A wear-resistant sealing coating resistant to salt spray corrosion and its preparation method

By employing a Co-based alloy and composite coating design on the surface of titanium alloys, a silver thermal conductive network and a dual lubricant system are constructed, solving the problems of insufficient stability and salt spray corrosion resistance of the sealing coating on the titanium alloy surface at high temperatures, thus achieving effective protection of the blade tip and improved rotor stability.

CN123108463APending Publication Date: 2026-11-17INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611292504.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, the sealing coating on the titanium alloy surface has poor stability at high temperature, insufficient resistance to salt spray corrosion, and the accumulation of frictional heat during high-speed scraping leads to severe blade tip wear. The coating is prone to adhesive wear, resulting in poor rotor running stability and premature corrosion failure in marine environments.

Method used

Using a Co-based alloy as the bonding layer, a composite coating consisting of a Co-based alloy, polyphenylene ester, hexagonal boron nitride, eutectic calcium fluoride/barium fluoride, and silver is prepared by supersonic flame and atmospheric plasma spraying technology to form a continuous or discontinuous silver thermally conductive network. The dual lubricant system provides lubrication performance across the entire temperature range, and a high-porosity pore network is formed through the thermal decomposition of polyphenylene ester.

Benefits of technology

It achieves efficient and stable sealing protection of the coating at high temperatures of 500~800 ℃, reduces blade tip wear, improves rotor stability, and enhances salt spray corrosion resistance, thus solving the high temperature stability and corrosion resistance problems existing in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108463A_ABST
    Figure CN123108463A_ABST
Patent Text Reader

Abstract

This invention discloses a salt spray corrosion resistant wearable sealing coating and its preparation method, belonging to the technical field of metal material surface protective coatings. The coating comprises a Co-based alloy bonding underlayer and a composite wearable surface layer; the wearable surface layer is composed of a Co-based alloy, polystyrene, hexagonal boron nitride, eutectic calcium fluoride / barium fluoride, and silver, wherein polystyrene serves as a pore-forming agent, hexagonal boron nitride as a first lubricant, eutectic calcium fluoride / barium fluoride as a second lubricant, and silver as a thermally conductive component. This invention avoids high-temperature interdiffusion between the Co-based bonding underlayer and the titanium alloy substrate; utilizes silver to construct an efficient thermally conductive network, suppressing frictional thermal damage to the blade tips during high-speed scraping; and employs a dual-lubricant compounding strategy, which not only provides synergistic lubrication over a wide temperature range, preventing adhesive wear, but also mitigates galvanic corrosion between metal components. This coating is suitable for high-temperature sealing conditions in titanium alloy compressors in marine environments, effectively protecting blade tips and maintaining rotor operational stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of protective coating technology for metal material surfaces, specifically to a wearable sealing coating resistant to salt spray corrosion and its preparation method, which is suitable for sealing applications of titanium alloy compressors for aero-engines in marine environments at medium and high temperatures of 500~800 ℃. Background Technology

[0002] High thrust-to-weight ratio, low fuel consumption rate, and high service safety are core development indicators for advanced aero-engines. To meet these performance requirements, aero-engine compressors are undergoing iterative upgrades towards higher speeds, higher operating temperatures, and higher pressure ratios. High-temperature titanium alloys, with their low density, high specific strength, excellent medium- and high-temperature mechanical properties, and thermal stability, are gradually replacing traditional nickel-based high-temperature alloys and becoming key structural materials for the next generation of high-performance aero-engines.

[0003] Precise control of the compressor-stator clearance in aero-engines is a core technology for improving engine aerodynamic efficiency, reducing fuel consumption, and extending the overall service life of the engine. Under high-speed compressor operation, blades may experience slight radial misalignment due to factors such as high-temperature thermal expansion, aerodynamic load impact, and engine surge. This can easily lead to hard scraping contact between the blade tips and the casing inner wall. Without effective protection, irreversible wear at the blade tips will occur, not only reducing airtightness but also potentially inducing fatigue cracks, seriously threatening the safety and lifespan of the entire engine.

[0004] Preparing a wearable sealing coating on the inner surface of the casing is a recognized effective method for solving the above problems. Its core principle is that during scraping contact, the blade tip preferentially scrapes the coating rather than itself, forming an ideal operating clearance while absorbing energy and suppressing vibration, thereby protecting the integrity of the rotor structure. An ideal wearable sealing coating must possess the following characteristics: suitable hardness (low and controllable), good bonding strength, structural and performance stability at high temperatures, and excellent wearability without damaging the wear-bearing parts during high-speed scraping. Furthermore, when operating in high-humidity, high-salt-spray marine environments, the wearable sealing coating must also possess certain corrosion resistance, especially given its multiphase, porous, and multilayered composite structure design, which is highly susceptible to corrosive media penetration and galvanic corrosion due to differences in corrosion potential between different materials, leading to premature coating failure.

[0005] To address the technical challenge of abrasive sealing of titanium alloy surfaces, several sealing coating solutions have been disclosed in the existing technology. However, all of them have unavoidable technical defects and are difficult to adapt to the harsh service conditions of 500~800 ℃ in marine environments.

[0006] A patent search revealed Chinese patent publication number CN114045454A, which discloses a titanium fire-resistant wear-resistant sealing coating and its preparation method. This coating employs a three-layer composite structure: a NiCrAl base layer, a nano-zirconia intermediate layer, and an AlSi / BN top layer, possessing good bonding strength, thermal insulation, and wear resistance. However, its core functional layer, the AlSi / BN system, has limited high-temperature resistance, making it suitable only for low-temperature titanium alloy compressors operating at 450 ℃ and below, and unsuitable for the medium-to-high temperature service environment of high-temperature titanium alloy compressors (500~800 ℃).

[0007] For example, Chinese Patent Publication No. CN109554657A discloses a graded-structure anti-titanium fire wear-resistant sealing coating and its preparation method. This coating uses NiCrAlY as the bonding underlayer and employs a yttrium-stabilized zirconium oxide and aluminum-silicon / boron nitride composite system to prepare a graded-structure surface layer. The graded-structure design optimizes the coating's thermal expansion matching and bonding strength, achieving both anti-titanium fire and wear-resistant sealing effects. However, the NiCrAlY bonding underlayer in this solution is prone to severe elemental interdiffusion with the titanium alloy matrix at high temperatures, forming a brittle phase and deteriorating the matrix's mechanical properties, posing a significant application risk.

[0008] For example, Chinese Patent Publication No. CN110747428A discloses an integrated flame-retardant sealing coating for titanium alloy surfaces, its preparation method, and its application. This solution uses a titanium-zirconium amorphous alloy as the flame-retardant bonding layer, avoiding the high-temperature interdiffusion problem between the NiCrAl bonding layer and the titanium alloy substrate. Simultaneously, NiCrAl-bentonite is selected as the wear-resistant surface layer, suitable for the medium-to-high temperature service temperature range of titanium alloys. However, this NiCrAl-bentonite surface layer has inherent performance defects: a low thermal diffusivity and high overall hardness. During high-speed scraping, frictional heat is difficult to dissipate quickly, easily accumulating locally at the blade tip, causing high-temperature softening, oxidation, or even local melting of the blade tip, leading to severe blade tip wear. This not only fails to effectively protect the blades but also exacerbates rotor mass imbalance, making it difficult to meet the safe service requirements of the compressor.

[0009] In summary, current technologies lack a wearable sealing coating system that can simultaneously ensure long-term stable operation of high-temperature titanium alloy compressors at 500–800 °C, effectively suppress frictional heat damage and protect blade tips under high-speed scraping conditions, and also possess salt spray corrosion resistance. Therefore, developing a salt spray corrosion-resistant wearable sealing coating and its preparation method that is compatible with titanium alloy substrates, possesses medium-to-high temperature stability, excellent wearability, and low blade tip wear damage characteristics is a pressing technical challenge that needs to be addressed in this field. Summary of the Invention

[0010] The purpose of this invention is to address the technical defects of existing titanium alloy surface sealing coatings, such as poor high-temperature stability and adaptability, insufficient salt spray corrosion resistance, high-speed scraping frictional heat accumulation, severe blade tip wear, easy adhesion wear of the coating, poor rotor operation stability, and premature corrosion failure. This invention provides a wearable sealing coating resistant to salt spray corrosion and its preparation method. By optimizing the coating component system, microstructure, and preparation process, the above-mentioned technical problems are comprehensively solved, achieving efficient, stable, and long-lasting sealing protection for titanium alloy compressors of aero-engines under operating conditions of 500~800 ℃.

[0011] The present invention provides a salt spray corrosion resistant abrasive sealing coating, comprising an adhesive underlayer and an abrasive toplayer. The adhesive underlayer is a Co-based alloy coating, and the abrasive toplayer is a composite coating composed of a Co-based alloy, polystyrene, hexagonal boron nitride, eutectic calcium fluoride / barium fluoride, and silver. Polystyrene serves as a pore-forming agent, hexagonal boron nitride as a first lubricant, eutectic calcium fluoride / barium fluoride as a second lubricant, and silver as a thermally conductive component. The Co-based alloy coating is either a CoCrAlY coating or a CoCrAlYSi coating. The chemical composition of the CoCrAlY coating is: 15.0~25.0 wt.% Cr, 10.0~15.0 wt.% Al, 0.2~1.0 wt.% Y, with the balance being Co. The chemical composition of the CoCrAlYSi coating is: 15.0~25.0 wt.% Cr, 10.0~15.0 wt.% Al, 0.2~1.0 wt.% Y, 0.2~1.0 wt.% Si, with the balance being Co. The mass percentages of each component in the wearable surface layer are as follows: 60.0~80.0 wt.% Co-based alloy, 5.0~10.0 wt.% polyphenylene oxide, 5.0~15.0 wt.% hexagonal boron nitride, 5.0~20.0 wt.% eutectic calcium fluoride / barium fluoride, and 4.0~12.0 wt.% silver.

[0012] In the eutectic calcium fluoride / barium fluoride, the content of calcium fluoride is 30.0~40.0 wt.%, and the balance is barium fluoride.

[0013] The Co-based alloy raw materials in the bonding underlayer and the wearable surface layer are all spherical powders. The Co-based alloy powder used to prepare the bonding underlayer has a particle size of 15~45 μm, and the Co-based alloy powder used to prepare the wearable surface layer has a particle size of 35~80 μm. The polystyrene and hexagonal boron nitride are irregular powders with a particle size of 30~150 μm. The eutectic calcium fluoride / barium fluoride is a spherical powder with a particle size of 20~65 μm. The silver is a spherical powder with a particle size of 20~60 μm.

[0014] The thickness of the adhesive underlayer is 60~150 μm and the porosity is less than 2%; the thickness of the wear-resistant surface layer is 600~1500 μm and the porosity is 40.0~70.0%.

[0015] In the wearable surface layer, silver is distributed in a continuous or discontinuous network, and eutectic calcium fluoride / barium fluoride is dispersed between the Co-based alloy skeleton and silver.

[0016] The bonding strength between the coating and the titanium alloy substrate is not less than 30 MPa.

[0017] This invention further provides a method for preparing the above-mentioned salt spray corrosion resistant wear-resistant sealing coating, comprising the following steps: (1) Preparation of abrasive surface coating powder: Weigh the raw material powder according to the proportion and place it in a mixing bottle. Mix mechanically for 2-6 hours to obtain a uniformly mixed powder to be sprayed. (2) Cleaning and degreasing of titanium alloy substrate: Use alcohol or acetone to clean the area of ​​the titanium alloy substrate to be sprayed to remove surface oil. (3) Surface roughening treatment of titanium alloy substrate: The area of ​​the titanium alloy substrate to be coated after step (2) is roughened by sandblasting using a sandblasting machine. The surface roughness after sandblasting is not less than Ra 3.5 μm. (4) Preparation of bonding underlayer: Co-based alloy powder is sprayed onto the surface of the titanium alloy substrate after step (3) using a supersonic flame spraying process to form a bonding underlayer; (5) Preparation of wearable surface layer: The wearable surface layer powder prepared in step (1) is sprayed onto the surface of the bonding underlayer prepared in step (4) using atmospheric plasma spraying process to form wearable surface layer. (6) Thermal decomposition of pore-forming agent and formation of pore network: The coating prepared in step (5) is heat-treated to completely decompose and volatilize the polyphenylene ester, forming a pore network with a porosity of 40.0~70.0%.

[0018] In step (1), before mixing the wearable surface layer raw material powder, eutectic calcium fluoride / barium fluoride bulk material is prepared by melting or sintering. Then, eutectic calcium fluoride / barium fluoride powder with a particle size of less than 2000 mesh is obtained by crushing and high-energy ball milling. Finally, spherical powder is obtained by atomization granulation treatment.

[0019] In step (4), the parameters of the supersonic flame spraying process are: gas (propane) flow rate 50~80 L / min, oxygen flow rate 180~300 L / min, carrier gas (nitrogen) flow rate 8~15 L / min, air flow rate 300~500 L / min, powder feeding rate 20~40 g / min, spraying distance 200~300 mm, and spray gun moving speed 250~500 mm / s.

[0020] In step (5), the parameters of the atmospheric plasma spraying process are as follows: main gas (Ar) flow rate 25~40 L / min, secondary gas (H2) flow rate 6~9 L / min, carrier gas (N2) flow rate 4~10 L / min, current 400~600 A, spraying power 25~40 kW, powder feeding rate 20~35 g / min, spraying distance 75~150 mm, and spray gun moving speed 150~300 mm / s.

[0021] In step (6), the parameters of the heat treatment process are: heating rate 5~20 ℃ / min, heat treatment temperature 550~600 ℃, holding time 5~10 h, followed by furnace cooling.

[0022] Advantages of this invention: (1) In this invention, CoCrAlY or CoCrAlYSi is selected as the bonding underlayer material, which avoids the problem of element interdiffusion between the Ni base layer and the titanium alloy matrix at high temperature, forming a brittle phase. Co-based alloys and titanium alloys have good microstructure compatibility and excellent high-temperature stability, which can meet the long-term service requirements of 500~800 ℃. At the same time, the Co-based alloy skeleton in the surface layer maintains sufficient mechanical strength at high temperature, overcoming the defects of aluminum-based and copper-based sealing coatings that cannot be used for long-term service above 650 ℃ due to melting point limitation or high-temperature softening.

[0023] (2) This invention introduces a high thermal conductivity silver component into the wearable surface layer. Silver has extremely high thermal conductivity (approximately 429 W / m·K) and is distributed in a continuous or discontinuous network pattern between the Co-based alloy skeleton in the coating, constructing a highly efficient heat conduction channel. Under high-speed scraping conditions, frictional heat can be rapidly conducted and dissipated into the coating interior through the silver network, avoiding local heat accumulation at the blade tip. This fundamentally solves the problem of high-temperature softening, oxidation, or even melting of the blade tip due to the low thermal diffusivity of existing coatings, and achieves effective protection for titanium alloy blades.

[0024] (3) This invention employs a dual lubricant system design, using hexagonal boron nitride as the first lubricant to provide stable lubrication in the room temperature to medium temperature range, and eutectic calcium fluoride / barium fluoride as the second lubricant, which activates and exerts excellent lubrication performance in the high temperature range above 500 ℃. The two components work synergistically to achieve lubrication and anti-adhesion effects across the entire temperature range of 500~800 ℃. More importantly, the eutectic calcium fluoride / barium fluoride forms a low shear strength lubricating film at high temperatures, effectively preventing direct contact between the coating and the titanium alloy blade tip, avoiding adhesive wear, thereby ensuring the mass balance of each blade tip and maintaining rotor stability.

[0025] (4) The present invention uses atomization granulation technology to prepare eutectic calcium fluoride / barium fluoride spherical powder, which makes it melt more fully during the spraying process and uniformly dispersed between the Co-based alloy skeleton and silver. The electrical insulation properties of eutectic calcium fluoride / barium fluoride can effectively block the galvanic corrosion channel between the Co-based alloy and silver, thereby improving the corrosion resistance of the coating.

[0026] (5) In this invention, polystyrene is used as a pore-forming agent. It is completely decomposed and volatilized by heat treatment at 550~600 ℃ to form a three-dimensional interconnected pore network with a porosity of 40.0~70.0%. The high porosity reduces the overall hardness and cutting resistance of the coating, allowing the blade tip to easily scrape the coating during scraping, giving full play to the wear-resistant sealing function, while avoiding damage to the blade.

[0027] (6) The CoCrAlY / CoCrAlYSi bonding underlayer exhibits excellent high-temperature oxidation resistance. The synergistic effect of Al and Cr elements forms a dense Al2O3 / Cr2O3 composite oxide film, effectively blocking oxygen diffusion into the substrate. Y and Si elements refine the oxide film grains and improve the adhesion of the oxide film. This underlayer system has a stable microstructure at high temperatures and exhibits good thermal expansion matching with both the titanium alloy substrate and the Co-based alloy surface layer, ensuring the reliability of the coating under thermal cycling conditions.

[0028] In summary, this invention, through the synergistic effect of multiple technical means such as Co-based bonding underlayer design, silver thermal conductive network construction, dual lubricant compounding, and wearable surface layer structure control, proposes for the first time a complete solution for a wearable sealing coating adapted to the salt spray corrosion resistance of titanium alloy surfaces under medium-high temperature service conditions of 500~800℃, which has significant technological progress. Attached Figure Description

[0029] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments: Figure 1 This is a schematic cross-sectional view of a high-temperature wear-resistant sealing coating on a titanium alloy surface according to the present invention. Explanation of the labels in the schematic diagram: 1-Titanium alloy substrate, 2-Adhesive underlayer, 3-Abrasive surface layer, 4-Porosity generated after thermal decomposition of polyphenylene ester, 5-Hexagonal boron nitride, 6-Eutectic calcium fluoride / barium fluoride, 7-Silver; Figure 2 This is a schematic diagram of the microstructure of the wearable surface layer of the present invention, showing that silver is distributed in a continuous network between the Co-based alloy skeleton; Figure 3 This is a schematic diagram of the microstructure of the wearable surface layer of the present invention, showing that silver is distributed in a discontinuous network pattern between the Co-based alloy skeleton; Figure 4 This is a comparison diagram of the porosity changes of the wearable surface layer before and after heat treatment in Embodiment 1 of the present invention; Figure 5 The friction coefficient curves of the coating in Example 1 of the present invention at different temperatures show the synergistic effect of the dual lubricants of hexagonal boron nitride and eutectic calcium fluoride / barium fluoride. Figure 6 The ratio of tip wear to coating wear depth after a high-speed scratch test of the coating in Embodiment 1 of the present invention demonstrates the protective effect of the coating on the tip. Detailed Implementation

[0030] The present invention will be further described below with reference to specific embodiments. However, these descriptions are only for further illustrating the features and advantages of the present invention and are not intended to limit the present invention. All other embodiments based on the embodiments of the present invention, without creative effort by those skilled in the art, are within the protection scope of the present invention. In the following embodiments, unless specific process parameters and test methods are specified, they are all conventional processes and national standard test methods. Materials or instruments whose manufacturers are not specified are all commercially available conventional products.

[0031] Preparation of eutectic calcium fluoride / barium fluoride powder In all embodiments of the present invention, the eutectic calcium fluoride / barium fluoride powder used in the wearable surface layer needs to be prepared in advance. Specifically, eutectic calcium fluoride / barium fluoride bulk material is first prepared by melting or sintering, then irregular eutectic calcium fluoride / barium fluoride powder with a particle size of less than 2000 mesh is obtained by crushing and high-energy ball milling, and finally spherical powder is obtained by atomization granulation treatment.

[0032] (1) Taking the melt crushing method as an example: Weigh 30.0~40.0 wt.% calcium fluoride and the balance barium fluoride according to the mass ratio, place the mixed powder in a graphite crucible, heat it to 1300~1400 ℃ under inert gas protection to completely melt it, hold it at the temperature for 1~2 h to fully homogenize the melt, and then cool it to room temperature with the furnace to obtain a eutectic ingot. Then, use a crusher and a high-energy ball mill to coarsely crush, finely crush and grind the ingot, and then sieve it to obtain irregular eutectic calcium fluoride / barium fluoride powder with a particle size of less than 2000 mesh. Finally, through atomization granulation and sieving, obtain spherical powder with a particle size of 20~65 μm.

[0033] (2) Taking the sintering and crushing method as an example: 30.0~40.0 wt.% of calcium fluoride and the balance of barium fluoride are weighed according to the mass ratio, mixed in a mixer for 4~8 h, and then cold-pressed under a pressure of 20~30 MPa. Subsequently, it is sintered at 1100~1200 ℃ for 4~6 h in an inert atmosphere to obtain sintered blocks. Then, the blocks are subjected to a series of treatments such as crushing, grinding, sieving, atomization granulation and sieving to obtain spherical powder with a particle size of 20~65 μm.

[0034] Coating preparation steps The salt spray corrosion resistant wear-resistant sealing coating of the present invention is prepared according to the following steps: (1) Preparation of abrasive surface coating powder Weigh the following raw material powders according to the design composition of the wearable surface layer: Co-based alloy (spherical powder, particle size 35~80 μm) 60.0~80.0 wt.%; polystyrene (irregular powder, particle size 30~150 μm) 5.0~10.0 wt.%; hexagonal boron nitride (irregular powder, particle size 30~150 μm) 5.0~15.0 wt.%; eutectic calcium fluoride / barium fluoride (irregular powder, particle size 20~65 μm) 5.0~20.0 wt.%; silver (spherical powder, particle size 20~60 μm) 4.0~12.0 wt.%. Place the weighed powders in a mixing bottle and mechanically mix at 50~150 r / min for 2~6 h at room temperature to obtain a uniformly mixed powder for spraying.

[0035] (2) Cleaning and degreasing of titanium alloy substrate The titanium alloy substrate area to be coated is wiped or ultrasonically cleaned with alcohol or acetone to thoroughly remove surface oil and contaminants. After cleaning, the substrate surface is dried with clean compressed air to ensure surface cleanliness.

[0036] (3) Surface roughening treatment of titanium alloy substrate The titanium alloy substrate area to be coated after step (2) was roughened by sandblasting using a sandblasting machine. White or brown fused alumina was used as the sandblasting medium, with a particle size of 24-60 mesh, a sandblasting pressure of 0.4-0.7 MPa, a sandblasting angle of 75-90°, and a sandblasting distance of 100-200 mm. After sandblasting, residual sand particles on the substrate surface were blown away with clean compressed air. The surface roughness after treatment was not less than Ra 3.5 μm, preferably Ra 4.0-6.0 μm.

[0037] (4) Preparation of adhesive underlayer A supersonic flame spraying process was used to spray Co-based alloy powder (CoCrAlY or CoCrAlYSi, spherical, particle size 15~45 μm) onto the surface of the titanium alloy substrate treated in step (3) to form a bonding underlayer. The supersonic flame spraying process parameters were: fuel gas (propane) flow rate 50~80 L / min, oxygen flow rate 180~300 L / min, carrier gas (nitrogen) flow rate 8~15 L / min, air flow rate 300~500 L / min, powder feeding rate 20~40 g / min, spraying distance 200~300 mm, and spray gun moving speed 250~500 mm / s. Within the above parameter range, a bonding underlayer with high density, low oxide content, and excellent bonding strength could be obtained. The thickness of the bonding underlayer was controlled to be 60~150 μm, and the porosity was less than 2%.

[0038] (5) Preparation of wearable surface layer Atmospheric plasma spraying was used to spray the abrasive topcoat powder prepared in step (1) onto the surface of the bonding underlayer prepared in step (4) to form an abrasive topcoat. The atmospheric plasma spraying process parameters were as follows: main gas (Ar) flow rate 25~40 L / min, secondary gas (H2) flow rate 6~9 L / min, carrier gas (N2) flow rate 4~10 L / min, current 400~600 A, spraying power 25~40 kW, powder feeding rate 20~35 g / min, spraying distance 75~150 mm, and spray gun moving speed 150~300 mm / s. Within the above parameter range, the full melting or semi-molten deposition of each component powder can be guaranteed, while avoiding premature decomposition and volatilization of polystyrene. The sprayed thickness of the abrasive topcoat was controlled to be 600~1500 μm.

[0039] (6) Thermal decomposition of pore-forming agent and formation of pore network The coating prepared in step (5) is placed in a box-type resistance furnace or a vacuum heat treatment furnace for heat treatment to allow the polystyrene to completely decompose and volatilize, forming a porous network with a porosity of 40.0~70.0%. The heat treatment process parameters are: heating to 550~600 ℃ at a heating rate of 5~20 ℃ / min, holding for 5~10 h, and then cooling to room temperature with the furnace.

[0040] After the aforementioned heat treatment, polystyrene completely decomposes into CO2 and H2O gases, leaving pores in the coating corresponding to its original particle size and morphology. Since the original polystyrene powder has a particle size of 30–150 μm and an irregular shape, the pores formed after thermal decomposition constitute an irregularly shaped, interconnected three-dimensional pore network with a porosity of 40.0–70.0%. This high porosity structure significantly reduces the overall hardness and cutting resistance of the coating, allowing the blade tip to scrape the coating with lower resistance during scraping.

[0041] Microstructure characteristics of coating The cross-sectional structure of the salt spray resistant wear-resistant sealing coating prepared by the above method is as follows: Figure 1 As shown, it includes a titanium alloy substrate 1, an adhesive underlayer 2 coated on the substrate surface, and a wearable surface layer 3 coated on the adhesive underlayer surface. In the wearable surface layer, the pores 4 generated after the thermal decomposition of polystyrene are irregularly shaped and interconnected; hexagonal boron nitride 5 is uniformly distributed between the Co-based alloy skeleton as a first lubricant; eutectic calcium fluoride / barium fluoride 6 is fully melted and dispersed between the Co-based alloy skeleton and silver; silver 7 is distributed in a continuous network... Figure 2 The network shown is either discontinuous or in discontinuous. Figure 3 As shown, these are distributed between the Co-based alloy skeletons, forming highly efficient heat conduction channels.

[0042] It should be noted that the distribution pattern of silver is closely related to the amount of silver added and the spraying process parameters. When the silver content is 4.0~8.0 wt.%, silver tends to be distributed in a discontinuous network pattern; when the silver content is 8.0~12.0 wt.%, silver tends to be distributed in a continuous network pattern. Both distribution patterns can achieve the construction of heat conduction channels, but the continuous network distribution has higher thermal conductivity and is suitable for higher temperature or higher scraping linear speed conditions; the discontinuous network distribution, while ensuring a certain thermal conductivity, is conducive to maintaining sufficient structural integrity of the coating.

[0043] Example Example 1 This embodiment provides a wear-resistant sealing coating resistant to salt spray corrosion, the preparation method of which includes the following steps: (1) Preparation of eutectic calcium fluoride / barium fluoride powder: 35.0 wt.% calcium fluoride and 65.0 wt.% barium fluoride were weighed according to the mass ratio, and eutectic powder was prepared by melting, crushing and atomizing granulation. Spherical powder with a particle size of 20~65 μm was obtained by sieving.

[0044] (2) Preparation of abrasive surface coating powder: Weigh the following raw material powders according to the following mass percentages: CoCrAlYSi alloy (spherical, particle size 35~80 μm, chemical composition: Cr 20.0 wt.%, Al 12.0 wt.%, Y 0.5 wt.%, Si 0.5 wt.%, balance Co) 70.0 wt.%; polystyrene (irregular, particle size 30~120 μm) 8.0 wt.%; hexagonal boron nitride (irregular, particle size 30~150 μm) 6.0 wt.%; eutectic calcium fluoride / barium fluoride (spherical, particle size 20~65 μm) 8.0 wt.%; silver (spherical, particle size 20~50 μm) 8.0 wt.%. Place the above powders in a mixing bottle and mechanically mix at a speed of 100 r / min for 4 h to obtain a uniformly mixed powder to be sprayed.

[0045] (3) Cleaning and degreasing of titanium alloy substrate: Use alcohol to ultrasonically clean the area of ​​the titanium alloy substrate to be sprayed to remove surface oil stains, and then blow dry with clean compressed air.

[0046] (4) Surface roughening treatment of titanium alloy substrate: 24-mesh white corundum sand is used to roughen the area of ​​the substrate to be coated by sandblasting. The sandblasting pressure is 0.5 MPa, the sandblasting angle is 90°, the sandblasting distance is 150 mm, and the surface roughness after treatment is Ra 5.0 μm.

[0047] (5) Preparation of the bonding substrate: CoCrAlYSi powder (spherical, particle size 15~45μm) was sprayed onto the substrate surface using a supersonic flame spraying process. The process parameters were: fuel gas (propane) flow rate 65 L / min, oxygen flow rate 240 L / min, carrier gas (nitrogen) flow rate 12 L / min, air flow rate 400 L / min, powder feed rate 30 g / min, spraying distance 250 mm, and spray gun moving speed 350 mm / s. The thickness of the bonding substrate was controlled at 100±20 μm, and the measured porosity was 1.5%.

[0048] (6) Preparation of the abrasive surface layer: The powder prepared in step (2) was sprayed onto the surface of the bonding substrate using an atmospheric plasma spraying process. The process parameters were as follows: main gas (Ar) flow rate 32 L / min, secondary gas (H2) flow rate 8 L / min, carrier gas (N2) flow rate 7 L / min, current 500 A, spraying power 32 kW, powder feeding rate 28 g / min, spraying distance 110 mm, and spray gun moving speed 220 mm / s. The thickness of the abrasive surface layer in the sprayed state was controlled to be 1100±50 μm.

[0049] (7) Thermal decomposition of pore-forming agent and formation of pore network: The above coating is placed in a box-type resistance furnace and heated to 580 ℃ at a heating rate of 10 ℃ / min, held for 8 h, and then cooled to room temperature with the furnace.

[0050] Testing showed that the porosity of the wearable surface layer obtained in this embodiment was 61.4%. The porosity change before and after heat treatment is shown below. Figure 4 As shown, by Figure 4 As can be seen, the porosity increased significantly from 8.6% in the sprayed state to 61.4% after heat treatment, indicating that the polystyrene had completely decomposed and formed a three-dimensional interconnected pore network. The bonding strength between the coating and the titanium alloy substrate was 37.9 MPa, meeting the requirement of not less than 30 MPa.

[0051] The friction coefficient test results of the coating in this embodiment at different temperatures are as follows: Figure 5 As shown. By Figure 5It can be seen that at room temperature, hexagonal boron nitride plays a dominant lubricating role, with the friction coefficient remaining stable at 0.58~0.65; at 600 ℃, eutectic calcium fluoride / barium fluoride is activated and synergistically lubricates with hexagonal boron nitride, further reducing the friction coefficient to 0.25~0.35, demonstrating the synergistic lubrication effect of the dual lubricant system over a wide temperature range.

[0052] High-speed scratch test results are as follows Figure 6 As shown, the experimental conditions were: scraping linear velocity 350 m / s, feed rate 5 μm / s, and scraping depth 500 μm. The results showed that the tip wear was only 20% of the coating wear depth, indicating that the coating preferentially undergoes controlled cutting under high-speed scraping conditions, resulting in minimal tip material wear and excellent protection for the tip.

[0053] Example 2 The difference between this embodiment and Embodiment 1 is that the amount of CoCrAlY alloy in the wearable surface layer composition is 80.0 wt.%, polystyrene 5.0 wt.%, hexagonal boron nitride 5.0 wt.%, eutectic calcium fluoride / barium fluoride 6.0 wt.%, and silver 4.0 wt.%, while the remaining steps and parameters are the same as in Embodiment 1. The coating obtained in this embodiment has a porosity of 44.5% and a bonding strength of 36.8 MPa. The silver is distributed in a discontinuous network, making it suitable for working conditions below 600 °C and with medium scratching linear speeds.

[0054] Example 3 The difference between this embodiment and Embodiment 1 is that the amount of CoCrAlYSi alloy in the wearable surface layer composition is 60.0 wt.%, polystyrene 10.0 wt.%, hexagonal boron nitride 12.0 wt.%, eutectic calcium fluoride / barium fluoride 12.0 wt.%, and silver 6.0 wt.%, the heat treatment temperature is 550 ℃, and the holding time is 10 h. The remaining steps and parameters are the same as in Embodiment 1. The coating obtained in this embodiment has a porosity of 66.7% and a bonding strength of 33.6 MPa. The silver is distributed in a discontinuous network, which is suitable for working conditions with high porosity and low cutting force requirements.

[0055] Example 4 The difference between this embodiment and Embodiment 1 is that the silver content in the wearable surface layer is increased to 10.0 wt.%, the CoCrAlY alloy is adjusted to 67.0 wt.%, the eutectic calcium fluoride / barium fluoride is 9.0 wt.%, and the remaining components remain unchanged (polyphenylene ester 8.0 wt.%, hexagonal boron nitride 6.0 wt.%). Simultaneously, the heat treatment heating rate is adjusted to 15 ℃ / min, the heat treatment temperature to 590 ℃, and the holding time to 6 h. The remaining steps and parameters are the same as in Embodiment 1. The coating obtained in this embodiment has a porosity of 53.1% and a bonding strength of 36.2 MPa. The silver is distributed in a continuous network, making it suitable for high heat flux density scraping conditions.

[0056] Example 5 The difference between this embodiment and Embodiment 1 is that the bonding underlayer uses a CoCrAlY coating with the chemical composition of Cr 22.0 wt.%, Al 13.0 wt.%, Y 0.6 wt.%, and the balance being Co; the wear-resistant surface layer uses a CoCrAlY-based alloy with a dosage of 65.0 wt.%, polystyrene 8.0 wt.%, hexagonal boron nitride 5.0 wt.%, eutectic calcium fluoride / barium fluoride 15.0 wt.%, and silver 7.0 wt.%, and the process parameters are the same as in Embodiment 1. The bonding underlayer porosity of the coating obtained in this embodiment is 1.2%, and the overall coating bonding strength is 34.3 MPa, all of which meet the design requirements.

[0057] Comparative Example 1 The difference between this comparative example and Example 1 is that no silver component is added to the wearable surface layer, and the amount of CoCrAlYSi alloy is increased to 78.0 wt.%, while the remaining components and process parameters are the same as in Example 1. In the high-speed scratch test (under the same conditions as in Example 1), the resulting coating showed a tip wear of 154% of the coating wear depth, and the tip exhibited obvious signs of high-temperature oxidation discoloration and melting, indicating that without a silver heat-conducting network, frictional heat could not be effectively dissipated, causing thermal damage to the tip.

[0058] Comparative Example 2 The difference between this comparative example and Example 1 is that only hexagonal boron nitride (14.0 wt.%) was added as a single lubricant to the wearable surface layer, and eutectic calcium fluoride / barium fluoride was not added. The remaining components and process parameters were the same as in Example 1. The resulting coating had a friction coefficient of over 0.65 at 600 °C. After high-speed scraping, severe adhesion and material transfer appeared on the coating surface, indicating that a single lubricant cannot meet the lubrication requirements of medium-high temperature and wide temperature range.

[0059] Comparative Example 3 The difference between this comparative example and Example 1 is that the eutectic calcium fluoride / barium fluoride powder added to the wearable surface layer is an irregular powder of 20~65 μm, while the remaining components and process parameters are the same as in Example 1. The corrosion potential of the resulting coating in 5% NaCl solution (-0.579 V vs. Pt) is lower than that of Example 1 (-0.418 V vs. Pt), and the corrosion current density (4.23 × 10⁻⁶) is lower. -6 A·cm -2 The value is greater than that of Example 1 (2.31 × 10⁻⁶). -6 A·cm -2 This indicates that the spherical eutectic calcium fluoride / barium fluoride powder is more evenly distributed in the coating, acts as a barrier between the CoCrAlYSi alloy and silver, and improves the corrosion resistance of the coating.

[0060] In summary, this invention, through the synergistic design of a Co-based alloy bonding underlayer, a silver-containing thermally conductive network, and a wearable surface layer with a dual lubrication system, combined with optimized spraying and heat treatment processes, has successfully developed a wearable sealing coating suitable for medium-high temperature service conditions of 500~800℃ on titanium alloy surfaces. It has excellent bonding strength, controllable porosity, excellent full-temperature-range lubrication performance, and efficient heat conduction capability, effectively solving the technical problems of rotor-stator clearance control and blade tip protection in high-temperature titanium alloy compressors, and has significant engineering application value.

[0061] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

[0062] Matters not covered in this invention are common knowledge.

[0063] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A salt spray resistant abrasive sealing coating, comprising an adhesive underlayer and an abrasive toplayer, characterized in that: The bonding underlayer is a Co-based alloy coating, and the wearable surface layer is a composite coating composed of Co-based alloy, polyphenylene ester, hexagonal boron nitride, eutectic calcium fluoride / barium fluoride and silver, wherein polyphenylene ester is a pore-forming agent, hexagonal boron nitride is a first lubricant, eutectic calcium fluoride / barium fluoride is a second lubricant, and silver is a thermally conductive component. The Co-based alloy coating is either a CoCrAlY coating or a CoCrAlYSi coating. The chemical composition of the CoCrAlY coating is: 15.0~25.0 wt.% Cr, 10.0~15.0 wt.% Al, 0.2~1.0 wt.% Y, with the balance being Co. The chemical composition of the CoCrAlYSi coating is: 15.0~25.0 wt.% Cr, 10.0~15.0 wt.% Al, 0.2~1.0 wt.% Y, 0.2~1.0 wt.% Si, with the balance being Co. The mass percentages of each component in the wearable surface layer are as follows: 60.0~80.0 wt.% Co-based alloy, 5.0~10.0 wt.% polyphenylene oxide, 5.0~15.0 wt.% hexagonal boron nitride, 5.0~20.0 wt.% eutectic calcium fluoride / barium fluoride, and 4.0~12.0 wt.% silver.

2. The abrasive sealing coating resistant to salt spray corrosion according to claim 1, characterized in that, In the eutectic calcium fluoride / barium fluoride, the content of calcium fluoride is 30.0~40.0 wt.%, and the balance is barium fluoride.

3. The abrasive sealing coating resistant to salt spray corrosion according to claim 1, characterized in that, The Co-based alloy raw materials in the bonding underlayer and the wearable surface layer are all spherical powders. The Co-based alloy powder used to prepare the bonding underlayer has a particle size of 15~45 μm, and the Co-based alloy powder used to prepare the wearable surface layer has a particle size of 35~80 μm. The polystyrene and hexagonal boron nitride are irregular powders with a particle size of 30~150 μm. The eutectic calcium fluoride / barium fluoride is a spherical powder with a particle size of 20~65 μm. The silver is a spherical powder with a particle size of 20~60 μm.

4. The abrasive sealing coating resistant to salt spray corrosion according to claim 1, characterized in that, The thickness of the adhesive underlayer is 60~150 μm and the porosity is less than 2%; the thickness of the wear-resistant surface layer is 600~1500 μm and the porosity is 40.0~70.0%.

5. The abrasive sealing coating resistant to salt spray corrosion according to claim 1, characterized in that, In the wearable surface layer, silver is distributed in a continuous or discontinuous network, and eutectic calcium fluoride / barium fluoride is dispersed between the Co-based alloy skeleton and silver; the bonding strength between the coating and the titanium alloy substrate is not less than 30 MPa.

6. A method for preparing a salt spray corrosion resistant wear-resistant sealing coating according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Preparation of abrasive surface coating powder: Weigh the raw material powder according to the proportion and place it in a mixing bottle. Mix mechanically for 2-6 hours to obtain a uniformly mixed powder to be sprayed. (2) Cleaning and degreasing of titanium alloy substrate: Use alcohol or acetone to clean the area of ​​the titanium alloy substrate to be sprayed to remove surface oil. (3) Surface roughening treatment of titanium alloy substrate: The area of ​​the titanium alloy substrate to be coated after step (2) is roughened by sandblasting using a sandblasting machine. The surface roughness after sandblasting is not less than Ra 3.5 μm. (4) Preparation of bonding underlayer: The Co-based alloy powder described in claim 3 is sprayed onto the surface of the titanium alloy substrate after step (3) using a supersonic flame spraying process to form a bonding underlayer; (5) Preparation of wearable surface layer: The wearable surface layer powder prepared in step (1) is sprayed onto the surface of the bonding underlayer prepared in step (4) using atmospheric plasma spraying process to form wearable surface layer. (6) Thermal decomposition of pore-forming agent and formation of pore network: The coating prepared in step (5) is heat-treated to completely decompose and volatilize the polyphenylene ester, forming a pore network with a porosity of 40.0~70.0%.

7. The method for preparing a salt spray resistant wear-resistant sealing coating according to claim 6, characterized in that, In step (1), before mixing the wearable surface layer raw material powder, eutectic calcium fluoride / barium fluoride bulk material is prepared by melting or sintering. Then, eutectic calcium fluoride / barium fluoride powder with a particle size of less than 2000 mesh is obtained by crushing and high-energy ball milling. Finally, spherical powder is obtained by atomization granulation treatment.

8. The method for preparing a salt spray resistant wear-resistant sealing coating according to claim 6, characterized in that, In step (4), the parameters of the supersonic flame spraying process are: gas (propane) flow rate 50~80 L / min, oxygen flow rate 180~300 L / min, carrier gas (nitrogen) flow rate 8~15 L / min, air flow rate 300~500 L / min, powder feeding rate 20~40 g / min, spraying distance 200~300 mm, and spray gun moving speed 250~500 mm / s.

9. The method for preparing a salt spray resistant wear-resistant sealing coating according to claim 6, characterized in that, In step (5), the parameters of the atmospheric plasma spraying process are as follows: main gas (Ar) flow rate 25~40 L / min, secondary gas (H2) flow rate 6~9 L / min, carrier gas (N2) flow rate 4~10 L / min, current 400~600 A, spraying power 25~40 kW, powder feeding rate 20~35 g / min, spraying distance 75~150 mm, and spray gun moving speed 150~300 mm / s.

10. The method for preparing a salt spray resistant wear-resistant sealing coating according to claim 6, characterized in that, In step (6), the parameters of the heat treatment process are: heating rate 5~20 ℃ / min, heat treatment temperature 550~600 ℃, holding time 5~10 h, followed by furnace cooling.

Citation Information

Patent Citations

  • Gradient-structure anti-titanium-fire abradable sealing coating and preparation method thereof

    CN109554657A

  • Titanium alloy surface inflaming retarding sealing integrated coating and preparing method an application thereof

    CN110747428A

  • Titanium fire resistant abradable sealing coating and preparation method thereof

    CN114045454A