An integrated composite electrode and an alkaline water electrolysis hydrogen production device including the composite electrode.
By using an integrated composite electrode and a magnetic field-assisted lattice oxygen mechanism, the problems of high interfacial resistance, bubble accumulation, and high overpotential of oxygen evolution reaction in traditional alkaline water electrolysis devices have been solved, achieving low-voltage and high-efficiency hydrogen production.
Patent Information
- Application Number
- CN202611423718.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
In traditional alkaline water electrolysis hydrogen production devices, the separation of the electrode and the diaphragm leads to increased interfacial contact resistance, bubble accumulation, high overpotential of oxygen evolution reaction, long ion conduction path, and the diaphragm is easily damaged by high temperature treatment.
An integrated composite electrode structure is adopted, in which the current collector, catalyst layer and membrane layer are integrated into one through hot pressing. Combined with magnetic field assistance and CeO2 activation of lattice oxygen mechanism, the interfacial resistance and oxygen evolution reaction overpotential are reduced.
It achieves zero-gap operation, significantly reduces cell voltage, reduces bubble ohmic impedance, improves catalyst layer utilization, reduces oxygen evolution reaction activation energy, and enhances mechanical stability.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
[0001] Invention Title: An Integrated Composite Electrode and an Alkaline Water Electrolysis Hydrogen Production Device Containing the Composite Electrode Background Technology
[0002] Alkaline water electrolysis (AWE) for hydrogen production is one of the mainstream technologies for green hydrogen production. Traditional alkaline electrolyzers employ a split structure, where the anode and cathode are separately assembled with the diaphragm. This split structure presents the following technical problems: Firstly, there is an interfacial gap between the electrode and the diaphragm, which increases the interfacial contact resistance. At the same time, bubbles accumulate in the gap, further increasing the ohmic impedance and raising the tank voltage.
[0003] Secondly, the traditional method of separating and assembling the membrane (such as the Zirfon composite membrane) and the electrode cannot achieve zero-gap operation, resulting in a long ion conduction path and low utilization of the catalyst layer.
[0004] Third, the oxygen evolution reaction (OER) is limited by the scaling relation under alkaline conditions, with a theoretical overpotential limit of approximately 370 mV, which is difficult for the traditional adsorption evolution mechanism (AEM) to overcome. Simultaneously, the OO bonding step in OER is spin-forbidden in some systems—the substrate (H₂O / OH⁻) of the OER is a spin singlet state, while the product O₂ is a spin triplet state. When the catalyst does not contain magnetic components that can provide spin polarization, this spin state transition is hindered, further increasing the activation energy. The lattice oxygen mechanism (LOM) bypasses the 370 mV lower limit of AEM, which is locked by the scaling relation, by allowing lattice oxygen to participate in OO bonding.
[0005] Fourth, existing technologies include methods for heat treatment of PTFE-based composite materials at high temperatures (such as above 350°C), but the decomposition temperature of PTFE is about 327°C. Such high-temperature treatment can easily lead to the decomposition of PTFE, the generation of gas, pore blockage, and structural damage.
[0006] Therefore, there is an urgent need for an electrode structure and electrolysis device that can reduce interfacial resistance, shorten ion conduction paths, and synergistically reduce the overpotential of the oxygen evolution reaction. Summary of the Invention
[0007] The purpose of this invention is to provide an integrated composite electrode that integrates the current collector, catalyst layer and membrane layer into an inseparable whole structure through hot pressing, thereby achieving zero-gap operation and reducing interfacial contact resistance and bubble resistance.
[0008] Another objective of this invention is to provide an alkaline water electrolysis hydrogen production device that reduces the overpotential of the oxygen evolution reaction through the synergistic effect of magnetic field assistance and CeO2 activation of lattice oxygen mechanism.
[0009] To achieve the above objectives, the present invention provides the following technical solution: An integrated composite electrode comprises a first catalyst layer, a first current collector layer, a membrane layer, a second current collector layer, and a second catalyst layer stacked sequentially. Both the first and second catalyst layers are nickel foam-based catalyst supports; both the first and second current collector layers are woven nickel meshes; the membrane layer is a PTFE composite membrane containing cerium and lanthanum, wherein CeO2 and La2O3 are introduced during the PTFE film formation stage; and each layer is hot-pressed into an integrated, indivisible structure.
[0010] The first current collector layer and the first catalyst layer, and the second current collector layer and the second catalyst layer are preferably fixed by ultrasonic welding or laser welding, with a welding density of 20 to 50 weld points per square centimeter. After welding, the interfacial contact resistance of the composite skeleton is significantly lower than that of the unwelded stacked structure.
[0011] Compared with the prior art, the present invention has the following beneficial effects: First, zero-gap operation is achieved through integrated hot pressing molding, and the interface contact resistance is less than half of the interface contact resistance between the separate electrode and the diaphragm assembly (this value is the theoretical expectation of the upper limit of the design, and the actual value needs to be verified by actual measurement), which significantly reduces the tank voltage.
[0012] Second, the magnetic field is set parallel to the electrode surface to generate a Lorentz force F=J×B, which promotes the detachment of bubbles from the electrode surface and reduces the ohmic impedance and coverage of the bubbles.
[0013] Third, CeO2 activates the lattice oxygen mechanism (LOM), bypassing the 370 mV overpotential limit locked by scaling relation in the traditional adsorption evolution mechanism (AEM).
[0014] Fourth, the magnetic components in the anode catalyst layer exhibit spin polarization under the influence of a magnetic field. This spin polarization effect, along with the lattice oxygen mechanism, synergistically reduces the activation energy of the oxygen evolution reaction at the same rate-determining step. The phase composition and magnetic order state of the magnetic components need to be confirmed by actual measurement using magnetic measurement methods such as a vibrating sample magnetometer (VSM).
[0015] Fifth, the micropore drilling process is carried out after hot pressing and cooling, which effectively avoids the PTFE melt from flowing back and clogging the channels during the hot pressing stage. The area density of the micropores is 5%~15%, which establishes sufficient ion conduction channels while ensuring mechanical strength.
[0016] Sixth, after hot pressing integration, the diaphragm layer and the braided nickel mesh current collector layers on both sides form a tight bond at the interface, which reduces the contact resistance at the interface (this effect is theoretically expected, and the actual value needs to be verified by actual measurement), which is different from the interface state where the diaphragm and the electrode are separated in the split assembly structure.
[0017] Seventh, the first current collector layer and the first catalyst layer, and the second current collector layer and the second catalyst layer are fixed by welding. Compared with the stacked structure that relies solely on hot pressing, welding can ensure a strong metallurgical bond between the mesh and the nickel foam, reduce the interfacial contact resistance, and improve the mechanical stability of the integrated structure in long-term operation. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the cross-section of an integrated composite electrode stacked structure (a five-layer hot-pressed integrated structure consisting of a foamed nickel catalyst layer, a braided nickel mesh current collector layer, a membrane layer, a braided nickel mesh current collector layer, and a foamed nickel catalyst layer).
[0019] Figure 2 The process flow diagram for hot-press integrated manufacturing is as follows (seven steps: sandblasting pretreatment → welding → cold pressing preforming → drying + hot pressing → cooling and depressurization → micro-hole drilling → loading + activation).
[0020] Figure 3 This is a schematic diagram of a magnetic field-assisted electrolysis device (the magnetic field direction is parallel to the electrode surface, and the Lorentz force F=J×B directs the detachment of bubbles).
[0021] Figure 4 A schematic diagram of the integrated synergistic mechanism (zero gap decreases interfacial resistance, magnetic field spin polarization effect, CeO2 lattice oxygen LOM bypasses AEM wall, and four-frame convergence limited by concentrated alkali conditions).
[0022] Figure 5 To creatively demonstrate the experimental design of five groups (A. Baseline / B. Magnetic field only / C. CeO2 only / D. Integrated only / E. Full combination). Detailed Implementation
[0023] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.
[0024] Example 1: Fabrication of an integrated composite electrode (0) Pretreatment of nickel mesh by sandblasting: The woven nickel mesh is sandblasted, and the woven nickel mesh is a twill weave structure; the sandblasting medium is white corundum or brown corundum, the abrasive particle size is 60~120 mesh, and the sandblasting pressure is 0.3~0.6 MPa; the surface roughness Ra of the nickel mesh after sandblasting reaches 0.8~3.2 μm (measured according to GB / T 1031) to enhance the mechanical anchoring effect between the catalyst layer and the nickel mesh; after sandblasting, the residual sand is removed by ultrasonic cleaning with deionized water.
[0025] (0.5) Welding: The sandblasted woven nickel mesh (30 mesh, 0.25 mm wire diameter, 3 strands twisted together; 30 mesh was chosen instead of the denser 40 mesh because the 40 mesh has an open area ratio of only about 27.9%, and the PTFE melt is more likely to accumulate and solidify at the mesh openings during hot pressing, causing blockage; while the 30 mesh has an open area ratio of about 41.4%, which reduces the risk of blockage while ensuring mechanical strength, and also facilitates the discharge of bubbles generated by electrolysis through the mesh layer and reduces the ohmic resistance of the bubbles) and nickel foam (thickness 1.3-1.4 mm, porosity ≥95%) are ultrasonically welded together to form a "foam-mesh" composite skeleton (where the nickel foam is the catalyst layer located on the outside, and the woven nickel mesh is the current collector layer facing the diaphragm side). The welding density is 20-50 weld points per square centimeter, and the interfacial contact resistance of the composite skeleton after welding is no more than half that of the unwelded stacked structure. Ultrasonic welding parameters: frequency 20kHz, amplitude 20~40 μm, welding pressure 0.2~0.4 MPa, welding time 0.1~0.3 s / point. After welding, check the thinning amount of foamed nickel at the weld point. The thinning amount shall not exceed 20% of the original thickness. This thinning amount is only for local thinning at the weld point. The overall compression of the hot pressing process is controlled by step (3). The sandblasting pretreatment and welding are completed continuously within 4 hours to avoid secondary oxidation of the fresh nickel surface after sandblasting.
[0026] (1) Cold pressing preforming: The "foam-mesh" composite skeleton obtained in step (0.5) and the PTFE composite membrane (thickness 100 μm, porosity 50%~70%, pore size 0.1~0.5 μm, with CeO2 and La2O3 introduced during the film formation stage, total content 5~50 wt%, preferably 10~20 wt%) are stacked in the order of "composite skeleton-membrane-composite skeleton", with the woven nickel mesh of each composite skeleton facing the membrane and the foam nickel facing outward. The membrane is held under pressure at 1.3~1.5 MPa and room temperature for 3~5 minutes to remove interlayer air. The foam nickel catalyst layer is not loaded with catalyst before hot pressing. The catalyst loading is carried out after hot pressing and drilling to avoid the influence of high temperature hot pressing on the catalyst crystal phase. The welded composite skeleton should be put into the cold pressing and hot pressing process as soon as possible, or the hot pressing is carried out in an inert atmosphere (N2 / Ar) to suppress the secondary oxidation of the fresh nickel surface after sandblasting.
[0027] (2) Drying: Dry at 60°C for 4 hours to remove residual moisture and solvent.
[0028] (3) Hot pressing: The hot pressing temperature is selected based on the interfacial bonding behavior of PTFE and braided nickel mesh under hot pressing. PTFE softens and begins to flow and penetrate into the mesh of the braided nickel mesh above 280°C, and does not undergo thermal decomposition below 300°C. The purpose of this temperature range is to form an interpenetrating network structure of braided nickel mesh and PTFE through the softening and flow of PTFE, thereby reducing the interfacial contact resistance, rather than changing the crystal phase or activity of the catalyst (the catalyst is loaded only after hot pressing). The pressure is maintained at 280~300°C and 3.2~3.5 MPa for 5~10 minutes. This temperature is higher than the softening temperature of PTFE but lower than its decomposition temperature (approximately 327°C), allowing PTFE to penetrate into the mesh of the braided nickel mesh, forming an interpenetrating network structure to fix the current collector and the diaphragm. After hot pressing, the total thickness is controlled at 1.0~1.5 mm, and the nickel foam is compressed to about 1 / 3 to 1 / 2 of its original thickness. Pressure is maintained and cooled to below 100°C before pressure is released to prevent the rapid cooling of PTFE from generating internal stress.
[0029] (4) Cooling: Pressure should be maintained and cooled to below 100°C before depressurization and natural cooling to room temperature to prevent PTFE from rapidly cooling and generating internal stress that could lead to delamination or warping.
[0030] (5) Micropore drilling: After hot pressing and cooling, through-holes penetrating the nickel foam catalyst layer are drilled on the hot-pressed integral body. The pore diameter is 10~30 μm and the area density is 5%~15%, establishing ion conduction channels. The membrane layer retains a microporous structure of 0.1~0.5 μm for gas barrier. The through-holes and the micropores of the membrane layer are functionally separated to avoid cross-diffusion of gas due to excessively large pore size. The drilling process is carried out after hot pressing and cooling to avoid PTFE melt backflow and blockage of the channels during the hot pressing stage. The 10~30 μm through-holes can be achieved by ultrafast laser processing, such as femtosecond laser processing or laser processing with Bessel beam shaping, to obtain straight holes with high depth-to-diameter ratio and low taper at a large depth-to-diameter ratio.
[0031] (6) Supported catalyst: NiFe-CeO2 catalyst supported on nickel foam on the anode side (Ni:Fe atomic ratio of about 3:1, Ce atomic percentage of 2.5%~3.5%, preferably about 3%); Raney Ni catalyst supported on nickel foam on the cathode side. Citric acid, in an amount equal to the total amount of metal ions, is added to the supporting solution as a complexing agent. The citric acid is analytical grade to ensure that the metal ions are stably dispersed in the supporting solution.
[0032] (7) Post-loading treatment: After loading is completed, the integrated electrode is vacuum dried (60°C, 4 hours), followed by electrochemical activation treatment - in 35 wt% KOH at 80°C, a constant potential of 1.2~1.5 V is applied for 30~60 minutes to fully convert the NiFe-CeO2 catalyst into the active phase.
[0033] Example 2: Alkaline water electrolysis hydrogen production device The integrated composite electrode prepared in Example 1 was assembled in an alkaline electrolytic cell using zero-gap assembly. Magnetic field generating components were installed on both sides of the electrode, with the magnetic field direction essentially parallel to the electrode surface and a magnetic induction intensity of 0.5–3 T. The electrolyte was a 35 wt% KOH aqueous solution, and the operating temperature was 80–90°C.
[0034] As an optional operating mode, the alkaline water electrolysis hydrogen production device can be configured with two sets of the integrated composite electrode modules. The two sets of electrode modules operate alternately, that is, one set is in electrolysis operation mode, and the other set is in open-circuit static mode. During the static mode, the iron deposited on the surface of the cathode catalyst layer redissolves back into the electrolyte under open-circuit conditions, allowing the iron concentration in the electrolyte to recover. The iron redox peak area of the anode catalyst layer in operation is periodically collected. When the iron redox peak area drops below a preset proportion of the initial value, the other set of electrode modules is switched to operation. The iron redox peak area is linearly related to the number of iron active sites, serving as a quantitative switching criterion that can be collected online. The switching trigger timing is determined based on the change of this signal, rather than simply being driven by a fixed time period. For reference, the iron concentration in the electrolyte should preferably be controlled below 1 ppm, preferably utilizing the natural iron background concentration of about 0.2 ppm in industrial electrolytes, without the need for additional iron salts. The iron deposition-dissolution cycle on the cathode can complete a reversible cycle within a few hours in a low-concentration system. The above optional operating modes are a preliminary description of the principle, and their specific switching cycles, rest periods and other parameters need to be determined through experimental verification.
Claims
1. An integrated composite electrode, characterized in that, It includes a first catalyst layer, a first current collector layer, a membrane layer, a second current collector layer, and a second catalyst layer stacked sequentially, wherein: Both the first and second catalyst layers are nickel foam-based catalyst supports; Both the first current collector layer and the second current collector layer are woven nickel meshes, located on opposite sides of the diaphragm layer, respectively. The membrane layer is a polytetrafluoroethylene (PTFE) composite membrane containing cerium and lanthanum, in which CeO2 and La2O3 are doped; The first catalyst layer, the first current collector layer, the membrane layer, the second current collector layer, and the second catalyst layer are integrally formed into an inseparable structure by hot pressing.
2. The integrated composite electrode according to claim 1, characterized in that, The first current collector layer and the first catalyst layer, and the second current collector layer and the second catalyst layer are fixed by welding; the welding is ultrasonic welding or laser welding, the welding density is 20 to 50 weld points per square centimeter, and the contact resistance of the interface after welding is not greater than half of that of the unwelded stacked structure.
3. The integrated composite electrode according to claim 2, characterized in that, The woven nickel mesh is pre-treated by sandblasting before welding. The sandblasting pre-treatment and welding are completed continuously within 4 hours. The welded composite skeleton is put into cold pressing and hot pressing processes as soon as possible, or the hot pressing is carried out in an inert atmosphere (N2 / Ar) to suppress secondary oxidation of the fresh nickel surface after sandblasting.
4. The integrated composite electrode according to claim 1, characterized in that, The first catalyst layer is an anode catalyst layer supported on a NiFe-CeO2 catalyst; the second catalyst layer is a cathode catalyst layer supported on a Raney Ni catalyst.
5. The integrated composite electrode according to claim 1, characterized in that, The hot pressing temperature is 280–300°C, the pressure is 3.2–3.5 MPa, and the holding time is 5–10 minutes.
6. The integrated composite electrode according to claim 1, characterized in that, The integrated structure has through-holes that penetrate the nickel foam catalyst layer. The through-holes have a pore size of 10–30 μm and a pore area density of 5%–15%, which are used to establish ion conduction channels. The membrane layer retains a microporous structure with a pore size of 0.1–0.5 μm for gas barrier. The through-holes and the micropores of the membrane layer are structurally and functionally separated.
7. The integrated composite electrode according to claim 1, characterized in that, The woven nickel mesh has a twill weave structure with a mesh count of 30 and a wire diameter of 0.25 mm. It adopts a multi-strand twisted structure, with 2 to 5 strands, preferably 3 strands. The porosity of the foamed nickel is not less than 95%.
8. An alkaline water electrolysis hydrogen production device, characterized in that, The integrated composite electrode comprising any one of claims 1 to 7, and: A magnetic field generating component that generates a magnetic field substantially parallel to the surface of the integrated composite electrode; The electrolyte is a 30%–40% (w / w) aqueous solution of potassium hydroxide (KOH).
9. The alkaline water electrolysis hydrogen production apparatus according to claim 8, characterized in that, The integrated composite electrode has a zero-gap assembly structure, and the interfacial contact resistance between the diaphragm layer and the current collector layer in the integrated composite electrode is less than half of the interfacial contact resistance between the separate electrode and the diaphragm assembly.
10. The alkaline water electrolysis hydrogen production apparatus according to claim 8, characterized in that, The magnetic field generating component produces a magnetic induction intensity of 0.5 to 3 T.
11. The integrated composite electrode or alkaline water electrolysis hydrogen production device according to claim 4 or 8, characterized in that, The NiFe-CeO2 catalyst has an atomic ratio of Ni to Fe of approximately 3:1 and an atomic percentage of Ce of 2.5% to 3.5%, preferably 3%.
12. A method for producing hydrogen through alkaline water electrolysis, characterized in that, Using the alkaline water electrolysis hydrogen production apparatus according to any one of claims 8 to 11, electrolysis is performed in the presence of the magnetic field, wherein: The magnetic field is basically parallel to the surface of the integrated composite electrode, generating a Lorentz force F=J×B, which directionally promotes the detachment of precipitated bubbles from the electrode surface and reduces the ohmic resistance of the bubbles. The CeO2 activates the lattice oxygen mechanism (LOM) and reduces the overpotential of the oxygen evolution reaction (OER).
13. The alkaline water electrolysis method for hydrogen production according to claim 12, characterized in that, The magnetic components in the anode catalyst layer exhibit a spin polarization effect under the action of the magnetic field. This spin polarization effect and the lattice oxygen mechanism work together at the same rate-determining step to reduce the activation energy of the oxygen evolution reaction.