A high-throughput thin film preparation apparatus and method for atomic layer deposition
By combining a combined vacuum chamber and a programmable mask control system, high-throughput thin film preparation using atomic layer deposition technology has been achieved, solving the problems of long R&D cycles and high costs in existing technologies, and improving the R&D efficiency of thin film materials and the efficiency of process parameter screening.
Patent Information
- Application Number
- CN202611556286.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing atomic layer deposition technology requires a large number of repeated experiments when optimizing process parameters, resulting in long research and development cycles, low efficiency and high costs, making it difficult to efficiently explore new high-performance thin film materials.
By employing a combined vacuum chamber and programmable mask control system, along with multiple atomic layer deposition sources and a movable substrate, parallel fabrication and precise control of thin films under various conditions can be achieved. Through precise mask movement and coordinated regulation of deposition sources, high-throughput thin film fabrication can be realized.
It significantly improves the R&D efficiency of thin film materials, shortens the R&D cycle, and reduces costs. It enables parallel deposition of different thicknesses, compositions, and stacked structures in a single substrate loading process, breaking through the efficiency bottleneck of traditional processes.
Smart Images

Figure CN123108532A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thin film material preparation technology, and in particular to a high-throughput thin film preparation apparatus and method using atomic layer deposition. Background Technology
[0002] Atomic Layer Deposition (ALD) is a chemical vapor deposition (CVD) technique that enables the fabrication of large-area, highly conformal, and uniformly thick nanoscale thin films on complex three-dimensional surfaces with single-atom-layer precision. It has significant applications in integrated circuits, microelectromechanical systems (MEMS), and display devices. The growth quality and performance of the films prepared using this technique are highly dependent on various process parameters, including thickness, precursor type and dosage, growth cycle number, and the cycle ratio of different material layers. Currently, to optimize these process parameters and obtain films with specific properties, it is necessary to sequentially and independently adjust various parameters on different substrates and grow a large number of samples with different parameters for experimentation. However, each experiment requires the establishment and stabilization of a specific growth temperature and high vacuum environment, which often takes far longer than the actual film growth time. Extensive repetitive experiments are required to explore multiple key parameters and ultimately determine the optimal process window, resulting in a lengthy, inefficient, and costly research and development cycle, severely hindering the exploration and development of high-performance novel thin film materials. Therefore, the inventors found that it was a problem to be solved to provide a high-throughput parallel preparation method for ALD that could significantly improve experimental efficiency, shorten the R&D cycle, and reduce costs.
[0003] In view of this, the present invention is hereby proposed. Summary of the Invention
[0004] The purpose of this invention is to provide a high-throughput thin film preparation apparatus and method based on atomic layer deposition, which can improve the efficiency of preparing high-throughput thin films based on atomic layer deposition, shorten the research and development cycle, reduce costs, and thus solve the above-mentioned technical problems existing in the prior art.
[0005] The objective of this invention is achieved through the following technical solution:
[0006] A high-throughput thin film fabrication apparatus for atomic layer deposition includes:
[0007] A modular vacuum chamber consists of an inner cavity and an outer cavity nested outside the inner cavity.
[0008] The outer cavity is equipped with an electrically movable cavity door, which can be electrically controlled to open or close to realize the loading and unloading of the substrate.
[0009] The inner cavity includes an upper cavity and a lower cavity that can be opened and closed. A spray device is provided in the upper part of the upper cavity, which can spray an atomic layer deposition source into the lower part of the inner cavity. A movable substrate base is fixedly provided in the bottom of the lower cavity. The movable substrate base can support the substrate and heat the substrate. The position of the movable substrate base corresponds to the spray device.
[0010] The movable substrate base is fixedly disposed in the lower cavity; the driving device is connected to the lower cavity and can drive the lower cavity and the movable substrate base to move synchronously in the vertical direction, so as to adjust the distance between the movable substrate base and the spraying device, and to switch the lower cavity relative to the upper cavity between the closed position and the substrate loading position.
[0011] The upper cavity is provided with a plasma inlet at its top, which extends out of the outer cavity;
[0012] The input pipeline has its outlet end connected to the spray device inside the top of the inner cavity, and its inlet end extends to the outside of the outer cavity. It is provided with a carrier gas inlet that can be connected to a carrier gas source and a deposition source inlet that can be connected to a vaporized atomic layer deposition source.
[0013] A mask is disposed within the inner cavity and above the substrate supported by the movable substrate base. The mask is fixedly connected to a programmable mask control system disposed outside the outer cavity and can move precisely above the substrate under the drive and control of the programmable mask control system.
[0014] A high-throughput thin film preparation method using atomic layer deposition, employing the high-throughput thin film preparation apparatus for atomic layer deposition described in this invention, includes the following steps:
[0015] Step 1: Determine the key process parameters that affect thin film deposition. The key process parameters include: substrate temperature, types of precursors and co-reactants, pulse time of opening the atomic layer deposition source bottle valve, and purge time after closing the valve.
[0016] Step 2: Place the substrate in the sample slot of the movable substrate base of the device, and use the mechanical limiting structure at the edge of the sample slot to ensure the positional accuracy of the substrate.
[0017] Step 3: Select the desired target patterned mask and assemble it into the positioning slot of the mask fixing frame; then, drive the mask to move precisely through the programmable mask control system of the device to achieve precise alignment between the mask pattern and the preset deposition area on the substrate;
[0018] Step 4: After setting the substrate temperature, precursor and co-reactant types, pulse time, purge time and deposition cycle number determined in Step 1, start the deposition process and make the spray device of the apparatus start spraying.
[0019] Step 5: After completing the deposition under the current set conditions, the programmable mask control system moves the mask to the next preset position according to the predetermined program, adjusts the thin film deposition parameters, and performs deposition of the newly set thin film deposition parameters in the new area on the substrate; or keeps the mask position unchanged, changes the thin film deposition parameters, and achieves the growth of a multilayer stacked thin film at the same position on the substrate.
[0020] Step 6: For different substrates or different regions of the same substrate, different metal precursors and co-reactants are sequentially sprayed using a spraying device, and growth cycles are set. Combined with mask position programming, high-throughput thin film preparation with programmable composition, thickness, and stacking order is achieved.
[0021] Compared with the prior art, the high-throughput thin film preparation apparatus and method for atomic layer deposition provided by the present invention have the following advantages:
[0022] (1) By employing a combined vacuum chamber, integrating multiple atomic layer deposition sources, and combining a mask whose displacement is precisely controlled by a programmable mask control system, the material can only be deposited onto a designated area of the substrate through the mask apertures during the deposition process. This device enables the parallel preparation of thin films under various conditions, significantly accelerating the screening process for thin film deposition conditions and greatly improving the efficiency of thin film material research. It effectively solves the problems of long process parameter screening cycles, limited sample size for single experiments, and high trial-and-error costs in existing atomic layer deposition technologies.
[0023] (2) By adopting a variety of movable and replaceable masks and their combination designs, efficient regional deposition layouts can be achieved, enabling the rapid preparation of films of different thicknesses. Furthermore, by combining the synergistic control of multiple atomic layer deposition sources, films of different thicknesses, multiple components, and different stacked structures can be deposited in parallel on multiple substrates at different locations on the substrate base, or in different regions on a single substrate, breaking through the efficiency bottleneck of traditional processes.
[0024] (3) It can maintain the continuous stability of the internal environment of the deposition chamber (including temperature, vacuum and atmosphere) during a single substrate loading process, and deposit thin film materials with different thicknesses, multiple components and different stacking sequences in parallel batches, which significantly improves the efficiency of thin film material research and development. Attached Figure Description
[0025] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a schematic diagram of the high-throughput deposition apparatus for atomic layer deposition provided in an embodiment of the present invention.
[0027] Figure 2 This is a three-dimensional structural schematic diagram of a high-throughput deposition apparatus for atomic layer deposition provided in an embodiment of the present invention.
[0028] Figure 3 A flowchart of a high-throughput deposition method for atomic layer deposition provided in an embodiment of the present invention.
[0029] Figure 4 This is a flowchart of a method for depositing thin films of different thicknesses on the same substrate according to an embodiment of the present invention; wherein, Figure A1 is a schematic diagram of the initial deposition, Figure B1 is a schematic diagram of the intermediate deposition, and Figure C1 is a schematic diagram of the final deposition.
[0030] Figure 5 The present invention provides a flowchart of a method for depositing thin films with different doping and stacked structures on the same substrate; wherein, Figure A2 is a schematic diagram of the first type of precursor deposition, Figure B2 is a schematic diagram of the second type of precursor deposition, and Figure C2 is a schematic diagram of the final ordered stacked thin film deposition.
[0031] Figure 6 The diagram illustrates the replacement of masks with different patterned hole structures and the parallel thin film deposition effect achieved on the substrate by combining different masks, as provided in the embodiments of the present invention. Detailed Implementation
[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them, and do not constitute a limitation on the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the protection scope of the present invention.
[0033] First, the following explanations are provided for the terms that may be used in this article:
[0034] The term "and / or" means that either or both can be achieved simultaneously. For example, X and / or Y means that it includes both "X" or "Y" as well as the three cases of "X and Y".
[0035] The terms "comprising," "including," "containing," "having," or other similar semantic descriptions should be interpreted as non-exclusive inclusion. For example, including a technical feature element (such as raw material, component, ingredient, carrier, dosage form, material, size, part, component, mechanism, device, step, process, method, reaction conditions, processing conditions, parameter, algorithm, signal, data, product or article of manufacture, etc.) should be interpreted as including not only the expressly listed technical feature element, but also other technical feature elements that are not expressly listed and are well-known in the art.
[0036] The term "composed of" excludes any technical features not expressly listed. When used in a claim, it closes the claim to exclude all technical features other than those expressly listed, except for associated conventional impurities. If the term appears only in a clause of a claim, it limits the claim to the elements expressly listed in that clause; elements recited in other clauses are not excluded from the overall claim.
[0037] Unless otherwise explicitly specified or limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this document according to the specific circumstances.
[0038] The terms “center,” “longitudinal,” “lateral,” “length,” “width,” “thickness,” “up,” “down,” “front,” “back,” “left,” “right,” “vertical,” “horizontal,” “top,” “bottom,” “inner,” “outer,” “clockwise,” and “counterclockwise” indicate the current orientation or positional relationship, and are only for the convenience and simplification of description, and do not explicitly or implicitly suggest that the device or component referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this document.
[0039] The technical solution provided by this invention will be described in detail below. Contents not described in detail in the embodiments of this invention are prior art known to those skilled in the art. Where specific conditions are not specified in the embodiments of this invention, they shall be performed according to conventional conditions in the art or conditions recommended by the manufacturer. Reagents or instruments used in the embodiments of this invention whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0040] like Figure 1 As shown, an embodiment of the present invention provides a high-throughput thin film fabrication apparatus for atomic layer deposition, comprising:
[0041] The combined vacuum chamber consists of an inner cavity 12 and an outer cavity 11 nested outside the inner cavity 12.
[0042] The outer cavity 11 is equipped with an electrically movable cavity door, which can be electrically controlled to open or close to realize the loading and unloading of the substrate.
[0043] The inner cavity 12 includes an openable and closable upper cavity 121 and a lower cavity 122. A spray device 13 is provided in the upper part of the upper cavity 121. The spray device 13 can spray an atomic layer deposition source into the lower part of the inner cavity 12. A movable substrate base 14 is fixedly provided in the bottom of the lower cavity 122. The movable substrate base 14 can support the substrate 22 and heat the substrate 22. The position of the movable substrate base 14 corresponds to the spray device 13.
[0044] The movable substrate base 14 is fixedly disposed in the lower cavity 122; the driving device is connected to the lower cavity 122 and can drive the lower cavity 122 and the movable substrate base 14 to move synchronously in the vertical direction, so as to adjust the distance between the movable substrate base 14 and the spray device 13, and switch the lower cavity 122 relative to the upper cavity 121 between the closed position and the substrate loading position;
[0045] The upper cavity 121 is provided with a plasma inlet at its top, which extends out of the outer cavity;
[0046] The input pipe 20 has its outlet end connected to the spray device 13 inside the top of the inner cavity 12, and its inlet end extends to the outside of the outer cavity 11. It is provided with a carrier gas inlet that can be connected to the carrier gas source 21 and a deposition source inlet that can be connected to the vaporized atomic layer deposition source.
[0047] The mask 18 is disposed in the inner cavity 12 and above the substrate supported by the movable substrate base 14. The mask 18 is fixedly connected to the programmable mask control system 17 disposed outside the outer cavity 11 and can move precisely above the substrate 22 under the drive control of the programmable mask control system 17.
[0048] Preferably, the electrically sliding cavity door on the outer cavity 11 of the above-mentioned device includes: a door body, a drive mechanism, and a position detection component; wherein, the door body is installed on the outer cavity 11;
[0049] The electric drive mechanism is connected to the door body and can drive the door body to move between the open position and the closed position; preferably, the drive mechanism consists of a stepper motor and a lead screw transmission assembly, the stepper motor is connected to the door body via the lead screw transmission assembly and can drive the door body to move between the open position and the closed position.
[0050] The position detection component is disposed on the outer cavity 11 and can detect the open and closed states of the door.
[0051] The drive mechanism can operate according to a preset program and the positioning signal fed back by the position detection device, thereby automatically opening or closing the door.
[0052] Furthermore, the aforementioned device also includes:
[0053] Carrier gas source 21, programmable gas flow valve assembly 16, and multi-channel atomic layer deposition source 15;
[0054] The carrier gas source 21 is connected to the carrier gas inlet of the input pipeline 20;
[0055] The multi-channel atomic layer deposition source 15 is connected to the deposition source inlet of the input pipeline 20 via the programmable gas flow valve assembly 16, and the flow rate of the vaporized atomic layer deposition source mixed with the carrier gas can be quantitatively controlled by the programmable gas flow valve assembly 16.
[0056] Preferably, in the above-described apparatus, the deposition source inlet has multiple inlets, each of which is connected to the carrier gas inlet;
[0057] The multi-path atomic layer deposition source 15 includes multiple precursor source bottles and co-reactant bottles, which are respectively connected to multiple input ports. Each precursor source bottle and connecting pipeline is equipped with an independent temperature control module. The independent temperature control module can maintain the stability of the precursor temperature and prevent condensation, deposit contamination or blockage in the pipeline.
[0058] Furthermore, the aforementioned device also includes:
[0059] A plasma generator 19 is located at the top of the outer cavity 11. The plasma outlet of the plasma generator 19 is sealed to the plasma inlet at the top of the upper cavity 121 and is connected to the spray device 13 in the inner cavity 12 through the plasma inlet.
[0060] Preferably, in the above-mentioned device, the movable substrate base 14 is provided with a sample groove that can precisely limit the positioning of the substrate;
[0061] The mask plate 18 is installed and fixed by the positioning slot of the mask plate fixing frame, and more than one mask plate 18 can be installed in the positioning slot;
[0062] The input pipeline 20 is equipped with a heating device, which can control the temperature of the input pipeline.
[0063] Preferably, in the above-mentioned device, the spraying device 13 is a pulse spraying device; the spraying device 13 and related source pipelines are all integrated with heating devices, which can control the temperature of the source pipelines and spray heads.
[0064] Preferably, in the above-mentioned device, the programmable mask control system 17 adopts a programmable displacement controller. The programmable displacement controller is fixedly connected to the mask 18 through a vacuum linear transmission linkage device, and can drive the mask 18 to make precise displacement in the horizontal plane above the substrate 22 in the inner cavity, matching the spraying cycle of different atomic layer deposition sources.
[0065] Specifically, the high-throughput thin film fabrication apparatus for atomic layer deposition mentioned above includes:
[0066] The system comprises a combined vacuum chamber, a spray device 13, a movable substrate base 14, a multi-channel atomic layer deposition source 15, a programmable gas flow valve assembly 16, a programmable mask control system 17, a mask 18, and a plasma generator 19. The combined vacuum chamber consists of an inner cavity 12 and an outer cavity 11 nested around it, forming a nested structure to optimize the vacuum environment and temperature stability of the inner cavity. The outer cavity 11 has a door that can be opened and closed via program control for substrate loading and unloading. The spray device 13 is located at the top of the inner cavity 12 of the combined vacuum chamber and is used to uniformly spray the atomic layer deposition source onto the substrate base below. The movable substrate base 14 is located below the spray device 13 and is used to support and heat the substrate. The movable substrate base 14 can be fixedly connected to the lower cavity 122 of the inner cavity and serves as a drive mechanism. The device is driven by a Z-axis precision stepper motor, which allows the two to move up and down in tandem under the motor's drive. The motor's controllable movement enables the opening and closing of the upper cavity 121 of the inner cavity 12, facilitating substrate loading and unloading. The multi-channel atomic layer deposition source 15 is flexibly controlled by a programmable gas flow valve assembly 16, which pulse-delivers various metal precursors and co-reactants into the combined vacuum chamber 12. The programmable mask control system 17 works in conjunction with a replaceable mask 18, precisely controlling the precise movement of the mask 18 and the pulse timing of the programmable gas flow valve assembly 16 to precisely regulate the thin film deposition process on the substrate. The plasma generator 19, located at the top of the combined vacuum chamber, generates plasma that reacts with the atomic layer deposition source, providing various co-reactants. This device can deposit thin films with different thicknesses, doping concentrations, and stacked structures in parallel on multiple substrates at different locations on the movable substrate base 14, or in different regions of a single substrate, thereby achieving high-throughput fabrication.
[0067] like Figure 3As shown, this invention also provides a method for preparing high-throughput thin films by atomic layer deposition, using the above-described high-throughput thin film preparation apparatus by atomic layer deposition, including the following steps:
[0068] Step 1, determine the key process parameters affecting thin film deposition: the key process parameters include: substrate temperature, types of precursors and co-reactants, pulse time of opening the atomic layer deposition source bottle valve and purge time after closing;
[0069] The substrate temperature (T) is controlled collaboratively by a movable substrate base and a cavity heating system; different types of precursors and co-reactants are selectively provided by the multi-channel atomic layer deposition source 15 and the programmable gas flow valve assembly 16 of the device; the pulse time (t) pulse ) and purging time (t) purge This is achieved by precisely controlling the opening and closing sequence of the gas flow valve through a pre-programmed control system.
[0070] Step 2: Place the substrate in the sample slot of the movable substrate base 14 of the device, and use the mechanical limiting structure at the edge of the sample slot to ensure the positional accuracy of the substrate.
[0071] Step 3: Select the desired target patterned mask 18 and assemble it into the positioning slot of the mask fixing frame; then, drive the mask 18 to move precisely through the programmable mask control system 17 of the device to achieve precise alignment between the mask pattern and the preset deposition area on the substrate.
[0072] Step 4: After setting the substrate temperature, precursor and co-reactant types, pulse time, purge time and deposition cycle number determined in Step 1, start the deposition process and make the spray device 13 of the apparatus start spraying.
[0073] Step 5: After completing the deposition under the current set conditions, the programmable mask control system 17 controls the mask 18 to move to the next preset position according to the predetermined program, adjusts the thin film deposition parameters, and performs deposition of the newly set thin film deposition parameters in the new area on the substrate; or keeps the position of the mask 18 unchanged, changes the thin film deposition parameters, and achieves the growth of a multilayer stacked thin film at the same position on the substrate.
[0074] Step 6: Different metal precursors and co-reactants are sequentially sprayed onto different substrates or different regions of the same substrate using the spray device 13, and growth cycles are set. Combined with mask position programming, high-throughput thin film preparation with programmable composition, thickness, and stacking order is achieved.
[0075] Preferably, the above method further includes:
[0076] According to design requirements, patterned masks with different aperture sizes and arrangements can be replaced; or, different masks can be combined and used simultaneously, and the temporal changes of the displacement sequence of each mask and the ALD source parameters can be controlled in a coordinated manner to perform high-throughput design of the deposition area on the substrate. This improves deposition efficiency, enables rapid deposition of thin film samples under various conditions, and thus completes the efficient screening and optimization of multivariate deposition conditions.
[0077] To more clearly demonstrate the technical solution and its effects provided by the present invention, the following detailed description of the solution provided by the embodiments of the present invention is provided with reference to specific examples.
[0078] Example 1
[0079] like Figure 1 As shown, this embodiment provides a high-throughput thin film fabrication apparatus for atomic layer deposition, including: a combined vacuum chamber (including an outer cavity 11 and an inner cavity 12), a spray device 13, a movable substrate pedestal 14, a multi-channel atomic layer deposition source 15, a programmable gas flow valve assembly 16, a programmable mask control system 17, a replaceable mask 18, and a plasma generator 19; wherein,
[0080] The combined high-vacuum chamber consists of an inner cavity 12 and an outer cavity 11 nested outside the inner cavity, forming a nested combined chamber structure. The inner cavity 12 consists of an upper cavity 121 and a lower cavity 122. The lower cavity 122 can move in coordination with the movable substrate base 14 and can be opened and closed with the upper cavity 121 through controllable movement. When opened, the substrate can be loaded. The outer cavity can be pre-evacuated to a low vacuum state, serving as a pre-buffer zone and leakage barrier for the high vacuum environment of the inner cavity, effectively improving the vacuum holding capacity and ultimate vacuum level of the inner cavity. At the same time, the outer cavity also serves as a thermal insulation layer, reducing the interference of external environmental temperature fluctuations on the stability of the inner cavity's operating temperature.
[0081] The spray device 13 is located at the top of the vacuum cavity and is used to spray atomic layer deposition sources into the cavity. The spray device 13 and related source pipelines are all integrated with a heating device for temperature control of the pipelines and spray heads. Temperature control prevents condensation or residue from occurring during the vaporization and transport of different atomic layer deposition sources, thereby ensuring the purity of the atomic layer deposition sources entering the cavity and avoiding cross-contamination.
[0082] The movable substrate base 14 is disposed in the inner cavity to support and heat the substrate, and is positioned opposite the top spray device 13. The inner cavity provides a high back vacuum and a stable deposition environment. The inner cavity 12 is cylindrical, allowing the vaporized atomic layer deposition source to be sprayed uniformly from top to bottom onto the substrate base, ensuring a uniform flow distribution of the vaporized atomic layer deposition source inside the cavity. The bottom of the movable substrate base 14 integrates a Z-axis precision stepper motor, which can be controllably moved in the vertical direction to precisely adjust the distance between it and the spray device 13. The controllable movement enables the opening and closing of the inner cavity 12 for substrate loading.
[0083] The multi-path atomic layer deposition source 15 includes: multiple precursor source bottles and co-reactants; wherein, each precursor source bottle and connecting pipeline is equipped with an independent temperature control module (including a heating device and a temperature sensor) to maintain the temperature stability of the precursor and prevent condensation or deposit contamination or blockage in the pipeline; the multi-path co-reactants mainly include: ozone (generated by high-purity oxygen through an ozone generator, the power of the ozone generator and the input gas flow rate can be independently adjusted, so as to output ozone with precise and controllable concentration), water vapor, plasma oxygen, etc.
[0084] The programmable gas flow valve assembly 16 is used to quantitatively control the flow rate of the vaporized atomic layer deposition source mixed with the carrier gas. The programmable gas flow valve assembly 16, together with the multi-channel atomic layer deposition source 15, is used to realize the growth of multi-element doped thin films, while the multi-channel, finely tunable co-reactants provide a broad and flexible process space for high-throughput thin film growth, supporting the parallel preparation of complex composition and stacked structure thin films.
[0085] The programmable mask control system 17 is connected to the mask 18 disposed in the inner cavity via a vacuum linear transmission linkage device that penetrates the inner and outer cavity walls. The programmable mask control system 17 employs a programmable displacement controller to drive the mask to make precise displacements within the inner cavity via the vacuum linear transmission linkage device. This system can achieve movement in both the X and Y axes. Movement along each axis is achieved through built-in, independently programmable stepper motors. The vacuum linear transmission linkage device is equipped with a position feedback module, which, combined with a multi-axis cooperative motion control algorithm, performs real-time calculations and adjustments to match the spraying cycle of different atomic layer deposition sources, thereby ensuring that the alignment accuracy between the mask pattern and the substrate meets the preset process requirements.
[0086] The mask 18 is mounted on the vacuum linear transmission linkage of the programmable mask control system 17 via a fixed frame, with a standardized positioning slot in the center of the fixed frame. The replaceable mask 18 has a fixed external dimension that matches the standardized positioning slot, and this mechanical interface constraint ensures high positional repeatability after replacement and assembly. Different mask 18 have specific patterned hole arrays (the size and arrangement of which can be customized) as mask patterns, used to achieve partitioned deposition, multi-component deposition, or parallel deposition of thin films of different thicknesses on the substrate surface in a single process.
[0087] The plasma generator 19 is located at the top of the equipment chamber. The working gas introduced into the chamber forms a stable and uniform plasma under the action of a high-frequency and high-voltage electric field. The plasma is then introduced into the spray device 13 through the gas outlet and sprayed onto the unshielded area on the substrate to react with the atomic layer deposition source deposited on the thin film.
[0088] like Figure 2 The diagram shows a three-dimensional representation of the main structure of the combined high-vacuum cavity and the programmable mask control system, which mainly includes an outer cavity 11, an inner cavity 12, a spray device 13, a movable substrate base 14, a programmable mask control system 17, and a replaceable mask 18.
[0089] like Figure 3 As shown, the specific implementation steps for high-throughput thin film deposition using the above-mentioned device are as follows: First, the substrate is precisely placed in the sample slot on the substrate base 14, ensuring alignment between the substrate and the sample slot to achieve accurate mapping between the substrate coordinates and the programmed mask coordinates, ensuring the accuracy of the deposition area division. Simultaneously, the selected replaceable mask 18 is embedded into the positioning slot of the mask control system. After closing the inner cavity 12 and evacuating to the set back vacuum level, the deposition parameters are set through the program control system, and the system temperature, gas flow rate, and other parameters are allowed to stabilize. Subsequently, the stepper motors of each axis of the program-driven vacuum transmission device move the mask to the initial coordinate position preset by the program. Then, the precursor source type, co-reactant type, deposition temperature T, and precursor pulse time t required for the current deposition area are selected through program control. pulse , purging time t purge The number of deposition cycles is set; deposition is performed after the parameters stabilize. After deposition in the current area is completed, the program control system drives the mask to move to the next target area. The deposition parameters are adjusted according to the required film characteristics (thickness / composition / layer structure) for the new area, and the above deposition process is repeated until the entire preset area of the substrate is covered. After deposition in all areas is completed, programmed cooling is performed. Once the chamber temperature drops to a safe threshold, the vacuum is released and the sample is removed, completing the entire high-throughput film deposition process.
[0090] Example 2
[0091] This embodiment provides a high-throughput thin film preparation method using atomic layer deposition, employing the high-throughput thin film preparation apparatus for atomic layer deposition described in Example 1, such as... Figure 4 , 5 As shown, it includes the following steps:
[0092] 1) A holeless mask is used, and its position is determined by the programmable mask control system 17 to expose only the left 1 / 3 of the substrate (as shown in the attached diagram). Figure 4 Figure A1 shows the arrows in Figure A1, which represent the spraying of vaporized atomic layer deposition sources. In actual growth, these arrows correspond to the individual spraying of atomic layer deposition sources and co-reactants, or, more complexly, the ordered spraying of various oxide component sources. The red rectangles on the substrate represent the thin films formed after the atomic layer deposition sources react with the co-reactants. Preset deposition parameters are executed, including precursor source type, co-reactant type, deposition temperature T, and precursor pulse time t. pulse , purging time t purge And the number of deposition cycles, at which point the precursor can only be deposited in the exposed area and react to form a film on the substrate surface, while no deposition occurs in the shaded area.
[0093] 2) Move the mask to the new coordinates to expose the left 2 / 3 of the substrate (as shown in the attached image). Figure 4 (See Figure B1). A second deposition was performed while keeping the deposition parameters and cycle number constant. The thickness of this deposition in the newly exposed 1 / 3 region was approximately the same as that of the first deposition, while the thickness of the left 1 / 3 region, having undergone two depositions, was approximately the same as that of the two depositions. This achieved a stepped thickness distribution on the substrate surface in a single process.
[0094] 3) Programmatically move the mask to expose the entire substrate area (as shown in the attached image). Figure 4 As shown in Figure C1), a third deposition was performed with the same deposition parameters and number of cycles, ultimately forming a three-tier thickness gradient structure on the substrate surface that increases layer by layer from right to left (the thickness is approximately the thickness obtained from one, two, and three depositions, respectively).
[0095] Based on the above operations, parallel growth of different components and ordered stacked structures can be achieved. For example:
[0096] 1) First, grow a single-component film with three-order thickness gradients (as shown in the attached image). Figure 5 (A2 in the text). Switch the second precursor source type, co-reactant type, deposition temperature T, and precursor pulse time t. pulse , purging time t purge Deposition can be performed using parameters such as the number of deposition cycles, and in conjunction with a mask control system, a second type of precursor gradient deposition can be formed (as shown in the attached figure). Figure 5 (B2 in the text) to achieve high-throughput integrated deposition with dual variables of thickness and composition.
[0097] 2) By repeating the aforementioned high-throughput deposition method with multiple components, and through programmed control of the deposition cycle number, precursor / co-reactant combination, and mask movement path, multilayer heterogeneous stacked structures can be further constructed on existing dual-gradient thin films (as shown in the attached figure). Figure 5 (C2 in the text). The mask configuration design, regional exposure accuracy, deposition parameter settings, and displacement timing are all executed collaboratively by the program control system to achieve efficient preparation of complex thin film materials.
[0098] In this embodiment, the mask configuration, deposition cycle number, precursor combination, and movement path are all supported by a programmable control system, which can customize the construction of thin film materials with arbitrary thickness, multiple components, and stacked structures, significantly improving the research and development efficiency of new materials.
[0099] Example 3
[0100] This embodiment provides a high-throughput thin film fabrication method using atomic layer deposition. It employs the high-throughput thin film fabrication apparatus of Embodiment 1, and is a high-throughput thin film deposition method based on programmable combined masks. Through multi-level mask configuration design and coordinated control, the fabrication efficiency of complex composition gradient thin films is significantly improved. The specific implementation process is shown in the attached figure. Figure 6 As shown, it includes the following steps:
[0101] 1) Two sets of photomasks can be designed and customized (e.g., Figure 6 As shown in the mask plates 61 and 62, their fixed outer dimensions match the positioning slots of the mask plate frame to ensure positional accuracy. Furthermore, the hole structures of each mask plate are distributed differently in shape, position, and size. The two can be used in combination to improve high-throughput efficiency.
[0102] 2) Embed the selected mask into the positioning slot of the mask control system. After the cavity environment stabilizes, perform the first deposition on the entire substrate without using the mask, and form the first thin film using uniform deposition conditions.
[0103] 3) Using mask 61, and controlled by the program, in four deposition areas (corresponding to deposition effects as shown in the image) Figure 6 In Figure 63 (where grayscale represents the thickness of the deposited film), differentiated deposition conditions are set to construct a second type of film with different thicknesses.
[0104] 4) Switch to mask 62 (whose aperture length is equal to the side length of mask 61, and its width is one-sixth of that side length). Through precise program movement, 24 independent deposition regions are formed. Each region completes the deposition of the third type of thin film under different conditions, achieving efficient and high-throughput deposition of three types of thin films and twenty-four regions on the substrate (e.g., deposition effect). Figure 6 (As shown in 64).
[0105] The high throughput efficiency advantage of this embodiment lies in the fact that when preparing a film with a similar heterogeneous structure (containing 24 regions) composed of three thin films, a maskless method would require independent deposition of the three thin films (a total of 72 times), while this method utilizes a synergistic combination of two masks (such as...). Figure 6 Masks 61 and 62 in the image are deposited in parallel during a single load to achieve the same goal.
[0106] Building on this, by expanding the mask combination scheme, the spatiotemporal efficiency of high-throughput thin film deposition can be further optimized by designing and combining a variety of masks.
[0107] The masking effect of the present invention's mask in high-throughput thin film deposition was verified by performing the following steps in conjunction with an atomic layer deposition process:
[0108] 1) A mask is placed in the atomic layer deposition cavity, with part of the substrate in the mask-shaded area and part of the substrate in the unshaded area.
[0109] 2) Using three oxygen source formulations—water (H2O), ozone (O3), and plasma oxygen (O2 plasma)—under standard conditions, hafnium zirconium oxide (Hf) was subjected to treatment. 0.5 Zr 0.5 O2) Thin film is deposited independently.
[0110] 3) After three depositions, the thickness of the deposited film was characterized by X-ray reflectance testing. No film growth was detected on the substrate in the completely shielded area of the mask, while film growth under the corresponding standard conditions was detected on the substrate in the unshielded area. This proves that the mask can completely block the deposition of atomic layer deposition sources and co-reactants, achieving precise regional selectivity of deposition (as shown in Table 1).
[0111] Table 1 presents preliminary verification data on the effect of the mask on the thickness control of the deposited thin film.
[0112]
[0113] In summary, the apparatus and method of this invention, by coordinating and controlling the precise movement of the programmable mask and the pulse delivery of different deposition sources, achieve precise control of the high-throughput thin film deposition process. This enables the parallel deposition of thin films with varying thicknesses, doping concentrations, and stacked structures on multiple substrates at different locations on the substrate pedestal, or in different regions of the same substrate. This apparatus facilitates rapid screening of deposition conditions, significantly improving the efficiency of thin film material development.
[0114] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims. The information disclosed in the background section is intended only to enhance the understanding of the overall background technology of the present invention and should not be construed as an admission or implication in any way that such information constitutes prior art known to those skilled in the art.
Claims
1. A high-throughput thin film preparation apparatus for atomic layer deposition, characterized in that, include: The combined vacuum chamber consists of an inner cavity (12) and an outer cavity (11) nested outside the inner cavity (12); The outer cavity (11) is provided with an electrically movable cavity door, which can be electrically controlled to open or close to realize the loading and unloading of the substrate; The inner cavity (12) includes an upper cavity (121) and a lower cavity (122) that can be opened and closed. A spray device (13) is provided in the upper part of the upper cavity (121). The spray device (13) can spray an atomic layer deposition source into the lower part of the inner cavity (12). A movable substrate base (14) is fixedly provided in the bottom of the lower cavity (122). The movable substrate base (14) can support and heat the substrate (22). The position of the movable substrate base (14) corresponds to the spray device (13). The movable substrate base (14) is fixedly disposed in the lower cavity (122); the driving device is connected to the lower cavity (122) for driving the lower cavity (122) and the movable substrate base (14) to move synchronously in the vertical direction, so as to adjust the distance between the movable substrate base (14) and the spray device (13), and to switch the lower cavity (122) relative to the upper cavity (121) between the closed position and the substrate loading position; The upper cavity (121) is provided with a plasma inlet at its top, and the plasma inlet extends out of the outer cavity; The input pipeline (20) has its outlet end connected to the spray device (13) at the top of the inner cavity (12), and its inlet end extends to the outside of the outer cavity (11). It is provided with a carrier gas inlet that can be connected to the carrier gas source (21) and a deposition source inlet that can be connected to the vaporized atomic layer deposition source. A mask (18) is disposed in the inner cavity (12) and above the substrate supported by the movable substrate base (14). The mask (18) is fixedly connected to a programmable mask control system (17) disposed outside the outer cavity (11) and can move precisely above the substrate (22) under the drive and control of the programmable mask control system (17).
2. The high-throughput thin film preparation apparatus for atomic layer deposition according to claim 1, characterized in that, Also includes: Carrier gas source (21), programmable gas flow valve assembly (16), and multi-channel atomic layer deposition source (15); The carrier gas source (21) is connected to the carrier gas inlet of the input pipeline (20); The multi-channel atomic layer deposition source (15) is connected to the deposition source inlet of the input pipeline (20) via the programmable gas flow valve assembly (16), and the flow rate of the vaporized atomic layer deposition source mixed with the carrier gas can be quantitatively controlled by the programmable gas flow valve assembly (16).
3. The high-throughput thin film preparation apparatus for atomic layer deposition according to claim 2, characterized in that, The sedimentation source inlet has multiple inlets, each of which is connected to the carrier gas inlet; The multi-path atomic layer deposition source (15) includes multiple precursor source bottles and multiple co-reactants, which are respectively connected to multiple input ports. Each precursor source bottle and connecting pipeline is equipped with an independent temperature control module. The independent temperature control module can maintain the stability of the precursor temperature and prevent condensation, deposit contamination or blockage in the pipeline.
4. The high-throughput thin film preparation apparatus for atomic layer deposition according to any one of claims 1-3, characterized in that, Also includes: A plasma generator (19) is located at the top of the outer cavity (11). The plasma outlet of the plasma generator (19) is sealed to the plasma inlet at the top of the upper cavity (121), and is connected to the spray device (13) in the inner cavity (12) through the plasma inlet.
5. The high-throughput thin film preparation apparatus for atomic layer deposition according to any one of claims 1-3, characterized in that, The movable substrate base (14) is provided with a sample groove that can precisely limit the position of the substrate; The mask (18) is installed and fixed by the positioning slot of the mask fixing frame, and more than one mask (18) can be installed in the positioning slot. The input pipeline is equipped with a heating device, which can control the temperature of the input pipeline.
6. The high-throughput thin film preparation apparatus for atomic layer deposition according to any one of claims 1-3, characterized in that, The spray device (13) adopts a pulse spray equipment; The spray device (13) and related source pipelines are all integrated with heating devices, which can control the temperature of the source pipelines and spray heads. The electrically operated sliding door on the outer cavity (11) includes: a door body, a drive mechanism, and a position detection component; wherein the door body is installed on the outer cavity (11). The electric drive mechanism is connected to the door body and can drive the door body to move between the open position and the closed position. The position detection element is disposed on the outer cavity (11) and can detect the open and closed states of the door; the drive mechanism can act according to the position signal fed back by the position detection element to stop the door in the open or closed position.
7. The high-throughput thin film preparation apparatus for atomic layer deposition according to any one of claims 1-3, characterized in that, The programmable mask control system (17) adopts a programmable displacement controller. The programmable displacement controller is fixedly connected to the mask (18) through a vacuum linear transmission linkage device. It can drive the mask (18) to make precise displacement in the horizontal plane above the substrate (22) in the inner cavity (12) to match the spraying cycle of different atomic layer deposition sources. The drive device uses a Z-axis precision stepper motor.
8. A method for preparing high-throughput thin films by atomic layer deposition, characterized in that, The high-throughput thin film fabrication apparatus using atomic layer deposition according to any one of claims 1-7 includes the following steps: Step 1: Determine the key process parameters that affect thin film deposition. The key process parameters include: substrate temperature, types of precursors and co-reactants, pulse time of opening the atomic layer deposition source bottle valve, and purge time after closing the valve. Step 2: Place the substrate in the sample slot of the movable substrate base (14) of the device, and use the mechanical limiting structure at the edge of the sample slot to ensure the positional accuracy of the substrate. Step 3: Select the desired target patterned mask (18) and assemble it into the positioning slot of the mask fixing frame; then, drive the mask (18) to move precisely through the programmable mask control system (17) of the device to achieve precise alignment between the mask pattern and the preset deposition area on the substrate; Step 4: After setting the substrate temperature, precursor and co-reactant types, pulse time, purge time and deposition cycle number determined in Step 1, start the deposition process and make the spray device (13) of the device start spraying. Step 5: After completing the deposition under the current set conditions, the mask (18) is moved to the next preset position by the programmable mask control system (17) according to the predetermined program. The thin film deposition parameters are adjusted, and the new area on the substrate is deposited according to the newly set thin film deposition parameters; or the position of the mask (18) is kept unchanged, the thin film deposition parameters are changed, and the growth of the stacked sequence thin film is achieved at the same position on the substrate. Step 6: For different substrates or different regions of the same substrate, different metal precursors and co-reactants are sequentially sprayed by the spray device (13), and the deposition cycle number is set. Combined with the mask position programming, high-throughput thin film preparation with programmable composition, thickness and stacking order is realized.
9. The high-throughput thin film preparation method of atomic layer deposition according to claim 8, characterized in that, Also includes: Replace with patterned masks of different apertures and arrangements as required by the design. Alternatively, different masks can be used simultaneously, and the displacement sequence of each mask and the temporal changes of the ALD source parameters can be controlled in a coordinated manner to perform high-throughput design of the deposition area on the substrate.
10. The high-throughput thin film preparation method of atomic layer deposition according to claim 8 or 9, characterized in that, The substrate temperature is controlled by the movable substrate base (14) and the cavity heating system in coordination; different types of precursors and co-reactants are provided by the multi-channel atomic layer deposition source (15) and the programmable gas flow valve assembly (16) of the device in combination; the pulse time and purge time are achieved by the precise control of the opening and closing sequence of each programmable gas flow valve through a predetermined control program integrated inside the programmable gas flow valve assembly (16).