furnace and evacuate it to a vacuum level of 3.5 × 10⁻⁶. -3 Pa, fill the furnace with 99.99wt% high-purity argon gas to a pressure of -0.06MPa to isolate it from air and prevent oxidation.
[0025] ② The alloy is repeatedly smelted no less than 5 times. During the 2nd and 4th smelting, magnetic stirring is turned on for 30 seconds to promote uniform diffusion of elements and eliminate micro-component segregation.
[0026] ③ After melting, the material is allowed to cool naturally in the furnace to obtain the as-cast state (VCoNi). 94 Al3Ti3 medium entropy alloy ingot.
[0027] like Figure 1 As shown, V 18 Co 42 Ni 40 Medium-entropy alloy heat treatment strengthening preparation process: Step A: Vacuum arc melting and casting of ingots (same as (VCoNi)) 94 Al3Ti3 smelting parameters).
[0028] Raw material pretreatment, vacuum melting, and magnetic stirring processes are fully compatible with (VCoNi). 94 Al3Ti3 was used to prepare as-cast dendritic V 18 Co 42 Ni 40 Alloy ingots.
[0029] Step B: Special vacuum homogenization annealing treatment.
[0030] ① Place the ingot into an SLG1400-100A vacuum tube furnace and evacuate it to a vacuum level of 6.67 × 10⁻⁶. -3 Pa.
[0031] ② The heating rate is 5℃ / min, the temperature is raised to 850℃, and the temperature is held constant for 30min to release the residual casting stress and eliminate dendrite segregation.
[0032] ③ Slowly cool to room temperature at 3℃ / min in the furnace to obtain annealed modified high strength and toughness V 18 Co 42 Ni 40 Medium entropy alloy.
[0033] The method for preparing VCoNi alloy includes the following steps: (1) Raw material pretreatment Select V, Co, and Ni metal particles with a purity ≥99.9wt%; sandpaper is used to remove the oxide scale on the surface of the particles, and the particles are weighed precisely according to the formula; they are placed in a KQ2200DA ultrasonic cleaner and ultrasonically cleaned with anhydrous ethanol for 30 minutes, and then air-dried to eliminate surface oxidation contamination.
[0034] (2) Vacuum arc melting casting of ingots ① Place the dried metal raw material into a DHL-500 vacuum arc furnace and evacuate it to a vacuum level of 3.2 × 10⁻⁶. -3 Pa, fill the furnace with 99.99wt% high-purity argon gas to a pressure of -0.07MPa to isolate it from air and prevent oxidation.
[0035] ② The alloy is repeatedly smelted no less than 5 times. During the 2nd and 4th smelting, magnetic stirring is turned on for 30 seconds to promote uniform diffusion of elements and eliminate micro-component segregation.
[0036] ③After smelting, the mixture is naturally cooled in the furnace to obtain a cast VCoNi medium-entropy alloy ingot.
[0037] Comparative Example 1 V 18 Co 42 Ni 40 Medium-entropy alloy preparation process: Step A: Vacuum arc melting and casting of ingots (same as (VCoNi)) 94 Al3Ti3 smelting parameters).
[0038] The raw material pretreatment, vacuum melting, and magnetic stirring processes are completely consistent with those in Example 1 (VCoNi). 94 Al3Ti3 was used to prepare as-cast dendritic V 18 Co 42 Ni 40 Alloy ingots.
[0039] Tensile specimen preparation: Dog-bone shaped tensile specimens were prepared by wire cutting, with parallel section dimensions of 10mm × 2.0mm × 1.5mm; they were then progressively ground and polished using 400# to 2000# silicon carbide sandpaper before testing. The results are shown in Table 2.
[0040] Performance testing standards: Tensile test: INSTRON 5982 universal testing machine, strain rate before yielding 1.25 × 10⁻⁶ -3 s -1 After yielding, 2.5 × 10 -3 s -1 .
[0041] Hardness test: FM-300 Vickers hardness tester, load 100N, hold for 10s, take the average value of 10 effective indentations.
[0042] Friction and wear: HSR-2M reciprocating friction tester, Si3N4 grinding ball diameter 6mm, load 10N, frequency 5Hz, amplitude 5mm, test for 30min.
[0043] Tissue and structural characterization: The samples were observed after being etched with aqua regia (HCl:HNO3=3:1) for 30 seconds using an Ultimate IV XRD diffractometer (Cu target λ=0.15406nm, scanning 10°~90°) and an OLYMPUS-GX53 metallographic microscope.
[0044] Table 2 Test Results
[0045] I. Quasi-static mechanical properties 1. Oxidation Matrix Analysis of VCoNi Before and After Stretching Figure 2 A represents the original metallographic structure of the as-cast VCoNi alloy. Figure 2 Figure B shows the microstructure of the alloy after room temperature quasi-static tensile testing. The as-cast VCoNi alloy has relatively fine and uniform grains, with a dense grain arrangement and no coarse grains or obvious structural defects. After room temperature high-strain tensile deformation, the microstructure of the alloy changed significantly. The grains showed obvious elongation along the direction of tensile stress, and the interface shape between grains was distorted due to plastic flow. Under continuous external load, dislocations continuously accumulated and grew at the grain boundaries, and the degree of local grain deformation gradually increased. The orientation characteristics of the microstructure clearly show the coordinated grain slip and flow behavior during plastic deformation. This microstructure change is consistent with the continuous work hardening characteristics exhibited by the room temperature tensile curve, demonstrating from a microscopic perspective the intrinsic principle that the VCoNi single-phase FCC alloy relies on grain slip to complete plastic deformation.
[0046] 2. (VCoNi) 94 OM analysis of Al3Ti3 before and after stretching Figure 3 In the middle, A represents the as-cast state (VCoNi). 94 The original metallographic structure of Al3Ti3 Figure 3 In the middle, B is (VCoNi). 94 The microstructure of Al3Ti3 after quasi-static stretching at room temperature. The as-cast modified alloy exhibits typical multi-scale mixed grain characteristics, with a wide range of grain sizes, and fine and large grains interspersed without obvious preferred orientation. The grain configuration is a microstructure characteristic caused by the solid solution modification of Al and Ti elements, which is also the reason for the good plasticity potential of the modified alloy. After large plastic deformation at room temperature, the original equiaxed grains of the alloy undergo large tensile distortion along the load direction. The grains are elongated, twisted, and exhibit obvious deformation orientation. The grain boundary morphology is significantly bent under the action of plastic flow. The multi-scale grains exhibit different deformation behaviors during deformation. Fine grains first coordinate intergranular slip and disperse local stress, while large grains are gradually elongated with deformation. The anisotropy of the microstructure reflects the deformation process in which multi-scale grains jointly bear and disperse stress. Compared with the microstructure of VCoNi alloy after stretching, the mixed-grain structure can alleviate the local stress concentration. This explains the improvement of alloy plasticity after Al and Ti microalloying from the perspective of microstructure, which is consistent with the changes in room temperature tensile mechanical properties mentioned earlier.
[0047] 3. V before and after heat treatment at 850℃ 18 Co42 Ni 40 OM analysis before and after stretching Figure 4 A is V 18 Co 42 Ni 40 Metallographic images of the medium-entropy alloy show a typical dendritic morphology, with clearly visible dendrites exhibiting a distinct crystal orientation. The dendrite spacing is 50–100 μm. Due to the rapid cooling rate, the dendrites exhibit a fine internal structure, while a small amount of discontinuous segregated phases exist between the dendrites. During solidification, the alloy transforms from a liquid phase to α-FCC dendrites. (V) 18 Co 42 Ni 40 In medium-entropy alloys, Co and Ni elements form compositional segregation during solidification, and rapid solidification leads to dendrite refinement.
[0048] Figure 4 B is V 18 Co 42 Ni 40 Metallographic images of the as-cast tensile fracture show a uniform grayscale distribution with no obvious zoning or localized deformation zones. The dendrite morphology remains largely unchanged, although dendrite arms exhibit bending and twisting. The interdendritic distribution is continuous, but the morphology is somewhat elongated. The bending of the dendrite arms is due to dislocation slip causing plastic deformation of the dendrite trunks. The absence of obvious slip bands indicates relatively uniform alloy deformation and the absence of concentrated shear bands. The alloy undergoes coordinated deformation leading to elongation of the interdendritic region, without early cracking, localized stress concentration, or porosity. Based on the microstructure before the tensile test, it can be inferred that the as-cast V... 18 Co 42 Ni 40 The tensile fracture process of medium-entropy alloys. During tension, the alloy first undergoes uniform slip, followed by work hardening, then neck formation, and then micropores initiate, grow, and aggregate between dendrites, ultimately leading to ductile fracture of the alloy.
[0049] Figure 4 C in the middle is V after annealing at 850℃ 18 Co 42 Ni 40 Metallographic images of the medium-entropy alloy show fragmented dendrites, no longer maintaining a complete dendritic structure. The microstructure tends towards equiaxed formation, but retains some directional traces. The dark phase is diffusely distributed, no longer forming a continuous network. The grain size is significantly refined, with numerous annealing twins appearing. The second phase particles are small, dispersed, and uniformly distributed in the matrix. These characteristics indicate that V 18 Co 42 Ni 40 The medium-entropy alloy undergoes significant microstructure homogenization during annealing at 850℃, resulting in the formation of equiaxed crystals and refining the grain size. Simultaneously, the formation of twinned structures after annealing further refines the grain size.
[0050] Figure 4 D is V 18 Co 42 Ni 40 Metallographic images of a medium-entropy alloy subjected to tensile fracture after annealing at 850℃. The images clearly show numerous micropores and microcracks, with significant microstructural refinement, especially in areas of concentrated deformation. Numerous circular / elliptical micropores are precursors to dimples. Due to localized deformation, preferential nucleation in soft areas leads to uneven pore distribution, alternating between dense and sparse zones. Deformation twinning results in twinning, and recrystallization during dynamic recovery / heat treatment further refines the matrix. Undissolved precipitates become nucleation sites for pores. The densely pored areas exhibit extremely high pore density and large pore size, with a swirling matrix morphology, representing the final fracture zone. Some pores have coalesced, forming crack fronts. The transitional deformation zone shows a more uniform pore distribution. Clear parallel striations are visible due to deformation twinning, with the twins at approximately 45° to the direction of maximum shear stress. The microstructure shows significant elongation and refinement. The uniformly pored areas have smaller and sparser pores, but fine twin traces are still visible, indicating a uniform deformation zone away from necking. Based on the microstructure, V can be inferred. 18 Co 42 Ni 40 The tensile fracture process of a medium-entropy alloy in the annealed state at 850℃. First, elastic deformation occurs, and dislocations move within the fine grains. Subsequently, the interaction between twinning and dislocations leads to an increase in work hardening stress. Micropores nucleate, grow, and aggregate at the second phase and grain boundaries, eventually forming necking, and finally the alloy fractures.
[0051] 4. VCoNi and (VCoNi) 94 XRD analysis of Al3Ti3 before and after stretching This experiment used an X-ray diffractometer from Rigaku Ultimate IV in Japan to analyze as-cast VCoNi and (VCoNi). 94 Crystal structure analysis was performed on the Al3Ti3 alloy. A thoroughly polished but uncorroded sample was placed in a metal frame and fixed in the center using double-sided tape, ensuring the sample surface was flush with the frame. The sample was then fed into an XRD instrument, with a scanning range of 10°–90° and a scanning rate of 5 deg / min; the wavelength and step size were 0.154 deg and 0.02 deg, respectively. The obtained data was imported into JADE for analysis, and the processed data was imported into Origin for plotting. Figure 5 As shown.
[0052] For cast VCoNi alloy and (VCoNi) 94 X-ray diffraction analysis was performed on the Al3Ti3 alloy, and the results are as follows: Figure 5 As shown in the figure. The figure shows the as-cast VCoNi alloy and (VCoNi) alloy. 94X-ray diffraction results of Al3Ti3 modified alloy. The diffraction spectrum of the undoped Al and Ti VCoNi alloy showed only one set of characteristic diffraction peaks corresponding to the face-centered cubic (FCC) crystal structure, matching the standard diffraction positions of the (111), (200), and (220) crystal planes of the FCC structure. No additional impurity diffraction peaks were generated in the spectrum, confirming that the as-cast VCoNi alloy formed a single FCC-type solid solution phase under this preparation process. All elemental atoms were uniformly dissolved in the crystal lattice, without elemental segregation or intermetallic compound precipitation. After adding Al and Ti atoms larger than the matrix to the (VCoNi) alloy... 94 The diffraction pattern of the Al3Ti3 alloy still shows the three characteristic diffraction peaks of FCC crystals, but no characteristic diffraction signals of Al-Ti intermetallic compounds are present. This indicates that Al and Ti elements are not precipitated in large quantities as second-phase particles, but rather dissolved into the VCoNi alloy lattice through substitutional solid solution. Compared with the matrix alloy, all diffraction peaks of the modified sample have shifted towards the lower 2θ direction. According to Bragg's diffraction law, a decrease in diffraction angle means an increase in interplanar spacing, which is due to the lattice expansion caused by the replacement of the original matrix atoms by large-sized Al and Ti atoms, resulting in an increase in the lattice constant. In addition, the diffraction baseline of the modified alloy is slightly raised, and the diffraction peaks are slightly broadened. This is due to lattice distortion caused by the dissolution of foreign atoms and the accumulation of microscopic internal stress, which reduces the integrity of the crystal lattice. Based on the XRD diffraction characteristics, it can be seen that the doping of trace Al and Ti elements achieves lattice solid solution modification while maintaining the crystal structure of VCoNi alloy FCC, without destroying the phase composition characteristics of the matrix single-phase solid solution.
[0053] like Figure 5 As shown, the XRD pattern of the annealed state at 850℃ exhibits optimal structural characteristics, with peaks approaching the sharpness of the as-cast state. This indicates that annealing at 850℃ refines and homogenizes the grains, thereby improving the overall material properties. The accurate peak alignment indicates consistent lattice constants and the disappearance of compositional segregation, consistent with the characteristics of equiaxed fine-grained microstructures formed after significant microstructural homogenization. Secondly, the narrower peaks indicate more uniform grain size. The broadening effect of diffraction peaks from finer grains and the improvement in lattice integrity mutually constrain each other, resulting in peaks with both sufficient intensity and good resolution. Furthermore, the pattern obtained after annealing at 850℃ still lacks significant second-phase diffraction peaks, or only exhibits a few weak impurity peaks. This is because the higher annealing temperature dissolves the already formed σ phase, allowing the brittle phase to re-enter the matrix or form dispersed fine particles, thus eliminating the problems caused by the presence of a continuous network.
[0054] Room temperature tensile micro-area XRD test results are as follows Figure 6As shown. The diffraction pattern of the deformed VCoNi alloy sample shows only one set of characteristic diffraction peaks matching the FCC crystal structure, corresponding to the (111), (200) and (220) crystal plane positions, respectively. The diffraction peaks are sharp, confirming that the matrix maintains a single FCC solid solution configuration before and after tensile deformation; after the addition of Al and Ti, (VCoNi) 94 The Al3Ti3 gold diffraction pattern did not show characteristic diffraction signals of intermetallic compounds different from those of the FCC matrix. Even if precipitates exist at the microscopic level, they maintain a good coherent relationship with the matrix. The lattice distortion effect caused by coherent strain is ultimately reflected in the width of the diffraction peaks. Due to the high-density dislocations and residual internal stress in the lattice caused by tensile plastic deformation, the diffraction baselines of both alloys increased to varying degrees. Moreover, no new phase diffraction peaks were generated after large-strain stretching, indicating that the precipitate structure inside the alloy is stable under tensile load and will not decompose or undergo phase transformation. From the perspective of phase change, the micro-precipitates coherent with the matrix can achieve precipitation strengthening by pinning dislocations and restricting grain boundary movement. The multi-level mixed crystal structure induced by Al and Ti doping controls the plastic rheological properties, thus explaining from the perspective of crystal phase that the modified alloy has slightly lower strength but higher plasticity than the matrix.
[0055] 5. VCoNi and (VCoNi) 94 Room temperature mechanical properties analysis of Al3Ti3 Figure 7 It is a VCoNi alloy and (VCoNi) 94 The engineering stress-strain curves of Al3Ti3 alloy under quasi-static tensile stress at room temperature. The as-cast VCoNi alloy exhibits excellent high-strength properties, with an ultimate tensile strength of approximately 1070 MPa and a fracture strain of 24%. Its mechanical properties are related to its uniform equiaxed fine-grained single-phase FCC matrix containing a large number of high-density annealed twins. Fine-grained strengthening and twinning strengthening together endow the material with high tensile strength. The homogeneous solid solution matrix, free of second-phase precipitation, ensures good work hardening throughout the tensile deformation stage. After the addition of Al and Ti, (VCoNi)... 94The mechanical properties of the Al3Ti3 alloy exhibited a cyclical change. The peak tensile strength decreased to around 750 MPa, but the plastic deformation capacity was significantly improved, with the fracture elongation of the green curve specimen increasing to 39%. Based on the preceding microstructure analysis, Al and Ti solid solution doping altered the alloy grain morphology, forming a multi-scale mixed-grain structure. The refined grains better coordinate deformation between grains during plastic deformation and delay local necking, thus improving plasticity. Simultaneously, the mechanical degradation caused by grain size inhomogeneity is much greater than the strengthening gain caused by element solid solution, ultimately leading to a decrease in overall alloy strength and a significant increase in plasticity. The lower fracture strain of the blue curve specimen in the test is due to differences in local microstructure uniformity in the as-cast specimens and minor casting defects causing variations in mechanical properties. The comprehensive tensile results show that Al and Ti microalloying optimized the strength-plasticity ratio of the VCoNi alloy by controlling the matrix grain morphology and size distribution, effectively expanding the alloy's plastic deformation range with a slight sacrifice in tensile strength.
[0056] Depend on Figure 7 It can be seen that annealing at 850℃ V 18 Co 42 Ni 40 The medium-entropy alloy has a yield strength of 550 MPa, a tensile strength of 850 MPa, and an elongation after fracture of 18%. At this point, V... 18 Co 42 Ni 40 The medium-entropy alloy exhibits a significant improvement in both strength and ductility. Tensile strength is 130% higher than that of the as-cast alloy, and elongation is 50% higher. It also shows a high work hardening rate, with the curve rising continuously until fracture, exhibiting no obvious necking followed by a rapid decline, and a relatively gradual fracture process. Combined with the microstructure, V... 18 Co 42 Ni 40 Medium-entropy alloys may undergo microstructural homogenization upon annealing at 850℃, forming fine and uniform equiaxed grains. The fracture curve rises continuously until fracture, without significant necking, then rapidly declines, indicating a relatively gradual fracture process. Combined with the microstructure, V... 18 Co 42 Ni 40 Medium-entropy alloys may undergo microstructure homogenization when annealed at 850℃, forming a fine and uniform equiaxed crystal structure.
[0057] II. Microhardness Figure 8 It is as-cast VCoNi and (VCoNi) 94 The average Vickers hardness histogram of Al3Ti3 alloy; the average hardness of VCoNi alloy is 257.6 HV, obtained by adding Al and Ti elements (VCoNi).94 The average hardness of the Al3Ti3 alloy reached 337.9 HV, an increase of 29.9% compared to the original. According to the original test data distribution, the hardness of the VCoNi alloy ranged from 224.2 to 345.2, showing low data dispersion. The modified alloy, however, ranged from 248.5 HV to 567 HV. The locally higher hardness values are due to variations in grain size in the as-cast structure and microscopic elemental segregation. Based on the aforementioned metallographic changes, the increased alloy hardness is achieved through multiple strengthening mechanisms. Al and Ti atoms dissolve into the FCC matrix lattice via substitution, and the difference in atomic size causes lattice distortion. Solid solution strengthening increases the resistance to dislocation slip. Furthermore, Al and Ti doping alters the solidification process, transforming the matrix from a uniform equiaxed crystal to a multi-scale mixed crystal. Fine-grained regions rely on fine-grain strengthening to limit grain boundary migration and dislocation multiplication. The combined strengthening effects of these mechanisms result in better resistance to indentation deformation. The macroscopic hardness results directly demonstrate the control effect of Al and Ti microalloying on the microstructure of VCoNi alloy, and the difference in hardness is related to the better wear resistance of the modified alloy in subsequent friction and wear tests.
[0058] like Figure 8 As shown, for the as-cast V 18 Co 42 Ni 40 Analysis of the medium-entropy alloy data showed an average hardness of 234.3 HV across eight data sets. Hardness testing revealed that the hardness values of the as-cast alloy ranged from 203.3 HV to 267.0 HV, a difference of 63.7 HV, representing a relative fluctuation of approximately 27.2%. This indicates poor homogeneity of the as-cast microstructure and significant dispersion in the hardness data. Metallographic analysis further revealed a typical dendritic morphology in the as-cast alloy, with compositional segregation existing in the dendrite trunks and interdendritic regions. The dendrite trunks were enriched in high-melting-point V, while the interdendritic regions were primarily enriched in Co and Ni.
[0059] like Figure 8 As shown, for V annealed at 850℃ 18 Co 42 Ni 40Data analysis of medium-entropy alloys showed an average hardness of 335.3 HV across eight data sets. The data ranged from 248.5 HV to 385.6 HV, a difference of 137.1 HV, representing a relative fluctuation of approximately 40.9%. Combining metallographic and XRD results, annealing at 850℃ resulted in significant microstructure homogenization, forming an equiaxed fine-grained structure. XRD analysis indicated that the brittle phases largely dissolved after annealing at 850℃, forming a near-single-phase FCC solid solution, thus eliminating the contribution of precipitation strengthening to hardness. Regarding the significant dispersion, upon reviewing the original data, it was noted that after removing the maximum value of 392.5 HV and the minimum value of 211.3 HV, two maxima of 248.5 HV and 385.6 HV remained. This indicates that the microstructure annealed at 850℃ contains two regions with different properties: a higher hardness region characterized by well-refined grains and a small amount of dispersed precipitates, and a lower hardness region characterized by excessive recrystallization, grain growth, and softening. Under high magnification tensile metallographic observation, there are also obvious regional divisions, with a dense area on the left and a porous area on the right coexisting. This heterogeneity in the structure is also reflected in the significant changes in hardness.
[0060] III. Metallographic Observation of Wear Figure 9 China A Figure 9 In the diagram, B represents VCoNi and (VCoNi) respectively. 94 The metallographic morphology of the friction and wear cross-section of Al3Ti3 alloys was uniformly scaled to 200 μm. Both alloys exhibited a surface plastic rheological layer that directionally extended along the friction sliding direction. However, due to differences in microstructure, the degree of surface wear damage and rheological characteristics differed significantly between the two. The VCoNi alloy showed a larger overall thickness of the wear rheological band, with numerous continuous spalling pits and large fragmentation damage on the wear surface. Under cyclic frictional shear loads, the surface material was prone to plastic tearing and blocky spalling. This phenomenon is because the matrix is a single-phase FCC solid solution structure, lacking a hard reinforcing phase to restrict plastic deformation. Frictional shear stress accumulates locally on the surface, continuously promoting unimpeded dislocation slip and causing surface fatigue spalling. After Al and Ti microalloying, (VCoNi)... 94 The Al3Ti3 alloy exhibits a more uniform distribution of wear rheological layer thickness, reduced size and density of surface spalling pits, and controlled excessive plastic rheology. The multi-scale mixed-grain structure within the alloy disperses frictional contact stress, allowing different grains to collectively bear the burden of consuming frictional work, preventing localized stress concentration and large-scale wear debris detachment, and improving the surface's resistance to shear deformation. These differences in cross-sectional wear morphology are consistent with room-temperature hardness test results. Al and Ti doping-induced grain configuration modifications improve the matrix surface's damage resistance, thereby enhancing the alloy's wear resistance.
[0061] IV. Friction Curve Analysis Figure 10 The friction and wear curves show that during the initial running-in phase (0–2 min), the friction coefficients of both materials rapidly increased from low values and exhibited significant fluctuations. Specifically, the initial friction coefficient of the VCoNi alloy was 0.66, while that of (VCoNi)... 94 The initial friction coefficient of the Al3Ti3 alloy was 0.61. During the initial running-in phase, the VCoNi curve showed a low value of 0.40 at 0.03 min, followed by a rapid increase; (VCoNi) 94 The Al3Ti3 curve dropped to 0.17 at 0.03 min and then quickly rebounded. This is because the micro-protrusions on the friction pair surface undergo plastic deformation, shearing, and fracture in the initial contact phase, causing a rapid increase in the actual contact area and consequently, a greater frictional resistance. Among them, (VCoNi) 94 The Al3Ti3 curve rises at a slower rate than the VCoNi curve, indicating that the surface of materials containing Al and Ti phases can form a transitional adaptation layer through slight wear to mitigate the sharp increase in the friction coefficient. After entering the transition stage (2–6 min), the VCoNi curve becomes relatively flat around 3 min, with significantly reduced fluctuations, and its friction coefficient mainly ranges between 0.50 and 0.60, indicating a fast break-in speed and strong break-in convergence ability; however, (VCoNi)... 94 The Al3Ti3 curve showed a slow upward trend, with its friction coefficient gradually increasing from approximately 0.57 at 2 minutes to approximately 0.61 at 6 minutes, before reaching a relatively stable state around 5 minutes. This indicates that the presence of Al and Ti reinforcing phases prolonged the break-in time, possibly due to their high hardness and influence on surface shear behavior. During the stable wear phase (6–10 minutes), the friction coefficients of both curves remained relatively constant, but significant differences existed between them. The VCoNi alloy exhibited a lower steady-state friction coefficient, averaging approximately 0.556, with a maximum value of 0.73 and a minimum of 0.40 throughout the process, fluctuating between 0.50 and 0.56 in steady state. The small fluctuation range suggests good self-lubrication or low shear strength during sliding contact, which is related to the fact that the solid solution composed of Co, Ni, and V readily produces oxides with anti-friction properties under frictional heat. In contrast, (VCoNi)… 94The Al3Ti3 alloy exhibits a significantly higher steady-state coefficient of friction, averaging approximately 0.594, reaching a maximum of 0.70, and a minimum of approximately 0.57 in the steady-state stage, with greater periodic fluctuations. Generally, the repeated processes of microcrack formation, wear debris accumulation, and spalling at the contact surface induce periodic fluctuations. Therefore, while the addition of Al and Ti can improve the material's hardness and wear resistance, it can also reduce the self-healing ability of the surface film or increase the ploughing effect between friction pairs, leading to an increase in the coefficient of friction and decreased stability. Under the experimental conditions, the VCoNi alloy exhibits a low coefficient of friction and stable wear, while (VCoNi)... 94 The Al3Ti3 alloy exhibits a high and fluctuating coefficient of friction due to the presence of a reinforcing phase.
[0062] VCoNi medium-entropy alloys with a single-phase FCC structure rely on dislocation slip for plastic deformation at room temperature. However, their uniform equiaxed fine-grained structure makes it difficult to coordinate local stress concentrations, thus limiting room-temperature plasticity. The addition of trace amounts of Al and Ti allows the alloy to maintain its FCC structure while forming a multi-scale mixed-grain structure. Through the synergistic deformation of fine-grain slip and coarse-grain twinning, stress is dispersed and microcrack initiation is suppressed, significantly improving room-temperature plasticity. Simultaneously, the combined effect of lattice distortion and solid solution strengthening increases hardness by approximately 30%, and wear resistance is improved by dispersing frictional contact stress and reducing surface spalling. Annealing at 850℃ effectively releases the deformation energy stored within the alloy, completely eliminating residual casting stress. Simultaneously, the randomly distributed dislocations within the alloy undergo slip and climb, and low-dislocation-density intact grains gradually replace the high-defect structure, achieving dynamic grain recovery and static recrystallization. At the same time, the Co, Ni, and V matrix atoms inside the alloy diffuse uniformly, the lattice distortion tends to be more regular, and the atomic arrangement order is significantly improved, avoiding the problem of abnormal grain growth caused by high-temperature over-annealing, and finally forming a mixed crystal structure with alternating fine and coarse grain gradients.
[0063] Therefore, this invention employs the aforementioned high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy and its preparation method. By simultaneously adding Al and Ti to the VCoNi matrix, a multi-scale mixed-grain structure is constructed while maintaining the single-phase FCC crystal structure, thereby simultaneously improving the alloy's plasticity, hardness, and wear resistance. Specifically targeting V... 18 Co 42 Ni 40 A precise 850℃ temperature-controlled annealing process has been developed for dendritic segregation alloys to break up dendrites and eliminate compositional segregation, resulting in a significant simultaneous improvement in strength, plasticity, and hardness. The accompanying vacuum arc melting and segmented magnetic stirring processes ensure uniform composition. This approach, with its low raw material costs and simple, easily scalable production, addresses the industry pain points of existing VCoNi medium-entropy alloys, such as insufficient plasticity, poor wear resistance, and weak performance of non-equiatomic as-cast alloys. It can be widely used in wear-resistant structural parts, plastically formed metal components, and other fields.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A high-strength, high-toughness, and wear-resistant VCoNi-based medium-entropy alloy, characterized in that, It includes Co, Ni, V, Al, and Ti metal particles with a purity of not less than 99.9 wt%, and chemical formulas VCoNi and (VCoNi). 94 Al x Ti y V 18 Co 42 Ni 40 The value of x ranges from 2 to 4, and the value of y ranges from 2 to 4.
2. The high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy according to claim 1, characterized in that: VCoNi contains 30.22 wt% V, 34.96 wt% Co, and 34.82 wt% Ni.
3. The high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy according to claim 1, characterized in that: The value of x is 3, the value of y is 3, and (VCoNi) 94 Al3Ti3 contains 29.03 wt% V, 33.58 wt% Co, 33.45 wt% Ni, 1.47 wt% Al, and 2.47 wt% Ti.
4. The high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy according to claim 1, characterized in that: V 18 Co 42 Ni 40 It contains 16.05 wt% V, 43.14 wt% Co, and 40.81 wt% Ni.
5. The method for preparing the high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy according to any one of claims 1-4, characterized in that, Includes the following steps: Step 1: Mix the metal particles, sand them with sandpaper to remove the oxide layer on the surface of the metal particles, weigh them, place them in an ultrasonic cleaner, ultrasonically clean them with anhydrous ethanol for 30 minutes, and air dry them naturally in the air to eliminate surface oxidation pollution. Step 2: Place the metal granule raw material into a vacuum electric arc furnace for melting, and evacuate to a vacuum level of 3.2 × 10⁻⁶. -3 ~3.5×10 -3 Pa, fill the furnace with 99.99wt% high-purity argon gas to a pressure of -0.04 to -0.08 MPa to isolate it from air and prevent oxidation; Step 3: The alloy is repeatedly melted no less than 5 times. During the 2nd and 4th melting, magnetic stirring is turned on for 30 seconds to promote uniform diffusion of elements and eliminate micro-component segregation. Step 4: After melting, allow the alloy to cool naturally in the furnace or perform heat treatment. For heat treatment, place the melted alloy in a vacuum furnace, maintaining a vacuum level of 6.6 × 10⁻⁶. -3 ~6.7×10 -3 Pa is used to prevent oxidation. The temperature is increased to the annealing temperature of 800-900℃ at a heating rate of 3-7℃ / min, held for 20-35min, and then cooled in the furnace at a rate of 3℃ / min to eliminate residual stress.
6. The method for preparing the high-strength, tough, and wear-resistant VCoNi-based medium-entropy alloy according to claim 5, characterized in that: In step 4, the heat treatment heating rate is 5℃ / min, the annealing temperature is 850℃, and the holding time is 30min.