HRB500cE hot-rolled corrosion-resistant aseismic steel bar and preparation method thereof

By controlling the content of elements such as Cr, Ni, Cu, Nb, V and other elements and the hot rolling process, a refined structure is formed, which solves the problem that HRB500cE steel bars are difficult to take into account between strength and plasticity, and achieves high strength, excellent corrosion resistance and Good ductility steel bars are suitable for construction needs in seawater environments.

CN119082621AActive Publication Date: 2024-12-06新余钢铁股份有限公司

Patent Information

Application Number
CN202411206733.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing HRB500cE steel bars are difficult to take into account both strength and plasticity, and have insufficient corrosion resistance, especially in seawater environments, and face severe challenges of chloride ion corrosion.

Method used

By controlling the content of elements such as Cr, Ni, Cu, Nb, V and hot rolling process, a refined ferrite and bainite structure is formed to prevent the abnormal growth of austenite grains and improve the corrosion resistance of the steel bars and Mechanical properties while maintaining high ductility.

Benefits of technology

It realizes the high strength, excellent corrosion resistance and good ductility of HRB500cE steel bars, reduces the cost of raw material formulation, and is suitable for construction needs in seawater corrosion-resistant environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082621A_ABST
    Figure CN119082621A_ABST
Patent Text Reader

Abstract

The invention discloses an HRB500cE hot-rolled corrosion-resistant aseismic steel bar and a preparation method thereof, and relates to the technical field of steel production. The microstructure of the steel bar comprises, by volume, 38-41% of ferrite, less than or equal to 10% of pearlite and the balance bainite. By controlling the content of Cr, Ni and Cu, oxidation of the steel bar can be prevented, and the corrosion resistance and mechanical property of the steel bar are improved; the contents of Nb and V and the contents of other elements are further controlled, the Nb-V composite carbonitride can prevent abnormal growth of austenite grains, the effect of refining ferrite grains is also achieved in the cooling process of austenite transformation, the lamellar spacing of pearlite is refined, and meanwhile a certain amount of bainite is obtained. According to the structure concept, the strength of the steel bar can be guaranteed, the corrosion resistance of the steel bar is improved, meanwhile, the extension plasticity of the steel bar is not reduced, and the problem that the strength and plasticity of the high-strength corrosion-resistant HRB500cE steel bar are difficult to consider at the same time is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel production, and in particular to a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar and a preparation method thereof. Background Art

[0002] HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar is a type of steel that is resistant to chloride ion corrosion. Therefore, it is widely used in the field of seawater corrosion resistance technology and can be used as a raw material for reinforced concrete buildings such as coastal ports, docks, and cross-sea bridges. Studies have shown that the losses caused by steel bar corrosion are six times the combined losses of natural disasters such as floods, fires, hurricanes, and earthquakes. Therefore, the disasters and losses caused by steel bar corrosion are huge. At the same time, the total length of my country's coastline exceeds 32,000 kilometers. With the increase of reinforced concrete buildings such as coastal ports, docks, and cross-sea bridges, more buildings are facing the severe challenge of chloride ion corrosion. In addition, the strength and plasticity of high-strength steel bars are usually difficult to balance. When the strength of the steel bar increases, its plasticity decreases accordingly. When the plasticity of the steel bar increases, the strength will be lower. Therefore, it is urgent to provide a HRB500cE steel bar with higher strength, better corrosion resistance, and both plasticity and strength.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar and a preparation method thereof.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar, wherein the element composition of the steel bar comprises, by mass percentage: C: 0.12-0.16wt%, Si: 0.40-0.60wt%, Mn: 1.00-1.35wt%, Cr: 0.70-1.10wt%, Cu: 0.30-0.60wt%, Ni:

[0007] 0.30~0.60wt%, Nb: 0.012~0.018wt%, V: 0.070~0.085wt%, Alt: 0.025~0.040wt%, P≤0.035wt%, S≤0.035wt%, N≤0.010wt%, O≤30ppm, and the balance is Fe and unavoidable impurities.

[0008] The volume content of the microstructure of the steel bar includes: ferrite is 38-41%, pearlite content is ≤10%, and the balance is bainite.

[0009] In a second aspect, the present invention provides a method for preparing HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars as described in any of the aforementioned embodiments, comprising continuously casting refined molten steel smelted in proportion into ingots, and hot rolling the ingots.

[0010] The hot rolling process includes heating the ingot for a long time at high temperature and then single-line rolling, and the single-line rolling is a multi-stage weak cold temperature controlled rolling.

[0011] The present invention has the following beneficial effects:

[0012] The present invention provides a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar and a preparation method thereof. By controlling the contents of Cr, Ni and Cu, oxidation of the steel bar can be prevented, and the corrosion resistance of the steel bar can be improved. Meanwhile, Ni and Cu can also improve the mechanical properties of the steel bar. The contents of Nb and V and other elements are further controlled. During the hot rolling process, strain can induce Nb-V composite carbonitrides to precipitate at the austenite grain boundary and play a pinning role, thereby preventing abnormal growth of austenite grains during the heating process, controlling austenite recrystallization during the rolling process, and relieving austenite. The recrystallized grains grow and the austenite grains are refined. At the same time, the Nb-V composite carbonitrides are further precipitated. In the cooling process of austenite transformation, small polygonal ferrite grains are obtained, which also plays a role in refining the ferrite grains, so that the ferrite grain size in the steel bar is significantly refined, and the pearlite lamellar spacing is refined. At the same time, a certain amount of bainite is obtained, which can ensure the strength of the steel bar and improve the corrosion resistance of the steel bar without reducing the ductility and plasticity of the steel bar, effectively solving the problem of the difficulty in balancing the strength and plasticity of the high-strength and corrosion-resistant HRB500cE steel bar. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0014] Figure 1 This is an electron microscope image of the HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0016] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0017] HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar is a type of steel that is improved on the basis of HRB500E steel and is resistant to chloride ion corrosion. HRB500cE steel has better corrosion resistance than HRB500E steel. Therefore, in order to ensure the excellent performance of HRB500cE steel, its element composition and proportion are relatively more complex, and the process control process precision requirements are also higher. However, with the increase of reinforced concrete buildings such as coastal ports, docks, and cross-sea bridges, the demand for HRB500cE steel with seawater corrosion resistance is also increasing. Therefore, how to reduce the cost of HRB500cE steel and improve the mechanical properties and corrosion resistance of HRB500cE steel at the same time is one of the goals that this field has been pursuing.

[0018] In a first aspect, the present invention provides a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar, wherein the element composition of the steel bar comprises, by mass percentage: C: 0.12-0.16wt%, Si: 0.40-0.60wt%, Mn: 1.00-1.35wt%, Cr: 0.70-1.10wt%, Cu: 0.30-0.60wt%, Ni:

[0019] 0.30~0.60wt%, Nb: 0.012~0.018wt%, V: 0.070~0.085wt%, Alt: 0.025~0.040wt%, P≤0.035wt%, S≤0.035wt%, N≤0.010wt%, O≤30ppm, and the balance is Fe and unavoidable impurities.

[0020] Among them, carbon is an effective strengthening element and an austenite-forming element, which plays a role in solid solution strengthening. At the same time, it can form more pearlite in the steel, further improving the strength of the steel. The C element can reduce the potential difference between the various areas inside the steel bar, thereby reducing the corrosion rate.

[0021] Nitrogen is beneficial to the pitting corrosion resistance of steel. However, carbonitrides enriched at grain boundaries are prone to intergranular corrosion, which reduces the corrosion resistance of steel. Therefore, it is necessary to control the content ratio of nitrogen and carbon elements and control the precipitation process of carbonitrides. In addition, carbonitrides can also reduce the plasticity of steel bars. Therefore, the joint control of nitrogen content and carbon content in steel bars is even more important. The present invention can take into account the strength and plasticity of steel bars by controlling the element content of C and N within the above range, and at the same time, it works together with other alloying elements to improve the corrosion resistance of steel bars.

[0022] Silicon mainly improves the strength of steel bars in the form of solid solution strengthening. It is also a deoxidizing element in steel and a ferrite-forming element. However, too high Si content will reduce the plasticity of the steel and deteriorate the welding performance of the steel bars.

[0023] Manganese is a weak carbide-forming element. Its role in smelting is to deoxidize and eliminate the effects of sulfur. It can also reduce the transformation temperature of austenite and refine ferrite grains, which is beneficial to improving the strength and toughness of steel bars. In addition, it can also strengthen ferrite by solid solution and combine with harmful element S to reduce the hot brittleness of steel bars; however, when the Mn content is too high, the plasticity, impact toughness, and welding performance of steel bars will all decrease.

[0024] Chromium can form a dense chromium oxide film in steel to effectively prevent the oxidation of steel bars and improve the corrosion resistance of the steel bar matrix. In addition, Cr is also one of the important elements for generating ferrite and carbide, and has an important influence on the organizational properties of steel bars. When the Cr content is too high, a large amount of bainite is easily generated in the steel bars, affecting the ductility and plasticity of the steel bars. Therefore, the Cr content needs to be controlled within a certain range to ensure that the steel bars contain a certain amount of bainite, but not to the extent that it affects the ductility and plasticity of the steel bars.

[0025] Nickel, copper and chromium are the main corrosion-resistant elements in steel bars. Nickel has strong corrosion resistance to acids and alkalis, which can improve the strength of steel bars while better maintaining the plasticity and toughness of steel bars. Copper has good resistance to atmospheric corrosion and can also improve the strength and toughness of steel bars.

[0026] Vanadium mainly precipitates fine V (C, N) structures and pins them on the austenite grain boundaries, thereby refining the austenite grains and improving strength and toughness.

[0027] During the heating and rolling process of the steel billet, niobium will form niobium carbonitride with carbon and nitrogen, and concentrate at the austenite grain boundary, effectively inhibiting the recrystallization of austenite. As a second phase particle, it prevents the growth of austenite grains and plays a role in grain refinement, thereby improving the strength and toughness of the steel bar. At the same time, the addition of Nb promotes the precipitation of fine Nb-V composite carbonitrides, further improving the strength and toughness matching of the steel bar.

[0028] Furthermore, the present invention controls the contents of nickel, copper, chromium, vanadium and niobium, so that the present invention can use relatively less nickel, copper and chromium to achieve the main anti-corrosion effect, combined with the fine-grained strengthening effect of vanadium and niobium composite, thereby reducing the raw material formula cost of the steel bar.

[0029] A small amount of aluminum can refine the grains and improve toughness. It also has antioxidant and corrosion resistance. Combined with chromium and silicon, it can improve the high-temperature corrosion resistance of steel bars.

[0030] By controlling the element composition of the steel bar within the above range, the volume content of the microstructure of the obtained steel bar includes: ferrite is 38-41%, pearlite content is ≤10%, and the balance is bainite. Since the content of pearlite is relatively small and the content of ferrite is 38-41%, the microstructure of the steel bar contains about 50% bainite, thereby ensuring the strength of the steel bar; in addition, the content of ferrite in the steel bar can ensure the plasticity of the steel bar. The combination of the two can make the yield strength, elongation after fracture and total elongation at maximum force of the steel bar excellent. In addition, controlling the bainite content in the steel bar can also make the steel bar have better corrosion resistance.

[0031] In an optional embodiment, the element composition of the steel bar includes, by mass percentage, C: 0.12-0.16wt%, Si: 0.40-0.60wt%, Mn: 1.00-1.35wt%, Cr: 0.70-1.10wt%, Cu: 0.30-0.45wt%, Ni: 0.30-0.45wt%, Nb: 0.012-0.018wt%, V: 0.070-0.080wt%, Alt: 0.025-0.040wt%, P≤0.035wt%, S≤0.035wt%, N≤0.010wt%, O≤30ppm, and the balance is Fe and unavoidable impurities. The element composition of the steel bar is further preferably controlled within the above range, so that HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars with good mechanical properties and good corrosion resistance can be obtained at the same time.

[0032] In an optional embodiment, the yield strength R of the hot-rolled corrosion-resistant and earthquake-resistant steel bar is eL ≥540MPa, tensile strength R m ≥850MPa, elongation A≥20.0%, total elongation at maximum force A gt ≥9.5%, R 0 m / R 0 eL ≥1.35, R 0 eL / R eL ≤1.18, average corrosion rate ≤4.1g / m 2 ·h, the relative corrosion rate is ≤67% compared with HRB500E steel bar.

[0033] In an optional embodiment, the volume content of the microstructure of the hot-rolled corrosion-resistant and earthquake-resistant steel bar includes: ferrite is 40-41%, pearlite content is ≤8%, the balance is bainite, and the grain size is above grade 9.5.

[0034] In order to improve the various properties of steel bars, in addition to controlling the elemental composition of the steel bars, the process also needs to be controlled to ensure that the composition of each element can form the expected bainite structure content, ferrite structure content and pearlite structure content.

[0035] In a second aspect, the present invention provides a method for preparing a steel bar as described in any one of the aforementioned embodiments, comprising continuously casting refined molten steel smelted in proportion into ingots, and hot rolling the ingots.

[0036] The hot rolling process includes heating the ingot for a long time at high temperature and then single-line rolling, and the single-line rolling is a multi-stage weak cold temperature controlled rolling.

[0037] In some embodiments, in order to clearly illustrate the preparation method of the HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar of the present invention, the method comprises the following steps:

[0038] S01. Molten steel smelting

[0039] In an optional embodiment, the process of molten steel smelting includes smelting molten iron in a converter to obtain molten steel, and then sending the molten steel to an argon station for argon blowing and then performing LF refining to obtain refined molten steel.

[0040] The purpose of molten steel smelting is to ensure that the content of each element in the refined molten steel is within the content range required by the steel grade. Therefore, in order to achieve the above goal, in the actual smelting process, the molten steel smelting process can also be adjusted according to the specific conditions of each furnace of molten steel. The following is a preferred molten steel smelting scheme provided by the present invention, which can quickly and accurately adjust the various components in the molten steel to within the range required by the steel grade.

[0041] Preferably, the converter smelting adopts conventional top and bottom combined oxygen converter smelting, argon is blown throughout the steel discharge process, and when 1 / 4 of the converter is discharged, aluminum source, silicon source, manganese source, chromium source, copper source, nickel source and scrap steel are added to the molten steel in sequence for deoxidation and alloying, and then the molten steel is sent to the argon station for argon blowing. In this way, not only can the content of some alloy elements in the molten steel be adjusted first, but argon blowing can also make the various components in the molten steel and the molten steel temperature more uniform.

[0042] Preferably, in order to improve the yield of various raw material alloys and achieve uniform distribution of the alloys, the argon blowing time of the argon station is greater than or equal to 6 minutes.

[0043] The silicon source may be ferrosilicon and / or silicomanganese. When the silicon source is ferrosilicon and silicomanganese, silicomanganese should be added to the molten steel first, and then ferrosilicon. In addition, silicomanganese can also be used as a manganese source to adjust the manganese content in the molten steel. The chromium source may be ferrochrome, and the copper and nickel sources may be copper plates and nickel plates, or their corresponding alloys may be used as raw materials.

[0044] The molten steel discharged from the argon station is sent to the LF furnace for refining through a ladle. In an optional embodiment, during the LF refining process, the mass ratio of lime to molten steel is 3-6 kg / t, and the mass ratio of fluorite to molten steel is 0.5-1 kg / t. Lime and fluorite are added to form slag during the LF smelting process and to assist the refining process in completing desulfurization and deoxidation.

[0045] Preferably, after adding lime and fluorite, electrification is applied to slag for 8 to 15 minutes.

[0046] Preferably, after the electroslag is slag-forming, a deoxidizer is added to make white slag, and a niobium source and a vanadium source are added to adjust the element content in the molten steel. When the refined molten steel temperature is 1600°C, the calcium wire is fed for 100 to 150 m, and the soft argon blowing time is greater than or equal to 10 min to obtain refined molten steel.

[0047] S02, continuous casting

[0048] The refined molten steel obtained in S01 is continuously cast into a plurality of ingots. In an optional embodiment, during the continuous casting process, the temperature of the molten steel during the continuous casting in the tundish is 1520-1560°C, and the casting speed is 2.2-3.0 m / min. By controlling the above continuous casting parameters, the continuous casting process can be ensured to proceed smoothly, and the leakage of the molten steel due to the high temperature of the molten steel during the continuous casting process can be avoided, and the phenomenon of agglomeration in the crystallizer due to the low temperature of the molten steel during the continuous casting process can be avoided.

[0049] S03, hot rolling

[0050] The ingot obtained after continuous casting of S02 is subjected to heat rolling. The heat rolling includes heating the ingot for a long time at high temperature and then single-line rolling. The single-line rolling is multi-stage weak cold temperature control rolling.

[0051] In an optional embodiment, during the high temperature and long heating process, the ingot stays in the heating furnace for more than 120 minutes, and the heating rate is 15-20°C / s. Preferably, the soaking zone temperature of the heating furnace is 1140-1180°C.

[0052] High temperature and long time heating can make the alloy elements in the steel bar fully dissolved, but the heating temperature of the ingot should not be too high. Too high heating temperature will not only cause coarse grains and damage the mechanical properties of the material, but also cause overburning of the crystals. Therefore, controlling the heating time and heating temperature of the ingot within the above range can ensure the full solution of the alloy elements without causing adverse effects.

[0053] Preferably, in order to ensure that the parameters of the above-mentioned high-temperature and long heating process meet the above-mentioned requirements, this can be achieved by controlling the temperature of the heating furnace, for example, the temperature of the heating section of the heating furnace is 990-1110°C.

[0054] Preferably, the heating section of the heating furnace includes a first heating section and a second heating section, the temperature of the first heating section is 990-1030°C, and the temperature of the second heating section is 1070-1110°C.

[0055] After the heating in the heating furnace is completed, the ingot enters the rolling mill for single-line rolling. The single-line rolling adopts multi-stage weak cold temperature control and rolling. In an optional embodiment, the multi-stage weak cold temperature control and rolling includes rough rolling, intermediate rolling, pre-finishing rolling and finishing rolling of the heated ingot, wherein rough rolling, intermediate rolling and pre-finishing rolling are pre-rolling processes, and the rolled product obtained after the pre-finishing rolling is the intermediate ingot, which is then controlled cooled and finish rolled to obtain the finished rolled product.

[0056] Preferably, the starting rolling temperature of the rough rolling is 990-1030°C. Too high or too low starting rolling temperature will be detrimental to the temperature-controlled rolling process and deformation control of the ingot. As the rolling temperature increases, the deformation increases, and recrystallization is more likely to occur. When the starting rolling temperature is controlled within the above range, the uniformity of the austenite structure after hot deformation is affected by the deformation and rolling temperature. Increasing the deformation and the rolling temperature is conducive to the uniform distribution of the austenite structure.

[0057] The processes of rough rolling, intermediate rolling and pre-finishing rolling can be carried out using existing rolling methods to obtain intermediate billets. Since the temperature of the steel bars will continue to rise during the rolling process, in order to better control the structural composition of the steel bars during the finishing rolling process, the intermediate billet needs to be cooled and temperature controlled before finishing rolling to prevent the temperature of the intermediate billet from being too high, which will cause the growth of unfavorable structures during the rolling process.

[0058] Preferably, the cooling rate of the intermediate billet before finish rolling is 5-15°C / s, and the start temperature of finish rolling is 960-1000°C. More preferably, the start temperature of finish rolling is 960-980°C.

[0059] As long as the cooling rate of the intermediate billet before finish rolling is controlled within the above range, and the finish rolling is carried out at the above start temperature of finish rolling, the adverse effect of temperature increase on the control of the steel bar structure can be offset. It is prevented that the temperature of the intermediate billet is too high, causing the austenite grains inside the structure to grow, or the temperature of the intermediate billet is too low, causing the structure to transform and precipitate secondary cementite. The present invention makes full use of the controlled rolling and controlled cooling method combined with the precipitation strengthening and fine grain strengthening effect of the carbonitride formed by the composite precipitation of Nb-V to obtain HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars with better structure performance.

[0060] Preferably, the cooling rate of the intermediate billet before finishing rolling is controlled by controlling the amount of water in the water piercer through which the intermediate billet passes before finishing rolling. For example, in some embodiments, both sets of water piercers before finishing rolling must be put into use, and the amount of water in the second set of water piercers is controlled to be greater than the amount of water in the first set of water piercers, and the difference in the amount of water between the two sets is 10-20%. By increasing the amount of water before finishing rolling, more cooling capacity is provided for the billet.

[0061] In order to control the high content of bainite structure in the steel bar, for example, the water volume of the first set of water piercers before the finish rolling can be controlled to be 80-90%, and the water volume of the second set of water piercers can be controlled to be 100%.

[0062] Preferably, after the intermediate billet is finished and the finished rolled piece is obtained, the finished rolled piece needs to be cooled and then sent to the cooling bed for cooling to ensure that the final structure and morphology of the steel bar meet the requirements. Specifically, the cooling rate of the finished rolled piece is less than or equal to 1.5°C / s, and the temperature of the cooling bed on the finished rolled piece is 950-990°C.

[0063] In order to ensure slow cooling of the steel bars after finish rolling, only the first two groups of water permeators are opened after finish rolling, and the last four groups are all closed. The water volume of the last group is 15-25% lower than that of the previous group. The finish-rolled parts are cooled by gradually lower cooling water volume, which achieves slow cooling of the finish-rolled parts and is conducive to the morphological transformation of the bainite structure in the formation organization.

[0064] For example, after finishing rolling, the water volume of the first group of water piercers is 100%, and the water volume of the second group of water piercers is 80%.

[0065] After cooling to the upper cooling bed temperature at the above cooling rate, the finished rolled piece is sent to the cooling bed for cooling. By controlling the high upper cooling bed temperature and the lower cooling rate, the composition and proportion of each tissue phase in the microstructure of the steel bar can be finely controlled.

[0066] Example 1

[0067] The present embodiment provides a HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar, whose element composition, measured by mass percentage, includes: C: 0.16wt%, Si: 0.52wt%, Mn: 1.21wt%, Cr: 0.79wt%, Cu: 0.40wt%, Ni: 0.40wt%, Nb: 0.016wt%, V: 0.073wt%, Alt: 0.031wt%, P: 0.019wt%, S: 0.009wt%, N: 0.0080wt%, O≤30ppm, and the remainder is Fe and unavoidable impurities.

[0068] This embodiment also provides a method for preparing HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars, comprising the following steps:

[0069] S01. Molten steel smelting

[0070] The molten iron is added into a conventional top and bottom double-blown oxygen converter for converter smelting. Argon is blown throughout the steel discharge process. When 1 / 4 of the steel is discharged from the converter, aluminum blocks, ferrosilicon, silicon manganese, ferrochrome, copper plates, nickel plates and scrap steel are added into the molten steel in turn for deoxidation and alloying. Then the ladle is sent to the argon station for argon blowing for 10 minutes.

[0071] The molten steel leaving the argon station is sent to the LF furnace for refining through a ladle. 500kg of lime and 100kg of fluorite are added as slag materials. After electrification for 10 minutes, deoxidizer is added to make white slag. At the same time, niobium iron, vanadium nitrogen alloy and other alloys are added to fine-tune the composition. After the composition temperature reaches 1600℃, 100m of pure calcium wire is fed and the soft argon blowing time is 12 minutes to obtain refined molten steel.

[0072] S02, continuous casting

[0073] The refined molten steel obtained from S01 was continuously cast into multiple ingots. The molten steel temperature during continuous casting in the tundish was 1550°C, the water volume of the continuous casting machine was 1.6L / t, and the casting speed was 2.5m / min.

[0074] S03, hot rolling

[0075] The ingot obtained after continuous casting of S02 was heated and rolled, and the ingot was kept in the heating furnace for 120 minutes at a heating rate of 15°C / s. The temperature of the first heating section of the heating furnace was 1000°C, the temperature of the second heating section was 1100°C, and the temperature of the soaking section was 1160°C.

[0076] After the ingot is heated in the heating furnace, it enters the rolling mill for rough rolling, intermediate rolling, pre-finishing rolling and finishing rolling in sequence. Among them, rough rolling, intermediate rolling and pre-finishing rolling are the pre-rolling processes, and the rolled product obtained after the pre-finishing rolling is the intermediate billet, which is then controlled cooled and finish rolled to obtain the finished rolled product.

[0077] The starting rolling temperature of the rough rolling is 1025°C. The intermediate billet obtained after the pre-finishing rolling is cooled to the starting rolling temperature of 980°C at a cooling rate of 10°C / s, and then the finishing rolling is carried out. After the finishing rolling, the finished rolled piece is obtained, and the cooling rate of the finished rolled piece is controlled to be 0.8°C / s, and the finished rolled piece is cooled to the temperature of 990°C on the cooling bed, and the finished rolled piece is sent to the cooling bed.

[0078] The HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar provided in this embodiment was placed under an electron microscope for observation, and the following results were obtained: Figure 1 The results are shown. Figure 1 It can be seen that the microstructure of steel bars is mainly ferrite and bainite, which contains a small amount of pearlite.

[0079] The preparation methods of Examples 2 to 5 and Comparative Examples 1 to 5 are similar to those of Example 1, except that the element ratios are different, as shown in Table 1, and the parameters of the hot rolling step are different, as shown in Table 2. In the table, S refers to the examples, and D refers to the comparative examples.

[0080] Table 1 Element composition of HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars (wt%)

[0081] C Mn S P Si Cr Ni Cu V Nb Alt N S1 0.16 1.21 0.009 0.019 0.52 0.79 0.40 0.40 0.073 0.016 0.031 0.0080 S2 0.12 1.16 0.001 0.011 0.51 0.80 0.39 0.40 0.085 0.017 0.035 0.0050 S3 0.12 1.10 0.008 0.017 0.51 0.79 0.39 0.40 0.085 0.015 0.026 0.0046 S4 0.14 1.19 0.002 0.012 0.53 0.79 0.42 0.38 0.080 0.013 0.039 0.0035 S5 0.15 1.25 0.009 0.018 0.54 0.79 0.40 0.42 0.070 0.017 0.021 0.0088 D1 0.16 1.20 0.009 0.018 0.51 0.80 0.40 0.41 0.075 0.010 0.035 0.0060 D2 0.15 1.18 0.008 0.017 0.52 0.79 0.42 0.39 0.080 0.002 0.025 0.0084 D3 0.07 1.25 0.008 0.018 0.54 0.99 0.45 0.45 0.085 0.015 0.038 0.0035 D4 0.14 1.24 0.008 0.017 0.52 1.20 0.45 0.45 0.085 0.016 0.038 0.0045 D5 0.14 1.24 0.008 0.017 0.52 1.00 0.45 0.45 0.002 0.035 0.038 0.0045

[0082] Table 2 Hot rolling process parameters

[0083]

[0084] Test Example 1

[0085] The performance of the HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars provided in Examples 1 to 5 and Comparative Examples 1 to 5 was tested, and the results shown in Tables 3 and 4 were obtained.

[0086] Among them, the yield strength is tested by GB / T 228.1 method, the tensile strength is tested by GB / T228.1 method, the maximum force total elongation is tested by GB / T 228.1 method, and the corrosion rate is tested by YB / T 4367 method.

[0087] Table 3 Performance of HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars

[0088] Table 4 Microstructure of HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars

[0089] Diameter(mm) Ferrite(%) Bainite (%) Pearlite(%) Grain size (grade) S1 25 38 54 8 10.0 S2 25 39 56 5 9.5 S3 28 39 56 5 9.5 S4 28 40 52 8 9.5 S5 36 41 51 8 9.5 D1 25 35 55 10 9.5 D2 25 36 49 15 9.5 D3 28 48 44 8 9.0 D4 32 35 60 5 9.5 D5 25 39 56 5 9.0

[0090] It can be seen from Table 3 and Table 4 that the steel bars provided by Examples 1 to 5 of the present invention have excellent comprehensive performance. They not only have better strength, but also have a yield strength of more than 540 MPa, a tensile strength of 850 to 885 MPa, a large total elongation at maximum force, and good ductility. At the same time, the steel bars of Examples 1 to 5 of the present invention also have better corrosion resistance and a low corrosion rate. Compared with ordinary HRB500E steel bars, the relative corrosion rate is smaller.

[0091] Comparative Examples 1 and 2 changed the content of Nb and the temperature of the soaking zone during hot rolling, which significantly reduced the mechanical properties of the steel bars. Comparative Example 3 reduced the carbon content and reduced the hot rolling time in the furnace, which also significantly reduced the mechanical properties of the steel bars. Comparative Example 4 changed the content of Cr. Although it had higher strength and corrosion resistance, its ductility was significantly reduced. Comparative Example 5 changed the content of V and Nb. It also had higher strength and corrosion resistance, but its ductility was significantly reduced.

[0092] In summary, the HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar and its preparation method provided by the present invention have at least the following advantages:

[0093] 1) By controlling the element composition and adopting a low-carbon + chromium, nickel, copper, aluminum, niobium and vanadium alloy system, the steel bar has excellent corrosion resistance and comprehensive mechanical properties through niobium and vanadium composite strengthening, high-temperature long heating and multi-stage weak controlled cooling technology. The overall comprehensive performance is excellent and is suitable for the use requirements of projects in chloride ion corrosion environments.

[0094] 2) Under the above-mentioned chemical composition design scheme, high-temperature long heating, high-temperature rolling, high-temperature cooling bed and cooling rate control technology are adopted to reduce the manufacturing cost while reducing the alloy cost, and further optimize the overall comprehensive performance of the obtained steel bar, which is suitable for actual production and processing, and the process operation is simple and easy to control, ensuring the smooth operation of the actual production conditions, and has higher social significance and economic effect.

[0095] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar, characterized in that: In terms of mass percentage, the element composition of steel bars includes: C: 0.12-0.16wt%, Si: 0.40-0.60wt%, Mn: 1.00-1.35wt%, Cr: 0.70-1.10wt%, Cu: 0.30-0.60wt%, Ni: 0.30~0.60wt%, Nb: 0.012~0.018wt%, V: 0.070~0.085wt%, Alt: 0.025~0.040wt%, P≤0.035wt%, S≤0.035wt%, N≤0.010wt%, O≤ 30ppm, the balance is Fe and unavoidable impurities; The volume content of the microstructure of the steel bar includes: ferrite content is 38-41%, pearlite content is ≤10%, and the balance is bainite.

2. The HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar according to claim 1, characterized in that: In terms of mass percentage, the element composition of the steel bar includes: C: 0.12-0.16wt%, Si: 0.40-0.60wt%, Mn: 1.00-1.35wt%, Cr: 0.70-1.10wt%, Cu: 0.30~0.45wt%, Ni: 0.30~0.45wt%, Nb: 0.012~0.018wt%, V: 0.070~0.080wt%, Alt: 0.025~0.040wt%, P≤0.035wt%, S≤0.035wt%, N≤0.010wt%, O≤30ppm, and the balance is Fe and unavoidable impurities.

3. The HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar according to claim 1, characterized in that: The yield strength R of the steel bar eL ≥540MPa, tensile strength R m ≥850MPa, elongation A≥20.0%, total elongation at maximum force A gt ≥9.5%, R 0 m / R 0 eL ≥1.35, R 0 eL / R eL ≤1.18, average corrosion rate ≤4.1g / m 2 ·h, the relative corrosion rate is ≤67% compared with HRB500E steel bar.

4. The HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bar according to claim 1, characterized in that: The volume content of the microstructure of the steel bar includes: ferrite is 40-41%, pearlite content is ≤8%, the balance is bainite, and the grain size is above grade 9.

5.

5. A method for preparing HRB500cE hot-rolled corrosion-resistant and earthquake-resistant steel bars according to any one of claims 1 to 4, characterized in that: The method comprises continuously casting the refined molten steel smelted in proportion into a casting billet, and hot rolling the casting billet; The hot rolling process includes heating the ingot for a long time at a high temperature and then single-line rolling, wherein the single-line rolling is multi-stage weak cold temperature-controlled rolling.

6. The preparation method according to claim 5, characterized in that: The multi-stage weak cooling temperature control rolling includes pre-rolling the heated ingot into an intermediate billet, and then cooling the intermediate billet and then finishing rolling it to obtain a finished rolled piece; The cooling rate of the intermediate billet before finishing rolling is 5-15°C / s, and the finishing rolling start temperature is 960-1000°C; Preferably, the finishing rolling start temperature is 960-980°C; Preferably, after the finish rolling of the intermediate billet is completed, the cooling rate of the finished rolled piece is less than or equal to 1.5°C / s, and the temperature of the cooling bed on the finished rolled piece is 950-990°C; Preferably, the process of pre-rolling the cast billet into an intermediate billet comprises performing rough rolling, intermediate rolling and pre-finish rolling on the cast billet, and the starting rolling temperature of the rough rolling is 990-1030°C.

7. The preparation method according to claim 5 or 6, characterized in that: During the high temperature and long heating process, the ingot is kept in the heating furnace for more than 120 minutes, and the heating rate is 15-20°C / s; Preferably, the soaking zone temperature of the heating furnace is 1140-1180°C; Preferably, the temperature of the heating section of the heating furnace is 990-1110°C; Preferably, the heating section of the heating furnace comprises a first heating section and a second heating section, the temperature of the first heating section is 990-1030°C, and the temperature of the second heating section is 1070-1110°C.

8. The preparation method according to claim 5, characterized in that: The preparation of the refined molten steel includes smelting molten iron in a converter to obtain molten steel, and sending the molten steel to an argon station for argon blowing and then LF refining; Preferably, argon is blown throughout the steel discharge process of the converter smelting. When 1 / 4 of the steel is discharged from the converter, aluminum source, silicon source, manganese source, chromium source, copper source, nickel source and scrap steel are sequentially added to the molten steel for deoxidation and alloying, and then the molten steel is sent to an argon station for argon blowing; Preferably, the argon blowing time of the argon station is greater than or equal to 6 minutes.

9. The preparation method according to claim 8, characterized in that: During the LF refining process, the mass ratio of lime to molten steel is 3-6 kg / t, and the mass ratio of fluorite to molten steel is 0.5-1 kg / t; Preferably, after adding lime and fluorite, electrification is applied to slag for 8 to 15 minutes; Preferably, after the electroslag is slag-forming, a deoxidizer is added to make white slag, and a niobium source and a vanadium source are added to adjust the element content in the molten steel. When the refined molten steel temperature is 1600°C, the calcium wire is fed for 100 to 150 m, and the soft argon blowing time is greater than or equal to 10 min.

10. The preparation method according to claim 5, characterized in that: During the continuous casting process, the temperature of the molten steel during continuous casting in the tundish is 1520-1560° C., and the casting speed is 2.2-3.0 m / min.

Citation Information

Patent Citations

  • Cl- corrosion resistant high-strength low-alloy steel bar and production method thereof

    CN101709434A

  • High-strength reinforced bar and production method for same

    CN102994883A

  • Corrosion-resistant reinforcement for reinforced concrete and preparation method of corrosion-resistant reinforcement

    CN111270141A

  • High-strength alloy cold heading steel B7 wire rod and production method thereof

    CN112680669A

  • Preparation method of high-speed single-line rolled HRB400E anti-seismic reinforcing steel bar

    CN116460141A

Cited By

  • 400MPa-grade low-temperature corrosion-resistant steel bar for frozen soil engineering and preparation method of low-temperature corrosion-resistant steel bar

    CN121718804A