Electrolytic production of magnesium-lithium alloys

By electrolyzing magnesium and lithium in stages in the same electrolytic cell and capturing lithium with liquid magnesium, the problems of long process flow, high energy consumption and difficult control in traditional magnesium-lithium alloy preparation methods have been solved, realizing large-scale production of magnesium-lithium alloys with uniform composition, high purity and low cost.

CN123108666APending Publication Date: 2026-11-17UNIV OF SCI & TECH BEIJING
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611248975.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional magnesium-lithium alloy preparation methods have long processes, high energy consumption, and high costs. Furthermore, the electrode potential difference between magnesium and lithium results in a narrow process window and high control difficulty.

Method used

Magnesium and lithium are electrolyzed in stages in the same electrolytic cell. The liquid magnesium generated in the early stage is used to capture the lithium deposited in the later stage. Magnesium-lithium alloying is achieved by configuring a molten salt electrolyte of potassium chloride and magnesium chloride, using an inert metal or graphite anode and a metal or conductive ceramic cathode, and controlling the electrolysis parameters.

Benefits of technology

It achieves uniform composition and high purity of magnesium-lithium alloys, with a short process flow, low equipment investment and operating costs, making it suitable for large-scale production. It avoids the problem of narrow-window parameter matching and realizes full-range composition adjustment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108666A_ABST
    Figure CN123108666A_ABST
Patent Text Reader

Abstract

This invention relates to the field of non-ferrous metal metallurgy, specifically to an electrolytic preparation method for magnesium-lithium alloys. The method includes: preparing a first molten salt electrolyte comprising potassium chloride and magnesium chloride; electrolyzing the first molten salt electrolyte with magnesium according to the parameters of the first electrolytic cell until the concentration of magnesium chloride in the first molten salt electrolyte is less than or equal to a preset concentration threshold, thereby obtaining a magnesium-electrolyzed molten salt electrolyte; adding lithium chloride to the magnesium-electrolyzed molten salt electrolyte to obtain a second molten salt electrolyte; and electrolyzing lithium according to the parameters of the second electrolytic cell to obtain a magnesium-lithium alloy. This invention electrolyzes magnesium and lithium in stages within the same electrolytic cell, utilizing the liquid magnesium generated in the initial electrolysis to capture the lithium deposited later, allowing the two metals to alloy directly in the cathode molten pool. This eliminates the intermediate step of separately preparing pure metals and then remelting them into an alloy, while also avoiding the parameter matching problems caused by differences in decomposition voltage in a co-electrolysis system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metal metallurgy technology, specifically to an electrolytic preparation method for magnesium-lithium alloys. Background Technology

[0002] Magnesium-lithium alloys are characterized by low density, high specific strength and specific stiffness, excellent damping performance and electromagnetic shielding performance, and are known as "ultra-light alloys". They have broad application prospects in aerospace, defense industry, 3C electronics, transportation and other fields.

[0003] Traditional magnesium-lithium alloy preparation methods mainly involve the doping method, which mixes pure metallic magnesium and pure metallic lithium in a certain proportion and then melts and casts them under a protective atmosphere. This requires the separate preparation of high-purity metallic magnesium and metallic lithium before a second melting and alloying process. The process is lengthy, energy-intensive, and costly. In addition, the chemical properties of metallic lithium are extremely reactive, which places stringent requirements on melting equipment and protective atmosphere, severely restricting the large-scale application of magnesium-lithium alloys.

[0004] To shorten the process and reduce production costs, the direct preparation of magnesium-lithium alloys via molten salt electrolysis has received widespread attention in recent years. This method involves the direct co-electrodeposition of magnesium and lithium from a chloride molten salt system to obtain the alloy in one step, eliminating the intermediate steps of separately preparing the elemental metals and then remelting them into an alloy. This approach offers significant advantages such as a shorter production process, lower energy consumption, and more uniform alloy composition. However, due to the electrode potential difference between magnesium and lithium, the magnesium chloride concentration must be strictly controlled within an extremely narrow window of 1–10 wt.%, resulting in a narrow process window and significant challenges for industrial-scale control. Summary of the Invention

[0005] (a) Purpose of the invention The purpose of this invention is to provide an electrolytic preparation method for magnesium-lithium alloys. By electrolyzing magnesium and lithium in stages in the same electrolytic cell, the liquid magnesium generated in the early electrolysis is used to capture the lithium deposited in the later stage, so that the two metals are directly alloyed in the cathode molten pool. This eliminates the intermediate step of preparing pure metals separately and then melting them into alloys, and avoids the parameter matching problem caused by the difference in decomposition voltage in the co-electrolysis system.

[0006] (II) Technical Solution To address the above problems, this invention provides an electrolytic preparation method for magnesium-lithium alloys, comprising: A first molten salt electrolyte is prepared, wherein the first molten salt electrolyte comprises potassium chloride and magnesium chloride; Using an electrolytic cell, the first molten salt electrolyte is subjected to magnesium electrolysis according to preset first electrolytic cell parameters until the concentration of magnesium chloride in the first molten salt electrolyte is less than or equal to a preset concentration threshold, thereby obtaining molten salt electrolyte after magnesium electrolysis. Lithium chloride is added to the molten salt electrolyte after magnesium electrolysis to obtain a second molten salt electrolyte; The second molten salt electrolyte is subjected to lithium electrolysis according to the preset parameters of the second electrolytic cell to obtain a magnesium-lithium alloy.

[0007] In another aspect of the present invention, preferably, the anode of the electrolytic cell is an inert metal or graphite, and the cathode of the electrolytic cell is a metal or conductive ceramic.

[0008] In another aspect of the present invention, preferably, the molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (0.5~2):1; the preset parameters of the first electrolytic cell include a first electrolysis temperature of 680~800℃, a first cathode current density of 0.5~5.0 A / cm², a first cell voltage of 3.5~7.0 V, and a first electrode spacing of 30~80 mm.

[0009] In another aspect of the present invention, preferably, the molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (1~1.5):1; the preset parameters of the first electrolytic cell include a first electrolysis temperature of 700~750℃, a first cathode current density of 1.0~2.5 A / cm², a first cell voltage of 4.5~6.0 V, and a first electrode spacing of 40~60 mm.

[0010] In another aspect of the present invention, preferably, the preset concentration threshold is 1 to 5 wt.% by mass percentage.

[0011] In another aspect of the present invention, preferably, the amount of lithium chloride added is 10-50% of the second molten salt electrolyte by mass percentage, and the amount of lithium chloride added is determined according to the lithium content in the target magnesium-lithium alloy and the amount of molten salt electrolyte after magnesium electrolysis.

[0012] In another aspect, preferably, the invention further includes the addition of additives and regulators when adding lithium chloride, said additives including potassium fluoride or sodium chloride, wherein the amount of said additives added is 1-8 wt.% of the second molten salt electrolyte. The regulator is potassium chloride.

[0013] In another aspect of the present invention, preferably, the preset parameters of the second electrolytic cell include a second electrolysis temperature of 350~450℃, a second cathode current density of 1.0~8.0 A / cm², a second cell voltage of 6.0~11.0 V, and a second electrode spacing of 40~100 mm.

[0014] In another aspect of the present invention, preferably, the concentration of lithium chloride in the second molten salt electrolyte is 20-40 wt.%; The preset parameters of the second electrolytic cell include a second electrolysis temperature of 380~420℃, a second cathode current density of 2.0~5.0 A / cm², a second cell voltage of 7.0~9.0 V, and a second electrode spacing of 50~80 mm.

[0015] In another aspect, preferably, the invention further includes: collecting the magnesium-lithium alloy from the electrolytic cell by skimming or siphoning.

[0016] (III) Beneficial Effects The above-described technical solution of the present invention has the following beneficial technical effects: This invention completes two stages of magnesium electrolysis and lithium electrolysis sequentially in the same electrolytic cell. First, liquid metallic magnesium is deposited using a first molten salt electrolyte containing magnesium ions. Then, lithium salt is added to the same electrolyte while switching electrolysis parameters, allowing lithium to be immediately captured and absorbed in situ by the existing liquid magnesium after deposition at the cathode, directly forming a magnesium-lithium alloy through liquid-phase diffusion. This completely avoids the parameter matching problem of existing co-electrodeposition methods, which require strict control of magnesium chloride concentration within a narrow range of 1–10 wt.%, and eliminates the limitation of co-deposition conditions caused by the approximately 0.4 V electrode potential difference between magnesium and lithium. By independently controlling the electrolysis parameters of the two stages, precise adjustment of the magnesium-lithium alloy composition across the entire range from the α phase (lithium < 5.7 wt.%) to the β phase (lithium > 10.3 wt.%) can be achieved. Utilizing the in-situ protection and rapid absorption mechanism of lithium by liquid magnesium, the magnesium-lithium alloy has uniform composition and high purity. The process is short, with low equipment investment and operating costs, and wide raw material adaptability, making it suitable for large-scale continuous production. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the structure of an electrolytic cell according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the overall process of one embodiment of the present invention; Figure label: 1: Tank body, 2: Anode assembly, 3: Cathode assembly, 4: Collection area, 5: Feeding system, 6: Heating and temperature control system, 7: Gas collection system. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and the accompanying drawings. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0019] The accompanying drawings show structural schematic diagrams according to embodiments of the present invention. These drawings are not drawn to scale, and some details have been enlarged for clarity, and some details may have been omitted. The shapes of the various regions and layers shown in the drawings, as well as their relative sizes and positional relationships, are merely exemplary and may deviate from reality due to manufacturing tolerances or technical limitations. Furthermore, those skilled in the art can design regions / layers with different shapes, sizes, and relative positions as needed.

[0020] Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0021] In the description of this invention, it should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0022] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0023] Example An electrolytic preparation method for magnesium-lithium alloys, utilizing the same electrolytic cell for electrolysis. Figure 1 A schematic diagram of the structure of an electrolytic cell according to an embodiment of the present invention is shown, as follows: Figure 1As shown, the electrolytic cell includes a tank body 1, an anode assembly 2, a cathode assembly 3, a collection area 4, a feeding system 5, a heating and temperature control system 6, and a gas collection system 7. The tank body 1 is made of a high-temperature resistant, molten salt corrosion resistant material, with an inner steel plate lined with nickel alloy or high-purity graphite. The tank body forms a sealed electrolytic chamber to contain the molten electrolyte and maintain a stable electrolytic environment. It also has reserved electrode mounting ports, a feeding port, and a gas outlet to meet the requirements of continuous electrolytic production. The anode assembly 2 is made of graphite or inert metal material, is adjustable in height, and is connected to the positive terminal of a DC power supply. The electrode spacing is controlled by adjusting the anode immersion depth. The current distribution within the electrolytic cell is optimized, and the cell voltage is reduced. The anode surface has good conductivity and resistance to chlorine corrosion. During electrolysis, chlorine ion discharge reaction mainly occurs to generate chlorine gas, ensuring long-term stable operation. The cathode assembly 3 can adopt a plate-shaped, rod-shaped, or bottom-type structure. The cathode material is preferably molybdenum, tungsten, or low-carbon steel. The cathode surface has liquid metal wettability to promote timely accumulation of electrodeposited metal and reduce adhesion loss. The cathode assembly is connected to the negative terminal of the DC power supply. The collection area 4 is located above the cathode of the electrolytic cell to receive and collect liquid metal products. Due to the density difference between the liquid magnesium-lithium alloy and the molten salt, the collection area... A flow guide plate, baffle, or collection tank can be installed to guide the continuous convergence of liquid metal and its separation from the electrolyte, thereby reducing metal re-oxidation or re-dissolution and improving product recovery rate. The feeding system 5 is used to quantitatively add materials to the electrolytic cell, such as magnesium chloride, lithium chloride, potassium fluoride, and potassium chloride. It can include a storage silo, metering device, screw feeder, or vibrating feeder. The feeding system controls the feeding based on the liquid level, electrolytic current, or molten salt composition. The heating and temperature control system 6 maintains the temperature inside the electrolytic cell, which can be in the range of 650~850℃. It is used to keep the molten salt in the electrolytic cell in a molten state and can employ resistance heating or induction heating. Alternatively, gas-assisted heating can be used. The temperature control system includes a temperature sensor, a controller, and a heating execution unit. It adjusts the heating power in real time through closed-loop feedback to keep the temperature fluctuation in the cell within a preset range. The gas collection system 7 is used to collect chlorine gas generated at the anode and may include a gas collection hood, corrosion-resistant gas pipelines, cooling and purification devices, and tail gas treatment devices. The chlorine gas released from the anode is transported to a chlorine storage or recycling system after being channeled through a closed system. It can also enter an absorption tower for purification to prevent chlorine gas leakage from causing equipment corrosion and environmental pollution. At the same time, it maintains stable atmospheric conditions in the electrolytic cell, improving production safety and resource utilization.

[0024] Figure 2 An overall flowchart of one embodiment of the present invention is shown, as follows: Figure 2As shown, the preparation method includes: preparing a first molten salt electrolyte, which comprises potassium chloride and magnesium chloride; the first molten salt electrolyte is a KCl-MgCl2 binary system, and the molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (0.5~2):1, specifically 0.5:1, 0.6:1, 0.8:1, 1.0:1, 1.2:1, 1.5:1, 1.8:1, or 2.0:1, or any value between the above values. The purpose of adding KCl is to lower the melting point and viscosity of the first molten salt electrolyte and improve its conductivity. Since KCl and MgCl2 can form a low-melting-point eutectic system, the molten salt can maintain good fluidity and ion migration ability at lower temperatures, thereby reducing electrolysis energy consumption, improving current distribution, increasing the mass transfer rate of magnesium ions and cathode deposition efficiency, while reducing equipment corrosion and magnesium volatilization loss under high-temperature conditions, and improving the stability of the electrolysis process. In this embodiment, the magnesium electrolysis does not require strict control of the magnesium chloride concentration within a narrow range. Instead, it is allowed to fluctuate naturally within a wider range as the electrolysis process and raw material replenishment occur. Stable electrolysis can be maintained without frequent detection and adjustment of the electrolyte composition, thereby reducing the complexity of process control and production costs. The eutectic point temperature of the KCl-MgCl2 system is 424℃ (KCl-MgCl2 molar ratio is approximately 58:42).

[0025] An electrolytic cell is used, with the anode being an inert metal or graphite, and the cathode being a metal or conductive ceramic. High-temperature conductive metals such as molybdenum, tungsten, nickel, and low-carbon steel, or conductive ceramic materials such as TiB2 and TiC, can be used. The anode is connected to the positive terminal of a DC power supply for the oxidation reaction of chloride ions to generate chlorine gas. The cathode is connected to the negative terminal of a DC power supply for the reduction and precipitation of magnesium and lithium ions. Preferably, the cathode surface has good wettability to liquid magnesium-lithium alloy to promote the timely aggregation and detachment of the precipitated liquid magnesium-lithium alloy from the electrode surface, reducing metal back-dissolution and side reactions, and improving current efficiency and magnesium-lithium alloy yield.

[0026] Magnesium electrolysis is performed on the first molten salt electrolyte according to the preset first electrolytic cell parameters until the concentration of magnesium chloride in the first molten salt electrolyte is less than or equal to the preset concentration threshold, thereby obtaining the molten salt electrolyte after magnesium electrolysis; the molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (0.5~2):1, specifically it can be 0.5:1, 0.6:1, 0.8:1, 1.0:1, 1.2:1, 1.5:1, 1.8:1 or 2.0:1, or any value between the above values, which can keep the molten salt system at a low melting point, suitable viscosity and high ionic conductivity, thereby ensuring that magnesium ions have good mass transfer ability, reducing the ohmic voltage drop of the electrolytic cell and improving current efficiency. The preset parameters for the first electrolytic cell include a first electrolysis temperature of 680~800℃, specifically 680℃, 700℃, 720℃, 740℃, 760℃, 780℃, or 800℃, or any value between these values. This ensures good fluidity and conductivity of the KCl-MgCl2 molten salt system while preventing excessively high temperatures from increasing magnesium volatilization losses and exacerbating equipment corrosion. The first cathode current density is 0.5~5.0 A / cm², specifically 0.5A / cm², 1.0A / cm², 1.5A / cm², 2.0A / cm², 2.5A / cm², 3.0A / cm², 3.5A / cm², 4.0A / cm², 4.5A / cm², or 5.0A / cm², or any value between these values. The first cell voltage is 3.5~7.0 A / cm². The voltage (V) can be 3.5V, 4.0V, 4.5V, 5.0V, 5.5V, 6.0V, 6.5V, or 7.0V, or any value between these values; the first electrode spacing is 30~80mm, specifically 30mm, 35mm, 40mm, 45mm, 50mm, 55mm, 60mm, 65mm, 70mm, 75mm, or 80mm, or any value between these values. During electrolysis, metallic magnesium is deposited in liquid form on the cathode surface. Due to the density of liquid magnesium (approximately 1.58 g / cm³),... 3 It is less than that of the first molten salt electrolyte (approximately 2.2~2.5 g / cm³). 3 The generated metallic magnesium will float to the electrolyte surface or collect in the collection area above the cathode, facilitating subsequent contact and alloying with the lithium generated during electrolysis. Furthermore, the concentration of magnesium chloride in the first molten salt electrolyte is less than or equal to a preset concentration threshold, which is 1~5 wt.% by mass percentage. The endpoint of magnesium electrolysis can be determined by the following method: when the electrolytic cell voltage rises significantly, exceeding 0.5V relative to the stable electrolysis stage, or the current efficiency decreases significantly, it indicates that the magnesium chloride concentration in the electrolyte has decreased to a level that cannot sustain normal magnesium electrolysis, at which point the magnesium electrolysis stage ends.

[0027] Furthermore, in this embodiment, the molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (1~1.5):1; the preset parameters of the first electrolytic cell include a first electrolysis temperature of 700~750℃, a first cathode current density of 1.0~2.5 A / cm², a first cell voltage of 4.5~6.0 V, and a first electrode spacing of 40~60 mm. A good balance can be achieved between the stability of the molten salt system, current efficiency, magnesium recovery rate, and unit energy consumption, which can further improve the continuous precipitation effect of liquid magnesium.

[0028] Anhydrous lithium chloride is added to the molten salt electrolyte after magnesium electrolysis to obtain a second molten salt electrolyte. A regulator, such as potassium chloride, can be added to adjust the overall composition of the second molten salt electrolyte. Since MgCl2 is continuously consumed during the first stage of electrolysis, the composition of the molten salt changes. Therefore, adding potassium chloride can adjust the proportions of each component in the second molten salt electrolyte, maintaining a suitable liquid phase region, ionic conductivity, and fluidity. The amount of lithium chloride added is 10-50% by mass of the second molten salt electrolyte, specifically 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50%, or any value between these values. The amount of lithium chloride added is determined based on the lithium content in the target magnesium-lithium alloy and the amount of molten salt electrolyte after magnesium electrolysis to ensure that the final magnesium-lithium alloy achieves the expected composition. Lithium chloride can be added all at once, or added in batches or continuously to the molten salt electrolyte after magnesium electrolysis. The second molten salt electrolyte is a ternary molten salt system of KCl-MgCl2-LiCl. LiCl serves as the source of lithium ions, providing lithium ions during subsequent electrolysis. KCl is used to lower the melting point of the system, improve the fluidity of the molten salt, and increase the conductivity. The residual MgCl2 can maintain the stability of the molten salt system composition and further improve the migration environment of lithium ions, giving the entire ternary molten salt system a wide liquid phase region and good electrolytic stability. To reduce electrolyte volatilization loss and lower the melting point, in this embodiment, an additive is added when lithium chloride is added. The additive includes potassium fluoride or sodium chloride. The amount of the additive added is 1 to 8 wt.% of the second molten salt electrolyte, specifically 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, or 8 wt.%, or any value between these values. When the additive is potassium fluoride, fluoride ions can improve the structure of the molten salt system, reduce the surface tension of the molten salt, reduce the volatilization loss of LiCl and MgCl2 at high temperatures, and also improve the wettability and ion migration ability of the molten salt. When the additive is sodium chloride, the composition of the molten salt can be further adjusted, the liquid phase region of the ternary molten salt system can be expanded, the system viscosity can be reduced, the flow properties can be improved, and the cost of molten salt raw materials can be reduced.

[0029] Lithium-ion alloy is obtained by lithium electrolysis of the second molten salt electrolyte according to preset second electrolytic cell parameters. The preset second electrolytic cell parameters include a second electrolysis temperature of 350~450℃, specifically 350℃, 380℃, 400℃, 420℃, 450℃, etc., or any value between these values. This ensures the second molten salt electrolyte remains fully molten and possesses good fluidity and ion migration ability, facilitating lithium ion migration to the cathode region. Simultaneously, it avoids excessively high temperatures leading to increased lithium chloride volatilization, accelerated liquid lithium evaporation loss, and increased electrolytic cell corrosion rate. The second cathode current density is 1.0~8.0 A / cm², and can be 1.0 A / cm², 2.0 A / cm², 3.0 A / cm², 4.0 A / cm², 5.0 A / cm², 6.0 A / cm², 7.0 A / cm², or 8.0 A / cm², etc., or any value between these values. This ensures the lithium ion reduction rate matches the lithium ion replenishment rate in the molten salt. The voltage of the second cell is 6.0~11.0V, which can be 6.0V, 7.0V, 8.0V, 9.0V, 10.0V, or 11.0V, or any value between these values; this allows lithium to be effectively deposited from the molten salt system while avoiding increased energy consumption and electrode side reactions caused by excessively high cell voltage. The spacing between the second electrodes is 40~100 mm, which can be 40mm, 50mm, 60mm, 70mm, 80mm, 90mm, or 100mm, or any value between these values, achieving a balance between reducing molten salt resistance loss and ensuring a safe distance between electrodes. Further, in this embodiment, the concentration of lithium chloride in the second molten salt electrolyte is 20~40 wt.%; the preset parameters of the second electrolytic cell include a second electrolysis temperature of 380~420℃, a second cathode current density of 2.0~5.0 A / cm², a second cell voltage of 7.0~9.0 V, and a second electrode spacing of 50~80 mm. It can achieve stable lithium deposition and in-situ alloying with liquid magnesium in the same electrolytic cell, reduce oxidation loss caused by intermediate transfer process, and improve the preparation efficiency, composition uniformity and product quality of magnesium-lithium alloy.

[0030] Furthermore, in this embodiment, the method further includes collecting the magnesium-lithium alloy from the electrolytic cell using a skimming-type mechanical scooping or siphoning method. Since the density of the magnesium-lithium alloy is lower than that of the molten salt electrolyte, the alloy floats on the electrolyte surface and can be collected using a skimming-type mechanical scooping or siphoning method. The collected alloy is cooled under an inert atmosphere to obtain a magnesium-lithium alloy ingot.

[0031] Example 1 The objective was to prepare an α-phase magnesium-lithium alloy with lithium content of 5 wt.%.

[0032] Anhydrous KCl and MgCl2 were mixed at a molar ratio of 1.2:1, with a total mass of 5 kg, and placed in an electrolytic cell and heated to 720℃ to melt. A 50 mm diameter high-purity graphite rod was used as the anode, and a low-carbon steel plate as the cathode, with a cathode current density of 1.5 A / cm². 2 Electrolysis was performed for 2 hours at a cell voltage of 5.2V, with a total charge of approximately 540Ah. Approximately 243g of metallic magnesium was deposited, and the MgCl2 concentration in the electrolyte decreased from an initial 42wt.% to approximately 5wt.%. The metallic magnesium generated during electrolysis floated on the electrolyte surface.

[0033] 500g of anhydrous LiCl was added to the electrolytic cell to achieve a LiCl mass fraction of approximately 25 wt.% in the molten salt, and the electrolysis temperature was adjusted to 400℃. The same cathode was maintained; at this point, the cathode surface was covered with a layer of liquid magnesium, and the cathode current density was 3.0 A / cm². 2 Electrolysis continued for 40 minutes at a cell voltage of 8.2V, with an applied charge of approximately 120Ah, resulting in the deposition of approximately 12.5g of metallic lithium. The newly deposited lithium was immediately absorbed by the liquid magnesium in the molten pool, forming a magnesium-lithium alloy.

[0034] After electrolysis, the floating magnesium-lithium alloy was skimmed off with a graphite spoon and cooled under argon protection to obtain approximately 255g of magnesium-lithium alloy. ICP analysis showed that the lithium content was 5.2wt.%, indicating that it was an α-phase magnesium-lithium alloy.

[0035] Example 2 The objective was to prepare a β-phase magnesium-lithium alloy with lithium content of 12 wt.%.

[0036] Approximately 200g of metallic magnesium was deposited. After switching the electrolyte, the lithium electrolysis time was 90 minutes, and the charge was approximately 260Ah. Approximately 27g of metallic lithium was deposited. The remaining parameters were the same as in Example 1, resulting in approximately 227g of magnesium-lithium alloy with a lithium content of 11.8wt.%, which was a β-phase magnesium-lithium alloy.

[0037] Example 3 When adding lithium chloride, 3 wt.% KF was added as an additive, and the remaining parameters were the same as in Example 1.

[0038] Example 4 The cathode current density during the magnesium electrolysis stage is 1.0 A / cm². 2 The remaining parameters are the same as in Example 1.

[0039] Example 5 The cathode current density during the magnesium electrolysis stage is 1.5 A / cm². 2 The remaining parameters are the same as in Example 1.

[0040] Example 6 The cathode current density during the magnesium electrolysis stage is 2.0 A / cm². 2The remaining parameters are the same as in Example 1.

[0041] Example 7 Anhydrous KCl and MgCl2 were mixed at a molar ratio of 0.5:1 and placed in an electrolytic cell, then heated to 680℃ to melt. A 50mm diameter high-purity graphite rod was used as the anode, and a low-carbon steel plate as the cathode, with a cathode current density of 0.5 A / cm². 2 Electrolysis was performed under a cell voltage of 3.5V, and the magnesium metal generated during the electrolysis process floated on the surface of the electrolyte.

[0042] Anhydrous LiCl was added to the electrolytic cell to achieve a LiCl mass fraction of approximately 10 wt.% in the molten salt, and the electrolysis temperature was adjusted to 350°C. The same cathode was maintained; at this point, the cathode surface was covered with a layer of liquid magnesium, and the cathode current density was 1.0 A / cm². 2 Electrolysis continues under a cell voltage of 6.0V, and the deposited lithium is immediately absorbed by the liquid magnesium in the molten pool to form a magnesium-lithium alloy.

[0043] After electrolysis, the floating magnesium-lithium alloy is skimmed off with a graphite spoon and cooled under argon protection to obtain the magnesium-lithium alloy.

[0044] Example 8 Anhydrous KCl and MgCl2 were mixed in a molar ratio of 2:1 and placed in an electrolytic cell, then heated to 800℃ to melt. A 50mm diameter high-purity graphite rod was used as the anode, and a low-carbon steel plate as the cathode, with a cathode current density of 5.0 A / cm². 2 Electrolysis was performed under a cell voltage of 7.0V, and the magnesium metal generated during the electrolysis process floated on the surface of the electrolyte.

[0045] Anhydrous LiCl was added to the electrolytic cell to achieve a LiCl mass fraction of approximately 50 wt.% in the molten salt, and the electrolysis temperature was adjusted to 450℃. The same cathode was maintained; at this point, the cathode surface was covered with a layer of liquid magnesium, and the cathode current density was 8.0 A / cm². 2 Electrolysis continues under a cell voltage of 11.0V, and the precipitated lithium is immediately absorbed by the liquid magnesium in the molten pool to form a magnesium-lithium alloy.

[0046] After electrolysis, the floating magnesium-lithium alloy is skimmed off with a graphite spoon and cooled under argon protection to obtain the magnesium-lithium alloy.

[0047] Example 9 Anhydrous KCl and MgCl2 were mixed in a 1:1 molar ratio and placed in an electrolytic cell, then heated to 700℃ to melt. A 50mm diameter high-purity graphite rod was used as the anode, and a low-carbon steel plate as the cathode, with a cathode current density of 1.0 A / cm². 2 Electrolysis was performed under a cell voltage of 4.5V, and the magnesium metal generated during the electrolysis process floated on the surface of the electrolyte.

[0048] Anhydrous LiCl was added to the electrolytic cell to achieve a LiCl mass fraction of approximately 20 wt.% in the molten salt, and the electrolysis temperature was adjusted to 380℃. The same cathode was maintained; at this point, the cathode surface was covered with a layer of liquid magnesium, and the cathode current density was 2.0 A / cm². 2 Electrolysis continues under a cell voltage of 7.0V, and the precipitated lithium is immediately absorbed by the liquid magnesium in the molten pool to form a magnesium-lithium alloy.

[0049] After electrolysis, the floating magnesium-lithium alloy is skimmed off with a graphite spoon and cooled under argon protection to obtain the magnesium-lithium alloy.

[0050] Example 10 Anhydrous KCl and MgCl2 were mixed at a molar ratio of 1.5:1 and placed in an electrolytic cell, then heated to 750℃ to melt. A 50mm diameter high-purity graphite rod was used as the anode, and a low-carbon steel plate as the cathode, with a cathode current density of 2.5 A / cm². 2 Electrolysis was performed under a cell voltage of 6.0V, and the magnesium metal generated during the electrolysis process floated on the surface of the electrolyte.

[0051] Anhydrous LiCl was added to the electrolytic cell to achieve a LiCl mass fraction of approximately 40 wt.% in the molten salt, and the electrolysis temperature was adjusted to 420℃. The same cathode was maintained; at this point, the cathode surface was covered with a layer of liquid magnesium, and the cathode current density was 5.0 A / cm². 2 Electrolysis continues under a cell voltage of 9.0V, and the precipitated lithium is immediately absorbed by the liquid magnesium in the molten pool to form a magnesium-lithium alloy.

[0052] After electrolysis, the floating magnesium-lithium alloy is skimmed off with a graphite spoon and cooled under argon protection to obtain the magnesium-lithium alloy.

[0053] Comparative Example 1 Magnesium-lithium alloys were prepared using a molten salt electrolytic co-electrodeposition method, a traditional co-deposition technique. A LiCl-KCl (mass ratio 1:1) electrolyte system was used, with MgCl2 added to maintain an initial concentration of 5 wt.%. Co-electrodeposition was performed at 670 °C using a graphite anode and a molybdenum cathode, with a cathode current density of 6.2 A / cm². 2 The cell voltage is approximately 7.0V. By controlling the MgCl2 concentration and the amount of electricity used in electrolysis, a magnesium-lithium alloy with a lithium content of approximately 8 wt.% is prepared.

[0054] Four hours after co-electrodeposition, ICP analysis revealed a lithium content of 6.5 wt.% in the alloy, lower than the target value of 8 wt.%, and the lithium content at different locations within the same batch of alloy varied by ±1.8 wt.%, indicating poor compositional uniformity. The current efficiency was approximately 76%, and the cell voltage fluctuation range was approximately ±600 mV. This is because the MgCl2 concentration continuously decreased during electrolysis, leading to a constant change in the effective magnesium ion concentration participating in co-deposition, resulting in unstable lithium deposition behavior. Metallographic observation of the alloy sample cross-section showed obvious compositional segregation regions, with the alloy structure consisting of an α-phase matrix and segregated phases.

[0055] Comparative Example 2 Magnesium-lithium alloys were prepared using a solid-state cathode diffusion method, a traditional diffusion process. A 5mm thick magnesium plate was used as the cathode, and LiCl-KCl (mass ratio 1:1) was used as the electrolyte. Electrolysis was performed at 450℃ with a current density of 0.1 A / cm². 2 Lithium is deposited on a solid magnesium cathode and diffused into the interior by controlling the cathode potential (refer to method CN101376992A).

[0056] After electrolysis, the cathode was removed for testing. ICP layer analysis revealed a lithium content of approximately 12 wt.% on the cathode surface, while the lithium content in the cathode core was only about 2 wt.%, showing a significant concentration gradient from the surface to the core, indicating extremely uneven alloy composition. Only one magnesium cathode could be processed per electrolysis cycle, and a new cathode had to be replaced after each cycle to continue, representing a typical intermittent operation. The current efficiency was approximately 65%, far lower than that of the embodiments of this invention. Metallographic observation of the alloy cross-section showed a clear gradient distribution of lithium elements from the surface to the core, rather than a uniform alloy structure.

[0057] Table 1 shows the detection results of Examples 1-10 and Comparative Examples 1 and 2. The detection method was ICP stratification analysis.

[0058] Table 1. Detection results of Examples 1-10 and Comparative Examples 1 and 2 As shown in Table 1, Examples 1-10 are superior to the comparative examples and completely avoid the parameter matching problem of existing co-electrodeposition methods that require strict control of magnesium chloride concentration within a narrow range of 1-10 wt.%, eliminating the limitation of co-deposition conditions by the approximately 0.4 V electrode potential difference between magnesium and lithium; by independently controlling the electrolysis parameters of the two stages, precise adjustment of the magnesium-lithium alloy composition across the entire range from α phase (lithium < 5.7 wt.%) to β phase (lithium > 10.3 wt.%) can be achieved.

[0059] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.

[0060] The present invention has been described above with reference to embodiments thereof. However, these embodiments are merely illustrative and not intended to limit the scope of the invention. The scope of the invention is defined by the appended claims and their equivalents. Various substitutions and modifications can be made by those skilled in the art without departing from the scope of the invention, and all such substitutions and modifications should fall within the scope of the invention.

[0061] Although embodiments of the present invention have been described in detail, it should be understood that various changes, substitutions, and modifications can be made to the embodiments of the present invention without departing from the spirit and scope of the invention.

[0062] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for the electrolytic preparation of a magnesium-lithium alloy, characterized in that, include: A first molten salt electrolyte is prepared, wherein the first molten salt electrolyte comprises potassium chloride and magnesium chloride; Using an electrolytic cell, the first molten salt electrolyte is subjected to magnesium electrolysis according to preset first electrolytic cell parameters until the concentration of magnesium chloride in the first molten salt electrolyte is less than or equal to a preset concentration threshold, thereby obtaining molten salt electrolyte after magnesium electrolysis. Lithium chloride is added to the molten salt electrolyte after magnesium electrolysis to obtain a second molten salt electrolyte; The second molten salt electrolyte is subjected to lithium electrolysis according to the preset parameters of the second electrolytic cell to obtain a magnesium-lithium alloy.

2. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, The anode of the electrolytic cell is an inert metal or graphite, and the cathode of the electrolytic cell is a metal or conductive ceramic.

3. The electrolytic preparation method of magnesium-lithium alloy according to claim 2, characterized in that, The molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (0.5~2):1; the preset parameters of the first electrolytic cell include a first electrolysis temperature of 680~800℃, a first cathode current density of 0.5~5.0 A / cm², a first cell voltage of 3.5~7.0 V, and a first electrode spacing of 30~80 mm.

4. The electrolytic preparation method of magnesium-lithium alloy according to claim 3, characterized in that, The molar ratio of potassium chloride to magnesium chloride in the first molten salt electrolyte is (1~1.5):1; the preset parameters of the first electrolytic cell include a first electrolysis temperature of 700~750℃, a first cathode current density of 1.0~2.5 A / cm², a first cell voltage of 4.5~6.0 V, and a first electrode spacing of 40~60 mm.

5. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, The preset concentration threshold, expressed as a percentage by mass, is 1 to 5 wt.%.

6. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, The amount of lithium chloride added is 10-50% of the second molten salt electrolyte by mass percentage, and the amount of lithium chloride added is determined according to the lithium content in the target magnesium-lithium alloy and the amount of molten salt electrolyte after magnesium electrolysis.

7. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, It also includes the addition of additives and regulators when adding lithium chloride, wherein the additives include potassium fluoride or sodium chloride, and the amount of the additives added is 1-8 wt.% of the second molten salt electrolyte. The regulator is potassium chloride.

8. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, The preset parameters of the second electrolytic cell include a second electrolysis temperature of 350~450℃, a second cathode current density of 1.0~8.0 A / cm², a second cell voltage of 6.0~11.0 V, and a second electrode spacing of 40~100 mm.

9. The electrolytic preparation method of magnesium-lithium alloy according to claim 8, characterized in that, The concentration of lithium chloride in the second molten salt electrolyte is 20~40 wt.%; The preset parameters of the second electrolytic cell include a second electrolysis temperature of 380~420℃, a second cathode current density of 2.0~5.0 A / cm², a second cell voltage of 7.0~9.0 V, and a second electrode spacing of 50~80 mm.

10. The electrolytic preparation method of magnesium-lithium alloy according to claim 1, characterized in that, Also includes: The magnesium-lithium alloy is collected from the electrolytic cell by skimming or siphoning.

Citation Information

Patent Citations

  • Method for preparing magnesium lithium alloy by fused salt electrolysis process

    CN101376992A