A high-selectivity tungsten CMP polishing slurry with mixed abrasives and its preparation method

By using a mixture of nano-alumina and silica abrasives in a tungsten CMP polishing slurry, and combining it with hyperbranched polyester-catechol bisphosphonic acid coupling compound and methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer, the problems of agglomeration and scratching of nano-alumina abrasives were solved, thereby improving the removal selectivity of tungsten oxide and the polishing quality.

CN123108567APending Publication Date: 2026-11-17TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611595999.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing tungsten CMP polishing slurries, nano-alumina abrasives easily scratch the tungsten and silicon oxide surfaces. Nano-alumina and silica particles are prone to agglomeration, and electrostatic effects affect dispersion stability. Furthermore, the adsorption effect of small molecule amino acid inhibitors is limited, making it difficult to balance tungsten removal rate, selectivity, and pattern area flatness.

Method used

A highly selective tungsten CMP polishing slurry with mixed abrasives, containing nano-alumina particles and negatively charged silica particles, is used. Hyperbranched polyester-catechol bisphosphonic acid coupling agent is used as a dispersant, and methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer is used as a tungsten inhibitor to regulate mechanical and chemical action, reduce agglomeration and scratching, and improve selectivity.

Benefits of technology

This approach achieves the goal of reducing surface scratches while maintaining tungsten removal rate, improving the tungsten to silicon oxide removal selectivity, reducing dish-like and dielectric layer erosion in the micro-tungsten pattern area, and improving surface roughness and intra-wafer uniformity after polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of semiconductor chemical mechanical polishing (CMP) technology, and discloses a highly selective tungsten CMP polishing slurry composed of mixed abrasive particles and its preparation method. The polishing slurry comprises a mixed abrasive consisting of nano-alumina particles and negatively charged silica particles, a hyperbranched polyester-catechol bisphosphonic acid coupling agent as a dispersant, a methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor, an oxidant, and deionized water. The dispersant is used to reduce the agglomeration and sedimentation of the two types of abrasive particles, and the tungsten inhibitor is used to regulate the chemical reactions on the tungsten surface. This invention can reduce the silicon oxide removal rate while maintaining the tungsten removal rate, reducing polished surface defects, dishing, and erosion, and is suitable for CMP polishing of patterned tungsten wafers at the 3 nm technology node.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor chemical mechanical polishing technology, and in particular to a mixed abrasive highly selective tungsten CMP polishing slurry and its preparation method. Background Technology

[0002] As semiconductor manufacturing processes advance to 3 nm and below technology nodes, tungsten is used to fill interconnect structures and contact vias. After tungsten film deposition, chemical mechanical polishing (CMP) is typically required to remove excess tungsten material from the wafer surface and create a flat surface between the tungsten layer and the silicon oxide dielectric layer. With decreasing device feature sizes, the requirements for controlling material removal selectivity, surface defects, dishing, etching, and on-wafer uniformity during tungsten CMP become increasingly stringent.

[0003] Existing tungsten CMP polishing slurries typically use nano-alumina as the abrasive, combined with oxidants and amino acid inhibitors to regulate the chemical reaction and material removal process of tungsten. Nano-alumina can provide strong mechanical grinding action, but its high hardness can easily cause strong mechanical action on the tungsten and silicon oxide surfaces during polishing, resulting in surface defects such as scratches, particles, or pits.

[0004] To reduce the mechanical damage caused by alumina abrasive alone, some polishing slurries use a mixture of alumina and silica. The addition of silica can modulate the overall mechanical action of the mixed abrasive; however, in acidic polishing slurry systems, nano-alumina and negatively charged silica have different surface charge properties, making the two types of abrasive particles prone to heterogeneous agglomeration due to electrostatic interactions. This agglomeration not only easily leads to sedimentation, affecting the dispersion stability and consistency of the polishing slurry, but the large-diameter agglomerates formed may also increase scratch defects on the wafer surface.

[0005] Regarding tungsten inhibitors, existing polishing slurries typically employ small-molecule amino acids such as lysine, histidine, or cysteine. While these small molecules can adsorb onto the tungsten surface, their adsorbed layer is prone to desorption under the mechanical action of the polishing pad and abrasive, making it difficult to continuously control non-target chemical corrosion on the tungsten surface. Although using a single polyamino acid as an inhibitor can improve adsorption stability, its functional groups are relatively limited, restricting its ability to synergistically regulate the chemical reactions and mechanical removal processes on the tungsten surface. This can easily affect the removal selectivity ratio between tungsten and silicon oxide, and cause dish-shaped and dielectric layer erosion in areas with fine tungsten patterns.

[0006] To address this, a highly selective tungsten CMP polishing slurry with mixed abrasives and its preparation method are proposed. Summary of the Invention

[0007] The purpose of this invention is to provide a highly selective tungsten CMP polishing slurry with mixed abrasives and its preparation method, in order to solve the problems that existing tungsten CMP polishing slurries using nano-alumina as abrasives are prone to scratching on the tungsten and silicon oxide surfaces, that nano-alumina and negatively charged silica are prone to agglomeration and sedimentation in acidic polishing slurries due to differences in surface charge, and that the adsorption of small molecule amino acids or homopolymer amino acid inhibitors on the tungsten surface is limited, making it difficult to simultaneously achieve the tungsten removal rate, the removal selectivity ratio between tungsten and silicon oxides, and the flatness of the patterned area.

[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution.

[0009] This invention provides a highly selective tungsten CMP polishing slurry with a mixed abrasive, comprising a mixed abrasive, a dispersant, a tungsten inhibitor, an oxidant, and deionized water. The mixed abrasive comprises nano-alumina particles and negatively charged silica particles. The dispersant is a hyperbranched polyester-catechol bisphosphonate coupling compound, wherein the hyperbranched polyester-catechol bisphosphonate coupling compound has a hyperbranched polyester backbone with terminal hydroxyl groups and residual carboxyl groups. The catechol-bisphosphonate coupling anchoring group is formed by dopamine and alendronate or pamidronate linked by a phosphonamide bond. The catechol-bisphosphonate coupling anchoring group is grafted onto the hyperbranched polyester backbone by forming amide bonds with some residual carboxyl groups of the hyperbranched polyester through the terminal amino groups retained by alendronate or pamidronate. The tungsten inhibitor is a methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer.

[0010] Furthermore, the alumina nanoparticles have a particle size of 80–250 nm, and the negatively charged silica particles have a particle size of 10–120 nm.

[0011] Furthermore, the mass ratio of the nano-alumina particles to the negatively charged silica particles is 1:(0.2~2).

[0012] Furthermore, the hyperbranched polyester is a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups, and the number average molecular weight of the hyperbranched polyester is 1500 to 20000.

[0013] Further, the bisphosphonic acid is alendronate or pamidronate; when the bisphosphonic acid is alendronate, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: catechol—CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)3—NH2; when the bisphosphonic acid is pamidronate, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: catechol—CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)2—NH2.

[0014] Furthermore, in the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer, the degree of polymerization of the polyhistidine segment is 10-100, and the degree of polymerization of the polycysteine ​​segment is 10-100.

[0015] Furthermore, the oxidant is hydrogen peroxide, and the pH of the mixed abrasive high-selectivity tungsten CMP polishing slurry is 2-5.

[0016] In addition, the present invention also provides a method for preparing a mixed abrasive highly selective tungsten CMP polishing slurry, comprising the following steps: S1. Polyols and polycarboxylic acids or anhydrides are prepolymerized and polycondensed in the presence of a catalyst, and then distilled under reduced pressure to obtain a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups; dopamine is reacted with alendronic acid or pamidronic acid in the presence of EDC and NHS to obtain a catechol-bisphosphonic acid coupling with terminal amino groups; the hyperbranched polyester and the catechol-bisphosphonic acid coupling are subjected to an amidation grafting reaction in the presence of DCC and DMAP, so that some of the residual carboxyl groups of the hyperbranched polyester form amide bonds with the terminal amino groups of the catechol-bisphosphonic acid coupling to obtain a hyperbranched polyester-catechol-bisphosphonic acid coupling dispersant; S2. Using amino-terminated polyethylene glycol monomethyl ether as an initiator, Nim-triphenylmethyl-L-histidine NCA monomer and S-tert-butyl-L-cysteine ​​NCA monomer are sequentially polymerized, and the protecting group is removed to obtain methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor. S3. Disperse nano-alumina particles and negatively charged silica particles in deionized water, add the hyperbranched polyester-catechol bisphosphonic acid coupling dispersant obtained in step S1 and stir. S4. Add the tungsten inhibitor and oxidant of the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer obtained in step S2, and adjust the pH to 2-5 to obtain the mixed abrasive high-selectivity tungsten CMP polishing slurry.

[0017] Further, in step S1, the polyol and the polycarboxylic acid or anhydride are prepolymerized at 40–120°C for 1–8 hours, then reacted at 60–250°C for 3–20 hours, and distilled under reduced pressure until the acid value is below 30 mg KOH / g, to obtain a hyperbranched polyester with a number average molecular weight of 1500–20000 and terminal hydroxyl groups and residual carboxyl groups; the temperature for the amidation grafting reaction of the hyperbranched polyester with the catechol-bisphosphonic acid coupling is 60–120°C.

[0018] Furthermore, the sequential polymerization in step S2 is carried out under anhydrous conditions and at 20–40°C, and the protecting groups are removed using trifluoroacetic acid.

[0019] Nano-alumina particles are used to provide the mechanical action required for the removal of materials from tungsten surfaces, while negatively charged silica particles are used to modulate the mechanical action of the mixed abrasive system and reduce the scratches caused by nano-alumina particles on tungsten and silicon oxide surfaces.

[0020] In hyperbranched polyester-catechol-bisphosphonic acid couplings, the catechol-bisphosphonic acid coupling anchoring group is grafted onto the hyperbranched polyester backbone by forming amide bonds with some residual carboxyl groups of the hyperbranched polyester through its terminal amino groups. The catechol and bisphosphonic acid groups form multi-site adsorption on the surface of abrasive particles, and the hyperbranched polyester backbone creates steric hindrance between abrasive particles, thereby reducing the aggregation between nano-alumina particles and negatively charged silica particles.

[0021] The polyhistidine and polycysteine ​​segments in the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer contain imidazole and thiol groups, respectively. These imidazole and thiol groups are adsorbed onto the tungsten surface to regulate its chemical reactions. Under the mechanical action of the polishing pad and the mixed abrasive, the reaction layer on the tungsten surface is removed, thus achieving a synergy between chemical and mechanical action.

[0022] The embodiments of the present invention have the following advantages due to the adoption of the above technical solutions: I. This invention uses nano-alumina particles and negatively charged silica particles to form a mixed abrasive. The nano-alumina provides mechanical removal, and the silica regulates the mechanical action of the mixed abrasive, thereby reducing scratches on the polished surface while maintaining the tungsten removal rate.

[0023] II. This invention uses a hyperbranched polyester-catechol-bisphosphonic acid coupling agent as a dispersant. The abrasive particles are anchored by the catechol and bisphosphonic acid groups, and the hyperbranched polyester skeleton forms steric hindrance, thereby reducing the aggregation and sedimentation of nano-alumina particles and negatively charged silica particles. The sedimentation rate of the sample with the added dispersant after standing for 7 days was 2.5%–6.0%.

[0024] III. This invention uses a methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer as a tungsten inhibitor. The imidazole groups in the polyhistidine segments and the thiol groups in the polycysteine ​​segments adsorb onto the tungsten surface, regulating the chemical reaction on the tungsten surface. This, combined with the mechanical action of the mixed abrasive, reduces the removal rate of silicon oxide and improves the removal selectivity ratio of tungsten to silicon oxide. The removal selectivity ratios in Examples 1-3 are 178:1 to 256:1.

[0025] Fourth, this invention regulates abrasive dispersion, mechanical removal, and tungsten surface chemical reactions by combining mixed abrasives, dispersants, and tungsten inhibitors, thereby reducing dish-like patterns, dielectric layer erosion, and surface defects in the micro-tungsten pattern area, and improving the surface roughness and intra-sheet uniformity after polishing. Detailed Implementation

[0026] This invention provides a highly selective tungsten CMP polishing slurry with a mixed abrasive and its preparation method. The mixed abrasive consists of nano-alumina particles and negatively charged silica particles. The nano-alumina particles have a particle size of 80–250 nm, and the negatively charged silica particles have a particle size of 10–120 nm. The mass ratio of the nano-alumina particles to the negatively charged silica particles is 1:(0.2–2).

[0027] The dispersant used is a hyperbranched polyester-catechol bisphosphonic acid coupling agent. The hyperbranched polyester is prepared by polycondensation of polyol and polycarboxylic acid or anhydride in the presence of a catalyst. It is first prepolymerized at 40-120°C for 1-8 hours, then reacted at 60-250°C for 3-20 hours, and then distilled under reduced pressure until the acid value is below 30 mg KOH / g, to obtain a hyperbranched polyester with a number average molecular weight of 1500-20000 and terminal hydroxyl groups and residual carboxyl groups.

[0028] Catechol-bisphosphonic acid conjugates are formed by the reaction of dopamine with alendronic acid or pamidronic acid. The terminal primary amino group of dopamine forms a phosphonamide bond with the p-OH group in alendronic acid or pamidronic acid, while the amino group at the other end of alendronic acid or pamidronic acid remains free.

[0029] When alendronic acid is used, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: Catechol —CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)3—NH2.

[0030] When pamidronate is used, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: Catechol —CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)2—NH2.

[0031] The hyperbranched polyester and catechol-bisphosphonic acid coupling compound were subjected to an amidation grafting reaction at 60–120 °C in the presence of DCC and DMAP, so that some of the residual carboxyl groups of the hyperbranched polyester formed amide bonds with the terminal amino groups retained in the catechol-bisphosphonic acid coupling compound, thereby obtaining a hyperbranched polyester-catechol-bisphosphonic acid coupling compound dispersant.

[0032] The tungsten inhibitor used was a methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer, wherein the degree of polymerization of the polyhistidine segment was 10–100, and the degree of polymerization of the polycysteine ​​segment was 10–100. Using amino-terminated polyethylene glycol monomethyl ether as an initiator, Nim-triphenylmethyl-L-histidine NCA monomer and S-tert-butyl-L-cysteine ​​NCA monomer were sequentially polymerized under anhydrous conditions and at 20–40°C. The protecting groups were then removed using trifluoroacetic acid to obtain the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer.

[0033] Example 1 1. Preparation of dispersants 0.1 mol pentaerythritol and 0.6 mol 2,2-dimethylolpropionic acid were added to a reactor, along with 0.5% p-toluenesulfonic acid by mass of the total reactants. The mixture was prepolymerized at 80°C for 4 hours under nitrogen protection, then heated to 180°C and reacted for 10 hours. The mixture was then distilled under reduced pressure until the acid value was below 30 mg KOH / g, yielding a hyperbranched polyester with a number average molecular weight of approximately 5000 and terminal hydroxyl groups and residual carboxyl groups.

[0034] 0.05 mol of dopamine hydrochloride and 0.05 mol of alendronate were reacted at room temperature for 24 hours in the presence of EDC and NHS to form a phosphonamide bond between the terminal primary amino group of dopamine and the P-OH group of alendronate, thus obtaining a catechol-alendronic acid conjugate that retains the terminal amino group.

[0035] 10 g of the above hyperbranched polyester and 5 g of catechol-alendronic acid coupling compound were dissolved in anhydrous DMF, and 0.5 g of DCC and 0.05 g of DMAP were added. The mixture was reacted at 80 °C for 12 hours to allow some of the residual carboxyl groups in the hyperbranched polyester to undergo amidation with the terminal amino groups retained in the catechol-alendronic acid coupling compound. After precipitation, washing and drying, the hyperbranched polyester-catechol bisphosphonic acid coupling compound dispersant was obtained.

[0036] 2. Preparation of tungsten inhibitors 1 mmol of amino-terminated polyethylene glycol monomethyl ether with a number average molecular weight of 2000 (Mn) was dissolved in anhydrous THF, and 20 mmol of Nim-triphenylmethyl-L-histidine NCA monomer was added. The mixture was polymerized at 25°C for 24 hours under nitrogen protection to form methoxy polyethylene glycol-b-polyhistidine segments.

[0037] 20 mmol of S-tert-butyl-L-cysteine ​​NCA monomer was added, and polymerization was initiated by the obtained active chain end. The reaction was continued at 25 °C for 24 hours. Trifluoroacetic acid was added to remove the protecting groups of histidine and cysteine ​​segments. After dialysis purification and lyophilization, methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor was obtained.

[0038] 3. Preparation of polishing slurry Nano-alumina particles with an average particle size of 120 nm and negatively charged silica particles with an average particle size of 60 nm were dispersed in deionized water, so that the contents of nano-alumina particles and negatively charged silica particles in the polishing solution were 5 wt%.

[0039] Add 0.5 wt% of hyperbranched polyester-catechol bisphosphonic acid coupling dispersant and stir until homogeneous. Then add 100 ppm of methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor and 1 wt% hydrogen peroxide. Adjust the pH to 3.0 using nitric acid or potassium hydroxide to obtain the mixed abrasive high-selectivity tungsten CMP polishing slurry of Example 1.

[0040] Example 2 In this embodiment, hyperbranched polyester-catechol bisphosphonic acid coupling dispersant and methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor were prepared according to the method of Example 1.

[0041] Nano-alumina particles with an average particle size of 150 nm and negatively charged silica particles with an average particle size of 40 nm were dispersed in deionized water, so that the contents of the two abrasives in the polishing solution were 5 wt% respectively, and the mass ratio of nano-alumina particles to negatively charged silica particles was 1:1.

[0042] Add 0.3 wt% of hyperbranched polyester-catechol bisphosphonic acid coupling dispersant and stir until homogeneous. Then add 150 ppm of methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor and 1 wt% hydrogen peroxide. Adjust the pH to 2.5 using nitric acid or potassium hydroxide to obtain the mixed abrasive high-selectivity tungsten CMP polishing slurry of Example 2.

[0043] Example 3 In this embodiment, a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups was prepared according to the method of Example 1.

[0044] Dopamine hydrochloride was reacted with pamidronate in the presence of EDC and NHS to form a phosphonamide bond between the terminal primary amino group of dopamine and the P-OH group of pamidronate, resulting in a catechol-pamidronic acid conjugate that retains the terminal amino group.

[0045] The obtained catechol-pamidoline coupling compound was subjected to an amidation grafting reaction with hyperbranched polyester in the presence of DCC and DMAP, so that some of the residual carboxyl groups of the hyperbranched polyester formed amide bonds with the terminal amino groups retained in the catechol-pamidoline coupling compound, thus obtaining a hyperbranched polyester-catechol bisphosphonic acid coupling compound dispersant.

[0046] A tungsten inhibitor of methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer was prepared by NCA sequential polymerization, wherein the degree of polymerization of the polyhistidine segment was 30 and the degree of polymerization of the polycysteine ​​segment was 20.

[0047] Nano-alumina particles with an average particle size of 100 nm and negatively charged silica particles with an average particle size of 80 nm were dispersed in deionized water, so that the content of the two abrasives in the polishing solution was 5 wt%.

[0048] Add 0.4 wt% of hyperbranched polyester-catechol bisphosphonic acid coupling dispersant and stir until homogeneous. Then add 100 ppm of methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor and 1 wt% hydrogen peroxide. Adjust the pH to 4.0 using nitric acid or potassium hydroxide to obtain the mixed abrasive high-selectivity tungsten CMP polishing slurry of Example 3.

[0049] Comparative Example 1 The polishing solution was prepared according to the method of Example 1, except that hyperbranched polyester-catechol bisphosphonic acid coupling agent was not added, and the other conditions were the same as in Example 1.

[0050] Comparative Example 2 The polishing solution was prepared according to the method of Example 1, except that 0.5 wt% of the hyperbranched polyester-catechol bisphosphonic acid coupling dispersant was replaced with 0.5 wt% of sodium polyacrylate dispersant, and the other conditions were the same as in Example 1.

[0051] Comparative Example 3 The polishing solution was prepared according to the method of Example 1, except that the 100 ppm methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor was replaced with 100 ppm lysine, and the other conditions were the same as in Example 1.

[0052] Comparative Example 4 The polishing solution was prepared according to the method of Example 1, except that the 100 ppm methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor was replaced with 100 ppm ε-poly-L-lysine homopolymer, and the other conditions were the same as in Example 1.

[0053] Test Example 1 The polishing slurries prepared in Examples 1-3 and Comparative Examples 1-4 were used for CMP polishing tests on 3 nm patterned tungsten wafers.

[0054] The polishing pressure was 2.0 psi, the platen rotation speed was 115 rpm, the polishing head rotation speed was 121 rpm, and the polishing fluid flow rate was 90 mL / min. The tungsten polishing rate, silicon oxide polishing rate, tungsten to silicon oxide removal selectivity ratio, and total surface defect density after polishing were tested. The test results are shown in Table 1.

[0055] Table 1 Polishing performance of each embodiment and comparative example

[0056] As shown in Table 1, the tungsten polishing rate in Examples 1-3 was 1780-1920 Å / min, the silicon oxide polishing rate was 7.5-10 Å / min, the tungsten to silicon oxide removal selectivity ratio was 178:1-256:1, and the total surface defect density was no higher than 8 defects / cm². 2 .

[0057] Comparative Example 1, without the addition of a dispersant, exhibited a silicon oxide polishing rate of 42.5 Å / min, a tungsten to silicon oxide removal selectivity ratio of 67:1, and a total surface defect density of no less than 50 defects / cm². 2 Comparative Example 2 used sodium polyacrylate dispersant, with a tungsten to silica removal selectivity ratio of 86:1, and a total surface defect density of not less than 25 defects / cm². 2 .

[0058] The above results indicate that when hyperbranched polyester-catechol bisphosphonic acid coupling dispersant and methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor are combined with mixed abrasives, the polishing rate of silicon oxide and the total surface defect density can be reduced while maintaining the tungsten polishing rate.

[0059] Test Example 2 1. Test Sample To compare the dispersing effects of different dispersants on the mixed abrasive composed of nano-alumina particles and negatively charged silica particles, test samples were prepared according to Table 2.

[0060] The content of nano-alumina particles and negatively charged silica particles in each test sample was 5 wt%, and the total solid content of the mixed abrasive was 10 wt%. To ensure consistent testing conditions for all samples, the pH of each sample was adjusted to 3.0.

[0061] Table 2 Dispersion stability test samples

[0062] Among them, samples 1 to 3 correspond to the amount of dispersant added in Examples 1 to 3, respectively.

[0063] 2. Static Settlement Test Take 100 mL of each test sample and place it in a graduated stoppered cylinder. Record the sedimentation layer height and total liquid level at 0, 1, 6, 12, 24, 48, 72 and 168 hours after standing.

[0064] The settlement rate is calculated using the following formula: R = H1 / H2 × 100%.

[0065] In the formula, R is the settling rate, in units of %; H1 is the height of the settling layer; and H2 is the total liquid level.

[0066] The test results are shown in Table 3.

[0067] Table 3. Changes in sedimentation rate of each sample over time

[0068] 3. Zeta potential and particle size distribution testing The zeta potential of each test sample was measured at 25℃ using a Zetasizer Nano ZS zeta potential analyzer. The larger the absolute value of the zeta potential, the more obvious the electrostatic repulsion between particles; when the absolute value of the zeta potential is not less than 30mV, it indicates that the system has corresponding dispersion stability.

[0069] The average particle size (D50) and polydispersity index (PDI) of the abrasive particles in each test sample were measured using a dynamic light scattering particle size analyzer at 25℃. Samples were taken at 0, 24, 72, and 168 hours after sample preparation. An increase in average particle size over time or a PDI greater than 0.3 indicates agglomeration of abrasive particles.

[0070] The zeta potential and particle size distribution of each sample after initial and 7 days of standing are shown in Table 4.

[0071] Table 4. Zeta potential and particle size distribution of each sample

[0072] As shown in Tables 3 and 4, the sedimentation rate of the dispersion control sample A, which did not contain a dispersant, was 15% after standing for 1 hour and 92% after standing for 7 days. The D50 increased from 120 nm to 580 nm and the PDI increased from 0.45 to 0.68.

[0073] The dispersion control sample B used sodium polyacrylate as a dispersant. After standing for 7 days, the sedimentation rate was 70%, the D50 increased from 95 nm to 215 nm, and the PDI increased from 0.28 to 0.48.

[0074] The sedimentation rates of samples 1–3 after standing for 7 days were 2.5%–6.0%, the Zeta potentials were -35.2–38.5 mV, the D50 was 92–102 nm, and the PDI was 0.16–0.22. Sample 1 had a dispersant addition of 0.5 wt%, and after standing for 7 days, the sedimentation rate was 2.5%, the D50 increased from 85 nm to 92 nm, and the PDI increased from 0.12 to 0.16.

[0075] The above results indicate that hyperbranched polyester-catechol bisphosphonic acid coupling dispersant can reduce the aggregation and sedimentation of nano-alumina particles and negatively charged silica particles.

[0076] Test Example 3 1. Wafer and polishing conditions A 12-inch, 300 mm diameter, 3 nm technology node patterned tungsten wafer was used. The wafer surface includes tungsten interconnect lines with linewidths and spacings of 14 nm / 14 nm, 16 nm / 16 nm, 20 nm / 20 nm, and 28 nm / 28 nm, and has a W / TiN / SiO2 stacked structure. The initial thickness of the tungsten film is approximately 1500 Å, and the thickness of the SiO2 dielectric layer is approximately 2000 Å.

[0077] A Reflexion LK 300 mm CMP polisher and an IC1010 polyurethane polishing pad were used. The polishing pad was dressed with a diamond dresser for 30 seconds before use.

[0078] Test group 1 used the polishing slurry of Example 1, test group 2 used the polishing slurry of Example 2, and test group 3 used the polishing slurry of Example 3; control group 1 used the polishing slurry of Comparative Example 1, and control group 2 used the polishing slurry of Comparative Example 3.

[0079] The polishing process parameters are shown in Table 5.

[0080] Table 5 Polishing process parameters for 3 nm patterned tungsten wafers

[0081] 2. Detection Method The tungsten removal rate was determined by measuring the sheet resistance of the tungsten film before and after polishing using a four-probe resistivity meter, and then converting this resistance into a change in tungsten film thickness. Nine locations were measured for each wafer, including the wafer center, wafer edge, and locations between the wafer center and edge. The average value of these nine locations was used to calculate the tungsten removal rate.

[0082] The SiO2 removal rate was measured using an elliptic polarization spectrometer to measure the change in the thickness of the SiO2 dielectric layer before and after polishing.

[0083] The W / SiO2 selectivity ratio is the ratio of the tungsten removal rate to the SiO2 removal rate.

[0084] The KLA-Tencor Surfscan SP5 dark field defect detection system was used to detect scratches, particles and pits on the surface of the polished wafer. The defect density with a size of not less than 50 nm and the total surface defect density were statistically analyzed.

[0085] The Veeco Dimension ICON atomic force microscope was used to scan tungsten line arrays with linewidths of 14 nm, 16 nm, 20 nm and 28 nm, with a scanning range of 5 μm × 5 μm, and the depth of the disc-shaped center of the tungsten lines was measured.

[0086] The erosion depth of the SiO2 dielectric layer in the high-density tungsten line region with a linewidth / spacing of 14 nm / 14 nm was measured using atomic force microscopy, and the root mean square roughness Rq of the polished tungsten surface was measured in a 1 μm × 1 μm area.

[0087] 3. Test Results The test results are shown in Table 6.

[0088] Table 6 Polishing performance of various polishing slurries on 3 nm patterned tungsten wafers

[0089] After polishing, the dish depth of the 14 nm linewidth tungsten line in test group 1 was 1.2 nm, the SiO2 dielectric layer erosion depth of the 14 nm / 14 nm high-density array region was 1.5 nm, and the tungsten surface roughness Rq was 0.18 nm.

[0090] In control group 1, no dispersant was added. The dish depth of the 28 nm linewidth tungsten line was 10.5 nm, the erosion depth of the 14 nm / 14 nm array region was 8.5 nm, and the total surface defect density was not less than 50 defects / cm². 2 The surface roughness Rq of tungsten is 0.65 nm.

[0091] The W / SiO2 selectivity ratios for test groups 1–3 ranged from 178:1 to 256:1, and the defect density with a size not less than 50 nm was not higher than 2 defects / cm². 2 The total surface defect density is no higher than 8 defects / cm³. 2The dish depth of the 14 nm linewidth tungsten lines is 1.0–1.5 nm, and the dish depth of the 28 nm linewidth tungsten lines is 2.2–3.5 nm; the etching depth of the 14 nm / 14 nm array region is 1.2–1.8 nm, the surface roughness Rq is 0.15–0.22 nm, and the in-wafer non-uniformity WIWNU is 2.8%–3.8%.

[0092] In test group 2, the W / SiO2 selectivity ratio was 256:1, and the total surface defect density was no higher than 3 defects / cm². 2 The dish depth of the 14 nm linewidth tungsten line is 1.0 nm, the dish depth of the 28 nm linewidth tungsten line is 2.2 nm, and the etch depth of the 14 nm / 14 nm array region is 1.2 nm.

[0093] The above test results show that the mixed abrasive high-selectivity tungsten CMP polishing slurry prepared in the embodiments of the present invention can be used for chemical mechanical polishing of patterned tungsten wafers at the 3 nm technology node, and can control the W / SiO2 selectivity ratio, surface defects, dish shape, erosion, surface roughness and intra-wafer non-uniformity under the test conditions.

[0094] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various variations or substitutions within the technical scope disclosed in the present invention, and these should all be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A highly selective tungsten CMP polishing slurry comprising mixed abrasives, a dispersant, a tungsten inhibitor, an oxidant, and deionized water, characterized in that, The mixed abrasive comprises nano-alumina particles and negatively charged silica particles; the dispersant is a hyperbranched polyester-catechol bisphosphonate coupling compound, wherein the hyperbranched polyester-catechol bisphosphonate coupling compound uses a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups as the backbone, and the catechol-bisphosphonate coupling anchoring group is formed by dopamine and alendronic acid or pamidronic acid linked by a phosphonamide bond. The catechol-bisphosphonate coupling anchoring group is grafted onto the hyperbranched polyester backbone by forming amide bonds with some residual carboxyl groups of the hyperbranched polyester through the terminal amino groups retained by alendronic acid or pamidronic acid; the tungsten inhibitor is a methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer.

2. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, The alumina nanoparticles have a particle size of 80–250 nm, and the negatively charged silica particles have a particle size of 10–120 nm.

3. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, The mass ratio of the nano-alumina particles to the negatively charged silica particles is 1:(0.2~2).

4. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, The hyperbranched polyester is a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups, and the number average molecular weight of the hyperbranched polyester is 1500 to 20000.

5. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, The bisphosphonic acid is alendronate or pamidronate; when the bisphosphonic acid is alendronate, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: catechol—CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)3—NH2; when the bisphosphonic acid is pamidronate, the catechol-bisphosphonic acid coupling anchoring group includes the following linkage structure: catechol—CH2—CH2—NH—P(=O)(OH)—C(OH)(PO3H2)—(CH2)2—NH2.

6. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, In the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer, the degree of polymerization of the polyhistidine segment is 10-100, and the degree of polymerization of the polycysteine ​​segment is 10-100.

7. The high-selectivity tungsten CMP polishing slurry with mixed abrasives according to claim 1, characterized in that, The oxidant is hydrogen peroxide, and the pH of the mixed abrasive high-selectivity tungsten CMP polishing slurry is 2-5.

8. A method for preparing a mixed abrasive highly selective tungsten CMP polishing slurry, characterized in that, Includes the following steps: S1. Polyols and polycarboxylic acids or anhydrides are prepolymerized and polycondensed in the presence of a catalyst, and then distilled under reduced pressure to obtain a hyperbranched polyester with terminal hydroxyl groups and residual carboxyl groups; dopamine is reacted with alendronic acid or pamidronic acid in the presence of EDC and NHS to obtain a catechol-bisphosphonic acid coupling with terminal amino groups; the hyperbranched polyester and the catechol-bisphosphonic acid coupling are subjected to an amidation grafting reaction in the presence of DCC and DMAP, so that some of the residual carboxyl groups of the hyperbranched polyester form amide bonds with the terminal amino groups of the catechol-bisphosphonic acid coupling to obtain a hyperbranched polyester-catechol-bisphosphonic acid coupling dispersant; S2. Using amino-terminated polyethylene glycol monomethyl ether as an initiator, Nim-triphenylmethyl-L-histidine NCA monomer and S-tert-butyl-L-cysteine ​​NCA monomer are sequentially polymerized, and the protecting group is removed to obtain methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer tungsten inhibitor. S3. Disperse nano-alumina particles and negatively charged silica particles in deionized water, add the hyperbranched polyester-catechol bisphosphonic acid coupling dispersant obtained in step S1 and stir. S4. Add the tungsten inhibitor and oxidant of the methoxy polyethylene glycol-b-polyhistidine-b-polycysteine ​​triblock copolymer obtained in step S2, and adjust the pH to 2-5 to obtain the mixed abrasive high-selectivity tungsten CMP polishing slurry.

9. The method for preparing the mixed abrasive high-selectivity tungsten CMP polishing slurry according to claim 8, characterized in that, In step S1, the polyol and the polycarboxylic acid or anhydride are prepolymerized at 40–120°C for 1–8 hours, then reacted at 60–250°C for 3–20 hours, and distilled under reduced pressure until the acid value is below 30 mg KOH / g, to obtain a hyperbranched polyester with a number average molecular weight of 1500–20000 and terminal hydroxyl groups and residual carboxyl groups; the temperature for the amidation grafting reaction of the hyperbranched polyester with the catechol-bisphosphonic acid coupling is 60–120°C.

10. The method for preparing the mixed abrasive high-selectivity tungsten CMP polishing slurry according to claim 8, characterized in that, The sequential polymerization in step S2 was carried out under anhydrous conditions at 20–40°C, and the protecting groups were removed using trifluoroacetic acid.