A corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers and its preparation method

By constructing a nickel-based composite coating on the surface of the heat exchanger and embedding core-shell composite microparticles to form a sandwich structure, the corrosion, wear, and fouling problems of the heat exchanger under high temperature and high pressure environments are solved, thereby improving corrosion resistance, wear resistance, and fouling resistance, extending equipment life and reducing operation and maintenance costs.

CN123108680APending Publication Date: 2026-11-17YANGTZE NORMAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611306547.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing heat exchanger coatings are prone to corrosion, wear, and fouling under high temperature, high pressure, and complex corrosive media environments, leading to shortened equipment lifespan and increased operation and maintenance costs. Existing technologies cannot simultaneously solve the multiple failure problems of corrosion, wear, and fouling.

Method used

A nickel-based composite coating is used to construct a sandwich microstructure by embedding core-shell composite microparticles in the nickel coating. The core-shell composite microparticles consist of a wear-resistant core composed of silicon carbide and aluminum oxide, an intermediate bridging layer of graphene oxide, and a hydrophobic modification layer of polytetrafluoroethylene. Combined with a multi-component anion-cation compound dispersant and a symmetrical pulse electrodeposition process, a dense nickel-based composite coating is formed.

Benefits of technology

It significantly improves the corrosion resistance, wear resistance and scale resistance of the coating, extends the service life of equipment, reduces operation and maintenance costs, adapts to high temperature alternating working conditions, and has strong coating adhesion to prevent media penetration and particle peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108680A_ABST
    Figure CN123108680A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal surface treatment and heat exchanger protection technology, specifically to a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers and its preparation method. The composite coating employs a sandwich microstructure consisting of an inner nickel substrate, an intermediate layer containing (SiC / Al2O3)@graphene oxide@PTFE core-shell composite microparticles, and a surface layer of dense nickel. It is prepared on a pretreated substrate surface using a multi-component anion-cation composite dispersion system combined with a symmetrical pulse electrodeposition process, incorporating stirring and an ultrasonic composite flow field. The core-shell microparticles utilize SiC-Al2O3 multiphase ceramic powder as a wear-resistant core, graphene oxide as an anti-corrosion bridging layer, and PTFE as a hydrophobic modification layer. These microparticles are partially embedded within the nickel coating and partially exposed on the coating surface, locked together by the double-layer nickel intercalation. This invention can simultaneously improve the coating's corrosion resistance, wear resistance, and scale resistance, resulting in strong coating adhesion, low internal stress, and excellent plating solution dispersion stability, effectively extending the service life of the heat exchanger.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal surface treatment and heat exchanger protection technology, specifically to a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers and its preparation method. Background Technology

[0002] Heat exchangers are core heat exchange equipment in industries such as chemical, power, and metallurgy. Their inner walls are subjected to high temperature, high pressure, and complex corrosive media environments for extended periods, making them prone to coupled failures due to corrosion, wear, and scale buildup. This significantly shortens equipment lifespan and increases maintenance costs; even a mere 1mm of scale can reduce heat exchange efficiency by more than 10%, hindering continuous and stable production. Existing technologies, such as Chinese patent CN1228467C, disclose a nickel-phosphorus-based composite coating containing silicon carbide and polytetrafluoroethylene (PTFE). This technology uses a chemically plated nickel-phosphorus alloy as the substrate, directly and physically mixing hard silicon carbide powder and PTFE powder, and simultaneously depositing them to obtain a two-phase hybrid composite coating. This coating balances basic wear resistance with short-term hydrophobic lubrication, and the chemical plating process has strong adaptability to workpiece shapes.

[0003] However, the aforementioned nickel-phosphorus-based composite coating still has significant technical shortcomings. It only uses two types of particles for simple physical mixing, resulting in poor interfacial bonding between inorganic ceramic particles and organic fluoroplastics, and the powder is prone to agglomeration in the plating solution. All functional particles are randomly dispersed inside the nickel-phosphorus matrix, while polytetrafluoroethylene, which serves as a lubricating phase, is directly exposed on the coating surface and is easily lost under long-term media erosion. At the same time, there are a large number of gaps and micropores at the interface between the particles and the metal matrix, allowing corrosive media to easily penetrate into the coating. This technology uses only a single type of surfactant to disperse the powder, which has limited ability to stabilize multiphase nanoparticles. The powder needs to undergo high-temperature modification pretreatment in advance, making the process relatively complex. Furthermore, it adopts a chemical autocatalytic deposition method, which cannot control grain growth through electrical parameters. The coating grain size is large, the internal residual stress is high, and the bonding strength between the coating and the metal matrix is ​​limited, making it prone to microcracks under alternating temperature environments.

[0004] In addition, other similar coating technologies in the industry also have their own limitations. Nickel plating with only graphene can only improve corrosion resistance, but does not have wear resistance, hydrophobic and scale inhibition capabilities; core-shell powder with two-layer coating structure lacks hydrophobic modification components; ordinary DC electroplating lacks flow field synergistic control methods, making it difficult to eliminate powder agglomeration and coating porosity defects. At present, there is no integrated coating solution that can simultaneously solve the multiple failure problems of corrosion, wear and scale accumulation in heat exchange equipment under high-temperature conditions.

[0005] Therefore, in view of the above situation, there is an urgent need to develop a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers and its preparation method, so as to overcome the shortcomings in current practical applications. Summary of the Invention

[0006] The purpose of this invention is to provide a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers and its preparation method, so as to solve the problems mentioned in the background art.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] A corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers includes a nickel coating deposited on the surface of a workpiece substrate, and core-shell composite microparticles dispersed and embedded inside the nickel coating. The nickel-based composite coating as a whole consists of an inner nickel substrate, an intermediate layer with distributed core-shell composite microparticles, and a surface dense nickel layer forming a sandwich microstructure.

[0009] The core-shell composite microparticles use a multiphase ceramic powder composed of silicon carbide and aluminum oxide as the wear-resistant core, graphene oxide as the intermediate bridging coating layer, and polytetrafluoroethylene as the outer hydrophobic modification layer; part of the core-shell composite microparticles are embedded inside the nickel plating layer, and part of them are exposed on the outer surface of the nickel plating layer.

[0010] As a further aspect of the present invention: the core-shell composite microparticles are uniformly dispersed between the inner nickel substrate and the surface dense nickel, and the surface dense nickel fills the interfacial gaps of the core-shell composite microparticles to block the penetration channels of the corrosive medium and inhibit the corrosive medium from penetrating into the coating.

[0011] As a further aspect of the present invention: the total thickness of the nickel-based composite coating is 25μm to 35μm;

[0012] The core-shell composite microparticles account for 8.0 wt% to 12.0 wt% of the mass of the coating.

[0013] The exposed core-shell composite particles account for 10% to 30% of the total area.

[0014] As a further aspect of the present invention: the water contact angle of the nickel-based composite coating is 130° to 150°, the micro Vickers hardness is not less than 580 HV, and the neutral salt spray test durability time is not less than 480 h.

[0015] The corrosion current density is not higher than 3.0 × 10⁻⁶. -7 A / cm 2 The wear rate is no higher than 4.0 × 10⁻⁶. -6 mm 3 / (N·m), the amount of dirt adhering under simulated working conditions for 72 hours should not exceed 5.0 mg / cm³. 2 The peel strength of the coating is not less than 55 N / cm.

[0016] As a further embodiment of the present invention: the substrate is a carbon steel substrate, an aluminum alloy substrate, or a copper alloy substrate;

[0017] When the substrate is an aluminum alloy substrate, a dense zinc transition layer is also provided between the substrate and the inner nickel substrate.

[0018] A method for preparing the above-mentioned anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers specifically includes the following steps:

[0019] (1) Substrate pretreatment: The workpiece substrate surface is successively ground and polished, ultrasonically degreased, and surface activated, and then washed with water for later use;

[0020] (2) Preparation of core-shell composite microparticle dispersion: Silicon carbide nanoparticles and aluminum oxide nanoparticles were added to graphene oxide aqueous dispersion and subjected to first ultrasonic dispersion treatment to obtain an intermediate suspension of graphene oxide-coated ceramic particles.

[0021] Polytetrafluoroethylene emulsion was added to the intermediate suspension, and then subjected to a second ultrasonic dispersion treatment to obtain a (SiC / Al2O3)@graphene oxide@polytetrafluoroethylene core-shell composite microparticle suspension.

[0022] (3) Preparation of composite plating solution: Add a multi-component anion and cation compound dispersant to the nickel-based plating solution, stir evenly, and then add the core-shell composite microparticle suspension. Mix by mechanical stirring and ultrasonication to obtain a uniform and stable composite plating solution.

[0023] (4) Pulse electrodeposition: The pretreated substrate is used as the cathode and the nickel plate is used as the anode. A symmetrical pulse electrodeposition process is used for deposition. During the deposition process, mechanical stirring and ultrasonic action are applied simultaneously to form a nickel-based composite coating with a sandwich microstructure on the substrate surface.

[0024] As a further aspect of the present invention: the multi-component anionic and cationic compound dispersant is composed of anionic dispersant, nonionic dispersant and cationic dispersant;

[0025] The anionic dispersant is composed of sodium dodecyl sulfate and sodium hexametaphosphate, or of sodium dodecyl sulfate, sodium hexametaphosphate and sodium α-alkenyl sulfonate;

[0026] The nonionic dispersant is polyethylene glycol, and the cationic dispersant is polyquaternium-10.

[0027] As a further aspect of the present invention: the nickel-based plating solution uses nickel sulfate and nickel chloride as the main salts, boric acid as the pH buffer, and also adds sodium citrate complexing agent and sodium saccharin brightener.

[0028] As a further aspect of the present invention: the process parameters for the pulse electrodeposition are as follows:

[0029] The pulse frequency is 50Hz–90Hz, the duty cycle is 30%–50%, and the cathode current density is 2A / dm².2 ~4A / dm 2 The plating solution temperature is 50℃~60℃, and the distance between the anode and the cathode is 5cm~7cm.

[0030] As a further aspect of the present invention: in step (1), when the substrate is an aluminum alloy substrate, a zinc transition layer is prepared by a double zinc immersion process after surface activation treatment;

[0031] The double zinc immersion process is as follows: first, zinc is immersed once, then zinc is removed by nitric acid solution, and then zinc is immersed a second time.

[0032] Compared with the prior art, the beneficial effects of the present invention are:

[0033] The system employs a multi-component anion-cation compound dispersion system combined with an ultrasonic-stirring composite flow field, resulting in a sedimentation rate of ≤6% after 48 hours of standing of the plating solution, with no obvious particle agglomeration. At the same time, it eliminates the need for separate powder modification, simplifies the production process, and is compatible with industrial-grade raw materials.

[0034] By bidirectionally encapsulating and locking the core and shell of multifunctional microparticles with an inner nickel substrate and a dense outer nickel layer, wear-resistant ceramics, corrosion-resistant graphene oxide, and hydrophobic polytetrafluoroethylene are embedded in the coating and the microparticles are partially exposed on the coating surface, preventing the polytetrafluoroethylene from falling off due to surface wear. The nickel layer seals the micropores between the particles, blocking the penetration channels of corrosive media and inhibiting the penetration of corrosive media into the coating. The core and shell microparticles are pinned by the nickel coating, and no peeling of the core and shell microparticles was observed under the conditions of hot and cold cycles and long-term media scouring, which can adapt to the high-temperature alternating operating conditions of heat exchangers.

[0035] In terms of corrosion resistance, the coating undergoes a salt spray test for ≥480 hours, with a corrosion current density ≤3.0×10⁻⁶. -7 A / cm 2 Graphene oxide can form a continuous passivation barrier to block corrosion ions; in terms of wear resistance, silicon carbide and aluminum oxide synergistically improve the micro Vickers hardness of the coating to ≥580HV, and the wear rate to ≤4.0×10⁻⁶. -6 mm 3 / (N·m), capable of withstanding long-term scouring by the medium; in terms of anti-fouling performance, the PTFE constructs a highly hydrophobic surface with a water contact angle of 130°~150°, and the amount of dirt adhering under 72h simulated working conditions is ≤5.0mg / cm³. 2 It can alleviate the problem of heat exchange efficiency reduction caused by scale; at the same time, the coating has excellent adhesion, the coating peel strength is ≥55N / cm, and no cracks are generated after 10 cycles of cold and hot cycling from -40℃ to 120℃.

[0036] The symmetrical pulse electrodeposition method can refine the grains and release the internal stress of the coating. It is compatible with various heat exchanger substrates such as carbon steel, aluminum alloy and copper alloy. The formula range is wide, which can relax the requirements for water quality and equipment precision. It has high production efficiency and can be used in batches for the protection treatment of large heat exchange pipelines in the chemical, power and metallurgical fields. Attached Figure Description

[0037] Figure 1 This is a flowchart illustrating the preparation process of the nickel-based composite coating in an embodiment of the present invention.

[0038] Figure 2 This is a schematic diagram of the microstructure of the nickel-based composite coating in an embodiment of the present invention.

[0039] Figure 3 This is a schematic diagram of the longitudinal cross-section of the nickel-based composite coating in an embodiment of the present invention.

[0040] Figure 4 This is a microscopic morphology diagram of the substrate cross-section before coating preparation in an embodiment of the present invention.

[0041] Figure 5 This is a cross-sectional microstructure of the nickel-based composite coating prepared in the embodiments of the present invention.

[0042] In the figure: 1-workpiece substrate, 2-inner nickel substrate, 3-intermediate layer of core-shell composite microparticles, 4-surface dense nickel. Detailed Implementation

[0043] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0044] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.

[0045] Please see Figures 1-5 The present invention provides a method for preparing a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers, the specific steps of which are as follows:

[0046] (1) Mechanical grinding and polishing: The surface of the workpiece substrate 1 is ground step by step with 400# to 2000# sandpaper, and then mechanical polishing is performed to control the surface roughness Ra of the substrate to be ≤0.08μm;

[0047] (2) Ultrasonic degreasing: The polished substrate is placed in a 5% sodium hydroxide solution and ultrasonically degreased at 60°C. After removal, it is washed with multi-stage countercurrent water until the substrate surface is completely wetted.

[0048] (3) Surface activation: The degreased substrate is placed in a 10% to 15% dilute nitric acid aqueous solution and activated at room temperature for 40 seconds to remove the surface oxide film. After removal, it is washed with water until neutral.

[0049] (4) Preparation of transition layer: For aluminum alloy substrate, a dense zinc transition layer with a thickness of 80-150 nm is prepared by double zinc immersion process; the double zinc immersion adopts the conventional alkaline zinc immersion process in this field. After the first zinc immersion, the zinc is removed by 50% nitric acid solution by volume fraction, and then the second zinc immersion is performed. The single zinc immersion time is 30-60 s and the zinc immersion temperature is 20-30℃; for carbon steel and copper alloy substrate, this step is omitted and the subsequent electrodeposition process is directly entered.

[0050] The substrate is immediately transferred to the plating solution for electrodeposition after pretreatment to avoid re-oxidation of the surface.

[0051] The following examples and comparative examples all use the same electrodeposition conditions and post-processing procedures. The formulation components of each example all fall within the formulation protection scope of this invention. The performance differences of the coatings with different component contents are verified only by adjusting the amount of functional particles and dispersants added. The comparative examples use the same basic plating solution system and process conditions to form a performance comparison with the solution of this invention.

[0052] During the electrodeposition process, mechanical stirring at 500–600 r / min and ultrasonic treatment at 150–190 W are simultaneously activated. After electrodeposition, the sample is washed multiple times with deionized water to remove residual plating solution from the surface, and then vacuum dried at 55–65 °C to obtain the finished coating sample.

[0053] Example 1: Nickel-based composite coating with low core-shell particle content

[0054] This embodiment provides a method for preparing a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers, as detailed below:

[0055] 1. Plating solution formula (per 1L of plating solution):

[0056] Basic components: 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 0.25g sodium saccharin;

[0057] Functional enhancement phase: 0.6g graphene oxide, 7.0g silicon carbide nanoparticles, 0.3g aluminum oxide nanoparticles, and 6mL polytetrafluoroethylene emulsion with a solid content of 50%.

[0058] Compound dispersant: Sodium dodecyl sulfate 0.8g, sodium hexametaphosphate 0.4g, polyethylene glycol 0.4g, sodium α-alkenyl sulfonate 0.1g, polyquaternium-10 0.05g;

[0059] The remainder is deionized water.

[0060] 2. Preparation of core-shell composite microparticle dispersion:

[0061] Pre-disperse graphene oxide, silicon carbide nanoparticles, aluminum oxide nanoparticles, and polytetrafluoroethylene emulsion in the prescribed amounts. First, add silicon carbide nanoparticles and aluminum oxide nanoparticles to the graphene oxide aqueous dispersion and ultrasonically disperse at 150–190 W for 20–30 min to ensure that the graphene oxide sheets fully coat the surface of the ceramic particles, forming an intermediate suspension of graphene oxide-coated ceramic particles. Then, add polytetrafluoroethylene emulsion to the intermediate suspension and continue ultrasonic dispersion for 10–15 min to ensure that the polytetrafluoroethylene particles are uniformly adsorbed on the surface of the graphene oxide shell, forming a (SiC / Al2O3)@graphene oxide@polytetrafluoroethylene core-shell composite particle suspension. Filter through a 0.5 μm filter membrane to remove micron-sized agglomerates before use.

[0062] The above dispersion process can achieve uniform and stable dispersion of multiphase particles without high-temperature modification of the powder, effectively improving the poor interfacial compatibility between inorganic ceramic particles and organic polytetrafluoroethylene particles, and ensuring the stable formation of a three-layer core-shell structure.

[0063] 3. Preparation of composite plating solution:

[0064] Take deionized water at 48–52°C and dissolve the prescribed amounts of nickel sulfate, nickel chloride, boric acid, and sodium citrate in sequence, stirring until completely dissolved. Add the compound dispersant to the above base plating solution, stir evenly, and then add the prepared core-shell composite microparticle suspension. Mix mechanically and ultrasonically for 15–20 minutes. Finally, add sodium saccharin and replenish with deionized water to a final volume of 1 L. After circulating filtration through a 0.2 μm filter membrane, adjust the pH of the plating solution to 3.9 using dilute sulfuric acid or sodium hydroxide solution.

[0065] Sodium dodecyl sulfate and sodium hexametaphosphate are the core functional components of the anionic dispersion system. The combination of the two can maintain the dispersion stability of core-shell particles through electrostatic repulsion and chelation. Sodium α-alkenyl sulfonate is a high-temperature resistant synergistic component, which further enhances the long-term dispersion performance at the working temperature of the plating solution.

[0066] The multi-component anion-cation complex dispersion system can maintain the uniform dispersion of core-shell particles for a long time by relying on the synergistic effect of charge repulsion and steric hindrance, thus avoiding particle sedimentation and agglomeration.

[0067] 4. Pulse electrodeposition:

[0068] High-purity nickel plates were used as the anode, and the pretreated heat exchange substrate was used as the cathode. The anode and cathode were arranged in parallel with a spacing of 5–7 cm. The plating solution was kept at a constant temperature of 55°C, and mechanical stirring and ultrasonication were simultaneously activated. The pulse electrodeposition parameters were set as follows: pulse frequency 70 Hz, duty cycle 40%, and forward current density 3 A / dm³. 2 The reverse current and the forward current have symmetrical amplitudes. Forward electroplating and reverse electrolysis are carried out alternately, and the deposition time is 60 minutes.

[0069] Symmetric pulse electrodeposition can promote ion diffusion in the plating bath through intermittent power-off, refine the plating grains, and release residual stress inside the plating layer. Combined with a combined flow field of stirring and ultrasound, it can make the core-shell particles uniformly suspended and orderly embedded in the plating layer, gradually forming a sandwich microstructure of inner nickel substrate - middle layer with core-shell composite particles - surface dense nickel.

[0070] 5. Coating structure and properties:

[0071] The total thickness of the nickel-based composite coating prepared in this embodiment is 28-30 μm, the mass percentage of metallic nickel in the coating is 91.0 wt%, and the mass percentage of (SiC / Al2O3)@graphene oxide@polytetrafluoroethylene core-shell composite particles is 9.0 wt%. Cross-sectional morphology observation shows that core-shell microparticles are uniformly embedded between the inner nickel substrate 2 and the surface dense nickel 4, forming an intermediate layer 3 of core-shell composite microparticles. The tips of some core-shell microparticles are exposed on the coating surface. Based on the total area of ​​the outer surface of the coating, the area of ​​core-shell microparticles exposed on the coating surface accounts for 10% to 15% (this exposed area ratio can be controlled by adjusting the amount of core-shell composite microparticles added to the plating solution, the pulse electrodeposition current density, and the stirring speed). No obvious particle agglomeration defects or penetrating micropores were observed in the sample. The nickel coating encapsulates and pins the core-shell microparticles, effectively sealing the gaps between particles and blocking the penetration channels of corrosive media. The nickel phase firmly fixes the main body of the microparticles inside the coating, with only the tips of the microparticles exposed locally, which can alleviate the problem of rapid loss of the polytetrafluoroethylene phase due to surface wear.

[0072] Testing revealed that the peel strength of the coating in this embodiment was 60–64 N / cm, the neutral salt spray durability was 500–530 h, and the corrosion current density was 2.4–2.9 × 10⁻⁶. -7 A / cm 2 Under simulated operating conditions for 72 hours (using a common method for simulating calcium carbonate fouling in heat exchangers, with calcium ion concentration of 350 mg / L and bicarbonate concentration of 220 mg / L, and after 72 hours of constant temperature 60℃ circulation immersion, the mass of calcium carbonate deposited per unit area was measured), the fouling amount on the medium was 3.4–4.1 mg / cm³. 2The micro Vickers hardness is 590–620 HV, the steady-state friction coefficient is 0.11–0.13, the water contact angle is 130–136°, the particle settling rate after the plating solution has been left to stand for 48 hours is 4.0%–4.6%, and no cracks or peeling were observed in the plating sample after 10 cycles of thermal cycling from -40℃ to 120℃.

[0073] Example 2: Nickel-based composite coating with high core-shell particle content

[0074] This embodiment provides a method for preparing a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers, as detailed below:

[0075] 1. Plating solution formula (per 1L of plating solution):

[0076] Basic components: 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 0.25g sodium saccharin;

[0077] Functional enhancement phase: 0.9g graphene oxide, 7.5g silicon carbide nanoparticles, 0.5g aluminum oxide nanoparticles, and 7mL polytetrafluoroethylene emulsion with a solid content of 65%.

[0078] Compound dispersant: Sodium dodecyl sulfate 1.0g, sodium hexametaphosphate 0.6g, polyethylene glycol 0.5g, sodium α-alkenyl sulfonate 0.2g, polyquaternium-10 0.10g;

[0079] The remainder is deionized water.

[0080] 2. Preparation of core-shell composite microparticle dispersion:

[0081] The preparation method is the same as in Example 1, and a stable core-shell composite microparticle suspension is finally obtained for use.

[0082] 3. Preparation of composite plating solution:

[0083] The preparation method is the same as in Example 1, except that the pH of the plating solution is adjusted to 3.9.

[0084] 4. Pulse electrodeposition:

[0085] The process parameters are completely consistent with those of Example 1.

[0086] 5. Coating structure and properties:

[0087] The nickel-based composite coating prepared in this embodiment has a total thickness of 28–32 μm, with metallic nickel accounting for 89.7 wt% and core-shell composite particles accounting for 10.3 wt%. The coating structure is dense and continuous, with most of the core-shell composite powder embedded inside the nickel coating, and some particles exposed on the coating surface. Based on the total surface area of ​​the coating, the area of ​​the core-shell particles exposed on the coating surface accounts for 15%–22%, and the interfacial bonding performance between the particles and the nickel coating is excellent. Silicon carbide and aluminum oxide synergistically construct a wear-resistant skeleton, graphene oxide forms a continuous anti-corrosion barrier, and polytetrafluoroethylene imparts hydrophobic and anti-scaling properties to the coating, achieving a synergistic effect of multiple functions including wear resistance, corrosion prevention, and hydrophobic and anti-scaling properties.

[0088] Testing revealed that the peel strength of the coating in this embodiment was 62–68 N / cm, the neutral salt spray durability was 530–560 h, and the corrosion current density was 2.1–2.5 × 10⁻⁶. -7 A / cm 2 The fouling concentration in the simulated working conditions over 72 hours was 3.2–3.8 mg / cm³. 2 The micro Vickers hardness is 620-650 HV, the steady-state friction coefficient is 0.10-0.12, the water contact angle is 134-142°, the particle settling rate after the plating solution has been left to stand for 48 hours is 4.2%-5.1%, and no cracks or peeling were observed in the plating sample after 10 cycles of thermal cycling from -40℃ to 120℃.

[0089] Example 3: Nickel-based composite coating with high core-shell particle content

[0090] This embodiment provides a method for preparing a corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers, as detailed below:

[0091] 1. Plating solution formula (per 1L of plating solution):

[0092] Basic components: 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 0.25g sodium saccharin;

[0093] Functional enhancement phase: 1.0 g graphene oxide, 9.0 g silicon carbide nanoparticles, 0.7 g aluminum oxide nanoparticles, and 10 mL polytetrafluoroethylene emulsion with a solid content of 70%.

[0094] Compound dispersant: Sodium dodecyl sulfate 1.2g, sodium hexametaphosphate 0.8g, polyethylene glycol 0.6g, sodium α-alkenyl sulfonate 0.3g, polyquaternium-10 0.15g;

[0095] The remainder is deionized water.

[0096] 2. Preparation of core-shell composite microparticle dispersion:

[0097] The preparation method is the same as in Example 1, and a stable core-shell composite microparticle suspension is finally obtained for use.

[0098] 3. Preparation of composite plating solution:

[0099] The preparation method is the same as in Example 1, except that the pH of the plating solution is adjusted to 3.9.

[0100] 4. Pulse electrodeposition:

[0101] The process parameters are completely consistent with those of Example 1.

[0102] 5. Coating structure and properties:

[0103] The total thickness of the nickel-based composite coating prepared in this embodiment is 30–33 μm, with metallic nickel accounting for 88.4 wt% and core-shell composite particles accounting for 11.6 wt%. A dense nickel layer is formed on the surface, and the tips of some core-shell composite particles can be exposed on the outer surface of the coating. Based on the total area of ​​the outer surface of the coating, the area of ​​core-shell particles exposed on the coating surface accounts for 22%–30%. The increased proportion of core-shell particles in the coating increases the proportion of effective polytetrafluoroethylene components that can play a role on the coating surface, further enhancing the hydrophobic and anti-scaling properties.

[0104] Testing revealed that the peel strength of the coating in this embodiment was 61–66 N / cm, the neutral salt spray durability was 510–540 h, and the corrosion current density was 2.3–2.7 × 10⁻⁶. -7 A / cm 2 The fouling concentration in the simulated working conditions over 72 hours was 3.0–3.6 mg / cm³. 2 The micro Vickers hardness is 600-630 HV, the steady-state friction coefficient is 0.09-0.11, the water contact angle is 140-150°, the particle settling rate after the plating solution has been left to stand for 48 hours is 4.5%-5.3%, and no cracks or peeling were observed in the plating sample after 10 cycles of thermal cycling from -40℃ to 120℃.

[0105] Comparative Example 1: Pure Nickel Plating

[0106] To verify the performance gain of the composite coating of this invention, a pure nickel coating was set as a blank control example. The plating solution formulation (per 1L of plating solution): 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 0.25g sodium saccharin, with the balance being deionized water; the pH value of the plating solution was 3.9.

[0107] The substrate pretreatment, electrodeposition process and post-treatment process are completely consistent with those in Example 1.

[0108] Testing revealed that the pure nickel plating thickness in this comparative example was 28–31 μm, the peel strength was 33–38 N / cm, the neutral salt spray durability was 140–160 h, and the corrosion current density was 8.2–9.6 × 10⁻⁶. -6 A / cm 2 The amount of fouling under simulated operating conditions over 72 hours was 15.6–16.8 mg / cm³. 2 The micro Vickers hardness is 300-330 HV, the steady-state friction coefficient is 0.33-0.38, the water contact angle is 58-65°, and a small number of microcracks appear in the coating after 10 cycles of thermal cycling from -40℃ to 120℃.

[0109] Comparative Example 2: Nickel-Silicon Carbide Composite Coating

[0110] A single-component composite coating with only silicon carbide particles was set up as a comparative example. The plating solution formula (per 1L of plating solution): 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 7.0g silicon carbide nanoparticles, 1.0g sodium dodecyl sulfate, 0.25g sodium saccharin, with the balance being deionized water; the pH value of the plating solution was 3.9.

[0111] The substrate pretreatment, electrodeposition process and post-treatment process are completely consistent with those in Example 1.

[0112] Testing revealed that the coating thickness in this comparative example was 29–32 μm, the peel strength was 42–47 N / cm, the neutral salt spray durability was 260–290 h, and the corrosion current density was 4.3–5.4 × 10⁻⁶. -6 A / cm 2 The amount of fouling under simulated operating conditions over 72 hours was 7.2–8.0 mg / cm³. 2 The micro Vickers hardness is 440–470 HV, the steady-state coefficient of friction is 0.19–0.23, the water contact angle is 72–80°, the particle settling rate after the plating solution has been left to stand for 48 hours is 7.8%–9.2%, and after 10 cycles of hot and cold cycling from -40°C to 120°C, occasional microcracks are observed in the coating.

[0113] Comparative Example 3: Nickel-PTFE Composite Coating

[0114] A single-component composite coating with only polytetrafluoroethylene (PTFE) particles was set up as a comparative example. The plating bath formulation (per 1L of plating bath): 240g nickel sulfate, 28g nickel chloride, 40g boric acid, 2.0g sodium citrate, 6mL PTFE emulsion with 50% solids content, 1.0g sodium dodecyl sulfate, 0.25g sodium saccharin, with the balance being deionized water; the pH of the plating bath was 3.9.

[0115] The substrate pretreatment, electrodeposition process and post-treatment process are completely consistent with those in Example 1.

[0116] Testing revealed that the coating thickness in this comparative example was 28–32 μm, the peel strength was 40–45 N / cm, the neutral salt spray durability was 270–300 h, and the corrosion current density was 4.0–5.1 × 10⁻⁶. -6 A / cm 2 The amount of dirt adhering under simulated operating conditions for 72 hours was 4.8–5.6 mg / cm³. 2 The micro Vickers hardness is 360-390 HV, the steady-state friction coefficient is 0.14-0.17, the water contact angle is 108-116°, the particle settling rate after the plating solution has been left to stand for 48 hours is 6.9%-8.3%, and after 10 cycles of hot and cold cycling from -40℃ to 120℃, occasional microcracks are observed in the coating.

[0117] As can be seen from the comparison of the above embodiments and comparative examples, the present invention, by designing a three-layer progressive core-shell composite microparticle and constructing a sandwich coating structure with double-layer nickel coating, combined with a multi-component compound dispersion system and a symmetrical pulse electrodeposition process, can significantly improve the corrosion resistance, wear resistance and anti-fouling performance of the coating, while also having higher coating adhesion and plating solution stability. It can adapt to the harsh service conditions of heat exchangers with high temperature alternation and media scouring, and effectively extend the service life of the equipment.

[0118] It should be noted that, in this invention, although the specification describes the embodiments, not every embodiment contains only one independent technical solution. This way of describing the specification is only for clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A corrosion-resistant and scale-resistant nickel-based composite coating for heat exchangers, comprising a nickel plating layer deposited on the surface of a workpiece substrate, and core-shell composite microparticles dispersed and embedded within the nickel plating layer, characterized in that, The nickel-based composite coating consists of a sandwich microstructure consisting of an inner nickel substrate, an intermediate layer with core-shell composite microparticles, and a surface layer of dense nickel. The core-shell composite microparticles use a multiphase ceramic powder composed of silicon carbide and aluminum oxide as the wear-resistant core, graphene oxide as the intermediate bridging coating layer, and polytetrafluoroethylene as the outer hydrophobic modification layer; part of the core-shell composite microparticles are embedded inside the nickel plating layer, and part of them are exposed on the outer surface of the nickel plating layer.

2. The anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 1, characterized in that, The core-shell composite microparticles are uniformly dispersed between the inner nickel substrate and the surface dense nickel. The surface dense nickel fills the interfacial gaps between the core-shell composite microparticles to block the penetration channels of corrosive media.

3. The anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 1, characterized in that, The total thickness of the nickel-based composite coating is 25 μm to 35 μm; The core-shell composite microparticles account for 8.0 wt% to 12.0 wt% of the mass of the coating. The exposed core-shell composite particles account for 10% to 30% of the total area.

4. The anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 1, characterized in that, The nickel-based composite coating has a water contact angle of 130° to 150°, a micro Vickers hardness of not less than 580 HV, and a neutral salt spray test durability of not less than 480 h. The corrosion current density is not higher than 3.0 × 10⁻⁶. -7 A / cm 2 The wear rate is no higher than 4.0 × 10⁻⁶. -6 mm 3 / (N・m), the amount of dirt adhering under simulated working conditions for 72 hours should not exceed 5.0 mg / cm³. 2 The peel strength of the coating is not less than 55 N / cm.

5. The anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 1, characterized in that, The substrate is a carbon steel substrate, an aluminum alloy substrate, or a copper alloy substrate; When the substrate is an aluminum alloy substrate, a dense zinc transition layer is also provided between the substrate and the inner nickel substrate.

6. A method for preparing a corrosion-resistant and scale-resistant nickel-based composite coating for a heat exchanger according to any one of claims 1-5, characterized in that, Specifically, the steps include the following: (1) Substrate pretreatment: The workpiece substrate surface is successively ground and polished, ultrasonically degreased, and surface activated, and then washed with water for later use; (2) Preparation of core-shell composite microparticle dispersion: Silicon carbide nanoparticles and aluminum oxide nanoparticles were added to graphene oxide aqueous dispersion and subjected to first ultrasonic dispersion treatment to obtain an intermediate suspension of graphene oxide-coated ceramic particles. Polytetrafluoroethylene emulsion was added to the intermediate suspension, and then subjected to a second ultrasonic dispersion treatment to obtain a (SiC / Al2O3)@graphene oxide@polytetrafluoroethylene core-shell composite microparticle suspension. (3) Preparation of composite plating solution: Add a multi-component anion and cation compound dispersant to the nickel-based plating solution, stir evenly, and then add the core-shell composite microparticle suspension. Mix by mechanical stirring and ultrasonication to obtain a uniform and stable composite plating solution. (4) Pulse electrodeposition: The pretreated substrate is used as the cathode and the nickel plate is used as the anode. A symmetrical pulse electrodeposition process is used for deposition. During the deposition process, mechanical stirring and ultrasonic action are applied simultaneously to form a nickel-based composite coating with a sandwich microstructure on the substrate surface.

7. The method for preparing the anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 6, characterized in that, The multi-component anionic and cationic compound dispersant is composed of anionic dispersant, nonionic dispersant and cationic dispersant; The anionic dispersant is composed of sodium dodecyl sulfate and sodium hexametaphosphate, or of sodium dodecyl sulfate, sodium hexametaphosphate and sodium α-alkenyl sulfonate; The nonionic dispersant is polyethylene glycol, and the cationic dispersant is polyquaternium-10.

8. The method for preparing the anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 6, characterized in that, The nickel-based plating solution uses nickel sulfate and nickel chloride as the main salts, boric acid as the pH buffer, and also contains sodium citrate complexing agent and sodium saccharin brightener.

9. The method for preparing the anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 6, characterized in that, The process parameters for the pulse electrodeposition are as follows: The pulse frequency is 50Hz–90Hz, the duty cycle is 30%–50%, and the cathode current density is 2A / dm². 2 ~4A / dm 2 The plating solution temperature is 50℃~60℃, and the distance between the anode and the cathode is 5cm~7cm.

10. The method for preparing the anti-corrosion and anti-fouling nickel-based composite coating for heat exchangers according to claim 6, characterized in that, In step (1), when the substrate is an aluminum alloy substrate, a zinc transition layer is prepared by a double zinc immersion process after surface activation treatment; The double zinc immersion process is as follows: first, zinc is immersed once, then zinc is removed by nitric acid solution, and then zinc is immersed a second time.

Citation Information

Patent Citations

  • Ni-P-base composite coating contg. silicon carbide and PTFE

    CN1228467C