A nickel plating process for laser welding aluminum alloy welding wire

By combining a self-made zinc citrate and citrate-phenylphosphonate nickel composite complex solution with a multi-step pretreatment process, the problem of high surface reflectivity of aluminum alloy welding wire was solved, achieving uniformity and adhesion of the coating, improving welding efficiency and quality, and making it suitable for aerospace, automobile manufacturing and rail transportation fields.

CN123108541APending Publication Date: 2026-11-17SHANDONG SHISHANG WELDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611602054.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Aluminum alloy welding wire has a high surface gloss, which strongly reflects the laser beam, resulting in insufficient penetration, low welding efficiency, and unstable weld quality. Existing nickel plating processes have problems such as incomplete removal of oxide film, poor coating adhesion, and unstable plating solution.

Method used

A nickel plating process for aluminum alloy welding wire was prepared by using a self-made zinc citrate and citrate-phenylphosphonate nickel composite complex solution, combined with degreasing, activation, brightening, zinc immersion and zinc stripping processes. By controlling the coating thickness and plating solution composition, the uniformity and adhesion of the coating were improved.

Benefits of technology

It significantly improves the adhesion and uniformity of the coating, increases the laser absorption rate of the weld, and enhances welding efficiency and weld formation quality, making it suitable for aerospace, automotive manufacturing, and rail transportation industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_28
    Figure SMS_28
  • Figure SMS_29
    Figure SMS_29
Patent Text Reader

Abstract

This invention discloses a nickel plating process for laser-welded aluminum alloy welding wire, belonging to the field of welding wire nickel plating technology. The process includes preparing zinc citrate by adding zinc oxide to a solution of citric acid monohydrate, followed by reaction, sieving, concentration, and drying; reacting nickel sulfate hexahydrate with sodium carbonate, washing the filter cake, and reacting it with a mixture of citric acid and phenylphosphonic acid to prepare a composite complex solution; sequentially degreasing, activating, and brightening the aluminum alloy welding wire; then performing zinc immersion, zinc stripping, and a second zinc immersion before being immersed in a nickel plating solution for plating; and finally, hot water treatment followed by drying and winding. This invention combines three pretreatment steps (degreasing, activation, and brightening) with zinc immersion, zinc stripping, and a second zinc immersion process, and introduces self-made zinc citrate into the zinc immersion solution, resulting in a zinc layer thickness variation coefficient as low as 3.0-3.6%, a coating peeling and detachment area ratio of only 0.6-1.5%, and a coating porosity as low as 6-18 cells / dm². 2 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nickel plating technology for welding wire, and specifically to a nickel plating process for the surface of laser welding aluminum alloy welding wire. Background Technology

[0002] Laser welding offers advantages such as concentrated heat input, a small heat-affected zone, high welding speed, and excellent weld formation, making it widely used in aerospace, automotive manufacturing, and rail transportation. Aluminum alloys, due to their low density, high specific strength, and good corrosion resistance, are core materials for lightweight structures. Using laser welding wire on aluminum alloys can achieve hydrogen vaporization and diffusion, increase weld penetration, and improve weld formation quality, resulting in significant engineering value.

[0003] However, aluminum alloy welding wire has a high surface gloss and strong reflection of the laser beam. Laser welding relies on the workpiece to absorb the heat source of the laser beam to achieve melting. However, the aluminum alloy surface has an absorption rate of less than 10% of the heat source of the laser beam, and a large amount of energy is reflected and lost, resulting in insufficient penetration, low welding efficiency, and unstable weld quality, which seriously restricts the large-scale application of aluminum alloy laser welding.

[0004] To reduce reflectivity, existing technologies attempt to plate nickel on the surface of aluminum alloy welding wire. However, problems include incomplete removal of the oxide film on the aluminum alloy surface, poor coating adhesion, and easy peeling. The thickness of the zinc plating layer is difficult to control in the pretreatment process, which directly affects the quality of subsequent nickel plating. Improper ratio of nickel salt and reducing agent in the plating solution leads to large fluctuations in the phosphorus content of the coating and unstable deposition rate, making it difficult to meet the strict requirements of laser welding for coating uniformity and absorption rate.

[0005] Based on this, the present invention designs a nickel plating process for the surface of laser welding aluminum alloy welding wire to solve the above problems. Summary of the Invention

[0006] To address the aforementioned shortcomings of existing technologies, this invention provides a nickel plating process for the surface of laser-welded aluminum alloy welding wire, comprising the following steps:

[0007] S1: Dissolve citric acid monohydrate in water to prepare an aqueous citric acid solution, add zinc oxide, heat and stir to react, sieve, collect the filtrate, concentrate and dry the filtrate to obtain zinc citrate;

[0008] S2: Nickel sulfate hexahydrate is dissolved in water to prepare an aqueous solution of nickel sulfate. An aqueous solution of sodium carbonate is added to react and a reaction mixture is obtained. The reaction mixture is centrifuged and the supernatant is discarded. The filter cake is collected and washed. Then it is reacted with a mixed acid aqueous solution composed of citric acid and phenylphosphonic acid to obtain a citric acid-phenylphosphonate nickel complex solution.

[0009] S3: Pass the aluminum alloy welding wire through degreasing solution, deionized water rinsing, activation solution, deionized water rinsing, brightening solution, and deionized water rinsing in sequence.

[0010] S4: The aluminum alloy welding wire treated in S3 is continuously passed through a zinc immersion solution, rinsed with deionized water, then continuously passed through a zinc stripping solution, rinsed with water, and then immersed in zinc again and rinsed with water; the zinc immersion solution is composed of zinc oxide, zinc citrate, sodium hydroxide, potassium sodium tartrate, ferric chloride hexahydrate and sodium nitrate.

[0011] S5: The aluminum alloy welding wire treated in S4 is continuously plated through a nickel plating solution, rinsed with water, then treated with hot water, dried and cooled to room temperature, and then wound up; the nickel plating solution is composed of a citrate-phenylphosphonate nickel complex solution, nickel sulfate hexahydrate, sodium citrate and sodium hypophosphite.

[0012] Furthermore, citric acid monohydrate is dissolved in deionized water to prepare a citric acid aqueous solution with a mass fraction of 30-50%. Zinc oxide is added to the citric acid solution at a molar ratio of zinc oxide to citric acid of 1:2-2.5. The solution is then heated to 60-90℃ and stirred at 150-300 r / min for 1-3 h. The solution is passed through a 200-400 mesh sieve, and the filtrate is collected. The filtrate is concentrated under reduced pressure at 60-80℃ and -0.095 to -0.08 MPa to 1 / 3-1 / 2 of its original volume. Then it is dried at 60-80℃ for 6-12 h to obtain zinc citrate for later use.

[0013] Furthermore, nickel sulfate hexahydrate is dissolved in deionized water to prepare a nickel sulfate aqueous solution with a concentration of 0.5-1.5 mol / L. A sodium carbonate aqueous solution (mass fraction 10-20%) with a nickel sulfate hexahydrate to sodium carbonate molar ratio of 1:1-1.2 is added to the nickel sulfate aqueous solution at 200-300 r / min over a period of 15-30 min. After all the ingredients are added, stirring is continued for 20-60 min to obtain the reaction mixture.

[0014] Centrifuge the reaction mixture, discard the supernatant, collect the filter cake, and wash it 2-3 times with 3-5 times the volume of deionized water at 60-80℃ for 3-4 minutes each time. Then transfer it to a reaction vessel and add a 20-40% (w / w) mixed acid aqueous solution (composed of citric acid and phenylphosphonic acid in a molar ratio of 1:0.3-1) at a molar ratio of nickel carbonate to total acid (the sum of the molar numbers of citric acid and gluconic acid) of 1:1.5-2.5. Stir at 200-300 r / min at ≤50℃ for 25-40 minutes, then raise the temperature to 60-90℃ and continue stirring for 1-3 hours. Pass the solution through a 200-400 mesh sieve to obtain a citric acid-nitrophenylphosphonate complex solution for later use.

[0015] Furthermore, the aluminum alloy welding wire is passed through the following treatment tanks sequentially at a constant linear speed. The aluminum alloy welding wire is continuously passed through the degreasing solution and treated at 40-55℃ for 3-6 minutes, then rinsed with deionized water for 15-30 seconds. Subsequently, it is continuously passed through the activation solution and treated at 25-40℃ for 10-30 seconds, then rinsed with deionized water for 15-30 seconds. Finally, it is continuously passed through the brightening solution and treated at room temperature for 5-15 seconds, then rinsed with deionized water for 15-30 seconds.

[0016] Furthermore, the degreasing solution is composed of 20-30 g / L sodium carbonate, 8-15 g / L trisodium phosphate, and 0.5-1.5 g / L sodium dodecyl sulfate;

[0017] Furthermore, the activation solution is composed of 15-30 g / L sodium hydroxide and 3-10 g / L sodium citrate dihydrate;

[0018] Furthermore, the light-emitting solution is composed of 100-200 mL / L nitric acid aqueous solution (mass fraction 65-68%) and 50-100 mL / L sulfuric acid aqueous solution (mass fraction 95-98%).

[0019] Furthermore, the S3-treated aluminum alloy welding wire is continuously passed through a zinc immersion solution, immersing in zinc at room temperature for 20-40 seconds, rinsing with deionized water for 15-30 seconds, and then continuously passed through a zinc stripping solution composed of 150-300 mL / L concentrated nitric acid (mass fraction 65-68%), stripping zinc at room temperature for 10-20 seconds, rinsing with deionized water for 15-30 seconds, and then immersing in zinc again for 10-25 seconds, rinsing with deionized water for 15-30 seconds.

[0020] Furthermore, the zinc immersion solution is composed of 60-100 g / L zinc oxide, 5-20 g / L zinc citrate, 400-500 g / L sodium hydroxide, 20-40 g / L potassium sodium tartrate, 1-2 g / L ferric chloride hexahydrate and 1-2 g / L sodium nitrate;

[0021] Furthermore, the S4-treated aluminum alloy welding wire is continuously plated in a nickel plating solution (pH 8.2-8.8) at 82-88℃ for 10-30 minutes, rinsed with deionized water for 20-40 seconds, then treated with deionized water at 80-95℃ for 20-60 seconds, dried at 40-60℃ for 10-30 minutes, cooled to room temperature, and then wound up.

[0022] Furthermore, the nickel plating solution is composed of a 3-5 g / L citrate-phenylphosphonate nickel complex solution (based on nickel), 30-43 g / L nickel sulfate hexahydrate, 45-55 g / L sodium citrate, and 15-25 g / L sodium hypophosphite.

[0023] Compared with the prior art, the beneficial effects of this invention are as follows:

[0024] 1. This invention combines three pretreatment steps—degreasing, activation, and brightening—with zinc immersion, zinc stripping, and a second zinc immersion process. Furthermore, it introduces self-made zinc citrate into the zinc immersion solution, resulting in a zinc layer thickness variation coefficient as low as 3.0-3.6%, a coating peeling / detachment area ratio of only 0.6-1.5%, and a coating porosity as low as 6-18 cells / dm². 2 This effectively solves the technical problems of incomplete removal of oxide film on aluminum alloy surface and difficulty in controlling the thickness of zinc plating layer, which lead to poor coating adhesion and easy peeling.

[0025] 2. This invention uses a self-made citrate-phenylphosphonate nickel composite as the nickel source for the nickel plating solution, combined with nickel sulfate, sodium citrate and sodium hypophosphite, to maintain the transmittance of the plating solution at 91.0-94.8% for 8 hours, stabilize the deposition rate at 14.8-17.2 μm / h, and reduce the phosphorus content fluctuation to only 0.22-0.32 wt%. Under continuous wire drawing conditions, the coefficient of variation of nickel layer thickness is as low as 3.8-5.0%, effectively overcoming the defects of existing plating solutions caused by improper ratio of nickel salt and reducing agent, such as easy decomposition of the plating solution, unstable deposition rate, and large fluctuations in plating composition and thickness.

[0026] 3. The nickel-plated aluminum alloy welding wire prepared by this invention has a coating hardness of 535-558HV0.1, and the time for the first appearance of rust in the neutral salt spray test is 86-132 hours. The absorption rate of 1064nm wavelength laser is increased to 33.0-38.5%, which is more than 280% higher than that of bare aluminum welding wire. The proportion of defect-free effective length of weld is 94.8-98.5%, which significantly reduces laser reflection loss, increases weld penetration, and improves welding efficiency and weld formation quality. It is suitable for laser welding of aluminum alloys in aerospace, automobile manufacturing, rail transportation and other fields. Detailed Implementation

[0027] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0028] Example 1: This example provides a nickel plating process for the surface of laser welding aluminum alloy welding wire, including the following steps:

[0029] S1: Dissolve citric acid monohydrate in deionized water to prepare a 50% citric acid aqueous solution. Add zinc oxide to the citric acid solution at a molar ratio of zinc oxide to citric acid of 1:2.5. Then heat to 90°C and stir at 300 r / min for 3 h. Pass through a 400-mesh sieve and collect the filtrate. Concentrate the filtrate under reduced pressure at 80°C and -0.08 MPa to half of the original volume. Then dry at 80°C for 12 h to obtain zinc citrate for later use.

[0030] S2: Dissolve nickel sulfate hexahydrate in deionized water to prepare a nickel sulfate aqueous solution with a concentration of 1.5 mol / L. Add a sodium carbonate aqueous solution (mass fraction 20%) with a nickel sulfate hexahydrate to sodium carbonate in a molar ratio of 1:1.2 at 300 r / min to the nickel sulfate aqueous solution. The addition time is 30 min. After all the materials are added, continue stirring for 60 min to obtain the reaction mixture.

[0031] Centrifuge the reaction mixture, discard the supernatant, collect the filter cake, and wash it three times with 80°C deionized water (5 times the volume of the filter cake) for 4 min each time. Then transfer it to a reaction vessel and add a 40% (w / w) mixed acid aqueous solution (composed of citric acid and phenylphosphonic acid in a 1:1 molar ratio) at a ratio of nickel carbonate to total acid (the sum of the molar numbers of citric acid and gluconic acid) of 1:2.5. Stir at 300 r / min for 40 min at ≤50°C, then raise the temperature to 90°C and continue stirring for 3 h. Pass the solution through a 400-mesh sieve to obtain a citric acid-nitrophenylphosphonate complex solution for later use.

[0032] S3: The aluminum alloy welding wire is passed through the following treatment tanks in sequence at a constant linear speed. The aluminum alloy welding wire is continuously passed through the degreasing liquid and treated at 55°C for 6 minutes. It is then rinsed with deionized water for 30 seconds. Subsequently, it is continuously passed through the activation liquid and treated at 40°C for 30 seconds. It is then rinsed with deionized water for 30 seconds. Finally, it is continuously passed through the brightening liquid and treated at room temperature for 15 seconds. It is then rinsed with deionized water for 30 seconds.

[0033] The degreasing solution consists of 30 g / L sodium carbonate, 15 g / L trisodium phosphate, and 1.5 g / L sodium dodecyl sulfate;

[0034] The activation solution consists of 30 g / L sodium hydroxide and 10 g / L sodium citrate dihydrate;

[0035] The light-emitting solution is composed of 200 mL / L nitric acid aqueous solution (68% by mass) and 100 mL / L sulfuric acid aqueous solution (98% by mass);

[0036] S4: The aluminum alloy welding wire treated with S3 is continuously passed through zinc immersion solution, zinc immersion at room temperature for 40s, rinsed with deionized water for 30s, and then continuously passed through zinc stripping solution composed of 300mL / L concentrated nitric acid (mass fraction 68%), zinc stripping at room temperature for 20s, rinsed with deionized water for 30s, then zinc immersion again for 25s, and rinsed with deionized water for 30s.

[0037] The zinc immersion solution consists of 100 g / L zinc oxide, 20 g / L zinc citrate, 500 g / L sodium hydroxide, 40 g / L potassium sodium tartrate, 2 g / L ferric chloride hexahydrate, and 2 g / L sodium nitrate.

[0038] S5: The aluminum alloy welding wire treated with S4 is continuously plated in nickel plating solution (pH 8.2-8.8) at 88℃ for 30 minutes, rinsed with deionized water for 40 seconds, then treated with deionized water at 95℃ for 60 seconds, dried at 60℃ for 30 minutes, cooled to room temperature, and then wound up.

[0039] The nickel plating solution consists of a 5 g / L citrate-phenylphosphonate nickel complex solution (based on nickel), a 43 g / L nickel sulfate hexahydrate, a 55 g / L sodium citrate, and a 25 g / L sodium hypophosphite.

[0040] Example 2: This example provides a nickel plating process for the surface of laser welding aluminum alloy welding wire, including the following steps:

[0041] S1: Dissolve citric acid monohydrate in deionized water to prepare a 30% citric acid aqueous solution. Add zinc oxide to the citric acid solution at a molar ratio of zinc oxide to citric acid of 1:2. Then heat to 60°C and stir at 150 r / min for 1 h. Pass the solution through a 200-mesh sieve and collect the filtrate. Concentrate the filtrate under reduced pressure at 60°C and -0.095 MPa to 1 / 3 of the original volume. Then dry at 60°C for 6 h to obtain zinc citrate for later use.

[0042] S2: Dissolve nickel sulfate hexahydrate in deionized water to prepare a nickel sulfate aqueous solution with a concentration of 0.5 mol / L. Add a sodium carbonate aqueous solution (mass fraction 10%) with a nickel sulfate hexahydrate to sodium carbonate in a molar ratio of 1:1 at 200 r / min. The addition time is 15 min. After all the materials are added, continue stirring for 20 min to obtain the reaction mixture.

[0043] Centrifuge the reaction mixture, discard the supernatant, collect the filter cake, and wash it twice with 3 times the volume of deionized water at 60°C for 3 min each time. Then transfer it to a reaction vessel and add a 20% (w / w) mixed acid aqueous solution (composed of citric acid and phenylphosphonic acid in a molar ratio of 1:0.3) at a molar ratio of nickel carbonate to total acid (the sum of the molar numbers of citric acid and gluconic acid). Stir at 200 r / min for 25 min at ≤50°C, then raise the temperature to 60°C and continue stirring for 1 h. Pass the solution through a 200-mesh sieve to obtain a citric acid-nitrophenylphosphonate complex solution for later use.

[0044] S3: Pass the aluminum alloy welding wire through the following treatment tanks in sequence at a constant linear speed. The aluminum alloy welding wire passes through the degreasing liquid continuously, is treated at 40°C for 3 minutes, rinsed with deionized water for 15 seconds, then passes through the activation liquid continuously, is treated at 25°C for 10 seconds, rinsed with deionized water for 15 seconds, then passes through the brightening liquid continuously, is treated at room temperature for 5 seconds, and rinsed with deionized water for 15 seconds.

[0045] The degreasing solution consists of 20 g / L sodium carbonate, 8 g / L trisodium phosphate, and 0.5 g / L sodium dodecyl sulfate;

[0046] The activation solution consists of 15 g / L sodium hydroxide and 3 g / L sodium citrate dihydrate;

[0047] The light-emitting solution is composed of 100 mL / L nitric acid aqueous solution (65% by mass) and 50 mL / L sulfuric acid aqueous solution (95% by mass);

[0048] S4: The aluminum alloy welding wire treated with S3 is continuously passed through the zinc immersion solution, immersed in zinc for 20s at room temperature, rinsed with deionized water for 15s, and then continuously passed through the zinc stripping solution composed of 150mL / L concentrated nitric acid (mass fraction 65%), zinc stripping for 10s at room temperature, rinsed with deionized water for 15s, then immersed in zinc again for 10s, and rinsed with deionized water for 15s.

[0049] The zinc immersion solution consists of 60 g / L zinc oxide, 5 g / L zinc citrate, 400 g / L sodium hydroxide, 20 g / L potassium sodium tartrate, 1 g / L ferric chloride hexahydrate and 1 g / L sodium nitrate.

[0050] S5: The aluminum alloy welding wire treated with S4 is continuously plated in nickel plating solution (pH 8.2-8.8) at 82℃ for 10 minutes, rinsed with deionized water for 20 seconds, then treated with deionized water at 80℃ for 20 seconds, dried at 40℃ for 10 minutes, cooled to room temperature, and then wound up.

[0051] The nickel plating solution consists of a 3 g / L citrate-phenylphosphonate nickel complex solution (based on nickel), a 30 g / L nickel sulfate hexahydrate, a 45 g / L sodium citrate, and a 15 g / L sodium hypophosphite.

[0052] Example 3: This example provides a nickel plating process for the surface of laser welding aluminum alloy welding wire, including the following steps:

[0053] S1: Dissolve citric acid monohydrate in deionized water to prepare a citric acid aqueous solution with a mass fraction of 45%. Add zinc oxide to the citric acid solution at a molar ratio of zinc oxide to citric acid of 1:2.5. Then heat to 70°C and stir at 200 r / min for 2 h. Pass through a 200 mesh sieve and collect the filtrate. Concentrate the filtrate under reduced pressure at 75°C and -0.09 MPa to 1 / 3 of the original volume. Then dry at 70°C for 8 h to obtain zinc citrate for later use.

[0054] S2: Dissolve nickel sulfate hexahydrate in deionized water to prepare a nickel sulfate aqueous solution with a concentration of 0.9 mol / L. Add a sodium carbonate aqueous solution (mass fraction 15%) with a nickel sulfate hexahydrate to sodium carbonate molar ratio of 1:1.2 at 220 r / min. The addition time is 20 min. After all the materials are added, continue stirring for 30 min to obtain the reaction mixture.

[0055] Centrifuge the reaction mixture, discard the supernatant, collect the filter cake, and wash it three times with 5 times the volume of deionized water at 65°C for 3 minutes each time. Then transfer it to a reaction vessel and add a 25% (w / w) mixed acid aqueous solution (composed of citric acid and phenylphosphonic acid in a molar ratio of 1:0.5) at a molar ratio of nickel carbonate to total acid (the sum of the molar numbers of citric acid and gluconic acid). Stir at 240 r / min for 30 minutes at ≤50°C, then raise the temperature to 70°C and continue stirring for 2 hours. Pass the solution through a 200-mesh sieve to obtain a citric acid-nitrophenylphosphonate complex solution for later use.

[0056] S3: Pass the aluminum alloy welding wire through the following treatment tanks in sequence at a constant linear speed. The aluminum alloy welding wire passes through the degreasing liquid continuously, is treated at 50°C for 5 minutes, rinsed with deionized water for 20 seconds, then passes through the activation liquid continuously, is treated at 30°C for 30 seconds, rinsed with deionized water for 30 seconds, then passes through the brightening liquid continuously, is treated at room temperature for 10 seconds, and rinsed with deionized water for 20 seconds.

[0057] The degreasing solution consists of 25 g / L sodium carbonate, 9 g / L trisodium phosphate, and 1.2 g / L sodium dodecyl sulfate;

[0058] The activation solution consists of 20 g / L sodium hydroxide and 5 g / L sodium citrate dihydrate;

[0059] The light-emitting solution is composed of 180 mL / L nitric acid aqueous solution (65% by mass) and 60 mL / L sulfuric acid aqueous solution (96% by mass);

[0060] S4: The aluminum alloy welding wire treated with S3 is continuously passed through the zinc immersion solution, immersed in zinc for 30s at room temperature, rinsed with deionized water for 20s, and then continuously passed through the zinc stripping solution composed of 200mL / L concentrated nitric acid (mass fraction 65%), zinc stripping for 15s at room temperature, rinsed with deionized water for 30s, then immersed in zinc again for 20s, and rinsed with deionized water for 20s.

[0061] The zinc immersion solution consists of 90 g / L zinc oxide, 8 g / L zinc citrate, 420 g / L sodium hydroxide, 25 g / L potassium sodium tartrate, 1.8 g / L ferric chloride hexahydrate and 1.6 g / L sodium nitrate.

[0062] S5: The aluminum alloy welding wire treated with S4 is continuously plated in nickel plating solution (pH 8.2-8.8) at 86℃ for 15 minutes, rinsed with deionized water for 30 seconds, then treated with deionized water at 90℃ for 30 seconds, dried at 45℃ for 20 minutes, cooled to room temperature, and then wound up.

[0063] The nickel plating solution consists of a 5 g / L citrate-phenylphosphonate nickel complex solution (based on nickel), a 38 g / L nickel sulfate hexahydrate, a 51 g / L sodium citrate, and a 19 g / L sodium hypophosphite.

[0064] Comparative Example 1: The difference between this comparative example and Example 3 is that zinc citrate in the zinc immersion solution is replaced with an equimolar amount of zinc oxide, while keeping the total zinc concentration of the zinc immersion solution unchanged.

[0065] Comparative Example 2: The difference between this comparative example and Example 3 is that, in S2, when preparing the mixed acid aqueous solution, phenylphosphonic acid was removed and replaced entirely with equimolar citric acid, while keeping the total molar amount of acid constant, to obtain a single nickel citrate complex solution.

[0066] Comparative Example 3: The difference between this comparative example and Example 3 is that the zinc stripping and secondary zinc immersion processes are removed in S4, and the welding wire after S3 is only immersed in zinc once for 30 seconds. After rinsing, it directly enters the nickel plating process in S5.

[0067] Comparative Example 4: The difference between this comparative example and Example 3 is that the brightening liquid treatment step is removed in S3. After the welding wire is treated with activation liquid and rinsed with deionized water, it directly enters the zinc immersion process in S4.

[0068] Comparative Example 5: The difference between this comparative example and Example 3 is that the citrate-phenylphosphonate nickel complex component was removed from the S5 nickel plating solution, and an equal molar amount of nickel sulfate hexahydrate was added to maintain the total nickel concentration of the plating solution unchanged.

[0069] Experimental Example 1: Referring to the definition, calculation rules, and test constraints of the deposition rate parameter specified in GB / T 13913-2008, the average thickness of the nickel-phosphorus alloy coating was measured on the welding wire sample processed by the process of this invention according to GB / T 6462-2025. The actual plating time of the sample was recorded, and the coating deposition rate (μm / h) was calculated according to the following formula:

[0070]

[0071] in, For coating deposition rate, The average thickness (μm) of the nickel-phosphorus alloy coating. The actual plating time (h) for the sample.

[0072] Experimental Example 2: According to GB / T 6462-2025, the local thickness of the zinc layer of the welding wire sample after the secondary zinc immersion process of this invention was measured. The measuring points were evenly distributed along the circumference of the welding wire cross-section (8 points) to obtain the original thickness data of the zinc layer at each measuring point. The coefficient of variation (%) of the zinc layer thickness was calculated according to the following formula:

[0073]

[0074]

[0075]

[0076] in, The arithmetic mean of the zinc plating thickness (μm) The measured thickness (μm) of the zinc plating layer at the i-th measuring point. Number of effective measurement points (dimensionless) Standard deviation (μm) of zinc plating thickness for the sample. This represents the coefficient of variation for the zinc plating layer thickness.

[0077] Experimental Example 3: According to GB / T 5270-2024, a cross-cut adhesion test was conducted on nickel-plated welding wire samples prepared using the process of this invention. After the test, images of the cross-cut test area were acquired, and the total test area of ​​the cross-cut grid and the area of ​​plating peeling off within the cross-cut area were obtained. The percentage of plating peeling off area was calculated using the following formula:

[0078]

[0079] in, The percentage of the area where the coating has peeled off. The area of ​​coating peeling off within the gridded area (mm) 2 ), Total test area of ​​the grid (mm²) 2 ).

[0080] Experimental Example 4: According to the phosphorus content detection method in GB / T 13913-2008, samples were taken from the nickel-plated welding wire prepared by the process of this invention. Five parallel samples were set up in each group, and the phosphorus mass fraction of the coating of each sample was measured. Five groups of measured phosphorus mass fraction data were obtained, and the range of fluctuation of phosphorus content in the coating (wt%) was calculated according to the following formula:

[0081]

[0082] in, The phosphorus content of the coating fluctuates extremely poorly. The maximum phosphorus mass fraction (wt%) of the 5 parallel samples. The minimum phosphorus mass fraction (wt%) among the 5 parallel samples.

[0083] Experimental Example 5: According to GB / T 9721-2006, the transmittance (%) of the nickel plating working solution prepared according to the process of this invention was measured at the initial stage and after 8 hours, using deionized water as a reference and a visible light wavelength of 600nm.

[0084] Experimental Example 6: According to GB / T 17721-1999, an iron reagent drop test was conducted on the nickel-plated welding wire sample prepared by the process of this invention. The total number of pore spots appearing within the specified test area was counted, and the porosity of the coating (number of spots / dm²) was directly obtained according to the area conversion relationship built into the standard. 2 ).

[0085] Experimental Example 7: The spectral reflectance of the nickel-plated welding wire sample prepared according to the process of this invention was measured using a near-infrared spectrometer equipped with an integrating sphere attachment at a commonly used laser welding wavelength of 1064 nm, in accordance with GB / T 6040-2019. Simultaneously, the surface roughness (μm) of the same sample was measured according to GB / T 6062-2009. The roughness was only used as a recording parameter and did not participate in the calculation. Based on the principle of energy conservation in opaque materials, the laser absorption rate (%) of the welding wire was calculated using the following formula:

[0086]

[0087] in, For laser absorption rate, The spectral reflectance (%) of the sample was measured at a wavelength of 1064 nm.

[0088] Experimental Example 8: Welded samples prepared using the welding wire of this invention and a unified fixed laser welding process were subjected to radiographic testing according to GB / T 3323. The total length of the inspected weld and the total length of the defect-free section inside the weld were measured. The percentage of the effective length of the defect-free section was calculated using the following formula:

[0089]

[0090] in, The percentage of defect-free effective length of weld, The total length (mm) of the defect-free section of the weld. The total length of the weld being inspected (mm).

[0091] Experimental Example 9: The local thickness of the nickel plating layer on the finished welding wire prepared by the continuous wire-to-wire plating process of this invention was measured according to GB / T 6462-2025. Samples were taken from the head, middle, and tail of the same coil of welding wire, resulting in a total of 9 effective measurement points. The measurement points were evenly distributed along the circumference of the welding wire cross-section at each sampling location. The original thickness data of the nickel plating layer at each measurement point were obtained. The arithmetic mean of the nickel plating layer thickness, the sample standard deviation, and the coefficient of variation (%) of the continuous wire-to-wire plating nickel layer thickness were calculated according to the following formulas:

[0092]

[0093]

[0094]

[0095] in, The arithmetic mean of the nickel plating thickness (μm) The measured thickness (μm) of the nickel plating at the i-th measuring point. The total number of valid measurement points (dimensionless). Standard deviation (μm) for nickel plating thickness samples. The coefficient of variation is the thickness of the nickel layer plated by continuous wire drawing.

[0096] Experimental Example 10: Micro Vickers hardness tests were conducted on the cross-section of nickel-plated welding wire samples prepared using the complete process of this invention, according to GB / T 4340.1-2024. Five effective measuring points were used for each sample group, distributed at different locations on the coating. Measured hardness data for each point were obtained. The arithmetic mean of the coating hardness and the hardness fluctuation range (HV0.1) were calculated using the following formula:

[0097]

[0098]

[0099] in, The hardness of the coating is the arithmetic mean (HV0.1). The micro Vickers hardness (HV0.1) of the coating at the i-th measuring point is given. For the number of effective measurement points, For coating hardness fluctuations are extremely poor, This represents the maximum value of the hardness test (HV0.1). This is the minimum value for hardness testing.

[0100] Experimental Example 11: A neutral salt spray test was conducted on the nickel-plated welding wire samples prepared by the process of this invention in accordance with GB / T 10125-2021. The test conditions were: sodium chloride mass concentration of 50 g / L, test chamber temperature of 35℃, pH controlled at 6.5-7.2, and the time (h) at which the first rust spots appeared on the sample was recorded.

[0101] The results are shown in the table below:

[0102]

[0103] As shown in the table above, the deposition rate of the coating in the examples was 14.8-17.2 μm / h, the coefficient of variation of the zinc immersion layer thickness was 3.0-3.6%, the percentage of coating peeling and detachment area was 0.6-1.5%, the phosphorus content fluctuated between 0.22-0.32 wt%, the transmittance of the plating solution after 8 hours was 91.0-94.8%, and the porosity of the coating was 6-18 cells / dm². 2 The laser absorption rate of the welding wire is 33.0-38.5%, the effective length of the weld without defects is 94.8-98.5%, the coefficient of variation of the nickel plating layer thickness in continuous wire feeding is 3.8-5.0%, the coating hardness is 535-558HV0.1, the hardness fluctuation is 15-30HV0.1, and the time to first corrosion is 86-132 hours. This indicates that the process of this invention can obtain nickel-plated aluminum alloy welding wire with good plating solution stability, uniform and dense coating, strong adhesion, high laser absorption rate, excellent weld quality, and good corrosion resistance. The laser absorption rate (33.0-38.5%) is more than 280% higher than that of bare aluminum welding wire (less than 10%), effectively solving the problem of excessively high laser reflectivity in aluminum alloy welding wire.

[0104] Comparative Example 1 replaced zinc citrate in the zinc immersion solution with an equimolar amount of zinc oxide, keeping the total zinc concentration constant. Compared with the embodiments of the present invention, the coefficient of variation of the zinc immersion layer thickness increased from 3.0-3.6% to 8.2%, the proportion of coating peeling and detachment area increased from 0.6-1.5% to 5.2%, and the porosity increased from 6-18 cells / dm². 2 Increased to 38 units / dm 2 The laser absorption rate decreased from 33.0-38.5% to 31.0%, the proportion of defect-free effective length of weld decreased from 94.8-98.5% to 89.5%, the coefficient of variation of continuous wire cutting thickness increased from 3.8-5.0% to 6.8%, and the time to first corrosion decreased from 86-132h to 42h. This indicates that the introduction of zinc citrate is beneficial to the uniform deposition of zinc layer, which can obtain a more uniform zinc immersion layer, thereby improving the adhesion, density and welding performance of subsequent coatings. After replacing it with zinc oxide, the uniformity of zinc layer decreased and the coating quality deteriorated across the board.

[0105] In Comparative Example 2, phenylphosphonic acid was removed during the preparation of the mixed acid aqueous solution in S2 and completely replaced with equimolar citric acid to obtain a single nickel citrate complex solution. Compared with the embodiments of the present invention, its phosphorus content fluctuation range increased from 0.22-0.32 wt% to 0.68 wt%, the transmittance of the plating solution after 8 hours decreased from 91.0-94.8% to 76.8%, the coefficient of variation of continuous wire drawing thickness increased from 3.8-5.0% to 6.2%, the hardness fluctuation range increased from 15-30 HV0.1 to 52 HV0.1, the coating hardness decreased from 535-558 HV0.1 to 510 HV0.1, and the porosity increased from 6-18 cells / dm². 2 Increased to 42 units / dm 2 The time to first rusting decreased from 86-132 hours to 38 hours, indicating that the synergistic complexation effect of phenylphosphonic acid and citric acid is better than that of citric acid alone. It can stabilize the supply rate of nickel source in the plating solution, inhibit the decomposition of the plating solution, and improve the uniformity of phosphorus content, thickness and hardness of the coating. After removing phenylphosphonic acid, the stability of the plating solution decreased, the fluctuation of the coating composition increased, and the corrosion resistance decreased.

[0106] Comparative Example 3 eliminated the zinc stripping and secondary zinc immersion processes. The welding wire treated with S3 underwent only one zinc immersion (30s) before directly entering the nickel plating process. Compared with the embodiments of the present invention, its zinc layer thickness variation coefficient increased from 3.0-3.6% to 12.0%, the proportion of plating peeling and detachment area increased from 0.6-1.5% to 8.5%, and the porosity increased from 6-18 cells / dm². 2 Increased to 55 units / dm 2 The laser absorption rate decreased from 33.0-38.5% to 28.5%, the proportion of defect-free effective length of weld decreased from 94.8-98.5% to 83.0%, and the time to first rust appearance decreased from 86-132h to 26h. All six indicators were the worst in their respective groups. In addition, the coefficient of variation of continuous wire drawing thickness increased to 9.5%, and the hardness fluctuation range increased to 45HV0.1, which were also significantly worse than the embodiments of the present invention. This indicates that the secondary zinc immersion process can obtain a more uniform and dense zinc layer than the primary zinc immersion process. It is a key process to ensure the coating adhesion, integrity and welding quality. After omitting this process, the zinc layer is coarse and uneven, the coating adhesion is poor and easy to fall off, and the laser absorption rate and weld quality are significantly reduced.

[0107] In Comparative Example 4, the brightening solution treatment step was removed in S3. The welding wire was directly introduced into the zinc immersion process after being treated with the activation solution. Compared with the embodiment of the present invention, the proportion of the coating peeling and detachment area increased from 0.6-1.5% to 6.0%, and the porosity increased from 6-18 particles / dm². 2 Increased to 48 units / dm 2The laser absorption rate decreased from 33.0-38.5% to 30.0%, the proportion of defect-free effective length of weld decreased from 94.8-98.5% to 86.5%, the coefficient of variation of continuous wire feed thickness increased from 3.8-5.0% to 7.8%, the coating hardness decreased from 535-558HV0.1 to 505HV0.1, and the time to first rust appearance decreased from 86-132h to 33h. This indicates that the brightening treatment can effectively remove the gray-black adhering substances remaining on the surface after the welding wire is activated, and obtain a clean activated surface, which is conducive to the uniform growth of subsequent zinc immersion and coating. After omitting the brightening treatment, the residual impurities on the surface affect the bonding and density of the coating, resulting in the deterioration of various properties.

[0108] Comparative Example 5 removed the citrate-phenylphosphonate nickel complex component from the S5 nickel plating bath and added an equimolar amount of nickel sulfate hexahydrate to maintain a constant total nickel concentration. Compared with the embodiments of the present invention, the phosphorus content fluctuation range increased from 0.22-0.32 wt% to 0.82 wt%, the initial transmittance of the plating bath decreased from 97.5-98.0% to 93.5%, the 8-hour transmittance decreased from 91.0-94.8% to 70.5%, the continuous wire-feed thickness variation coefficient increased from 3.8-5.0% to 10.8%, and the coating hardness increased from 535-5. The hardness dropped from 58HV0.1 to 500HV0.1, and the hardness fluctuation range increased from 15-30HV0.1 to 65HV0.1. In addition, the proportion of the effective length of the weld without defects decreased to 91.0%, and the time to first corrosion decreased to 46 hours. This indicates that the composite complex is the core component for maintaining the stability of the plating solution and the uniformity of the coating. It can effectively delay the decomposition of the plating solution, stabilize the phosphorus content, and ensure the consistency of the coating thickness under continuous wire feeding conditions. After removing the composite complex, the stability of the plating solution decreased sharply, the fluctuation of the coating composition and thickness increased, and the hardness and corrosion resistance decreased significantly.

[0109] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A nickel plating process for the surface of laser welding aluminum alloy welding wire, characterized in that, Includes the following steps: S1: Dissolve citric acid monohydrate in water to prepare an aqueous citric acid solution, add zinc oxide, heat and stir to react, sieve, collect the filtrate, concentrate and dry the filtrate to obtain zinc citrate; S2: Nickel sulfate hexahydrate is dissolved in water to prepare an aqueous solution of nickel sulfate. An aqueous solution of sodium carbonate is added to react and a reaction mixture is obtained. The reaction mixture is centrifuged and the supernatant is discarded. The filter cake is collected and washed. Then it is reacted with a mixed acid aqueous solution composed of citric acid and phenylphosphonic acid to obtain a citric acid-phenylphosphonate nickel complex solution. S3: Pass the aluminum alloy welding wire through degreasing solution, deionized water rinsing, activation solution, deionized water rinsing, brightening solution, and deionized water rinsing in sequence. S4: The aluminum alloy welding wire treated in S3 is continuously passed through a zinc immersion solution, rinsed with deionized water, then continuously passed through a zinc stripping solution, rinsed with water, and then immersed in zinc again and rinsed with water; the zinc immersion solution is composed of zinc oxide, zinc citrate, sodium hydroxide, potassium sodium tartrate, ferric chloride hexahydrate and sodium nitrate. S5: The aluminum alloy welding wire treated in S4 is continuously plated through a nickel plating solution, rinsed with water, then treated with hot water, dried and cooled to room temperature, and then wound up; the nickel plating solution is composed of a citrate-phenylphosphonate nickel complex solution, nickel sulfate hexahydrate, sodium citrate and sodium hypophosphite.

2. The nickel plating process for the surface of laser welding aluminum alloy welding wire according to claim 1, characterized in that, In step S1, citric acid monohydrate is dissolved in deionized water to prepare a citric acid aqueous solution with a mass fraction of 30-50%. Zinc oxide is added to the citric acid aqueous solution at a molar ratio of zinc oxide to citric acid of 1:2-2.

5. The solution is then heated to 60-90℃ and stirred at 150-300 r / min for 1-3 h. The solution is then sieved and the filtrate is collected. The filtrate is concentrated under reduced pressure at 60-80℃ and -0.095 to -0.08 MPa to 1 / 3-1 / 2 of its original volume. The solution is then dried at 60-80℃ for 6-12 h to obtain zinc citrate.

3. The nickel plating process for the surface of laser welding aluminum alloy welding wire according to claim 1, characterized in that, In step S2, nickel sulfate hexahydrate is dissolved in deionized water to prepare a nickel sulfate aqueous solution with a concentration of 0.5-1.5 mol / L. A sodium carbonate aqueous solution with a nickel sulfate hexahydrate to sodium carbonate molar ratio of 1:1-1.2 is added to the nickel sulfate aqueous solution at 200-300 r / min over a period of 15-30 min. After all the solution is added, stirring continues for 20-60 min to obtain the reaction mixture. The reaction mixture is centrifuged, the supernatant is discarded, and the filter cake is collected. The filter cake is washed 2-3 times with 3-5 times its volume of deionized water at 60-80℃ for 3-4 min each time.

4. The nickel plating process on the surface of laser welding aluminum alloy welding wire according to claim 3, characterized in that, In step S2, the washed filter cake is transferred to a reaction vessel, and a mixed acid aqueous solution with a mass fraction of 20-40% is added at a nickel carbonate to total acid molar ratio of 1:1.5-2.

5. The mixed acid aqueous solution consists of citric acid and phenylphosphonic acid in a molar ratio of 1:0.3-1. The mixture is stirred at 200-300 r / min for 25-40 min at ≤50℃, then heated to 60-90℃ and stirred for 1-3 h. The mixture is then sieved to obtain a citric acid-nitrophenylphosphonate composite complex solution.

5. The nickel plating process for the surface of laser welding aluminum alloy welding wire according to claim 1, characterized in that, In S3, the degreasing solution is composed of 20-30 g / L sodium carbonate, 8-15 g / L trisodium phosphate, and 0.5-1.5 g / L sodium dodecyl sulfate; the aluminum alloy welding wire is continuously passed through the degreasing solution and treated at 40-55℃ for 3-6 minutes, and then rinsed with deionized water.

6. The nickel plating process on the surface of laser welding aluminum alloy welding wire according to claim 5, characterized in that, S3 aluminum alloy welding wire, after degreasing and rinsing with deionized water, is continuously passed through an activation solution and treated at 25-40℃ for 10-30 seconds, then rinsed with deionized water. It is then passed through the light-emitting solution continuously and rinsed with deionized water; The activation solution is composed of 15-30 g / L sodium hydroxide and 3-10 g / L sodium citrate dihydrate; The light-emitting solution is composed of 100-200 mL / L nitric acid aqueous solution and 50-100 mL / L sulfuric acid aqueous solution.

7. The nickel plating process for the surface of laser welding aluminum alloy welding wire according to claim 1, characterized in that, In step S4, the zinc immersion solution consists of 60-100 g / L zinc oxide, 5-20 g / L zinc citrate, 400-500 g / L sodium hydroxide, 20-40 g / L potassium sodium tartrate, 1-2 g / L ferric chloride hexahydrate, and 1-2 g / L sodium nitrate. The aluminum alloy welding wire is continuously passed through the zinc immersion solution and immersed in zinc for 20-40 seconds at room temperature, then rinsed with deionized water.

8. The nickel plating process on the surface of laser welding aluminum alloy welding wire according to claim 7, characterized in that, In S4, the zinc is then continuously passed through a zinc stripping solution composed of 150-300 mL / L concentrated nitric acid for 10-20 seconds at room temperature, rinsed with deionized water, and then immersed in zinc again for 10-25 seconds, and rinsed with deionized water.

9. The nickel plating process on the surface of laser welding aluminum alloy welding wire according to claim 1, characterized in that, In step S5, the aluminum alloy welding wire treated in step S4 is continuously plated in a nickel plating solution at 82-88℃ for 10-30 minutes, rinsed with deionized water, then treated with deionized water at 80-95℃, dried at 40-60℃ for 10-30 minutes, cooled to room temperature, and then wound up. The nickel plating solution consists of a 3-5 g / L citrate-phenylphosphonate nickel complex solution, a 30-43 g / L nickel sulfate hexahydrate, a 45-55 g / L sodium citrate, and a 15-25 g / L sodium hypophosphite.