A low yield strength ratio 1400MPa grade medium manganese steel and its preparation method

By controlling the microstructure ratio of medium manganese steel through specific chemical composition and hot rolling combined with two-phase annealing process, the problem of excessively high yield strength ratio of medium manganese steel under high strength is solved, achieving a match between low yield strength ratio and high elongation. It is suitable for automotive safety structural components and has good industrial production adaptability and cost-effectiveness.

CN123108431APending Publication Date: 2026-11-17ANGANG STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611372568.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing medium-manganese steel has an excessively high yield strength ratio at high strength levels, making it difficult to balance low yield strength ratio, high elongation, and excellent impact energy absorption performance. Furthermore, it relies on special processes or expensive alloying elements, making it difficult to achieve mass production on conventional production lines.

Method used

Medium manganese steel with a specific chemical composition ratio, including elements such as C, Mn, Al, Si, and Mo, is combined with conventional hot rolling and two-phase annealing processes to control the ratio of ferrite, austenite, and martensite. The grains are refined through Mo microalloying and annealing processes to form a composite structure of soft and tough phases, metastable phases, and hard phases.

Benefits of technology

Achieving a yield strength ratio of ≤0.80 and a high elongation of ≥24% at a strength of 1400MPa, the material improves its impact energy absorption performance, making it suitable for automotive safety structural components and possessing good industrial production adaptability and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108431A_ABST
    Figure CN123108431A_ABST
Patent Text Reader

Abstract

This invention relates to the field of steel material preparation, specifically to a low yield strength ratio 1400MPa grade medium manganese steel and its preparation method. The medium manganese steel is composed of the following chemical composition by mass percentage: C: 0.22%–0.32%, Mn: 10.0%–13.0%, Al: 1.8%–2.8%, Si: 0.15%–0.45%, Mo: 0.10%–0.30%, P≤0.008%, S≤0.004%, with the balance being Fe and unavoidable impurities. The preparation method includes: homogenizing and holding the steel billet at 1200–1240℃, followed by hot rolling at a final rolling temperature of 800–860℃; then annealing in the two-phase region at 720–760℃ for 90–150 min, followed by air cooling to room temperature. This invention achieves a multiphase microstructure of ferrite, austenite, and martensite through the synergistic effect of Mo microalloying and two-phase annealing. The ferrite content is 25%–35%, and the austenite content is 20%–28%, with ferrite grain size of 1–3 μm and austenite grain size of 0.5–2 μm. The manganese steel produced in this invention has a tensile strength ≥1400 MPa, a yield strength ratio ≤0.80, and an elongation after fracture ≥24%, making it suitable for automotive safety structural components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of steel material preparation technology, specifically to a low yield strength ratio 1400MPa grade medium manganese steel and its preparation method. Background Technology

[0002] Medium-manganese steel (typically with a manganese content of 4%–12%), as a typical representative of third-generation advanced high-strength steel for automobiles, combines the low alloy cost and process applicability of first-generation high-strength steel with the high plasticity and high strength-ductility product of second-generation high-strength steel, making it one of the most promising materials in the field of automotive lightweighting. With the automotive industry's increasing demands for energy conservation and emission reduction, and the continuous tightening of collision safety standards, steel used in automotive structural components needs to possess excellent collision energy absorption performance while ensuring high strength, which places higher demands on the yield strength ratio of materials.

[0003] The yield strength ratio (the ratio of yield strength to tensile strength) is an important indicator for evaluating a material's ability to absorb impact energy. A lower yield strength ratio indicates a longer plastic deformation range after yielding, enabling the material to absorb more impact energy during a collision, thus improving vehicle safety. However, existing medium-manganese steels often face the problem of excessively high yield strength ratios at high strength levels. For example, Chinese patent application publication number CN107419196A discloses "Ultra-low carbon easy-to-weld medium-manganese automotive steel with controllable yield strength ratio and its preparation method," involving medium-manganese automotive steel with a yield strength ratio between 0.7 and 0.9. Chinese patent authorization publication number CN117144261B discloses "A room temperature quenched-partitioned medium-manganese steel with low yield strength ratio and high tensile strength and its preparation method," with the prepared medium-manganese steel having a yield strength ratio of 0.55 to 0.60 and a tensile strength of 1250 to 1350 MPa. Furthermore, some existing medium-manganese steels even have yield strength ratios exceeding 0.85. An excessively high yield strength ratio causes materials to yield prematurely during a collision, resulting in a narrow range of plastic deformation and insufficient energy absorption capacity, making it difficult to meet the requirements of automotive safety structural components for high collision energy absorption performance.

[0004] To address the aforementioned issues, researchers explored various technical approaches to reduce the yield strength ratio of medium-manganese steel. Chinese Patent CN110117755B discloses a method for preparing 980MPa grade low-yield-strength-ratio cold-rolled medium-manganese steel, producing a yield strength ≥400MPa, tensile strength ≥980MPa, and yield strength ratio ≤0.50. Chinese Patent CN115198191B discloses a method for preparing medium-manganese steel with a low yield strength ratio and low yield elongation, producing a yield strength ratio of 0.60–0.66. Chinese Patent Application CN119876553A discloses a method for preparing 1400MPa grade medium-manganese steel, producing a yield strength ratio of 0.3–0.306, a yield strength of 270–430MPa, and a tensile strength of 800–1400MPa.

[0005] Although the above technical solutions have made some progress in reducing the yield strength ratio, the following shortcomings still exist: (1) It is difficult to balance strength and yield strength ratio. Although the Chinese patent with authorization announcement number CN110117755B achieves a yield strength ratio ≤0.50, its tensile strength is only 980MPa, not reaching the 1400MPa level; the Chinese patent with authorization announcement number CN117144261B has a tensile strength of 1250~1350MPa, also not reaching the 1400MPa level, and a yield strength ratio of 0.55~0.60; although the Chinese patent document with application publication number CN119876553A achieves a tensile strength of 1400MPa and a very low yield strength ratio, its yield strength is only 270~430MPa. How to achieve a yield strength ratio ≤0.80 at a high strength level of 1400MPa is still a technical problem that needs to be solved in this field. (2) Insufficient precision in tissue regulation. The yield strength ratio of medium manganese steel is closely related to the ratio of soft phase (ferrite) to hard phase (martensite) in its microstructure. Existing technologies have reduced the yield strength ratio by controlling the ratio of ferrite to austenite through two-phase annealing, but the control precision of process parameters such as annealing temperature and holding time is insufficient, making it difficult to obtain a stable microstructure ratio and consistent mechanical properties in industrial production. (3) Reliance on special processes or expensive alloying elements. The realization of some low yield strength ratio medium manganese steels depends on special processes such as warm rolling and quenching-partitioning, which increases the production difficulty and equipment requirements, and is not conducive to mass production on conventional continuous annealing production lines.

[0006] In summary, existing medium-manganese steel technology still struggles to achieve a low yield strength ratio, high elongation, and excellent impact energy absorption performance at high strength levels. There is an urgent need to develop a medium-manganese steel and its preparation method that can stably control the yield strength ratio below 0.80 at a strength level of 1400MPa while also possessing good plasticity. Summary of the Invention

[0007] In order to overcome the shortcomings of high-strength medium-manganese steel with excessively high yield strength ratio and insufficient impact energy absorption capacity in the existing technology, this invention provides a medium-manganese steel with a low yield strength ratio of 1400MPa and its preparation method.

[0008] To achieve the above objectives, the present invention employs the following technical solution: A low yield strength ratio 1400MPa grade medium manganese steel is composed of the following chemical composition by weight percentage: C: 0.22%~0.32%, Mn: 10.0%~13.0%, Al: 1.8%~2.8%, Si: 0.15%~0.45%, Mo: 0.10%~0.30%, P≤0.008%, S≤0.004%, with the balance being Fe and unavoidable impurities.

[0009] The effect of selecting the above alloying elements and their contents: Carbon (C): Carbon is the most fundamental solid solution strengthening element in steel, significantly improving its strength through solid solution strengthening and precipitation strengthening. Simultaneously, carbon is an austenite stabilizing element, effectively improving the stability of retained austenite, lowering the martensite transformation initiation temperature (Ms point), and allowing for more retained austenite after annealing in the two-phase region. This, in turn, enables a full TRIP effect during deformation, improving the steel's plasticity and work hardening capacity. However, excessive carbon content can lead to component segregation in the cast billet and promote carbide precipitation, deteriorating the steel's weldability and toughness. Therefore, this invention controls the C content to be between 0.22% and 0.32%.

[0010] Manganese (Mn): Manganese is one of the most important alloying elements in this invention and a core element that distinguishes medium-manganese steel from traditional high-strength steel. Manganese is an austenite stabilizing element, significantly expanding the austenite phase region and lowering the martensitic transformation initiation temperature (Ms point). During two-phase annealing, Mn enriches in austenite, improving its thermodynamic stability and allowing a large amount of metastable austenite to be retained at room temperature. Furthermore, manganese strengthens the steel through solid solution without significantly impairing its plasticity. However, excessively high manganese content can easily lead to segregation in the cast billet, increasing production costs. Therefore, this invention controls the Mn content to be between 10.0% and 13.0%.

[0011] Aluminum (Al): Aluminum is a key deoxidizing and ferrite stabilizing element in this invention. Aluminum effectively inhibits cementite precipitation and promotes carbon enrichment in austenite, thereby enhancing the stability of retained austenite and the TRIP effect. Simultaneously, aluminum inhibits carbide formation, preventing carbides from disrupting the matrix and improving the steel's plasticity. Furthermore, as a lightweight element, aluminum can appropriately reduce the density of steel. However, excessive aluminum content promotes the formation of coarse δ-ferrite and κ-carbides, adversely affecting the steel's strength and toughness. Therefore, this invention controls the Al content to 1.8%–2.8%.

[0012] Silicon (Si): Silicon is a commonly used solid solution strengthening element in steel, possessing a certain austenite stabilizing effect, which helps stabilize retained austenite. Silicon can inhibit carbide precipitation and promote carbon enrichment into austenite, thereby improving the stability of retained austenite. However, excessive silicon content can adversely affect the toughness and surface quality of steel and increase welding difficulty. Therefore, this invention controls the Si content to 0.15%–0.45%.

[0013] Molybdenum (Mo): Molybdenum is the key microalloying element for achieving a low yield strength ratio in this invention. Molybdenum has a strong grain boundary pinning effect, which can effectively inhibit austenite grain growth and refine the grains. Molybdenum can also promote the formation of reverse-transformed austenite and regulate the ratio of soft ferrite to hard martensite, thereby reducing the yield strength ratio. In addition, molybdenum can suppress temper brittleness, adsorb and fix harmful impurities, and prevent them from segregating to grain boundaries. However, excessive molybdenum will generate coarse intermetallic compounds, which will adversely affect toughness and increase alloy cost. Therefore, the Mo content is controlled at 0.10% to 0.30% in this invention.

[0014] Sulfur (S) and phosphorus (P): Sulfur readily forms sulfide inclusions such as FeS and MnS in steel. These inclusions are typically located at grain boundaries and melt when the temperature reaches their melting point, leading to hot brittleness during hot deformation and significantly reducing the steel's toughness and fatigue performance. Phosphorus tends to segregate at grain boundaries, disrupting the continuity of the matrix, significantly reducing the steel's cold deformation capacity and low-temperature toughness, and deteriorating weldability. Therefore, this invention strictly controls the S content to ≤0.004% and the P content to ≤0.008% to minimize the adverse effects of harmful impurities on the mechanical and performance properties of the steel.

[0015] The microstructure of the aforementioned medium-manganese steel is ferrite + austenite + martensite, with a ferrite volume fraction of 25%–35% and an austenite volume fraction of 20%–28%. The average grain size of the ferrite is 1–3 μm, and the average grain size of the austenite is 0.5–2 μm. The tensile strength of the aforementioned medium-manganese steel is ≥1400 MPa, the yield strength ratio is ≤0.80, and the elongation after fracture is ≥24%.

[0016] The preparation method of the above-mentioned low yield strength ratio 1400MPa grade medium manganese steel includes the following steps: 1) Smelting to obtain molten steel, and continuously casting the molten steel into billets; 2) The cast billet is subjected to homogenization and heat preservation treatment at 1200-1240℃; 3) The homogenized and heat-insulated billet is hot-rolled at a final rolling temperature of 800-860℃; 4) The hot-rolled steel plate is subjected to two-phase annealing treatment at a temperature of 720-760℃ and a holding time of 90-150 minutes, and then air-cooled to room temperature.

[0017] Furthermore, in step 1), the smelting is either converter smelting or electric arc furnace smelting, and is subsequently refined by LF refining and RH vacuum refining; the continuous casting adopts full-process protective casting.

[0018] Furthermore, in step 2), the homogenization and heat preservation treatment time is 2 to 4 hours.

[0019] Furthermore, in step 3), the initial rolling temperature of the hot rolling is 1000–1100°C.

[0020] Furthermore, in step 3), the total deformation of the hot rolling is 50% to 80%.

[0021] Furthermore, in step 3), the hot rolling process employs multi-pass rolling, with 5 to 7 passes.

[0022] Furthermore, in step 4), the two-phase annealing process is carried out in an air atmosphere.

[0023] Furthermore, in step 4), the cooling rate of the air cooler is 1 to 10°C / s.

[0024] Compared with the prior art, the beneficial effects of the present invention are: 1. The synergistic design of composition and process enables precise control of the hard-soft phase ratio. This invention achieves precise control of the proportions of ferrite, austenite, and martensite through the synergistic combination of Mo microalloying and two-phase annealing. During homogenization heating and two-phase annealing, Mo pins grain boundaries and inhibits austenite grain growth, refining the microstructure before two-phase annealing. Furthermore, two-phase annealing at 720–760℃ allows the steel to undergo sufficient austenite reversal transformation in the α+γ two-phase region, with Mo's grain boundary pinning inhibiting the coarsening of the reversed austenite. The synergistic effect of these two processes stabilizes the ferrite volume fraction at 25%–35%, the austenite volume fraction at 20%–28%, with the balance being martensite, forming a composite microstructure of "soft and tough phase (ferrite) + metastable phase (austenite) + hard phase (martensite)". Ferrite, as the soft phase, reduces yield strength, while martensite, as the hard phase, ensures tensile strength. The metastable austenite provides continuous work hardening capability during deformation through the TRIP effect.

[0025] 2. The composition design achieved a fine-grained microstructure with a good balance of strength and plasticity. This invention achieves a fine-grained microstructure through a rational alloy element ratio design. Both C and Mn are austenite stabilizing elements, with Mn being the core element for obtaining a large amount of retained austenite. Through solid solution strengthening and lowering the martensite transformation initiation temperature (Ms point), sufficient retained austenite is obtained after annealing in the two-phase region. C further enhances the stability of austenite while simultaneously strengthening through solid solution. Al inhibits cementite precipitation and promotes carbon enrichment in austenite, thus enhancing the stability of the retained austenite. The addition of Mo further refines the grains, resulting in an average ferrite grain size of 1–3 μm and an average austenite grain size of 0.5–2 μm. The fine-grained microstructure not only contributes to strength through grain refinement strengthening but also effectively reduces the yield strength ratio, giving the material a longer plastic deformation range after yielding.

[0026] 3. The process design takes into account both performance regulation and adaptability to industrial production. This invention employs a conventional hot rolling process combined with two-phase annealing, avoiding the stringent equipment requirements of special processes such as warm rolling and quenching-partitioning. The final hot rolling temperature is controlled at 800–860℃ to ensure uniform microstructure; subsequently, two-phase annealing is performed at 720–760℃ for 90–150 minutes to allow C and Mn elements to fully distribute between the ferrite and austenite phases. This process can be implemented on a conventional continuous annealing production line, exhibiting good adaptability to industrial production while avoiding the cost increases associated with adding expensive alloying elements such as Ni, Cr, and V.

[0027] 4. The synergistic combination of composition and process enables the regulation of the tissue's thermodynamic stability. This invention achieves effective control over the thermodynamic stability of retained austenite through the synergistic combination of Mo microalloying and two-phase annealing. The addition of Mo improves the hardenability of austenite, allowing more austenite to be retained to room temperature during air cooling after two-phase annealing. Simultaneously, Mo pinning of grain boundaries inhibits grain growth, refines the austenite grain size, and further enhances austenite stability. Annealing temperatures of 720–760℃ combined with holding times of 90–150 min ensure sufficient enrichment of Mn into the austenite, giving the retained austenite appropriate thermodynamic stability at room temperature. This stability is sufficient to retain adequate retained austenite during cooling to room temperature, while also possessing sufficient metastability to sustain the TRIP effect during deformation, thus providing stable work hardening capability.

[0028] 5. The final mechanical properties achieve a good match between high strength and low yield strength ratio. Based on the combined effect of the above-mentioned composition design and process optimization, this invention achieves excellent comprehensive mechanical properties. The results of the examples show that the prepared medium-manganese steel has a tensile strength of 1410–1490 MPa, a yield strength of 1110–1180 MPa, a yield-to-tensile ratio stably controlled at 0.75–0.79 (all below 0.80), and an elongation after fracture of 24.5%–27%. This indicates that this invention achieves a good match between a low yield-to-tensile ratio and high elongation at a strength level of 1400 MPa, significantly improving the material's impact energy absorption performance and meeting the comprehensive performance requirements of high-strength steel for automotive safety structural components. Attached Figure Description

[0029] Figure 1 This is an optical metallographic photograph of the manganese steel prepared in Example 1 of the present invention.

[0030] Figure 2 This is a transmission electron microscope (TEM) image of the manganese steel prepared in Example 1 of the present invention. Detailed Implementation

[0031] This invention discloses a low yield strength ratio (1400 MPa) grade medium-manganese steel and its preparation method. Those skilled in the art can refer to this document and appropriately modify the process parameters to achieve the desired result. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this invention. The methods and applications of this invention have been described through preferred embodiments. Those skilled in the art can clearly modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit, and scope of this invention to realize and apply the technology of this invention.

[0032] The production process of this invention is as follows: smelting → continuous casting → homogenization and heat preservation → hot rolling → two-phase annealing → air cooling to room temperature. Specific process steps are as follows: (1) Smelting and continuous casting Molten steel is obtained by smelting according to the chemical composition described in this invention. Smelting can be carried out in a converter or electric arc furnace, followed by sequential LF refining and RH vacuum refining to remove harmful gases and inclusions, thereby improving the purity of the molten steel. The refined molten steel is then continuously cast using a fully protected casting process to reduce secondary oxidation, lower the inclusion content, and improve the quality of the cast billet. The steel is then continuously cast into billets of the required specifications.

[0033] (2) Homogenization and heat preservation treatment The continuously cast billet is subjected to homogenization holding treatment at 1200–1240℃. The purpose of homogenization holding treatment is to eliminate dendritic segregation generated during the solidification process of the billet, and to ensure that alloying elements (especially Mn and Mo) diffuse fully and uniformly, providing a billet with a uniform microstructure for subsequent hot rolling. The preferred homogenization holding time is 2–4 hours.

[0034] (3) Hot rolling The homogenized and heat-treated billet is then hot-rolled. The initial rolling temperature is 1000–1100℃, ensuring that rolling takes place in the austenite recrystallization or non-recrystallization zone. Rolling deformation breaks down and refines the original coarse as-cast structure. Hot rolling employs multiple passes, 5–7 passes, with a total deformation of 50%–80%, ensuring sufficient deformation accumulation and microstructure refinement. The final rolling temperature is 800–860℃. Ending rolling within this temperature range keeps the deformed austenite grains fine, providing a refined precursor structure for subsequent annealing. The hot-rolled steel sheet is then air-cooled to room temperature.

[0035] (4) Annealing in the two-phase region The hot-rolled steel sheet undergoes two-phase annealing. The annealing temperature is 720–760℃, and the holding time is 90–150 min. Within this temperature range, the steel's microstructure exists in the two-phase region of ferrite (α) and austenite (γ). The prolonged holding time allows for sufficient distribution of C and Mn elements between the ferrite and austenite, with Mn enriching in the austenite and improving its stability. Annealing is performed in air, eliminating the need for a protective atmosphere and reducing production costs. After annealing, the sheet is air-cooled to room temperature at a rate of 1–10℃ / s. During air cooling, some austenite transforms into martensite, while the austenite enriched with sufficient Mn and C remains at room temperature, forming a multiphase microstructure composed of ferrite, austenite, and martensite.

[0036] The present invention will be further illustrated below through specific embodiments. The chemical composition of the embodiments and comparative examples of the present invention is shown in Table 1, the homogenization heat preservation and hot rolling process is shown in Table 2, the two-phase annealing process is shown in Table 3, and the mechanical properties are shown in Table 4.

[0037] Table 1. Chemical composition (wt%) of the embodiments and comparative examples of the present invention.

[0038] Table 2. Homogenization, heat preservation, and hot rolling processes of the embodiments and comparative examples of the present invention.

[0039] Table 3 Two-phase annealing process of embodiments and comparative examples of the present invention.

[0040] Table 4 Mechanical properties of embodiments and comparative examples of the present invention

[0041] As shown in Table 4, the medium-manganese steel prepared in each embodiment of the present invention has a tensile strength of 1420–1500 MPa, a yield strength of 1050–1180 MPa, a yield-to-tensile ratio stably controlled at 0.74–0.79 (all below 0.80), and an elongation after fracture of 24.0%–27.5%. Each embodiment achieves a good match between a yield-to-tensile ratio ≤0.80 and an elongation ≥24% at a strength level of 1400 MPa.

[0042] Comparative Example 1 had a Mn content of 14.0% (exceeding the upper limit of 13.0% in this invention), with the remaining components and processes being the same as in Example 1. Table 4 shows that its tensile strength was 1510 MPa, yield strength was 1329 MPa, and yield-to-tensile ratio was 0.88, significantly higher than those of the embodiments of this invention. This indicates that when the Mn content exceeds 13.0%, the proportion of the soft and tough phase (ferrite) in the microstructure is insufficient, failing to effectively reduce the yield-to-tensile ratio, leading to deterioration of the impact energy absorption performance.

[0043] Comparative Example 2 did not add Mo (the remaining components and processes were the same as in Example 1). As shown in Table 4, its tensile strength was 1430 MPa, yield strength was 1187 MPa, and yield strength ratio was 0.83, which were higher than those of the embodiments of this invention. This indicates that without the addition of Mo, it is impossible to effectively inhibit austenite grain growth and promote the formation of reverse-transformed austenite, resulting in poorer microstructure uniformity and an increased yield strength ratio.

[0044] The above results show that, through the synergistic effect of Mo microalloying and two-phase annealing, the present invention achieves a good match between yield strength ratio ≤0.80 and elongation ≥24% at a strength level of 1400MPa, significantly improving the impact energy absorption performance of the material.

[0045] The low yield strength ratio 1400MPa grade medium manganese steel and its preparation method described in this invention are applicable to the field of automotive safety structural components, including but not limited to automotive anti-collision beams, door anti-collision bars, B-pillar reinforcements, bumpers, and other components requiring high collision energy absorption performance. This invention employs a conventional hot rolling combined with two-phase annealing process, avoiding the stringent equipment requirements of special processes such as warm rolling and quenching-partitioning. It can achieve mass production on existing continuous annealing production lines and has good prospects for industrial application.

[0046] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A low yield ratio 1400 MPa grade medium manganese steel, characterized in that, Composed of the following chemical components in weight percentage composition: C: 0.22%~0.32%, Mn: 10.0%~13.0%, Al: 1.8%~2.8%, Si: 0.15%~0.45%, Mo: 0.10%~0.30%, P≤0.008%, S≤0.004%, balance being Fe and unavoidable impurities; The microstructure of the medium manganese steel is ferrite + austenite + martensite, with the volume fraction of ferrite being 25% to 35% and the volume fraction of austenite being 20% ​​to 28%; the average grain size of the ferrite is 1 to 3 μm and the average grain size of the austenite is 0.5 to 2 μm.

2. The low yield strength ratio 1400MPa grade medium manganese steel according to claim 1, characterized in that, The medium manganese steel has a tensile strength ≥1400MPa, a yield strength ratio ≤0.80, and an elongation after fracture ≥24%.

3. A method of producing a low yield ratio 1400 MPa grade medium manganese steel according to any one of claims 1 or 2, characterized in that, Includes the following steps: 1) Smelting to obtain molten steel, and continuously casting the molten steel into billets; 2) The cast billet is subjected to homogenization and heat preservation treatment at 1200-1240℃; 3) The homogenized and heat-insulated billet is hot-rolled at a final rolling temperature of 800-860℃; 4) The hot-rolled steel plate is subjected to two-phase annealing treatment at a temperature of 720-760℃ and a holding time of 90-150 minutes, and then air-cooled to room temperature.

4. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 1), the smelting is either converter smelting or electric arc furnace smelting, and is subsequently refined by LF refining and RH vacuum refining; the continuous casting adopts full-process protective casting.

5. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 2), the homogenization and heat preservation treatment takes 2 to 4 hours.

6. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 3), the initial rolling temperature of the hot rolling is 1000-1100℃.

7. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 3), the total deformation of the hot rolling is 50% to 80%.

8. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 3), the hot rolling process is performed in multiple passes, with 5 to 7 passes.

9. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 4), the two-phase annealing process is carried out in an air atmosphere.

10. The method for preparing a low yield strength ratio 1400MPa grade medium manganese steel according to claim 3, characterized in that, In step 4), the air cooling rate is 1 to 10°C / s.

Citation Information

Patent Citations

  • Ultra-low carbon easily-welded medium-manganese automotive steel with controllable yield ratio and preparation method of automotive steel

    CN107419196A

  • A method for preparing 980MPa grade low yield strength ratio cold-rolled medium manganese steel

    CN110117755B

  • A method for preparing medium-manganese steel with low yield strength ratio and low yield elongation

    CN115198191B

  • A room temperature quenching-partitioning medium manganese steel with low yield ratio and high tensile strength and its preparation method

    CN117144261B

  • Preparation method of 1400 MPa-grade medium manganese steel

    CN119876553A