By depositing a high-entropy nitride coating on the surface of aluminum substrate micro-drills, the problems of poor coating hardness and wear resistance are solved, achieving long life and high reliability of aluminum substrate micro-drills under harsh processing conditions, which is suitable for the manufacture of heat dissipation substrates for LED lighting and high-power electronic devices.
Patent Information
- Application Number
- CN202611522025.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing micro-drill coatings on aluminum substrates have poor hardness and wear resistance, are easy to peel off, and cannot meet the increased heat dissipation requirements of LED lighting and high-power electronic devices. Furthermore, traditional coatings are prone to failure under harsh processing conditions.
A high-entropy nitride coating was used to deposit a (TiCrVZrNb)N coating on the surface of a micro-drilled aluminum substrate using micro-arc ion plating technology. This process included substrate pretreatment, plasma etching, bias voltage adjustment, and pulse power supply control, resulting in a dense single-face-centered cubic solid solution phase coating.
It significantly improves the hardness and wear resistance of aluminum substrate micro-drills, extends service life, reduces wear rate, and improves processing efficiency and reliability.
Smart Images

Figure CN123108480A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface engineering materials technology, specifically relating to a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates, and a method for preparing the high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates. Background Technology
[0002] Aluminum substrates, with their excellent thermal conductivity, electrical insulation, and machinability, are widely used in the manufacture of heat dissipation substrates for LED lighting, power modules, automotive electronics, and high-power devices. In the processing of aluminum-based printed circuit boards (MC-PCBs), micro-hole drilling is a crucial process for ensuring circuit continuity and heat dissipation efficiency. Since aluminum substrates are typically composed of an aluminum matrix and a high-hardness ceramic insulating layer (such as alumina or aluminum nitride), and given the high ductility and tendency for aluminum matrix to generate chips, micro-drills, during high-speed drilling, must simultaneously withstand the combined effects of severe abrasive wear from ceramic particles and adhesive wear from aluminum chips. This makes them highly susceptible to premature failure due to accelerated edge wear or chipping, leading to deteriorated drilling quality and increased processing costs.
[0003] To address the aforementioned issues, depositing a hard protective coating on the surface of micro-drills is an effective technique to extend their service life. Currently, coating materials used for surface protection of micro-drills mainly include binary or ternary nitrides such as TiN, TiAlN, CrN, and TiCN, which can improve the hardness and wear resistance of micro-drills to a certain extent. However, with the continuous increase in heat dissipation requirements from LED lighting and high-power electronic devices, the hardness and thickness of the ceramic insulating layer in aluminum substrates are constantly increasing. At the same time, micro-hole processing is developing towards smaller diameters and higher rotational speeds, making processing conditions increasingly demanding. Traditional coating systems can no longer meet the requirements of long life and high reliability for micro-drills in aluminum substrate micro-hole processing.
[0004] High-entropy alloy coatings are composed of five or more principal elements. This multi-principal element design allows high-entropy coatings to exhibit superior hardness and wear resistance compared to traditional binary / ternary nitride coatings. This design concept remains applicable to the field of high-entropy nitride coatings, providing a new material solution for improving the performance of micro-drill coatings used in micro-hole machining of aluminum substrates. The main existing technology for preparing micro-drill coatings is micro-arc ion plating, which combines the advantages of multi-arc ion plating and magnetron sputtering. The resulting coatings are dense, have low surface roughness, and excellent adhesion, making them suitable for high-quality coating preparation for micro-drills and other micro-tools. It offers advantages such as fast deposition rates and good film-substrate adhesion. However, while magnetron sputtering produces dense coatings, it suffers from thinness and susceptibility to peeling. The presence of molten droplets on the coating surface significantly increases surface roughness, making it prone to peeling during cutting. Summary of the Invention
[0005] One objective of this invention is to provide a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates, which solves the problems of poor hardness and wear resistance, and easy peeling of existing coatings.
[0006] Another object of the present invention is to provide a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates.
[0007] The first technical solution adopted in this invention is a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates, specifically as follows: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 2, substrate pretreatment; Step 3: Perform plasma etching; Step 4: Adjust the base bias voltage; Step 5: Adjust the duty cycle and peak current of the pulse power supply to deposit a TiCrVZrNb transition layer on the Cr transition layer; Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled, and the peak current of the pulse power supply is adjusted to deposit a (TiCrVZrNb)N working layer on the TiCrVZrNb transition layer.
[0008] The invention is further characterized in that: Step 1 is as follows: Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0009] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0010] Step 2 is as follows: Step 2.1: Grind and polish the substrate. After polishing, ultrasonically clean the substrate with ethanol solution for 20 minutes, then blow dry and place it in the vacuum chamber at a distance of 200 mm from the target. Step 2.2: The vacuum level inside the vacuum chamber is evacuated to 3.0 × 10⁻⁶. -3 Below Pa, the temperature inside the vacuum chamber is then heated to 100℃-300℃, followed by the introduction of 40 sccm of high-purity Ar gas into the vacuum chamber to stabilize the working pressure at 0.8 Pa.
[0011] The substrate can be made of either a single-crystal Si wafer or an M2 high-speed steel substrate; the M2 high-speed steel substrate has a size of Φ40mm×H4mm; the single-crystal Si wafer has a diameter of 100mm.
[0012] Step 3: The substrate bias voltage is -350V, and the etching time is 20min.
[0013] Step 4: Adjust the substrate bias voltage to -50V to -200V, and deposit the Cr transition layer for 10 minutes in constant current mode with a 2A DC power supply.
[0014] Step 5: Adjust the duty cycle of the pulse power supply to 10%-30%, the peak current to 5A-20A, and deposit the TiCrVZrNb transition layer; Step 6: Control the N2 flow rate to 4 sccm-16 sccm, adjust the peak current of the pulse power supply to 5A-20A, and deposit the (TiCrVZrNb)N working layer.
[0015] The second technical solution adopted in this invention is a high-entropy nitride wear-resistant coating for aluminum substrate micro-drills, which is prepared by depositing Cr targets and TiCrVZrNb targets on the surface of high-speed steel micro-drill substrates using a micro-arc ion plating system.
[0016] The invention is further characterized in that: The high-entropy nitride coating has a dense surface and a single face-centered cubic solid solution phase structure. The coating hardness is 27 GPa-31 GPa.
[0017] The beneficial effects of this invention are as follows: The high-entropy nitride wear-resistant coating for aluminum substrate micro-drills, using micro-arc ion plating technology, can effectively reduce surface defects during coating preparation, obtaining a coating that combines high hardness, excellent film-substrate adhesion, and good wear resistance. This significantly extends the service life of aluminum substrate micro-drills and can be widely applied in high-efficiency micro-hole drilling of aluminum substrates. Furthermore, thanks to its excellent mechanical properties, the coating exhibits good resistance to plastic deformation during wear, further reducing material loss and effectively extending the service life of the coating. Attached Figure Description
[0018] Figure 1(a) is a surface SEM image of the coating prepared in Example 5 of the present invention; Figure 1(b) is a surface SEM image of the coating prepared in Example 6 of the present invention; Figure 2(a) is a cross-sectional SEM image of the coating prepared in Example 5 of the present invention; Figure 2(b) is a cross-sectional SEM image of the coating prepared in Example 6 of the present invention; Figure 3 These are hardness and elastic modulus diagrams of the coatings prepared in Examples 5 and 6 of this invention; Figure 4(a) shows the scratch morphology and acoustic signal curve of the coating prepared in Example 5; Figure 4(b) is a graph showing the scratch morphology and acoustic signal curve of the coating prepared in Example 6. Detailed Implementation
[0019] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0020] The present invention provides a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling on aluminum substrates, specifically comprising: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0021] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0022] Step 2, substrate pretreatment; Step 2.1: Grind and polish the substrate. After polishing, ultrasonically clean the substrate with ethanol solution for 20 min-30 min, then blow dry and place it in the vacuum chamber at a distance of 190 mm-200 mm from the target. The substrate can be made of either single-crystal Si wafer or M2 high-speed steel substrate; the M2 high-speed steel substrate has a size of Φ40mm×H4mm; the single-crystal Si wafer has a diameter of 100mm; the single-crystal Si wafer is used for the coating microstructure; the M2 high-speed steel wafer is used for the coating mechanical and tribological properties.
[0023] Step 2.2: Use a mechanical pump and a molecular pump in succession to evacuate the vacuum chamber to a vacuum level of 3.0 × 10⁻⁶. -3 Below Pa, the temperature inside the vacuum chamber is then heated to 100℃-300℃, followed by the introduction of 40 sccm of high-purity Ar gas into the vacuum chamber to stabilize the working pressure at 0.8 Pa.
[0024] Step 3: Perform plasma etching; The substrate bias voltage was -350V, and the etching time was 20 minutes. Step 4: Adjust the base bias voltage; Deposit a Cr transition layer for 10 min in constant current mode with a 2A DC power supply; adjust the substrate bias voltage from -50V to -200V and deposit a Cr transition layer for 10 min in constant current mode with a 2A DC power supply. Step 5: Adjust the duty cycle and peak current of the pulse power supply to deposit a TiCrVZrNb transition layer on the Cr transition layer; Adjust the duty cycle of the pulse power supply to 10%-30%, and the peak current to 5A-20A to deposit a TiCrVZrNb transition layer; Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled, and the peak current of the pulse power supply is adjusted to deposit a (TiCrVZrNb)N working layer on the TiCrVZrNb transition layer.
[0025] The flow rate of N2 was controlled at 4 sccm-16 sccm, and the peak current of the pulse power supply was adjusted at 5A-20A to deposit a (TiCrVZrNb)N working layer.
[0026] Example 1 The present invention provides a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling on aluminum substrates, specifically comprising: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0027] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0028] Step 2, substrate pretreatment; Step 2.1: The substrate is a single-crystal Si wafer with a diameter of 100 mm; the single-crystal Si wafer is used for the coating structure; the substrate is polished, and after polishing, the substrate is ultrasonically cleaned with ethanol solution for 25 min, then dried and placed in a vacuum chamber at a distance of 190 mm from the target. Step 2.2: Use a mechanical pump and a molecular pump in succession to evacuate the vacuum chamber to a vacuum level of 3.0 × 10⁻⁶. -3 The pressure is below 0.8 Pa. Then the temperature inside the vacuum chamber is heated to 150°C. Next, 40 sccm of high-purity Ar gas is introduced into the vacuum chamber to stabilize the working pressure at 0.8 Pa.
[0029] Step 3: Perform plasma etching; the substrate bias voltage is -350V, and the etching time is 20min. Step 4: Adjust the substrate bias voltage; deposit the Cr transition layer for 10 min in DC power supply 2A constant current mode; adjust the substrate bias voltage to -50V, and deposit the Cr transition layer for 10 min in DC power supply 2A constant current mode. Step 5: Adjust the duty cycle and peak current of the pulse power supply to deposit a TiCrVZrNb transition layer on the Cr transition layer; adjust the duty cycle of the pulse power supply to 10% and the peak current to 5A to deposit the TiCrVZrNb transition layer. Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled at 4 sccm, and the peak current of the pulse power supply is adjusted to 5A to deposit a (TiCrVZrNb)N working layer.
[0030] Example 2 The present invention provides a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling on aluminum substrates, specifically comprising: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0031] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0032] Step 2, substrate pretreatment; Step 2.1: The substrate is an M2 high-speed steel substrate with a specification of Φ40mm×H4mm. The M2 high-speed steel substrate is used for the mechanical and tribological properties of the coating. The substrate is ground and polished. After polishing, the substrate is ultrasonically cleaned with ethanol solution for 30 minutes, then dried and placed in a vacuum chamber at a distance of 190mm from the target. Step 2.2: Use a mechanical pump and a molecular pump in succession to evacuate the vacuum chamber to a vacuum level of 3.0 × 10⁻⁶. -3 The pressure is below 0.8 Pa. Then the temperature inside the vacuum chamber is heated to 300°C. Next, 40 sccm of high-purity Ar gas is introduced into the vacuum chamber to stabilize the working pressure at 0.8 Pa.
[0033] Step 3: Perform plasma etching; the substrate bias voltage is -350V, and the etching time is 20min. Step 4: Adjust the substrate bias voltage; deposit the Cr transition layer for 10 min in DC power supply 2A constant current mode; adjust the substrate bias voltage to -200V, and deposit the Cr transition layer for 10 min in DC power supply 2A constant current mode. Step 5: Adjust the duty cycle and peak current of the pulse power supply to deposit a TiCrVZrNb transition layer on the Cr transition layer; adjust the duty cycle of the pulse power supply to 30% and the peak current to 20A to deposit the TiCrVZrNb transition layer. Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled at 4 sccm, and the peak current of the pulse power supply is adjusted to 20A to deposit a (TiCrVZrNb)N working layer.
[0034] Example 3 The high-entropy nitride wear-resistant coating for aluminum substrate micro-drilling prepared by the present invention is obtained by depositing Cr target and TiCrVZrNb target on the surface of high-speed steel micro-drilling substrate using a micro-arc ion plating system.
[0035] Example 4 The high-entropy nitride coating prepared in Example 3 has a dense surface and a single face-centered cubic (FCC) solid solution phase. The incorporation of nitrogen (N) causes severe lattice distortion within the crystal, restricting dislocation slip. Simultaneously, nitrogen atoms occupy interstitial lattice positions, forming strong covalent bonds (Me–N) with metals such as Ti, Cr, V, Zr, and Nb, effectively enhancing the intrinsic hardness of the coating, which ranges from 27 GPa to 31 GPa. This invention utilizes micro-arc ion plating technology to prepare a high-entropy nitride coating with a dense surface, good cross-section-to-substrate bonding, clear interface, and uniform thickness.
[0036] This invention relates to a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates. During the friction and wear process, the oxide layer generated in situ on the coating surface improves the contact state of the friction pair and reduces the interfacial shear strength, thereby significantly reducing the wear rate of the coating. Compared with existing multi-arc ion plating and magnetron sputtering coating deposition technologies, this invention produces a coating that combines high hardness, excellent film-substrate adhesion, and good wear resistance.
[0037] Example 5 The present invention provides a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling on aluminum substrates, specifically comprising: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0038] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0039] Step 2, substrate pretreatment; Step 2.1: The substrate is a single-crystal Si wafer; the diameter of the single-crystal Si wafer is 100mm; the single-crystal Si wafer is used for the coating structure; the substrate is ground and polished, and the polished substrate is ultrasonically cleaned with ethanol solution for 20min, then dried and placed in a vacuum chamber 200mm away from the target material. Step 2.2: Use a mechanical pump and a molecular pump in succession to evacuate the vacuum chamber to a vacuum level of 3.0 × 10⁻⁶. -3 The pressure is below Pa, then the temperature inside the vacuum chamber is heated to 100°C, and then 40 sccm of high-purity Ar gas is introduced into the vacuum chamber to stabilize the working pressure at 0.8 Pa. Step 3: Perform plasma etching with a substrate bias of -350V and an etching time of 20 minutes.
[0040] Step 4: Adjust the substrate bias voltage to -100V and deposit the Cr transition layer for 10 minutes in constant current mode with a DC power supply of 2A. Step 5: Adjust the pulse power supply duty cycle to 30% and the peak current to 15A to deposit the TiCrVZrNb transition layer; adjust the pulse power supply duty cycle to 10% and the peak current to 5A to deposit the TiCrVZrNb transition layer.
[0041] Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled at 16 sccm, and the peak current of the pulse power supply is adjusted to 15 A to deposit a (TiCrVZrNb)N working layer.
[0042] Example 6 The present invention provides a method for preparing a high-entropy nitride wear-resistant coating for micro-drilling on aluminum substrates, specifically comprising: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target and the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%.
[0043] Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
[0044] Step 2, substrate pretreatment; Step 2.1: The substrate is an M2 high-speed steel substrate with a specification of Φ40mm×H4mm. The M2 high-speed steel substrate is used for the mechanical and tribological properties of the coating. The substrate is ground and polished. After polishing, the substrate is ultrasonically cleaned with ethanol solution for 20 minutes, then dried and placed in a vacuum chamber 200mm away from the target. Step 2.2: Use a mechanical pump and a molecular pump in succession to evacuate the vacuum chamber to a vacuum level of 3.0 × 10⁻⁶. -3 Below Pa, the temperature inside the vacuum chamber is then heated to 300°C, and then 40 sccm of high-purity Ar gas is introduced into the vacuum chamber to stabilize the working pressure at 0.8 Pa. Step 3: Perform plasma etching with a substrate bias voltage of -350V and an etching time of 20 minutes. Step 4: Adjust the substrate bias voltage to -100V and deposit the Cr transition layer for 10 minutes in constant current mode with a DC power supply of 2A. Step 5: Adjust the pulse power supply duty cycle to 30% and the peak current to 15A to deposit the TiCrVZrNb transition layer; Step 6: Control the N2 flow rate to 12 sccm, adjust the peak current of the pulse power supply to 15 A, and deposit the (TiCrVZrNb)N working layer.
[0045] The coatings prepared in Examples 5 and 6 were characterized for surface and cross-sectional morphology using scanning electron microscopy (SEM, ZEISS Sigma 360); elemental composition was characterized using energy dispersive spectroscopy (EDS, OXFORD Xplore 30); crystal structure was characterized using X-ray diffraction (XRD), with a scanning range of 20°–90° and a scanning speed of 5° / min; and chemical bonding was characterized using X-ray photoelectron spectroscopy (XPS, Thermo Kalpha). The coatings prepared in Examples 5 and 2 were characterized for hardness and elastic modulus using a nano-indenter (Nano-Indenter G200). A Berkovich pyramidal diamond indenter was used in the test, with a maximum load of 10 mN and a holding time of 10 s. The Poisson's ratio was set to 0.32, and the indentation depth was 100 nm. Each sample was measured 5 times and the average value was taken to ensure the accuracy and reliability of the test results.
[0046] The wear resistance of the coatings prepared in Examples 5 and 6 was tested using a ball-disc tribo-wear testing machine (UMT-TriboLab type). The friction pair consisted of Si3N4 balls with a diameter of 6.35 mm, a rotation radius of 3 mm, a rotation speed of 200 rpm, a load of 3 N, and a friction test time of 30 min. The wear track width and depth were measured using a laser confocal microscope, and the specific wear rate K was then calculated by calculating the wear volume.
[0047] Example Test Results
[0048] As shown in Figures 1(a) and 1(b), both groups of coating surfaces exhibit typical cluster-like structural features; as shown in Figures 2(a) and 2(b), the coating structure is either layered or columnar, indicating that the nitrogen partial pressure has a significant impact on the crystal orientation growth of the coating.
[0049] The high-entropy nitride wear-resistant coating prepared by micro-arc ion plating technology has a hardness of about 30 GPa, such as... Figure 3 As shown, the interstitial solid solution of nitrogen atoms causes significant lattice distortion, effectively hindering dislocation movement and producing a strong solid solution strengthening effect. Secondly, nitrogen atoms can occupy interstitial positions and form strong covalent bonds (Me–N) with metallic elements such as Ti, Cr, V, Zr, and Nb, further improving the cohesive strength of the coating. Furthermore, combining the SEM cross-sectional morphologies of the coatings in Figures 2(a) and 2(b), it can be seen that the coating structure is dense with a high grain boundary density, and boundary strengthening also contributes.
[0050] The scratch test results of the coating are shown in Figures 4(a) and 4(b). The high-entropy nitride wear-resistant coating prepared by micro-arc ion plating technology exhibits excellent film-substrate adhesion strength. During the scratch test, the acoustic emission signal remained at the baseline level for most of the load range, with only a few points showing spikes. Furthermore, the scratch morphology showed that only slight scratches remained on the coating surface, without obvious cracking or peeling marks, indicating that crack propagation was effectively suppressed during the indenter loading process, and the film-substrate adhesion was at its best.
Claims
1. A method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates, characterized in that, Specifically: Step 1: Prepare a (TiCrVZrNb)Nx coating; Step 2, substrate pretreatment; Step 3: Perform plasma etching; Step 4: Adjust the base bias voltage; Step 5: Adjust the duty cycle and peak current of the pulse power supply to deposit a TiCrVZrNb transition layer on the Cr transition layer; Step 6: Using micro-arc ion plating technology, the flow rate of N2 is controlled, and the peak current of the pulse power supply is adjusted to deposit a (TiCrVZrNb)N working layer on the TiCrVZrNb transition layer.
2. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 1, characterized in that, Step 1 is as follows: Step 1.1: Weigh out the Cr target and TiCrVZrNb target. The atomic ratio of the Cr target to the TiCrVZrNb target is Ti:Cr:V:Zr:Nb = 1:1:1:1:
1. The purity of both the Cr target and the TiCrVZrNb target is not less than 99.99%. Step 1.2: The weighed Cr target is co-deposited with the TiCrVZrNb target; During the co-deposition process, a micro-arc ion plating system is used to apply a pulsed electric field between the cathode TiCrVZrNb target and the anode cavity, and a DC electric field between the cathode Cr target and the anode cavity.
3. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 2, characterized in that, Step 2 is as follows: Step 2.1: Grind and polish the substrate. After polishing, ultrasonically clean the substrate with ethanol solution for 20 minutes, then blow dry and place it in the vacuum chamber at a distance of 200 mm from the target. Step 2.2: The vacuum level inside the vacuum chamber is evacuated to 3.0 × 10⁻⁶. -3 Below Pa, the temperature inside the vacuum chamber is then heated to 100℃-300℃, followed by the introduction of 40 sccm of high-purity Ar gas into the vacuum chamber to stabilize the working pressure at 0.8 Pa.
4. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 3, characterized in that, The substrate can be made of either a single-crystal Si wafer or an M2 high-speed steel substrate; the M2 high-speed steel substrate has a size of Φ40mm×H4mm; the single-crystal Si wafer has a diameter of 100mm.
5. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 4, characterized in that, Step 3: The substrate bias voltage is -350V, and the etching time is 20min.
6. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 5, characterized in that, Step 4: Adjust the substrate bias voltage to -50V to -200V, and deposit the Cr transition layer for 10 minutes under constant current mode with a 2A DC power supply.
7. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 6, characterized in that, Step 5: Adjust the duty cycle of the pulse power supply to 10%-30%, the peak current to 5A-20A, and deposit the TiCrVZrNb transition layer.
8. The method for preparing a high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 7, characterized in that, Step 6: Control the N2 flow rate to 4 sccm-16 sccm, adjust the peak current of the pulse power supply to 5A-20A, and deposit the (TiCrVZrNb)N working layer.
9. A high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates, characterized in that, The Cr target and TiCrVZrNb target were deposited on the surface of a high-speed steel micro-drill substrate using a micro-arc ion plating system.
10. The high-entropy nitride wear-resistant coating for micro-drilling of aluminum substrates according to claim 9, characterized in that, The high-entropy nitride coating has a dense surface and a single face-centered cubic solid solution phase structure. The coating hardness is 27 GPa-31 GPa.