A method for producing high-strength hot-dip galvanized structural steel with a strength of 700MPa or higher.

By designing a low-carbon, high-manganese, and low-silicon composition and strengthening it with titanium alloy precipitation, combined with optimized rolling and hot-dip galvanizing processes, the problems of high cost and insufficient performance of existing 700MPa-grade hot-dip galvanized high-strength steel have been solved. This has resulted in hot-dip galvanized structural steel with high strength, low yield strength ratio, and good deformation performance, suitable for applications in multiple fields.

CN123108408APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611420150.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing 700MPa grade hot-dip galvanized high-strength steel has high production costs, a high yield strength ratio, and a high risk of cold working cracking, making it difficult to simultaneously meet the comprehensive requirements of high strength, high toughness, and excellent deformation performance.

Method used

The steel is designed with low carbon, high manganese, and low silicon content, and is strengthened by precipitation by adding titanium alloy. Combined with optimized rolling and hot-dip galvanizing processes, including controlled rolling and cooling, low-reduction cold rolling, and continuous hot-dip galvanizing, it produces high-strength, high-ductility hot-dip galvanized structural steel.

Benefits of technology

This technology enables the production of hot-dip galvanized structural steel with low cost, high strength, low yield strength ratio, and good deformation performance. It is suitable for applications such as building steel frames and engineering machinery, reducing material usage and processing costs, and enhancing market competitiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a production method for high-strength hot-dip galvanized structural steel with a strength of 700MPa or higher, belonging to the field of metal material processing and manufacturing technology. Its chemical composition by weight percentage is: C: 0.15–0.20%, Si: ≤0.08%, Mn: 0.85–1.05%, P ≤0.020%, S ≤0.010%, Alt: 0.020–0.050%, Ti: 0.065–0.105%, with the balance being Fe and unavoidable impurities. The specific production method is also disclosed. This invention, through innovative low-cost design, optimizes the rolling process using controlled rolling and cooling, and employs a low reduction rate in the cold rolling mill, resulting in hot-dip galvanized steel strip with excellent surface finish and shape. The product possesses comprehensive properties such as high strength, low yield strength ratio, high elongation, low cost, easy forming, and high corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material processing and manufacturing technology, and in particular relates to a production method for high-strength hot-dip galvanized structural steel with a strength of 700MPa or higher. Background Technology

[0002] High-strength hot-dip galvanized structural steel is widely used in building steel structures, engineering machinery, power transmission towers, highway guardrails, and other fields. It must meet requirements for high strength and high toughness, as well as good cold deformation and bending performance, and excellent corrosion resistance. Existing 700MPa grade hot-dip galvanized high-strength steels mostly employ microalloying designs with precious alloying elements such as Nb, V, and Mo, using fine-grain strengthening and precipitation strengthening to improve strength. However, this approach suffers from high production costs, a high yield strength ratio, and a high risk of cold working cracking. Some Nb-free designs, or those with high silicon content, are prone to hot-dip galvanizing defects such as incomplete galvanizing and orange peel texture, or have poor strength-ductility matching, making it difficult to simultaneously meet the comprehensive requirements of high strength, high toughness, and excellent deformation performance. Therefore, developing a low-cost, Nb-free, low-silicon structural steel that combines high strength, high elongation, low yield strength ratio, and good adaptability to hot-dip galvanizing processes has significant engineering application value and economic significance. Meanwhile, in the current harsh market environment of overcapacity and increasingly fierce competition in the steel market, effectively reducing product usage costs, continuously upgrading products, and improving product market competitiveness and industry position are key to the future vitality of enterprises. By developing high-strength, high-toughness, and high-corrosion-resistant flagship products, we can replace thinner raw materials with stronger ones, reduce the thickness of component plates, effectively reduce steel consumption, and reduce steel usage by more than 10%. At the same time, we can reduce processing, transportation, and assembly costs, and reduce overall procurement costs by 10-15%. This not only ensures the safety of engineering use but also effectively helps the industry to reduce costs and increase efficiency, while reducing carbon emissions. Economic benefits and efficiency are improved simultaneously, and both enterprises and customers achieve quality and efficiency improvements. Therefore, the development of hot-dip galvanized high-strength steel with a strength of 700MPa and above is of milestone significance.

[0003] A search revealed that patent number CN 116179960 A is titled "A Thin-Grade GI High-Strength Steel Strip with a Yield Strength of 700MPa and Its Production Method." This patent employs a design with low carbon (0.15~0.18%), high manganese (1.0~1.2%), and high silicon (0.15~0.22%) as its main components, supplemented with a small amount of niobium alloy. The final product achieves a high yield strength ≥700MPa, high tensile strength ≥720MPa, and a high yield-to-tensile strength ratio of 0.97~0.99. While this product is characterized by high strength and hardness, the high yield-to-tensile strength ratio, despite niobium's grain-refining effect and reduced yield-to-tensile strength ratio in steel, indicates that the yield and tensile strength values ​​are almost identical. This results in poor plasticity and deformation capacity of the finished product, lacking good seismic resistance, impact resistance, and deformation performance, severely limiting the material's versatility in application.

[0004] Compared to the searched patents, this invention uses a low-carbon (0.15~0.20%), high-manganese (0.85~1.05%), and low-silicon (≤0.08%) main component design, and adds relatively inexpensive titanium alloy for precipitation strengthening. Although the carbon content range in the component design is similar, the main strengthening elements silicon and manganese differ significantly. The comparison patent uses niobium for grain refinement strengthening, while this patent uses titanium for precipitation strengthening, resulting in a completely different strengthening mechanism. The finished product has a tensile strength ≥700MPa (average 750MPa) and an elongation of 10~19. With a yield strength ratio of 0.80~0.95, it ensures product strength while possessing good deformation and bending performance, resulting in superior overall performance. It can meet various application conditions such as high strength, high toughness, high corrosion resistance, and certain deformation capacity, leading to better usage costs and market prospects. At the same time, through the optimized material usage scheme of replacing thinner materials with stronger ones, the total amount of steel used is effectively reduced while ensuring structural safety and performance, further compressing material, transportation, and processing costs. By replacing low-strength, thicker materials with high-strength, thinner ones, raw material costs can be reduced by at least 10%, resulting in significant cost reduction for the product.

[0005] A search revealed that patent number CN 116334470 A, entitled "A Production Method of High-Strength Structural Steel SGC570," is designed with low carbon, low silicon, and medium manganese content. The product belongs to the ordinary carbon steel series, and the rolling process uses a low-temperature controlled cooling process to improve the product's strength. The yield strength is less than 600 MPa, and the tensile strength is ≥570 MPa. It has the characteristics of low manufacturing cost, high strength, and good corrosion resistance. It is mainly exported to Southeast Asia and is widely used in general indoor and outdoor building structures.

[0006] Compared to the searched patents, the composition design of this invention belongs to the low-alloy high-strength series of steels. The composition design and strength level are not the same as those of the comparative patents. Moreover, the process technology and strengthening concept are quite different, and the grain structure of the finished product is completely different. The grain structure of this patent is ferrite + precipitates, while the grain structure of the comparative patent is ferrite + pearlite. The application scenarios and uses of the final product are completely different.

[0007] A search revealed that patent number CN 112813342 A is titled "A hot-dip galvanized steel strip for light steel with a strength of 600MPa and its preparation method." The patent uses a design with low carbon (0.05~0.10%), high manganese (1.0~1.3%), and high silicon (0.05~0.25%) as the main components, and adds a small amount of niobium alloy (0.012~0.020%) for secondary grain refinement. The final product achieves a high yield strength ≥630MPa, high tensile strength ≥670MPa, and a high yield-to-tensile ratio of 0.96~0.98. While this product is characterized by high strength and hardness, due to the high yield-to-tensile ratio, the finished product has poor plasticity and deformation capacity, lacking good seismic resistance, impact resistance, and deformation performance, severely limiting the material's applications. Compared to the searched patents, this invention adopts a design with low carbon (0.15~0.20%), high manganese (0.85~1.05%), and low silicon (≤0.08%) as the main components, and adds inexpensive titanium alloy to enhance performance through precipitation. The composition design of this patent differs significantly from the comparative patents. The finished coil has a yield strength ≥600MPa, tensile strength ≥700MPa (average 750MPa), elongation 10~19%, and yield strength ratio 0.80~0.95. While ensuring product strength, the product manufacturing cost is lower, resulting in stronger market competitiveness and profitability. Through reasonable control of composition and process, a low yield strength ratio is achieved, and the final product has good deformation and bending performance, with superior overall performance, meeting the requirements of high strength, high toughness, and strong deformation capacity in various applications. Summary of the Invention

[0008] The purpose of this invention is to provide a production method for high-strength hot-dip galvanized structural steel with a strength of 700MPa or higher. This method utilizes a carbon and manganese chemical composition design to achieve solid solution strengthening and TiN / TiC precipitation strengthening, resulting in an innovative, low-cost design. The rolling process employs optimized controlled rolling and cooling techniques, and a low-reduction cold-rolling mill, among other processes, to obtain hot-dip galvanized steel strips with excellent surface finish and shape. The finished steel strip exhibits tensile strength ≥700MPa (average 750MPa), elongation 10-19%, and yield strength ratio 0.80-0.95. While ensuring product strength, the product possesses comprehensive properties such as high strength, low yield strength ratio, high elongation, low cost, easy forming, and high corrosion resistance, meeting the demand for highly corrosion-resistant materials in various fields such as building steel frames, engineering machinery, and transportation safety.

[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0010] This invention discloses a method for producing high-strength hot-dip galvanized structural steel with a strength of 700 MPa or higher. The main steps for preparing the steel plate of this invention are as follows:

[0011] (1) KR desulfurization → converter smelting → LF refining → RH refining → slab continuous casting;

[0012] (2) Slab heating → high pressure water descaling → fixed width press → E1R1 roughing mill rolling → E2R2 roughing mill rolling → (insulation cover) → flying shear head and tail → high pressure water descaling → F1~F7 finishing mill rolling → dense laminar flow cooling → coiling → pallet transport system → weighing → warehousing;

[0013] (3) Pickling and uncoiling → welding → tension leveling → pickling → rinsing → drying → trimming → rolling → coiling → weighing → marking → bundling → warehousing;

[0014] (4) Hot-dip galvanizing uncoiling → welding → entrance looper → cleaning → annealing furnace → zinc pot → post-galvanizing cooling → water quenching → intermediate looper → finishing machine → stretching and straightening machine → roller coating machine → dryer → air cooling device → exit looper → (edge ​​trimming) → surface inspection → (oiling) → sampling and inspection → coiling → bundling and weighing → packaging → warehousing.

[0015] The key process points are as follows, which will be elaborated on in detail:

[0016] Step 1: At the end of the KR process desulfurization, the sulfur content in the molten iron must be ≤0.010%, and the slag removal ratio on the surface of the molten iron ladle must be ≥90%. The converter tapping temperature must be controlled at ≥1620℃. During the tapping process, ferromanganese and ferroaluminum are added to the ladle to deoxidize and alloy the molten steel once, and carbon particles and top slag lime are added. The start and end of the converter tapping process uses a sliding plate slag blocking operation to prevent converter slag from falling into the ladle.

[0017] Step 2: After the ladle is in place in the LF refining process, it is heated and desulfurized by slag making. During the slag making process, quicklime is added and the refining slag is made to achieve the effect of white slag, and the content of (FeO+MnO) in the slag is less than 1.5%. Alloys such as aluminum iron and manganese iron, as well as carbon particles, are added to adjust the composition to the range of LF off-site composition. LF off-site ensures that the S content in the molten steel is ≤0.005% and the off-site temperature is ≥1620℃. After LF off-site, it is hoisted to RH vacuum treatment.

[0018] Step 3: RH deep vacuum treatment removes hydrogen and nitrogen from the molten steel, further improving its cleanliness. The circulating flow rate during RH vacuum treatment is set within the range of 120 m³ / min to 150 m³ / min; the vacuum level must be less than 1.3 mbar, and the deep vacuum treatment time is 20 to 25 minutes. During the vacuum treatment, titanium-iron alloy and metallic manganese are added to further adjust the composition of the molten steel. After deep vacuum treatment, the molten steel undergoes calcium treatment. During calcium treatment, 200 m of high-calcium wire is fed in, and a reasonable argon flow rate is controlled to prevent the molten steel from being exposed. After calcium treatment, the soft blowing time must be ≥8 minutes to promote the flotation of inclusions in the molten steel and improve its cleanliness. The chemical composition and temperature of the molten steel after removal from the casting machine must meet the casting machine's pouring requirements.

[0019] Step 4: During the casting process, the ladle is protected by argon gas throughout. A slag detection device is activated during the ladle pouring process to prevent slag from flowing into the tundish at the end of the ladle pouring. Constant casting speed control is used during the casting process, with the speed set within the range of 1.1 m / min to 1.8 m / min depending on the different pouring sections. The superheat of the tundish pouring is controlled between 15℃ and 30℃. Billet inspection: The center segregation of the continuously cast billet must not exceed Class B, grade 1.0, and the center porosity must not exceed grade 1.0.

[0020] Step 5: In the hot rolling process, the slab is heated in the furnace using either hot or cold charging. A suitable heating regime is selected based on the thickness requirements: heating temperature range 1230~1270℃, furnace time 150-230 min, soaking temperature range 1240~1280℃, soaking time 20-45 min, and furnace exit temperature 1240-1280℃.

[0021] Step 5: The rolling process includes roughing and finishing. Roughing is performed using a 2-stand mill, and finishing is performed using a 7-stand continuous variable crown mill. The final rolling temperature of the finishing mill is 870~910℃. Cooling is performed using a laminar flow continuous cooling system with a cooling code setting of mode 11. The upper cooling nozzles are set to open every other nozzle, and the lower cooling nozzles are set to open every two nozzles. The coiling temperature is controlled within the range of 550~610℃ depending on the thickness.

[0022] Step 6: In the pickling and rolling process, the reduction rate is controlled within the range of 50-76% according to the thickness requirements of the order. To ensure good adhesion of the coating to the strip surface in the next process, the surface roughness of the rolls in the pickling and rolling process is 2.0-3.0μm. After rolling, the surface roughness of the strip must be greater than 1.0μm to ensure good adhesion between the strip and the galvanized coating and to avoid defects such as incomplete coating, coating peeling, and cracks on the strip surface.

[0023] Step 7: The continuous hot-dip galvanizing process uses a vertical continuous annealing furnace. A reducing protective atmosphere is used for cooling inside the furnace. The heating / soaking temperature range is 710~740℃, the slow cooling temperature is 620~660℃, and the rapid cooling temperature is 420~470℃, depending on the strip thickness. The strip temperature entering the zinc pot is 460~470℃, and the temperature of the molten zinc in the zinc pot ranges from 450~470℃. The coating thickness is determined according to order requirements, selecting appropriate air knife pressure. The strip speed in the furnace zone varies from 70~130 m / min depending on the thickness. The elongation rate of the leveling machine is 0.5~0.8%, and the elongation rate of the tension leveler is ≤0.2%.

[0024] Its chemical composition by weight percentage is as follows: C: 0.15-0.20%, Si: ≤0.08%, Mn: 0.85-1.05%, P ≤0.020%, S ≤0.010%, Alt: 0.020-0.050%, Ti: 0.065-0.105%, with the balance being Fe and unavoidable impurities.

[0025] Furthermore, its chemical composition by weight percentage is: C: 0.17%, Si: 0.06%, Mn: 0.94%, P: 0.010%, S: 0.003%, Alt: 0.032%, Ti: 0.080%, with the balance being Fe and unavoidable impurities.

[0026] Furthermore, its chemical composition by weight percentage is: C: 0.17%, Si: 0.06%, Mn: 0.96%, P: 0.008%, S: 0.002%, Alt: 0.037%, Ti: 0.085%, with the balance being Fe and unavoidable impurities.

[0027] Furthermore, the specific details include: pre-treating the molten iron with desulfurization, achieving a sulfur content of 0.001% in the desulfurized KR molten iron leaving the station; adding 0.5 tons of desulfurizing agent during the treatment process; stirring for 15 minutes; removing slag more than once; achieving a slag removal rate of more than 90%; and setting the molten iron departure temperature T to 1350℃. A top-and-bottom blowing converter is used for smelting to decarburize and dephosphorize the molten iron to obtain steel. Argon is blown throughout the converter smelting process. 52 tons of scrap steel and 228 tons of molten iron are added to the converter. The converter tapping temperature is 1611℃, and the tapping carbon content is 0.06%. During the tapping process, ferromanganese and ferroaluminum are added to the ladle for deoxidation and alloying. Before and after tapping, a sliding plate slag-blocking operation is used to prevent slag from falling onto the steel. During the deoxidation and alloying process, 2800 kg of high-carbon ferromanganese and 1200 kg of ferroaluminum are added. A total of 20 tons of quicklime, dolomite, and iron-containing materials are added during the smelting process. Then, the molten steel after converter smelting undergoes LF ladle refining at a refining temperature of 1536℃. LF refining involves slag formation, deoxidation, desulfurization, and adjustment of composition and temperature. Alloying treatment is carried out in the early stage of LF treatment, with the addition of 90 kg of high-carbon ferromanganese, 450 kg of ferroaluminum, and 50 kg of ferrosilicon. 360 meters of calcium wire is fed for calcium treatment. After the alloying is completed and the slag forms white slag, calcium treatment is carried out, with a soft blowing time of 10 minutes. n. During the soft blowing process, molten steel leakage is prevented. The LF refining temperature at the station is 1611℃. Then, the molten steel after LF ladle refining is hoisted to the RH vacuum refining furnace. The RH refining temperature at the station is 1612℃. 8 minutes before the end of vacuum treatment, 380kg of ferrotitanium alloy is added. The vacuum treatment time is 14 minutes, and the RH temperature at the station is 1593℃. The casting machine superheat is 43℃, and the casting speed is 1.00m / min. After the ladle pouring is completed, the slag detection is activated and the automatic shut-off of the tundish slide plate is closed to avoid slag discharge from the tundish. After the slab undergoes quality inspection, it is loaded into the heating furnace. The hot-rolled slab thickness is 3.4mm, and the heating temperature is... The slab was heated to 1245℃ for 203 minutes, with a soaking time of 30 minutes, and exited at 1247℃. After heating, the slab underwent high-pressure water descaling. Width was determined using a width-fixing press, followed by a 2-stand roughing mill and a 7-stand CVC finishing mill, with a finishing temperature of 881℃. Laminar flow cooling was achieved using a continuous cooling method, and the coiling temperature was 585℃. The pickling process reduced the slab by 56%. The galvanizing process achieved a rolling thickness of 1.5mm, with an annealing furnace heating / soaking temperature of 723℃, a slow cooling temperature of 635℃, a rapid cooling temperature of 461℃, a zinc pot temperature of 460℃, and a coating thickness of 140g / m². 2 The speed of the steel strip in the furnace area is set to 90 m / min, the elongation rate of the leveling machine is 0.7%, and the elongation rate of the tension leveling machine is 0.1%.

[0028] Furthermore, the molten iron undergoes desulfurization pretreatment. The sulfur content of the desulfurized KR molten iron leaving the station is 0.001%. The amount of desulfurizing agent added during the treatment is 0.5 tons, the stirring time is 15 minutes, the slag is removed more than once, the slag removal rate is greater than 90%, and the molten iron departure temperature T is 1342℃. A top-and-bottom blowing converter is used for smelting to decarburize and dephosphorize the molten iron to obtain steel. Argon is blown throughout the converter smelting process. 50 tons of scrap steel and 230 tons of molten iron are added to the converter. The converter tapping temperature is 1611℃, and the carbon content of the tapped steel is 0.08%. During the tapping process, ferromanganese and ferroaluminum are added to the ladle for deoxidation and alloying. Before tapping... The steel was then tapped using a sliding plate slag-blocking operation to prevent slag from falling onto the steel. During the deoxidation and alloying process, 2800 kg of high-carbon ferromanganese and 990 kg of ferroaluminum were added. A total of 21 tons of quicklime, dolomite, and iron-containing materials were added during the smelting process. The molten steel from the converter was then subjected to LF ladle refining at a temperature of 1533℃. LF refining involved slag formation, deoxidation, desulfurization, and adjustment of composition and temperature. Before the LF treatment, alloying was performed by adding 400 kg of high-carbon ferromanganese, 500 kg of ferroaluminum, and 90 kg of ferrosilicon. 320 meters of calcium wire was fed in for calcium treatment. After alloying, when the slag formed white slag, calcium treatment was performed with a soft blowing time of 10 minutes. The soft-blowing process prevents molten steel leakage. The LF refining temperature at the station is 1615℃. Then, the molten steel after LF ladle refining is hoisted to the RH vacuum refining furnace. The RH refining temperature at the station is 1603℃. 400kg of ferrotitanium alloy is added 8 minutes before the end of vacuum treatment. The vacuum treatment time is 25 minutes, and the RH temperature at the station is 1562℃. The casting machine uses a superheat of 30℃ and a casting speed of 1.35m / min. After the ladle pouring is completed, the slag detection is activated and the automatic shut-off of the nozzle slide plate is closed to prevent slag from entering the tundish. After quality inspection of the slab, it is loaded into the heating furnace. The hot-rolled slab thickness is 5.0mm, and the heating temperature is... The slab was heated to 1250℃ for 210 minutes, with a soaking time of 40 minutes, and exited at 1255℃. After heating, the slab underwent high-pressure water descaling. Width was determined using a width-fixing press, followed by a 2-stand roughing mill and a 7-stand CVC finishing mill, with a finishing temperature of 900℃. Laminar flow cooling was achieved using a continuous cooling method, and the coiling temperature was 563℃. The pickling process reduced the slab by 50%. The galvanizing process achieved a rolling thickness of 2.5mm, with an annealing furnace heating / soaking temperature of 720℃, a slow cooling temperature of 631℃, a rapid cooling temperature of 450℃, a zinc pot temperature of 460℃, and a coating thickness of 270g / m². 2 The speed of the steel strip in the furnace area is set to 70 m / min, the elongation rate of the leveling machine is 0.7%, and the elongation rate of the tension leveling machine is 0.1%.

[0029] Furthermore, its mechanical properties meet the following requirements: yield strength 640~680MPa; tensile strength 720-760MPa; elongation 14-17%.

[0030] Furthermore, its mechanical properties meet the following requirements: yield strength 630~670MPa; tensile strength 735-742MPa; elongation 13.5-15%.

[0031] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0032] Through a rational chemical composition design and the aforementioned production method, a high-strength hot-dip galvanized structural steel with a tensile strength exceeding 700 MPa can be obtained. Compared to similar products on the market, which typically employ high-manganese chemical compositions and add niobium (a slightly more expensive solid solution strengthening element) to ensure good formability and high strength, this approach, while maintaining strength, fails to achieve a low yield strength ratio and high elongation, resulting in slightly inferior deformation resistance and formability. This patent, however, utilizes a low-carbon, high-manganese, low-silicon, and titanium microalloying design, without adding niobium, significantly reducing alloy costs. While ensuring product performance, it achieves a low yield strength ratio and high elongation, balancing high strength, high toughness, and excellent cold deformation and bending performance to meet the needs of various working conditions. The implementation and promotion of this patent can enrich the company's product structure, significantly improve profitability, enhance product quality and efficiency, and strengthen the company's market competitiveness.

[0033] Cost advantages: No precious alloys such as Nb, V, and Mo are added; titanium microalloying is used, reducing raw material costs by 15% to 25%; low silicon design reduces hot-dip galvanizing defects and lowers scrap rate.

[0034] Excellent balance of strength and plasticity: Low carbon and high manganese + nano-TiC precipitation reinforcement, yield strength ≥600MPa, tensile strength ≥700MPa, elongation 10%~19%, yield strength ratio 0.80~0.95, taking into account both high strength and excellent cold deformation and bending performance, no cracks after 180° cold bending.

[0035] Hot-dip galvanizing has strong adaptability: Si≤0.08%, which effectively inhibits abnormal growth of zinc-iron alloy layer, avoids defects such as incomplete galvanizing and orange peel texture, and produces a uniform and dense coating with excellent corrosion resistance.

[0036] Uniform microstructure and stability: Ferrite grains are 5μm to 10μm, and nano-TiC (≤20nm) is dispersed. It has small strength fluctuations and stable toughness, making it suitable for various working conditions such as construction, engineering machinery, and power transmission towers. Detailed Implementation

[0037] The present invention will be described in more detail below with reference to examples. These examples are merely descriptions of the best mode of implementation of the invention and do not limit the scope of the invention in any way.

[0038] Example 1

[0039] The molten iron underwent desulfurization pretreatment, with the sulfur content of the molten iron leaving the desulfurization station at 0.001%. The desulfurizing agent dosage was 0.5 tons, the stirring time was 15 minutes, the slag was removed more than once, the slag removal rate was greater than 90%, and the molten iron departure temperature (T) was 1350℃. A top-and-bottom blowing converter was used for smelting to decarburize and dephosphorize the molten iron to obtain steel. Argon was blown throughout the converter smelting process. 52 tons of scrap steel and 228 tons of molten iron were added to the converter. The converter tapping temperature was 1611℃, and the carbon content of the tapped steel was 0.06%. Ferromanganese and ferroaluminum were added to the ladle for deoxidation and alloying during the tapping process. Slag-blocking operations were used before and after tapping to prevent slag from falling into the ladle. 2800 kg of high-carbon ferromanganese and 1200 kg of ferroaluminum were added during the deoxidation and alloying process. A total of 20 tons of quicklime, dolomite, and iron-containing materials were used in the smelting process. The molten steel after converter smelting is then subjected to LF ladle refining at a refining temperature of 1536℃. LF refining involves slag formation, deoxidation, desulfurization, and temperature adjustment. Before the LF treatment, alloying is performed by adding 90 kg of high-carbon ferromanganese, 450 kg of ferroaluminum, and 50 kg of ferrosilicon. Calcium treatment is then performed by feeding 360 meters of calcium wire. After alloying, when the slag forms white slag, calcium treatment is carried out for 10 minutes of soft blowing, ensuring no exposed molten steel. The LF refining temperature at the station is 1611℃. The molten steel after LF ladle refining is then hoisted to the RH vacuum refining furnace at a refining temperature of 1612℃. Eight minutes before the end of vacuum treatment, 380 kg of ferrotitanium alloy (70% titanium content) is added. The vacuum treatment lasts for 14 minutes, and the RH temperature at the station is 1593℃. The chemical composition is supplied to the casting machine according to the table in Table 1. The casting machine uses a superheated temperature of 43℃ and a casting speed of 1.00 m / min. After the ladle pouring is completed, the slag detection system automatically closes the sprue slide to prevent slag from entering the tundish. After quality inspection of the slab, it is loaded into the heating furnace. The hot-rolled slab thickness is 3.4 mm, the heating temperature is 1245℃, the heating time is 203 min, the soaking time is 30 min, and the exit temperature is 1247℃. The heated slab is then subjected to high-pressure water descaling. The width is fixed using a width-fixing press, and a 2-stand roughing rolling (3+5 mode) and a 7-stand CVC finishing rolling are used, with a finishing rolling temperature of 881℃. Laminar flow cooling uses continuous cooling method 11, and the coiling temperature is 585℃. The reduction rate in the pickling rolling process is set at 56%. The galvanizing process has a rolling thickness of 1.5 mm, an annealing furnace heating / soaking temperature of 723℃, a slow cooling temperature of 635℃, a rapid cooling temperature of 461℃, a zinc pot temperature of 460℃, and a coating thickness of 140 g / m. 2 The steel strip speed in the furnace area is set to 90 m / min, the elongation rate of the leveler is 0.7%, and the elongation rate of the tension leveler is 0.1%. The corresponding mechanical properties of the finished product are shown in Table 2.

[0040] Example 2

[0041] The molten iron underwent desulfurization pretreatment, with the sulfur content of the molten iron leaving the desulfurization station at 0.001%. The desulfurizing agent dosage was 0.5 tons, the stirring time was 15 minutes, the slag removal was performed more than once, the slag removal rate was greater than 90%, and the molten iron departure temperature (T) was 1342℃. A top-and-bottom blowing converter was used for smelting to decarburize and dephosphorize the molten iron to obtain steel. Argon was blown throughout the converter smelting process. 50 tons of scrap steel and 230 tons of molten iron were added to the converter. The converter tapping temperature was 1611℃, and the carbon content of the tapped steel was 0.08%. Ferromanganese and ferroaluminum were added to the ladle for deoxidation and alloying during the tapping process. Slag-blocking operations were used before and after tapping to prevent slag from falling into the ladle. 2800 kg of high-carbon ferromanganese and 990 kg of ferroaluminum were added during the deoxidation and alloying process. A total of 21 tons of quicklime, dolomite, and iron-containing materials were used in the smelting process. The molten steel after converter smelting is then subjected to LF ladle refining at a refining temperature of 1533℃. LF refining involves slag formation, deoxidation, desulfurization, and temperature adjustment. Before the LF treatment, alloying is performed by adding 400 kg of high-carbon ferromanganese, 500 kg of ferroaluminum, and 90 kg of ferrosilicon. Calcium treatment is then performed by feeding 320 meters of calcium wire. After alloying, when the slag forms white slag, calcium treatment is carried out, with a soft blowing time of 10 minutes. During the soft blowing process, leakage of molten steel is strictly prohibited. The LF refining temperature at the station is 1615℃. The molten steel after LF ladle refining is then hoisted to the RH vacuum refining furnace at a refining temperature of 1603℃. Eight minutes before the end of vacuum treatment, 400 kg of ferrotitanium alloy (70% titanium content) is added. The vacuum treatment time is 25 minutes, and the RH temperature at the station is 1562℃. The chemical composition is supplied to the casting machine according to the table in Table 1. The casting machine uses a superheated temperature of 30℃ and a casting speed of 1.35m / min. After the ladle pouring is completed, the slag detection system automatically closes the sprue slide to prevent slag from entering the tundish. After quality inspection of the slab, it is loaded into the heating furnace. The hot-rolled slab thickness is 5.0mm, the heating temperature is 1250℃, the heating time is 210min, the soaking time is 40min, and the exit temperature is 1255℃. The heated slab is then subjected to high-pressure water descaling. The width is fixed using a width-fixing press, and a 2-stand roughing rolling (3+5 mode) and a 7-stand CVC finishing rolling are used, with a finishing rolling temperature of 900℃. Laminar flow cooling uses continuous cooling method 11, and the coiling temperature is 563℃. The reduction rate in the pickling rolling process is set at 50%. The galvanizing process has a rolling thickness of 2.5mm, an annealing furnace heating / soaking temperature of 720℃, a slow cooling temperature of 631℃, a rapid cooling temperature of 450℃, a zinc pot temperature of 460℃, and a coating thickness of 270g / m. 2 The steel strip speed in the furnace area is set at 70 m / min, the elongation rate of the leveling machine is 0.7%, and the elongation rate of the tension leveler is 0.1%. The corresponding mechanical properties of the finished product are shown in Table 2.

[0042] As can be seen from the actual chemical composition values ​​in Table 1 and the mechanical property test values ​​of the finished coils in Table 2, through Case Implementation 1 and 2, the chemical composition and mechanical properties of the produced steel coils meet the user requirements, and the product formability, strength, and corrosion resistance all meet the usage requirements.

[0043] Table 1 Chemical composition of finished casting machine products (%)

[0044] C Si Mn P S Alt Ca Ti Example 1 0.17 0.06 0.94 0.010 0.003 0.032 0.0010 0.080 Example 2 0.17 0.06 0.96 0.008 0.002 0.037 0.0016 0.085

[0045] Table 2 Mechanical properties of finished products corresponding to implementation cases

[0046] Thickness / mm Yield strength / MPa Tensile strength / MPa Elongation / % Example 1 (Multiple rolls from one furnace) 1.50 640~680 720~760 14.0~17.0 Example 2 (Multiple rolls from one furnace) 2.50 630~670 735~742 13.5~15.0

[0047] The above embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for producing high-strength hot-dip galvanized structural steel with a strength of 700MPa or higher, characterized in that, Includes the following steps: Step 1: When the KR process is desulfurized, the sulfur content in the molten iron should be ≤0.010%, and the slag removal ratio on the surface of the molten iron ladle should be ≥90%; the converter tapping temperature should be controlled at ≥1620℃; during the tapping process, ferromanganese and ferroaluminum are added to the ladle to deoxidize and alloy the molten steel once, and carbon particles and top slag lime are added; the start and end of the converter tapping process adopts the sliding plate slag blocking operation to prevent converter slag from falling into the ladle; Step 2: After the ladle is in place in the LF refining process, it is heated and desulfurized by slag making. During the slag making process, quicklime is added and the refining slag is made to achieve the effect of white slag, and the FeO+MnO content in the slag is less than 1.5%. Aluminum iron, manganese iron alloy and carbon particles are added to adjust the composition to the range of LF off-site composition. LF off-site ensures that the S content in the molten steel is ≤0.005% and the off-site temperature is ≥1620℃. After LF off-site, it is hoisted to RH vacuum treatment. Step 3: RH deep vacuum treatment removes hydrogen and nitrogen from the molten steel, further improving its cleanliness; the circulating flow rate during the RH vacuum treatment process is set within a range of 120m³. 3 / min~150 m 3 / min; the vacuum degree must be less than 1.3mbar, and the deep vacuum treatment time is 20min~25min; during the vacuum treatment process, titanium-iron alloy and metallic manganese are added to further adjust the composition of the molten steel. After the deep vacuum treatment, the molten steel is subjected to calcium treatment. During the calcium treatment process, 200~400m of high-calcium wire is fed in, and the argon flow rate is controlled reasonably to prevent the molten steel from being exposed; after the calcium treatment, the soft blowing time is guaranteed to be ≥8 minutes to promote the floating of inclusions in the molten steel and improve the control of the cleanliness of the molten steel. The chemical composition and temperature of the molten steel after displacement must meet the casting machine's pouring requirements; Step 4: Argon gas is used for protection throughout the casting process. The slag detection equipment is turned on during the ladle pouring process, and slag is prevented from flowing into the tundish at the end of the ladle pouring. Constant casting speed control is used during the casting process, and the casting speed is set in the range of 1.1m / min to 1.8m / min according to different casting sections. The superheat of the tundish pouring is controlled between 15℃ and 30℃. Billet inspection: The center segregation of the continuously cast billet shall not exceed Class B 1.0 grade, and the center porosity shall not exceed 1.0 grade. Step 5: In the hot rolling process, the slab is heated in the furnace by hot charging or cold charging; select the appropriate heating regime according to the thickness specification requirements, the heating temperature range is 1230~1270℃, the furnace time is 150-230min, the soaking temperature range is 1240~1280℃, the soaking temperature is 20-45min, and the furnace exit temperature is 1240-1280℃. Step 5: Rolling includes roughing and finishing. Roughing is done on a 2-stand mill, and finishing is done on a 7-stand continuous variable crown mill. The finishing temperature is 870~910℃. Cooling is done using a laminar flow continuous cooling system with a cooling code setting of mode 11. The upper cooling nozzles are set to open every other one, and the lower cooling nozzles are set to open every two. The coiling temperature is controlled within the range of 550~610℃ depending on the thickness. Step 6: Pickling and pickling process. The reduction rate is controlled within the range of 50-76% according to the thickness requirements of the order. In order to ensure good adhesion of the coating to the strip surface in the next process, the surface roughness of the rolls in the pickling and rolling process is 2.0-3.0μm. After rolling, the surface roughness of the strip should be greater than 1.0μm to ensure good adhesion between the strip and the galvanized coating and avoid defects such as incomplete coating, coating peeling and cracks on the strip surface. Step 7: Continuous hot-dip galvanizing process. The annealing process uses a vertical continuous annealing furnace. The furnace atmosphere should be a reducing protective atmosphere for cooling. The heating / soaking temperature range is 710~740℃, the slow cooling temperature is 620~660℃, and the rapid cooling temperature is 420~470℃, depending on the strip thickness. The strip temperature entering the zinc pot is 460~470℃, and the temperature of the molten zinc in the zinc pot ranges from 450~470℃. The coating thickness is determined according to the order requirements, and the appropriate air knife pressure is selected. The strip speed in the furnace area is 70~130m / min, depending on the thickness. The elongation of the leveling machine is 0.5~0.8%, and the elongation of the tension leveler is ≤0.2%. Its chemical composition by weight percentage is as follows: C: 0.15-0.20%, Si: ≤0.08%, Mn: 0.85-1.05%, P ≤0.020%, S ≤0.010%, Alt: 0.020-0.050%, Ti: 0.065-0.105%, with the balance being Fe and unavoidable impurities.

2. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 1, characterized in that, Its chemical composition by weight percentage is: C: 0.17%, Si: 0.06%, Mn: 0.94%, P: 0.010%, S: 0.003%, Alt: 0.032%, Ti: 0.080%, with the balance being Fe and unavoidable impurities.

3. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 1, characterized in that, Its chemical composition by weight percentage is: C: 0.17%, Si: 0.06%, Mn: 0.96%, P: 0.008%, S: 0.002%, Alt: 0.037%, Ti: 0.085%, with the balance being Fe and unavoidable impurities.

4. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 2, characterized in that, Specifically, it includes: The molten iron underwent desulfurization pretreatment, resulting in a sulfur content of 0.001% at the desulfurization KR station. The desulfurizing agent dosage was 0.5 tons, the stirring time was 15 minutes, slag was removed more than once, and the slag removal rate was greater than 90%. The molten iron departure temperature (T) was 1350℃. A top-and-bottom blowing converter was used for smelting to decarburize and dephosphorize the molten iron, yielding steel. Argon was blown throughout the converter smelting process. 52 tons of scrap steel and 228 tons of molten iron were added to the converter. The converter tapping temperature was 1611℃, and the carbon content at tapping was 0.06%. Ferromanganese and ferroaluminum were added to the ladle during tapping for deoxidation and alloying. Sliding was used before and after tapping. The steelmaking process involves slag blocking during tapping to prevent slag from falling onto the steel. During the deoxidation and alloying process, 2800 kg of high-carbon ferromanganese and 1200 kg of ferroaluminum are added. A total of 20 tons of quicklime, dolomite, and iron-containing materials are used in the smelting process. The molten steel from the converter is then subjected to LF ladle refining at a temperature of 1536℃. LF refining involves slag formation, deoxidation, desulfurization, and adjustment of composition and temperature. Before the LF treatment, alloying is performed by adding 90 kg of high-carbon ferromanganese, 450 kg of ferroaluminum, and 50 kg of ferrosilicon. 360 meters of calcium wire is fed in for calcium treatment. After alloying, when white slag forms, calcium treatment is performed, with a soft blowing time of 10 minutes. To prevent molten steel leakage, the LF refining furnace was set at a temperature of 1611℃. The molten steel after LF ladle refining was then hoisted to the RH vacuum refining furnace at a temperature of 1612℃. Eight minutes before the end of vacuum treatment, 380 kg of ferro-titanium alloy was added, and the vacuum treatment lasted 14 minutes, resulting in an RH departure temperature of 1593℃. The casting machine was used with a superheat of 43℃ and a casting speed of 1.00 m / min. After the ladle pouring was completed, the slag detection system was activated, and the automatic shut-off nozzle slide was closed to prevent slag from entering the tundish. After quality inspection, the slab was loaded into the heating furnace. The hot-rolled slab thickness was 3.4 mm, and the heating temperature was 12℃. The slab was heated to 45℃ for 203 minutes, with a soaking time of 30 minutes, and exited at 1247℃. After heating, the slab underwent high-pressure water descaling. Width was determined using a width-fixing press, followed by a 2-stand roughing mill and a 7-stand CVC finishing mill, with a finishing temperature of 881℃. Laminar flow cooling was performed using a continuous cooling method, and the coiling temperature was 585℃. The pickling process reduced the slab by 56%. The galvanizing process achieved a rolling thickness of 1.5mm, with an annealing furnace heating / soaking temperature of 723℃, a slow cooling temperature of 635℃, a rapid cooling temperature of 461℃, a zinc pot temperature of 460℃, and a coating thickness of 140g / m². 2 The speed of the steel strip in the furnace area is set to 90 m / min, the elongation rate of the leveling machine is 0.7%, and the elongation rate of the tension leveling machine is 0.1%.

5. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 3, characterized in that, The molten iron underwent desulfurization pretreatment, resulting in a sulfur content of 0.001% at the desulfurization KR station. The desulfurizing agent dosage was 0.5 tons, the stirring time was 15 minutes, slag was removed more than once, and the slag removal rate was greater than 90%. The molten iron departure temperature (T) was 1342℃. A top-and-bottom blown converter was used for smelting to decarburize and dephosphorize the molten iron, yielding steel. Argon was blown throughout the converter smelting process. 50 tons of scrap steel and 230 tons of molten iron were added to the converter. The converter tapping temperature was 1611℃, and the carbon content at tapping was 0.08%. Ferromanganese and ferroaluminum were added to the ladle during tapping for deoxidation and alloying. Slippage was used before and after tapping. The steelmaking process involves slag blocking during tapping to prevent slag from falling onto the steel. During the deoxidation and alloying process, 2800 kg of high-carbon ferromanganese and 990 kg of ferroaluminum are added. A total of 21 tons of quicklime, dolomite, and iron-containing materials are used in the smelting process. The molten steel from the converter is then subjected to LF ladle refining at a temperature of 1533℃. LF refining involves slag formation, deoxidation, desulfurization, and adjustment of composition and temperature. Before the LF treatment, alloying is performed by adding 400 kg of high-carbon ferromanganese, 500 kg of ferroaluminum, and 90 kg of ferrosilicon. 320 meters of calcium wire is fed in for calcium treatment. After alloying, when white slag forms, calcium treatment is performed, with a soft blowing time of 10 minutes. To prevent molten steel leakage, the LF refining furnace was set at a temperature of 1615℃ before leaving the furnace. The molten steel, after LF ladle refining, was then hoisted to the RH vacuum refining furnace at a temperature of 1603℃. Eight minutes before the end of the vacuum treatment, 400 kg of ferrotitanium alloy was added, and the vacuum treatment lasted 25 minutes, resulting in an RH departure temperature of 1562℃. The casting machine was used with a superheat of 30℃ and a casting speed of 1.35 m / min. After the ladle pouring was completed, the slag detection system was activated, and the automatic shut-off of the nozzle slide was performed to prevent slag from entering the tundish. After quality inspection, the slabs were loaded into the heating furnace. The hot-rolled slab thickness was 5.0 mm, and the heating temperature was 12℃. Heating was carried out at 50℃ for 210 minutes, with a soaking time of 40 minutes. The furnace exit temperature was 1255℃. The heated slab was then subjected to high-pressure water descaling. Width was determined using a width-fixing press, followed by 2-stand roughing and 7-stand CVC finishing rolling, with a finishing rolling temperature of 900℃. Laminar flow cooling was performed using continuous cooling method 11, with a coiling temperature of 563℃. The pickling process reduced the slab by 50%. The galvanizing process achieved a rolling thickness of 2.5mm, with an annealing furnace heating / soaking temperature of 720℃, a slow cooling temperature of 631℃, a rapid cooling temperature of 450℃, a zinc pot temperature of 460℃, and a coating thickness of 270g / m². 2 The speed of the steel strip in the furnace area is set to 70 m / min, the elongation rate of the leveling machine is 0.7%, and the elongation rate of the tension leveling machine is 0.1%.

6. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 4, characterized in that, Its mechanical properties meet the following requirements: yield strength 640~680MPa; tensile strength 720-760MPa; elongation 14-17%.

7. The method for producing high-strength hot-dip galvanized structural steel of grade 700MPa or above according to claim 5, characterized in that, Its mechanical properties meet the following requirements: yield strength 630~670MPa; tensile strength 735-742MPa; elongation 13.5-15%.

Citation Information

Patent Citations

  • Hot-dip galvanized steel strip for light steel with strength of 600MPa and preparation method thereof

    CN112813342A

  • Thin GI high-strength steel strip with yield strength of 700MPa and production method thereof

    CN116179960A

  • Production method of high-strength structural steel SGC570

    CN116334470A