A multi-gun plasma spraying apparatus and a method for preparing coatings
By using a multi-gun plasma spraying device and zoned spraying temperature control technology, the problems of low spraying efficiency and thermal deformation in existing technologies have been solved, achieving efficient preparation and uniformity of thick coatings, which is suitable for precision spraying of large-size thin-walled workpieces.
Patent Information
- Application Number
- CN202611325097.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing plasma spraying technology suffers from low spraying efficiency and workpiece thermal deformation when preparing radar absorbing coatings. In particular, cracking and peeling defects are prone to occur during the preparation of thick coatings. Furthermore, uneven thermal stress during the spraying process of large-sized thin-walled parts leads to unacceptable dimensional deformation.
A multi-gun plasma spraying device is adopted, which uses a six-axis robot to control multiple spray guns to spray in parallel. Combined with real-time temperature detection by an infrared temperature measurement module and protective gas injection, it can achieve zoned spraying and temperature control in synergy, ensuring uniform heating of all areas of the workpiece and reducing thermal stress.
It significantly improves spraying efficiency, shortens production cycle, ensures uniform coating thickness and no cracking defects, minimizes workpiece thermal deformation, is suitable for large-size thin-walled workpieces, and meets precision assembly requirements.
Smart Images

Figure CN123108465A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface engineering and functional coating preparation technology, and relates to a multi-gun plasma spraying device and a method for preparing coatings. Background Technology
[0002] Plasma spraying is a coating preparation technology that uses a plasma flame as a heat source. Its working principle is as follows: powdered coating material is introduced into the plasma flame and heated to a molten or semi-molten state. It is then accelerated and sprayed out through a spray gun, atomized into fine droplets by the high-speed airflow, and impacts the workpiece surface at high speed. During the impact, the droplets rapidly spread, cool, and solidify, accumulating layer by layer to form the plasma-sprayed coating layer.
[0003] Typical plasma spraying equipment mainly includes a plasma spraying power supply, spray gun, control cabinet, powder feeder, and cooling device. Spraying efficiency is one of the key factors affecting the economics of coating preparation. Currently, the power of plasma spray guns widely used both domestically and internationally is mostly concentrated in the range of 40 kW to 80 kW. To improve production efficiency, existing technologies tend to increase the spraying rate by increasing the spray gun power. For example, some literature has reported high-power plasma spray gun schemes with power progressively increased to 200 kW and even 450 kW. Although high-power spray guns can achieve coating thickness deposition in a shorter time, their input energy is significantly increased, leading to a sharp increase in plasma jet velocity. This exacerbates the uneven heat input of the substrate workpiece during the spraying process, easily causing the workpiece temperature to become too high and triggering thermal deformation.
[0004] Based on the above situation, existing plasma spraying technology still faces the following two core problems in preparing radar absorbing coatings: Firstly, single-gun spraying is inefficient, making it difficult to efficiently prepare thick coatings. Traditional single-gun spraying requires multiple layers to achieve the target thickness (e.g., ≥1.5 mm). This process not only takes tens of hours, but also easily accumulates residual stress inside the coating, leading to defects such as cracking, peeling, and even flaking, which severely restricts the engineering application of thick-walled microwave absorbing coatings.
[0005] Secondly, the substrate of the part is prone to thermal deformation during the spraying process. For large-sized thin-walled parts (such as afterburner components of aero engines), when using single-gun spraying, the difference in the relative position and heat exchange conditions between the edge area and the center of the workpiece and the plasma jet leads to a severe uneven heating. The resulting thermal stress can easily exceed the yield limit of the substrate, causing unacceptable dimensional deformation and affecting subsequent assembly and performance.
[0006] Therefore, there is an urgent need for a multi-gun plasma spraying device and a method for preparing coatings to overcome the above problems. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of the prior art and to propose a multi-gun plasma spraying device and a method for preparing coatings.
[0008] This invention discloses a multi-gun plasma spraying device, including a turntable and an infrared temperature measurement module. A placement plate is mounted on the turntable, and multiple workpiece clamping parts are mounted on the placement plate. Above the placement plate is a hollow protective gas support rod, on which multiple spray guns are mounted. The protective gas support rod is held by a six-axis robot. One end of the protective gas support rod is connected to a jetting mechanism, and the other end is sealed. Multiple gas nozzles are mounted on the protective gas support rod. The spray guns are connected to a powder feeding mechanism. The infrared temperature measurement module detects the workpiece temperature in real time and transmits the temperature signal to a control module.
[0009] Furthermore, the workpiece clamping part is arranged circumferentially along the placement disk.
[0010] Furthermore, the spray gun is snapped onto the protective gas support rod via a clip.
[0011] Furthermore, the moving speed of the six-axis robot is 1.0~1000mm / s.
[0012] Furthermore, the rotational speed of the turntable is 10~20 r / min.
[0013] Furthermore, the powder feeding mechanism includes 3 to 6 independent powder feeding channels, which are connected to the spray gun through the powder feeding channels.
[0014] Furthermore, the workpiece clamping part includes an L-shaped jaw, which is connected to the turntable.
[0015] Secondly, the present invention also discloses a method for preparing a coating using a multi-gun plasma spraying apparatus, the method comprising the following steps: Step 1: After cleaning, the workpiece is heat-treated and sandblasted, and then fixed on a turntable; Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod so that the axis of the spray gun is at 90° with the workpiece surface and the axis of the gas nozzle is at 50°~70° with the workpiece surface; set the spraying parameters and powder feeding parameters of the spray gun through the control module.
[0016] Furthermore, in step two, the spraying parameters include: current 400-600A, voltage 60-75V, and gas flow rate 40-50L / min.
[0017] Furthermore, in step two, the powder feeding parameters include: the matrix powder feeding rate is 25-50 g / min, and the microwave absorbing functional powder feeding rate is 20-35 g / min.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) Significantly improved spraying efficiency. This invention adopts a multi-gun parallel spraying method, dividing the entire spraying surface of the workpiece into multiple areas, with each spray gun responsible for its corresponding area. The coverage area of a single spraying stroke is increased several times, and the required spraying time is significantly shortened. Compared with single-gun spraying, the spraying efficiency can be increased by 3 to 5 times, and the time required to prepare a coating with a thickness of not less than 1.5 mm is shortened from at least 15 hours to less than 3 hours, greatly reducing the production cycle and manufacturing cost.
[0019] (2) It can achieve the preparation of thick coatings without cracking defects. By spraying in sections and using temperature control to relieve stress, the accumulated stress inside the coating is effectively released, so that the coating thickness can be stably reached 1.5 to 1.7 mm, and there are no defects such as cracking or peeling on the surface and inside of the coating. This overcomes the technical problem that traditional single-gun spraying of thick coatings is prone to cracking due to stress concentration.
[0020] (3) The workpiece exhibits minimal thermal deformation and high dimensional accuracy. This invention employs a six-axis industrial robot to precisely control the spray gun's trajectory (with a repeatability of 0.02 mm), achieving coordinated control of zoned spraying and cooling temperature. This ensures uniform heating across all areas of the workpiece, effectively suppressing deformation caused by thermal stress. Actual measurements show that the deformation of the substrate before and after spraying can be controlled within 0.5 mm, meeting the assembly and usage requirements of precision workpieces.
[0021] (4) Wide range of applications and good coating uniformity. This invention is applicable to large-sized thin-walled workpieces with a diameter of no more than 1m, and the coating thickness uniformity deviation does not exceed 5%. It has good adaptability to parts of different shapes and sizes and has broad engineering application prospects. Attached Figure Description
[0022] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.
[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a schematic diagram of the overall structure of the present invention; Figure 2 This is a schematic diagram of the spray gun structure of the present invention.
[0025] Wherein: 1 is the workpiece to be inspected; 2 is the workpiece clamping part; 3 is the turntable; 5 is the gas nozzle; 7 is the spray gun; 8 is the protective gas support rod; 9 is the infrared temperature measurement module. Detailed Implementation
[0026] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples consistent with some aspects of the invention as detailed in the appended claims.
[0027] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0028] On one hand, this invention discloses a multi-gun plasma spraying device, such as... Figure 1 As shown, the device includes a turntable 3 and an infrared temperature measurement module 9. The turntable 3 is equipped with a placement tray, which has multiple workpiece clamping parts 2. Above the placement tray is a hollow protective gas support rod 8, which has multiple spray guns 7. The protective gas support rod 8 is held by a six-axis robot. One end of the protective gas support rod 8 is connected to a jetting mechanism, and the other end is sealed. The protective gas support rod 8 has multiple gas nozzles 5. The spray guns 7 are connected to a powder feeding mechanism. The infrared temperature measurement module 9 detects the temperature of the workpiece 1 in real time and transmits the temperature signal to the control module.
[0029] Specifically, the spray gun 7 is a plasma spray gun, which is arranged in a rectangular shape on the protective gas support rod 8. The protective gas support rod 8 is hollow inside and is fastened to the six-axis robot. Each spray gun 7 is independently controllable and has an input end and an output end. The input end is for electricity, water, plasma gas, and spray powder. The output end is for plasma flame. The axis of the spray gun 7 forms an angle of 60-90° with the surface of the workpiece.
[0030] One end of the gas support rod 8 is connected to the jetting mechanism, and the other end of the protective gas support rod 8 is sealed. Multiple gas jet nozzles 5 are provided on the protective gas support rod 8. The infrared temperature measurement module 9 detects the temperature of the workpiece 1 in real time and transmits the temperature signal to the control module. After processing by the PLC, the control module controls the gas jet nozzles 5 to spray gas flow rate to reduce the surface temperature of the coating. The main purpose of compressed air is to cool the coating and reduce thermal stress.
[0031] Furthermore, the workpiece clamping part 2 is arranged along the circumference of the placement disk; Specifically, the longitudinal section of the workpiece clamping part 2 is "L" shaped, and the part is made of a bendable material. The bottom edge of the part is placed in the L-groove of the L-shaped clamping part to control the part to remain in a bent state. By adjusting the distance from the L-shaped clamping block to the center of the turntable, the side surface of the L-shaped clamping part is tightly fitted with the outer surface of the workpiece for fixation and restriction.
[0032] Furthermore, the spray gun 7 is snapped onto the protective gas support rod 8 via a clip.
[0033] Specifically, the spacing between the 7 spray guns is adjustable (80-300mm).
[0034] Furthermore, the moving speed of the six-axis robot is 1~1000mm / s.
[0035] Specifically, the six-axis industrial robot (moving speed 1-1000mm / s) ensures uniform movement of the spray gun 7 and uniform spraying, and is suitable for large workpieces with a diameter ≤1m.
[0036] Furthermore, the rotational speed of the turntable 3 is 10~20 r / min.
[0037] Specifically, a rotary motor is installed inside the turntable 3, and the output shaft of the rotary motor drives the placement plate to rotate. Alternatively, other mechanical mechanisms that can drive the placement plate to rotate are installed inside the turntable 3, which are not limited here. The rotation speed of the turntable 3 is 10~20 r / min, and it can rotate 360°. The turntable 3 works in conjunction with a six-axis industrial robot (moving speed 1-1000mm / s) to ensure that the plasma spray gun 7 moves at a uniform speed and the spraying is uniform. The rotating mechanism is suitable for large workpieces with a diameter ≤1m.
[0038] Furthermore, the powder feeding mechanism includes 3 to 6 independent powder feeding channels, which are connected to the spray gun 7 via the powder feeding channels.
[0039] Specifically, such as Figure 2 As shown, a coating can be sprayed onto the workpiece 1 using a spray gun 7. The spray gun 7 is connected to the powder feeder through a powder feeding channel (powder feeding pipe). There can be 3-6 powder feeding channels, and each powder feeding pipe is connected to a spray gun 7. The powder feeding channels can feed powder synchronously or alternately, conveying "matrix powder" (such as MCrAlY powder, where M is Ni, Co, or NiCo) and "functional powder", etc. Furthermore, the workpiece clamping part 2 includes an L-shaped jaw disposed at the bottom, which is connected to the turntable 3 via a T-shaped block.
[0040] Specifically, the turntable has several T-slots on its three surfaces, each containing a sliding T-block. The depth of the T-slot is greater than the height of the T-block, allowing it to slide freely within the slot. The T-blocks are machined with threaded holes, and the L-shaped jaws have countersunk through holes. When the screw passes through the countersunk through hole and engages with the threaded hole of the T-block, the T-block is pulled upwards by the screw, and its stepped end face presses tightly against the inner bearing surface of the T-slot, achieving overall locking and fixation through the friction of the contact surfaces.
[0041] On the other hand, the present invention discloses a method for preparing a coating using a multi-gun plasma spraying apparatus. This method, which uses a multi-gun plasma spraying apparatus, includes the following steps: Step 1: Heat treat and sandblast the cleaned workpiece 1, and then fix the workpiece 1 on the turntable 3; Specifically, workpiece pretreatment: The workpiece (diameter 1m, height 600mm) is degreased (300℃, 30min) and sandblasted (white corundum 80 mesh, 0.3MPa) in sequence. After pretreatment, the roughness Ra is 3.5μm. The workpiece is placed on a turntable with a rotation speed of 20r / min and fixed with L-shaped jaws.
[0042] Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod 8 so that the axis of the spray gun 7 is at 90° with the surface of the workpiece 1, and the axis of the gas nozzle 5 is at 50°~70° with the surface of the workpiece 1; set the spraying parameters and powder feeding parameters of the spray gun 7 through the control module.
[0043] Specifically, the robot position is adjusted so that the axis of the spray gun 7 is at a 90° angle to the workpiece surface; The axis of the protective gas nozzle 5 is at an angle of 50° to 70° to the workpiece surface; Plasma spray gun parameters: current 400-600A, voltage 60-75V, working gas (argon + hydrogen) flow rate 40-50L / min; Powder feeding parameters: Matrix powder (MCrAlY) powder feeding rate 25-50g / min, microwave absorbing functional powder powder feeding rate 20-35g / min; Step 3: The workpiece is rotated by the control module, and the spray gun 7 is sprayed up and down by the six-axis robot to obtain the pre-coated layer; during the spraying process, the surface temperature of the workpiece 1 is measured in real time by the infrared temperature measurement module 9 to adjust the temperature of the gas sprayed from the nozzle. Step 4: Allow the sprayed workpiece 1 to cool naturally to room temperature, then polish the pre-coated layer and perform high-temperature annealing heat treatment to obtain an integrated coating.
[0044] Example 1 This embodiment discloses a method for preparing a coating using a multi-gun plasma spraying apparatus. The method includes the following steps: Step 1: Heat treat and sandblast the cleaned workpiece 1, and then fix the workpiece 1 on the turntable 3; Specifically, the workpiece 1 (metal substrate (such as high-temperature alloy), 1m in diameter and 600mm in height) is cleaned with alcohol → heat treated (300℃, 30min; ensuring complete removal of oil stains and alcohol from the substrate) → sandblasted (grit size 80-200 mesh, roughness Ra2.5-5.3μm, to improve the adhesion between the coating and the substrate, 0.3MPa) → placed on a turntable 3, with a rotation speed of 20r / min, and fixed with L-shaped jaws 2 → the six-axis industrial robot connected to the multi-gun array mechanism is adjusted, with a moving speed of 500mm / s, so that the output end of the spray gun 7 is kept in a suitable position with the workpiece 1.
[0045] Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod 8 so that the axis of the spray gun 7 is at 90° with the surface of the workpiece 1, and the axis of the gas nozzle 5 is at 60° with the surface of the workpiece 1; set the spraying parameters and powder feeding parameters of the spray gun 7 through the control module.
[0046] Specifically, a rectangular array of three plasma spray guns (spaced 200mm apart) is used. The position of the six-axis robot is adjusted so that the 7th axis of the spray gun is at a 90° angle to the workpiece surface. The robot parameters are adjusted so that the distance between the output end of the plasma spray gun and the workpiece surface is 100mm, the axial translation speed of the plasma spray gun is 1.3mm / s, and the reciprocating translation distance is 200mm.
[0047] The axis of the protective gas nozzle 5 is at a 60° angle to the workpiece surface; Plasma spray gun parameters: current 500A, voltage 70V; plasma gas (argon flow rate 45L / min, hydrogen flow rate 8L / min) flow rate 53 L / min; Powder feeding parameters: matrix powder (NiCrAlY powder: particle size 20-50μm, flow rate 50s, powder feeding speed 25 g / min), microwave absorbing functional powder (particle size 20-70μm, flow rate 180s, powder feeding speed 28g / min); Step 3: The workpiece is rotated by the control module, and the spray gun 7 is sprayed up and down by the six-axis robot to obtain the pre-coated layer; during the spraying process, the surface temperature of the workpiece 1 is measured in real time by the infrared temperature measurement module 9 to adjust the temperature of the gas sprayed from the nozzle. Specifically, a "uniformly distributed, zoned heating" strategy is adopted: the workpiece is rotated (19 r / min) by the control module, and multiple guns move up and down simultaneously in axially uniform zones (total workpiece height H, n gun arrays) (gun speed 1.0 mm / s), with a moving distance of H / n, for spraying. The spraying distance is 100 mm, and the single spray thickness is 0.03 mm / layer. During the spraying process, the workpiece surface temperature is measured by the infrared temperature measurement module 9, and protective gas at appropriate pressure is released onto the workpiece surface through the nozzle. The cooling system is divided into... The support pressure is 0.3MPa~0.6MPa, with an angle of 70° to the workpiece surface. The position and height of the infrared thermometer are adjusted to measure the temperature of the entire area to be coated. The surface temperature of the coating is controlled at 130℃, and the protective gas is used for cooling and anti-oxidation. After the surface temperature of the coating decreases, the interlayer stress of the coating can be released. After multiple steps, the corresponding untreated coating is obtained. Two layers (metal bonding layer + radar absorbing layer) are sprayed in layers. First, the metal bonding layer is sprayed with a thickness of 70~110μm, and then the radar absorbing layer is sprayed with a thickness of 1.7mm.
[0048] Step 4: Allow the sprayed workpiece 1 to cool naturally to room temperature, then polish the pre-coated layer and perform high-temperature annealing heat treatment to obtain an integrated coating.
[0049] Specifically, after the workpiece is naturally cooled to room temperature after spraying, the coating surface is lightly polished (to remove the "burrs" on the edge of the substrate), and then subjected to a high-temperature annealing heat treatment at 900℃ for 120 minutes to finally obtain an integrated coating with a large thickness (≥1.5mm).
[0050] Performance testing: Coating bonding strength 6.2MPa, no oxidation after 100h heat treatment at 900℃, reflectivity ≤-5dB in 8-18GHz band, preparation efficiency improved by 300% compared to single gun.
[0051] Example 2 This embodiment discloses a method for preparing a coating using a multi-gun plasma spraying apparatus. The method includes the following steps: Step 1: Heat treat and sandblast the cleaned workpiece 1, and then fix the workpiece 1 on the turntable 3; Specifically, the workpiece 1 (metal substrate, such as high-temperature alloy, 1m in diameter and 600mm in height) is cleaned with alcohol → heat treated (300℃, 30min; ensuring complete removal of oil stains and alcohol from the substrate) → sandblasted (grit size 80-200 mesh, roughness Ra2.5-5.3μm, to improve the adhesion between the coating and the substrate, 0.3MPa) → placed on a turntable 3, with a turntable speed of 17r / min, and fixed with L-shaped jaws 2 → the six-axis industrial robot connected to the multi-gun array mechanism (the moving speed of the six-axis industrial robot is 1000mm / s) is adjusted so that the output end of the spray gun 7 is in a suitable position with the workpiece 1.
[0052] Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod 8 so that the axis of the spray gun 7 is at 90° with the surface of the workpiece 1, and the axis of the gas nozzle 5 is at 60° with the surface of the workpiece 1; set the spraying parameters and powder feeding parameters of the spray gun 7 through the control module.
[0053] Specifically, a rectangular array of three plasma spray guns (spaced 200mm apart) is used. The position of the six-axis robot is adjusted so that the 7th axis of the spray gun is at a 90° angle to the workpiece surface. The robot parameters are adjusted so that the distance between the output end of the plasma spray gun and the workpiece surface is 100mm, the axial translation speed of the plasma spray gun is 1.3mm / s, and the reciprocating translation distance is 200mm.
[0054] The axis of the protective gas nozzle 5 is at a 60° angle to the workpiece surface; Plasma spray gun parameters: current 400A, voltage 60V; plasma gas flow rate 40 L / min (argon flow rate 35L / min, hydrogen flow rate 5L / min). Powder feeding parameters: matrix powder (NiCrAlY powder: particle size 20-50μm, flow rate 19s, powder feeding speed 50g / min), microwave absorbing functional powder (particle size 20-70μm, flow rate 180s, powder feeding speed 35g / min); Step 3: The workpiece is rotated by the control module, and the spray gun 7 is sprayed up and down by the six-axis robot to obtain the pre-coated layer; during the spraying process, the surface temperature of the workpiece 1 is measured in real time by the infrared temperature measurement module 9 to adjust the temperature of the gas sprayed from the nozzle. Specifically, a "uniformly distributed, zoned heating" strategy is adopted: the workpiece is rotated (15 r / min) by the control module, and multiple guns move up and down simultaneously in axially uniform zones (total workpiece height H, n gun arrays) (gun speed 1.5 mm / s), with a moving distance of H / n, for spraying. The spraying distance is 100 mm, and the single spray thickness is 0.03 mm / layer. During the spraying process, the surface temperature of the workpiece is measured by the infrared temperature measurement module 9, and protective gas at appropriate pressure is released onto the workpiece surface through the nozzle. The cooling system is divided into... The support pressure is 0.3MPa~0.6MPa, with an angle of 70° to the workpiece surface. The position and height of the infrared thermometer are adjusted to measure the temperature of the entire area to be coated. The surface temperature of the coating is controlled at 130℃, and the protective gas is used for cooling and anti-oxidation. After the surface temperature of the coating decreases, the interlayer stress of the coating can be released. After multiple steps, the corresponding untreated coating is obtained. Two layers (metal bonding layer + radar absorbing layer) are sprayed in layers. First, the metal bonding layer is sprayed with a thickness of 70~110μm, and then the radar absorbing layer is sprayed with a thickness of 1.7mm.
[0055] Step 4: Allow the sprayed workpiece 1 to cool naturally to room temperature, then polish the pre-coated layer and perform high-temperature annealing heat treatment to obtain an integrated coating.
[0056] Specifically, after the workpiece is naturally cooled to room temperature after spraying, the coating surface is lightly polished (to remove the "burrs" on the edge of the substrate), and then subjected to a high-temperature annealing heat treatment at 900℃ for 120 minutes to finally obtain an integrated coating with a large thickness (≥1.5mm).
[0057] Performance testing: Coating bonding strength 6.2MPa, no oxidation after 100h heat treatment at 900℃, reflectivity ≤-5dB in 8-18GHz band, preparation efficiency improved by 300% compared to single gun.
[0058] Example 3 This embodiment discloses a method for preparing a coating using a multi-gun plasma spraying apparatus. The method includes the following steps: Step 1: Heat treat and sandblast the cleaned workpiece 1, and then fix the workpiece 1 on the turntable 3; Specifically, the workpiece 1 (metal substrate, such as high-temperature alloy, 1m in diameter and 600mm in height) is cleaned with alcohol → heat treated (300℃, 30min; ensuring complete removal of oil stains and alcohol from the substrate) → sandblasted (grit size 80-200 mesh, roughness Ra2.5-5.3μm, to improve the adhesion between the coating and the substrate, 0.3MPa) → placed on a turntable 3, with a turntable speed of 15r / min, and fixed with L-shaped chucks 2 → the six-axis industrial robot connected to the multi-gun array mechanism (the moving speed of the six-axis industrial robot is 5mm / s) is adjusted so that the output end of the spray gun 7 is in a suitable position with the workpiece 1.
[0059] Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod 8 so that the axis of the spray gun 7 is at 90° with the surface of the workpiece 1, and the axis of the gas nozzle 5 is at 60° with the surface of the workpiece 1; set the spraying parameters and powder feeding parameters of the spray gun 7 through the control module.
[0060] Specifically, a rectangular array of three plasma spray guns (spaced 200mm apart) is used. The position of the six-axis robot is adjusted so that the 7th axis of the spray gun is at a 90° angle to the workpiece surface. The robot parameters are adjusted so that the distance between the output end of the plasma spray gun and the workpiece surface is 100mm, the axial translation speed of the plasma spray gun is 1.3mm / s, and the reciprocating translation distance is 200mm.
[0061] The axis of the protective gas nozzle 5 is at a 60° angle to the workpiece surface; Plasma spray gun parameters: current 600A, voltage 75V; plasma gas (argon flow rate 40L / min, hydrogen flow rate 8L / min) flow rate 48 L / min; Powder feeding parameters: matrix powder (NiCrAlY powder: particle size 20-50μm, flow rate 50s, powder feeding speed 38 g / min), microwave absorbing functional powder (particle size 20-70μm, flow rate 180s, powder feeding speed 20g / min); Step 3: The workpiece is rotated by the control module, and the spray gun 7 is sprayed up and down by the six-axis robot to obtain the pre-coated layer; during the spraying process, the surface temperature of the workpiece 1 is measured in real time by the infrared temperature measurement module 9 to adjust the temperature of the gas sprayed from the nozzle. Specifically, a "uniformly distributed, zoned heating" strategy is adopted: the workpiece is rotated (13 r / min) by the control module, and multiple guns move up and down simultaneously in axially uniform zones (total workpiece height H, n gun arrays) (gun speed 1.5 mm / s), with a moving distance of H / n, for spraying. The spraying distance is 100 mm, and the single spray thickness is 0.03 mm / layer. During the spraying process, the workpiece surface temperature is measured by the infrared temperature measurement module 9, and protective gas at appropriate pressure is released onto the workpiece surface through the nozzle. The cooling system is divided into... The support pressure is 0.3MPa~0.6MPa, with an angle of 70° to the workpiece surface. The position and height of the infrared thermometer are adjusted to measure the temperature of the entire area to be coated. The surface temperature of the coating is controlled at 130℃, and the protective gas is used for cooling and anti-oxidation. After the surface temperature of the coating decreases, the interlayer stress of the coating can be released. After multiple steps, the corresponding untreated coating is obtained. Two layers (metal bonding layer + radar absorbing layer) are sprayed in layers. First, the metal bonding layer is sprayed with a thickness of 70~110μm, and then the radar absorbing layer is sprayed with a thickness of 1.7mm.
[0062] Step 4: Allow the sprayed workpiece 1 to cool naturally to room temperature, then polish the pre-coated layer and perform high-temperature annealing heat treatment to obtain an integrated coating.
[0063] Specifically, after the workpiece is naturally cooled to room temperature after spraying, the coating surface is lightly polished (to remove the "burrs" on the edge of the substrate), and then subjected to a high-temperature annealing heat treatment at 900℃ for 120 minutes to finally obtain an integrated coating with a large thickness (≥1.5mm).
[0064] Performance testing: Coating bonding strength 6.2MPa, no oxidation after 100h heat treatment at 900℃, reflectivity ≤-5dB in 8-18GHz band, preparation efficiency improved by 300% compared to single gun.
[0065] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.
[0066] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A multi-gun plasma spraying device, characterized in that, The system includes a turntable (3) and an infrared temperature measurement module (9). The turntable (3) is equipped with a placement tray, which is equipped with multiple workpiece clamping parts (2). Above the placement tray is a hollow protective gas support rod (8), which is equipped with multiple spray guns (7). The protective gas support rod (8) is held by a six-axis robot. One end of the protective gas support rod (8) is connected to the jetting mechanism, and the other end of the protective gas support rod (8) is sealed. The protective gas support rod (8) is equipped with multiple gas nozzles (5). The spray guns (7) are connected to the powder feeding mechanism. The infrared temperature measurement module (9) detects the temperature of the workpiece (1) in real time and transmits the temperature signal to the control module.
2. The multi-gun plasma spraying apparatus according to claim 1, characterized in that, The workpiece clamping part (2) is arranged along the circumference of the placement plate.
3. The multi-gun plasma spraying apparatus according to claim 1, characterized in that, The spray gun (7) is snapped onto the protective gas support rod (8) by a clip.
4. The multi-gun plasma spraying apparatus according to claim 1, characterized in that, The six-axis robot has a moving speed of 1~1000mm / s.
5. A multi-gun plasma spraying apparatus according to claim 1, characterized in that, The rotational speed of the turntable (3) is 10~20 r / min.
6. The multi-gun plasma spraying apparatus according to claim 1, characterized in that, The powder feeding mechanism includes 3 to 6 independent powder feeding channels, which are connected to the spray gun (7) through the powder feeding channels.
7. The multi-gun plasma spraying apparatus according to claim 1, characterized in that, The workpiece clamping part (2) includes an L-shaped jaw, which is connected to the turntable (3).
8. A method for preparing a coating using a multi-gun plasma spraying apparatus, characterized in that, The method uses the multi-gun plasma spraying apparatus according to any one of claims 1 to 7, and the method includes the following steps: Step 1: Heat treat and sandblast the cleaned workpiece (1), and then fix the workpiece (1) on the turntable (3); Step 2: Adjust the angle of the six-axis robot holding the protective gas support rod (8) so that the axis of the spray gun (7) is at 90° with the surface of the workpiece (1) and the axis of the gas nozzle (5) is at 50°~70° with the surface of the workpiece (1); set the spraying parameters and powder feeding parameters of the spray gun (7) through the control module. Step 3: The workpiece is rotated by the control module, and the spray gun (7) is sprayed up and down repeatedly by the six-axis robot to obtain the pre-coated layer; During the spraying process, the temperature of the workpiece (1) surface is measured in real time by the infrared temperature measurement module (9) in order to adjust the temperature of the gas sprayed from the nozzle; Step 4: After spraying, the workpiece (1) is naturally cooled to room temperature. The pre-coated coating is then polished and subjected to high-temperature annealing heat treatment to obtain an integrated coating.
9. A method for preparing a coating using a multi-gun plasma spraying apparatus according to claim 8, characterized in that, In step two, the spraying parameters include: current 400~600A, voltage 60~75V, and plasma gas flow rate of 40~55L / min.
10. A method for preparing a coating using a multi-gun plasma spraying apparatus according to claim 8, characterized in that, In step two, the powder feeding parameters include: the powder feeding speed of the matrix powder is 25-50 g / min, and the powder feeding speed of the microwave absorbing function powder is 20-35 g / min.