Film-forming solution and its treatment process for high corrosion resistance in micro-arc oxidation surface treatment
By optimizing the film-forming solution and process parameters, the mechanical properties and applicability issues in the micro-arc oxidation treatment of magnesium alloys were solved, achieving a magnesium alloy surface treatment with high corrosion resistance and low energy consumption, suitable for various alloy grades and complex configurations of automotive front assemblies.
Patent Information
- Application Number
- CN202610850543.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing micro-arc oxidation technology for magnesium alloys suffers from problems such as low mechanical properties, large film thickness, high power consumption, poor applicability, low production efficiency, and uneven surface treatment, making it difficult to meet the high corrosion resistance and lightweight requirements of automotive front assembly.
A film-forming solution containing silicates, metal acids, borates, nano-oxide particles, and vanadium-based ceramic particles is used. Combined with a dual-pulse DC power supply and optimized process parameters, magnesium alloys are subjected to micro-arc oxidation to form dense, thin films suitable for various alloy grades and complex configurations.
The generated oxide film has high mechanical properties, low porosity, low energy consumption, and strong adaptability, meeting the corrosion resistance and lightweight requirements of automotive front assembly, and reducing production costs and time.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of magnesium alloy surface treatment technology, specifically to a film-forming solution and its treatment process for a high corrosion-resistant micro-arc oxidation surface treatment process. Background Technology
[0002] With the rapid development of the automotive industry, the demand for lightweight vehicles is increasing. Magnesium alloys, due to their low density, high specific strength, and good shock absorption, are seeing a growing trend in automotive parts manufacturing, showing broad application prospects. Magnesium alloy automotive front fascia assemblies are one such important application component. However, magnesium alloys are chemically reactive and prone to corrosion during use, severely affecting their service life and safety. Therefore, surface treatment is necessary to improve their corrosion resistance and mechanical properties.
[0003] Micro-arc oxidation is an effective surface treatment method for magnesium alloys. It involves applying a high-voltage current to the metal surface, causing a spark discharge and generating a dense oxide film. This oxide film bonds firmly to the substrate and exhibits good corrosion resistance, wear resistance, and insulation. However, current micro-arc oxidation processes for magnesium alloys have several shortcomings. For example, the mechanical properties of the generated surface film are insufficient to meet the high strength requirements of automotive front assemblies; the film thickness is relatively large, increasing the weight and tolerance of parts, which is inconsistent with the trend towards lightweight and refined designs; the dense layer accounts for a small proportion, resulting in low efficiency in converting film thickness to various performance characteristics; the process consumes a lot of electricity, increasing production costs; the process time is long, reducing production efficiency; and its applicability to different magnesium alloy grades is poor. For large structural parts and exterior components, it is difficult to achieve uniform surface treatment and ensure a low surface defect rate. These factors limit its application in actual production.
[0004] Therefore, developing a high corrosion-resistant micro-arc oxidation surface treatment process for magnesium alloy automotive front assemblies that can generate high mechanical properties, low film thickness, high density layer ratio, low power consumption, short processing time, and is applicable to various alloy grades while ensuring the surface treatment effect of large die-cast structural parts and appearance parts with complex configurations is of great practical significance. Summary of the Invention
[0005] In view of the shortcomings of the existing magnesium alloy front assembly and existing micro-arc oxidation technology, this application provides a magnesium alloy micro-arc oxidation surface treatment process based on silicon-aluminum-boron composite oxide. This process can provide high corrosion resistance, high density, low porosity, high mechanical properties, high energy efficiency, low processing time, and has one or more of the following excellent adaptability to various alloy grades and various processing equipment.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a film-forming solution for a high corrosion-resistant micro-arc oxidation surface treatment process, comprising, by weight percentage: 0.5-1.5% silicate, 0.1-0.5% metal acid salt, 0.1-0.5% borate, 0.05-0.3% nano-oxide particles, 0.1-0.5% vanadium-based ceramic particles, 0.05-0.3% corrosion inhibitor, 0.01-0.1% organic additive, 0.02-0.08% metal alkali, 2%-5% buffer pair, and the remainder being deionized water and impurities.
[0007] Preferably, the silicate is one or a mixture of two of sodium silicate and potassium silicate; the metal acid salt is one or a mixture of sodium aluminate, potassium aluminate, sodium tungstate, and potassium tungstate; the borate is one or a mixture of sodium borate and potassium borate; the nano oxide particles are one or a mixture of nano silicon dioxide, nano titanium dioxide, and nano aluminum oxide with a particle size of 20-50 nm; and the vanadium-based ceramic particles are one or a mixture of vanadium-carbon ceramic particles and vanadium-nitrogen ceramic particles with a particle size of 50-100 nm.
[0008] Preferably, the corrosion inhibitor is one or a mixture of benzotriazole, methylbenzotriazole, mercaptobenzothiazole, 8-hydroxyquinoline, and 5-chloro-8-hydroxyquinoline; the organic auxiliary is one or a mixture of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyoxyethylene octylphenol ether, sodium gluconate, sucrose, glycerol, and triethanolamine; and the metal alkali is one or a mixture of two of sodium hydroxide and potassium hydroxide.
[0009] A high corrosion-resistant micro-arc oxidation surface treatment process suitable for magnesium alloy automotive front bulkhead assemblies includes: micro-arc oxidation treatment, using the aforementioned film-forming solution, employing a dual-pulse DC power supply (model DSA-600), and the following process parameters: current density 5-15A / dm²: AZ91D 8-10A / dm², AM60B 10-12A / dm², AZ31B 9-11A / dm²; voltage 200-400V: arc ignition 180-220V / 1min, stabilization 250-350V / 7-11min; duty cycle 10-30%: positive 20-25% + negative 5-10%; pulse frequency 500-1000Hz; tank temperature 25-35℃; and treatment time 8-12min.
[0010] A surface treatment method for a magnesium alloy automotive front bulkhead assembly includes sample pretreatment and the aforementioned micro-arc oxidation treatment; the sample pretreatment steps are as follows: the magnesium alloy front bulkhead assembly is sequentially subjected to alkaline degreasing, dilute nitric acid pickling, deionized water ultrasonic cleaning, spray rinsing, and drying.
[0011] Preferably, the magnesium alloy front assembly has dimensions of 300-400mm × 200-300mm and a wall thickness of 3-8mm; alkaline degreasing is performed by ultrasonic cleaning at 60-65℃ for 12-15 minutes; dilute nitric acid pickling is performed at 8-10% at room temperature for 2-3 minutes; deionized water ultrasonic cleaning is performed for 5 minutes; spray rinsing is performed 3 times; and drying is performed at 80℃ for 18-20 minutes.
[0012] Preferably, after micro-arc oxidation treatment, the oxide film properties are as follows: film thickness 15-20μm, dense layer ratio ≥80%, hardness 350-400HV, porosity 1.5-2.8%, salt spray resistance time ≥520 hours, and film thickness difference between inner and outer surfaces ≤25%.
[0013] Preferably, after hydrophobic sealing treatment, the oxide film performance is as follows: porosity ≤1.2%, salt spray resistance time ≥780 hours, and the change rate of hardness, film thickness, and dense layer ratio ≤1%.
[0014] Preferably, after hydrophobic sealing treatment, the magnesium alloy front assembly has a salt spray resistance (5% NaCl solution, GB / T10125) of ≥1200 hours and an appearance defect rate of ≤0.5%.
[0015] Preferably, the film-forming liquid is used in the micro-arc oxidation surface treatment of magnesium alloy automotive front bulkhead assembly (large die-cast part, size ≥300mm×200mm).
[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. The silicates, metal salts, borates and nano-oxide particles in the film-forming solution of this invention can significantly improve the density, hardness and wear resistance of the oxide film, giving the surface film high mechanical properties and corrosion resistance, and meeting the service life and mechanical strength requirements of magnesium alloy automotive front assembly.
[0017] 2. This invention adds a fixed amount of corrosion inhibitor, which ensures a low loss rate of the substrate during the micro-arc oxidation process and greatly reduces the stress unevenness caused by the phase selectivity of corrosion at the microscopic level; compared with the prior art, it greatly reduces the film cracks that appear after treatment.
[0018] 3. By optimizing the bath composition and process parameters, a thin and dense oxide film can be formed while shortening the process time, thereby reducing the weight and tolerance of parts and conforming to the development trend of automotive lightweighting.
[0019] 4. The synergistic effect of silicates, borates and metal salts makes the generated oxide film structure more compact, significantly increasing the proportion of the compact layer, which effectively enhances the corrosion resistance and mechanical properties of the oxide film.
[0020] 5. The process parameters of this invention have been optimized, reducing current density and voltage while ensuring the processing effect, thereby reducing the power consumption of the process and lowering production costs.
[0021] 6. The bath solution of the present invention has good adaptability to magnesium alloys of different compositions, and provides a similar film formation method for various magnesium alloys used in the automotive market, enabling effective surface treatment of magnesium alloy automotive front assemblies of various alloy grades. Attached Figure Description
[0022] Figure 1 This is a flowchart of the surface treatment method for the magnesium alloy automotive front bulkhead assembly of the present invention. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.
[0024] Reference Figure 1 As shown, in a first aspect, the present invention provides a magnesium alloy micro-arc oxidation film-forming solution formulation, the formulation comprising the following components by weight percentage: silicate: 0.5-1.5%, metal acid salt: 0.1-0.5%, borate: 0.1-0.5%, corrosion inhibitor: 0.05-0.3%, organic additive: 0.01-0.1%, metal alkali: 0.02-0.08%, nano-oxide particles: 0.05%-0.3%, the remainder being solvent, added elements and impurities, wherein the added elements include a mixture of carbon, nitrogen and vanadium, and the total weight percentage of the added elements is 0.1-0.5%.
[0025] Furthermore, the silicate is one or a mixture of two of sodium silicate and potassium silicate. As the main film-forming substance, silicate can provide sufficient silicon for the formation of the oxide film, promote the growth of the oxide film, and improve the density and hardness of the oxide film.
[0026] Furthermore, the metal salt is one or more of sodium aluminate, potassium aluminate, sodium tungstate, and potassium tungstate, and the metal salt has one or more functions such as participating in the formation process of oxide film, combining to form a denser film layer, optimizing the substrate surface, and improving the mechanical properties, density, and porosity of the film layer.
[0027] Furthermore, the borate is one or more of sodium borate and potassium borate. As an auxiliary film-forming substance, the borate can form a composite phase with the composite oxide film formed by silicate and metal acid salt. After combination, it has one or more effects of improving surface inertness, wear resistance, density and porosity.
[0028] Further, the corrosion inhibitor is one or more of benzotriazole, methylbenzotriazole, mercaptobenzothiazole, 8-hydroxyquinoline, and 5-chloro-8-hydroxyquinoline. Due to α-Mg and Mg... 17 Al 12 The surface properties of the phase and the growth direction of the oxide film in the micro-arc oxidation process are different. A certain amount of corrosion inhibitor can selectively protect the magnesium phase, which can improve the uniformity and density of the film, protect the integrity of the substrate in the process, and reduce the surface potential difference of the substrate.
[0029] Further, the organic additive is one or more of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyoxyethylene octylphenol ether, sodium gluconate, sucrose, glycerol, and triethanolamine. The organic additive has one or more functions, including reducing the surface tension of the bath, improving the wettability of the bath on the magnesium alloy surface, accelerating the escape of bubbles during the process, and enabling the oxide film to more uniformly cover the magnesium alloy surface.
[0030] Furthermore, the metal alkali is one or a mixture of two of sodium hydroxide and potassium hydroxide. The metal alkali can adjust the pH value of the bath solution, providing a suitable alkaline environment for the micro-arc oxidation reaction and promoting the formation of the oxide film.
[0031] Furthermore, the nano-oxide particles are one or more of nano-silica, nano-titanium dioxide, nano-alumina, nano-zinc oxide, and nano-manganese dioxide, or a mixture thereof. These nano-oxide particles can fill the pores of the oxide film, improving its density and mechanical properties, while also enhancing its wear resistance and corrosion resistance.
[0032] Furthermore, the added element is in the form of one or more of vanadium-carbon ceramic particles and vanadium-nitrogen ceramic particles in the film-forming solution.
[0033] Secondly, a process parameter for micro-arc oxidation surface treatment of magnesium alloys suitable for this bath system is provided. The process parameter includes the following parameters: current density: 5-15A / dm2, voltage: 200-400V, duty cycle: 10-30%, pulse frequency: 500-1000Hz.
[0034] Thirdly, a hydrophobic blocking agent formulation suitable for the micro-arc oxidation treatment is provided, the formulation comprising the following components by weight percentage: 4-6% silane coupling agent, 0.1-0.3% glacial acetic acid, 20-30% ethanol, and the remainder being solvents and impurities.
[0035] In a preferred embodiment, the magnesium alloy substrate can be pretreated before the anodizing process. Common treatments in the industry can be used, such as descaling, degreasing, weak alkali washing, and water washing.
[0036] The present invention will be further described below with reference to specific embodiments. It should be noted that the following embodiments are only examples for clearly illustrating the present invention and do not limit the present invention in any way.
[0037] Examples 1-2 The following detailed description is based on two sets of examples. In the examples, "parts" refers to "parts by weight," and the total weight of the film-forming liquid is 1000 parts. The object being treated is a die-cast sample of an AZ91D / AM60B / AZ31B magnesium alloy front assembly (350mm×220mm, wall thickness 3-8mm). The testing standards are GB / T4340.1, GB / T6462, and GB / T10125.
[0038] Example 1: Treatment of AZ91D magnesium alloy front assembly 1. Preparation of anodic oxidation electrolyte: Dissolve NaOH in 500 mL of deionized water by stirring. Prepare the solution according to the ratio in the table. After cooling, add sodium silicate / sodium aluminate / sodium borate and stir for 10 min. Add corrosion inhibitor / organic additive and stir for 5 minutes; After ultrasonically dispersing nano-SiO2 for 15 min, vanadium-carbon ceramic particles are added and ultrasonically dispersed for another 15 min. Aggregates larger than 50 nm are removed using a molecular sieve and a ceramic funnel. Deionized water is added to bring the volume to 1000 mL, and the pH is 9.2. This is the anodic oxidation electrolyte 1-5.
[0039] 2. Sample pretreatment: Degreasing: Alkaline degreasing agent (NaOH 5% + Na2CO3 3% + OP-10 1%), ultrasonicated at 60℃ for 15 minutes; Pickling: Immerse in 10% dilute nitric acid at room temperature for 3 minutes; Washing and drying: Ultrasonic treatment with deionized water for 5 minutes → Rinse 3 times → Dry at 80℃ for 20 minutes.
[0040] 3. Micro-arc oxidation process: Anode: AZ91D sample; Cathode: 316L stainless steel plate (area ratio 1.2:1). Parameters: Current density 8A / dm², arc ignition 200V / 1min, stable 250V / 7min, positive duty cycle 20%, negative duty cycle 5%, frequency 800Hz, tank temperature 25℃.
[0041] 4. The film-forming solution formulations are shown in Table 1 below.
[0042] Table 1. Film-forming solution ratio table for Example 1
[0043] Comparative Example 1A The comparative formulation is identical to that of Example 1 except that it does not contain metal salts, and the samples are processed using the same process.
[0044] Comparative Example 1B The comparative formulation is identical to that of Example 1 except that it does not contain borate, and the samples are processed using the same process.
[0045] Comparative Example 1C The comparative formulation is identical to that of Example 1 except that it does not contain nano-oxides, and the samples are processed using the same process.
[0046] Comparative Example 1D The comparative formulation is identical to that of Example 1 except that it does not contain vanadium-based ceramics, and the samples are processed using the same process.
[0047] 5. Performance Test Results The hardness, film thickness, and salt spray resistance of the cut samples after micro-arc oxidation were tested according to GB / T4340.1, GB / T6462, and GB / T10125 respectively. The proportion of dense layer, porosity, and appearance defect rate were obtained by scanning the cross-section of the cut samples with electron microscopy. The integrated test results are shown in Table 2 below.
[0048] Table 2 Test Results of Example 1
[0049] The table above shows that the anodic oxidation electrolyte provided by this invention can achieve excellent film formation on the AZ91D front assembly, and further explains the role of each component in the formulation: Metal salts (sodium aluminate): Their absence reduces the proportion of dense layer by 12% and the hardness by 60 HV, proving that their core function is to refine the film layer and improve its density. Borate (sodium borate): Its absence reduced salt spray resistance by 420h, proving that it is the key to improving the surface inertness of the film. Nano SiO2: Its absence reduced hardness by 30 HV and the proportion of dense layer by 8%, proving its role in filling pores; Vanadium-carbon ceramic particles: Their absence reduced salt spray resistance by 250 h, demonstrating their role in enhancing film-substrate adhesion and improving corrosion resistance stability.
[0050] Example 2: AM60B magnesium alloy front bulkhead assembly treatment, proportioning process: Consistent with Example 1 Sample pretreatment Degreasing: Ultrasonic treatment at 65℃ for 12 minutes; Pickling: 8% dilute nitric acid for 2 minutes; Drying: 80℃ for 18 minutes.
[0051] 3. Micro-arc oxidation process: Parameters: Current density 12A / dm², arc ignition 220V / 1min, stable 350V / 11min, duty cycle 30% (positive 25% + negative 5%), frequency 1000Hz, tank temperature 35℃.
[0052] 4. The film-forming solution formulations are shown in Table 3 below.
[0053] Table 3. Film-forming solution ratio table for Example 2
[0054] Comparative Example 2A The comparative formulation is identical to that of Example 2 except that it does not contain borate, and the samples are processed using the same process.
[0055] Comparative Example 2B The comparative formulation is identical to that of Example 2 except that it does not contain nano-oxides, and the samples are processed using the same process.
[0056] Comparative Example 2C The comparative formulation is identical to that of Example 2 except that it does not contain vanadium-based ceramics, and the samples are processed using the same process.
[0057] 5. Performance Test Results The performance testing method is described in Example 1, and the test results are shown in Table 4 below.
[0058] Table 4 Test Results of Example 2
[0059] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A film-forming solution for a high corrosion-resistant micro-arc oxidation surface treatment process, characterized in that, By weight percentage, it contains the following components: silicates 0.5-1.5%, metal salts 0.1-0.5%, borates 0.1-0.5%, nano-oxide particles 0.05-0.3%, vanadium-based ceramic particles 0.1-0.5%, corrosion inhibitors 0.05-0.3%, organic additives 0.01-0.1%, metal alkalis 0.02-0.08%, buffer pairs 2%-5%, and the remainder is deionized water and impurities.
2. The film-forming solution for high corrosion resistance process of micro-arc oxidation surface treatment according to claim 1, characterized in that: The silicate is one or a mixture of two of sodium silicate and potassium silicate; the metal acid salt is one or a mixture of sodium aluminate, potassium aluminate, sodium tungstate, and potassium tungstate; the borate is one or a mixture of sodium borate and potassium borate; the nano oxide particles are one or a mixture of nano silicon dioxide, nano titanium dioxide, and nano aluminum oxide with a particle size of 20-50 nm; the vanadium-based ceramic particles are one or a mixture of vanadium-carbon ceramic particles and vanadium-nitrogen ceramic particles with a particle size of 50-100 nm.
3. The film-forming solution for high corrosion resistance process of micro-arc oxidation surface treatment according to claim 1, characterized in that: The corrosion inhibitor is one or a mixture of benzotriazole, methylbenzotriazole, mercaptobenzothiazole, 8-hydroxyquinoline, and 5-chloro-8-hydroxyquinoline; the organic auxiliary is one or a mixture of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyoxyethylene octylphenol ether, sodium gluconate, sucrose, glycerol, and triethanolamine; and the metal alkali is one or a mixture of two of sodium hydroxide and potassium hydroxide.
4. A high corrosion-resistant micro-arc oxidation surface treatment process suitable for magnesium alloy automotive front assemblies, characterized in that, include: Micro-arc oxidation treatment uses the film-forming solution described in any one of claims 1-3, employs a dual-pulse DC power supply (model DSA-600), and has the following process parameters: current density 5-15A / dm²: AZ91D 8-10A / dm², AM60B 10-12A / dm², AZ31B 9-11A / dm²; voltage 200-400V: arc ignition 180-220V / 1min, stabilization 250-350V / 7-11min; duty cycle 10-30%: positive 20-25% + negative 5-10%; pulse frequency 500-1000Hz; tank temperature 25-35℃; and treatment time 8-12min.
5. A surface treatment method for a magnesium alloy automotive front bulkhead assembly, characterized in that, The sample pretreatment includes sample pretreatment and the micro-arc oxidation treatment as described in claim 4. The sample pretreatment steps are as follows: the magnesium alloy front assembly is sequentially subjected to alkaline degreasing, dilute nitric acid pickling, deionized water ultrasonic cleaning, spray rinsing, and drying.
6. The surface treatment method for the magnesium alloy automotive front bulkhead assembly according to claim 5, characterized in that, The magnesium alloy front assembly has dimensions of 300-400mm × 200-300mm and a wall thickness of 3-8mm. Alkaline degreasing is performed by ultrasonic cleaning at 60-65℃ for 12-15 minutes; dilute nitric acid pickling is performed at 8-10% at room temperature for 2-3 minutes; deionized water ultrasonic cleaning is performed for 5 minutes; spray rinsing is performed 3 times, and drying is performed at 80℃ for 18-20 minutes.
7. The surface treatment method for the magnesium alloy automotive front bulkhead assembly according to claim 5, characterized in that, After micro-arc oxidation treatment, the oxide film properties are as follows: film thickness 15-20μm, dense layer ratio ≥80%, hardness 350-400HV, porosity 1.5-2.8%, salt spray resistance time ≥520 hours, and film thickness difference between inner and outer surfaces ≤25%.
8. The surface treatment method for the magnesium alloy automotive front bulkhead assembly according to claim 5, characterized in that, After hydrophobic sealing treatment, the oxide film performance is as follows: porosity ≤1.2%, salt spray resistance time ≥780 hours, and the change rate of hardness, film thickness, and dense layer ratio ≤1%.
9. The surface treatment method for a magnesium alloy automotive front bulkhead assembly according to claim 5, characterized in that, After hydrophobic sealing treatment, the magnesium alloy front fascia assembly has a salt spray resistance of ≥1200 hours and an appearance defect rate of ≤0.5%.
10. The application of the film-forming liquid according to claim 1 in the micro-arc oxidation surface treatment of magnesium alloy automotive front bulkhead assembly.