An electroplated anodic coating
By constructing a composite structure of an inner iridium-tantalum active coating and an outer modified fluorine protective coating on a titanium-based anode, the problems of rapid consumption of organic brighteners and contamination by impurity ions during the electroplating process of the anode coating are solved, achieving high purity and uniformity of the coating and extending the service life of the anode.
Patent Information
- Application Number
- CN202611447480.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing titanium-based insoluble anodic coatings suffer from problems such as rapid oxidation and consumption of organic brighteners, contamination of the plating bath by impurity ions, weak interlayer adhesion, and uneven ion transport during electroplating, making them difficult to adapt to complex working conditions.
A bilayer composite structure consisting of an inner iridium-tantalum active coating and an outer modified fluorine-based protective coating is adopted. By constructing polymer-imprinted cavities within the fluorine polymer, preferential electron transfer catalysis of target metal ions is achieved, while selective suppression of side reactions of impurity ions is achieved.
Reduce organic brightener consumption, decrease coating defects, improve coating purity and uniformity, and extend anode life.
Smart Images

Figure CN123108708A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode coating technology, specifically to an electroplated anode coating. Background Technology
[0002] Electroplating, as one of the core processes in the field of surface engineering, is widely used in metal corrosion protection, decorative coating preparation, and functional surface modification. Among them, mainstream electroplating systems such as nickel plating, copper plating, and zinc plating all highly rely on the anodic process to maintain the ion balance of the plating solution and the efficiency of electrode reaction. Traditional soluble anodes have shortcomings such as uneven dissolution, large amount of anode sludge, and the need for frequent replenishment and maintenance. Therefore, titanium-based insoluble anodes have gradually become the mainstream choice in the industry due to their advantages such as dimensional stability, long service life, and strong adaptability to working conditions. With the rapid development of high-speed electroplating and precision electroplating technologies, various organic brighteners, leveling agents, and leveling agents are commonly added to electroplating solutions to improve the smoothness, uniformity, and density of the coating. At the same time, impurity metal ions such as iron, copper, and lead are inevitably introduced into the plating solution during the production process, which puts forward higher requirements for the functional integration of the anode. A single electrocatalytic active coating is no longer suitable for the complex plating solution environment.
[0003] In existing technologies, conventional titanium-based iridium-tantalum insoluble anodes are directly exposed to the electroplating solution. The high oxidation potential on the anode surface causes ineffective oxidation and decomposition of organic brighteners, resulting in rapid consumption of brighteners, a significant increase in electroplating production costs, and the generation of organic oxidation byproducts that continuously pollute the plating solution. To prevent brighteners from contacting the active coating, some technical solutions use fluorine-based polymer coatings as an outer protective layer, relying on the low surface energy and strong chemical inertness of fluorocarbon materials to achieve physical shielding. However, the intrinsic insulation of fluorine-based coatings significantly increases the anode mass transfer resistance and electrolytic cell voltage, and they lack ion selective permeability, making it impossible to distinguish between target metal ions and impurity ions. Impurity ions such as iron, copper, and lead can still undergo side reactions in the anode area, making it difficult to fundamentally improve the stability of the electroplating process. In addition, existing composite coatings are mostly prepared by simple blending coating, which has problems such as weak interlayer bonding, easy peeling and flaking under long-term electrochemical impact, and uneven distribution of ion transport channels, further limiting the service life of the anode and its adaptability to complex working conditions. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide an electroplating anolyte coating. It adopts a two-layer composite structure of an inner iridium-tantalum active coating and an outer modified fluorine-based protective coating. Fluorine-based polymers are used as the film-forming matrix to construct an organic photocatalyst physical barrier. At the same time, polymers prepared with the metal ions to be plated as templates are in situ composited inside the protective coating. Through the imprinted cavity that is perfectly matched with the spatial size, coordination configuration and charge distribution of the target ions, preferential electron transfer catalysis of the target metal ions is achieved, and the anolyte side reactions of impurity ions are selectively suppressed.
[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: an electroplating anolyte coating comprising an iridium-tantalum active coating and a modified fluorine-based protective coating; The iridium-tantalum active coating is laminated onto the surface of the pretreated titanium substrate, with a thickness of 0.1-100 μm; the baking temperature for preparing the iridium-tantalum active coating is 300-600℃. The modified fluorine-based protective coating is uniformly applied to the outer surface of the iridium-tantalum active coating, with a thickness of 0.01-20 μm, and is cured at a baking temperature of 120-400℃; a fluorine-based polymer is used as the film-forming matrix, and the polymer is uniformly dispersed inside the matrix. The polymer uses the metal ions to be plated as template ions and forms imprinted sites with specific recognition cavities through cross-linking polymerization of functional monomers. The imprinted sites match the target metal ions in terms of spatial size, coordination configuration and charge distribution, and have a preferential electron transfer catalytic effect on the target metal ions, while exhibiting electrochemical inertness to iron, copper and lead impurity metal ions.
[0006] Furthermore, the titanium substrate is any one of industrial pure titanium plate, titanium mesh or titanium rod, and the surface is pre-treated by degreasing, pickling and roughening, and baked at a high temperature of 400-700℃.
[0007] Furthermore, the fluorinated polymer is selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, perfluoroalkoxy resin, and fluorinated ethylene propylene copolymer.
[0008] Furthermore, the template ion is selected from Ni. 2+ Cu 2+ Zn 2+ Cr 3+ Any one of the following; the functional monomer is selected from one or more of methacrylic acid, acrylic acid, acrylamide, and vinylimidazole; the crosslinking agent is selected from divinylbenzene, ethylene glycol dimethacrylate, and trimethylolpropane triacrylate; the initiator is selected from azo or peroxide initiators.
[0009] Furthermore, a method for preparing an electroplated anodic coating includes the following steps: S1: The titanium substrate is degreased, pickled and roughened in sequence, rinsed clean and then baked and dried at high temperature to complete the pretreatment of the titanium substrate. S2: Prepare an iridium-tantalum precursor coating solution, coat it onto the surface of the pretreated titanium substrate and bake and sinter it. Repeat the coating-sintering cycle to the target thickness to obtain the inner iridium-tantalum active coating. S3: Prepare a prepolymer solution and mix it with a fluorine-based polymer dispersion to obtain a composite coating solution. Coat the surface of the iridium-tantalum active coating solution with the composite coating solution. After in-situ polymerization, baking and curing and template ion elution, repeat the coating-polymerization-elution cycle until the target thickness is reached to obtain a modified fluorine-based protective coating. S4: The workpiece with the double coating is then subjected to post-processing baking to eliminate internal stress in the coating and improve interfacial adhesion. After natural cooling, the finished product is obtained. Furthermore, the specific steps of S1 are as follows: The titanium substrate is placed in an alkaline degreasing solution, and surface oil is removed by ultrasonic cleaning. The alkaline degreasing solution is a 3%-8% sodium hydroxide aqueous solution. The ultrasonic power is 150-300W, and the cleaning time is 8-15 minutes. Through alkaline saponification and ultrasonic cavitation, rolling oil, rust-preventive oil, dust and other contaminants on the surface of the titanium substrate are removed, avoiding defects such as shrinkage craters, delamination and pinholes in the subsequent coating caused by oil contaminants, and improving the wettability and bonding foundation between the coating and the substrate surface.
[0010] After degreasing, the titanium substrate is rinsed with deionized water; then it is pickled and roughened by 8%-12% oxalic acid solution; the pickling temperature is 70-90℃ and the pickling time is 15-25min. The oxalic acid is used to corrode the titanium substrate to form a rough and uneven surface. Through the micro-corrosion effect of oxalic acid on the titanium surface, a uniform micro-uneven morphology and a large number of active sites are formed, which increases the mechanical anchoring area between the coating and the substrate.
[0011] After pickling, the surface of the titanium substrate is repeatedly rinsed with flowing deionized water until the pH of the rinsing wastewater is close to neutral.
[0012] Place the cleaned titanium substrate into a muffle furnace and bake at 400-700℃ for 20-40 minutes to remove moisture and residual trace organic acid impurities. After baking, allow it to cool to room temperature naturally with the furnace or remove it for later use.
[0013] Furthermore, the specific steps of S2 are as follows: The precursor coating liquid is loaded onto the surface of the pretreated titanium substrate by any of the following methods: brushing, immersion, or spraying; the spray gun pressure is 0.2-0.4 MPa during spraying; the immersion time is 10-30 seconds; brushing ensures complete wetting of the substrate surface. Under these process parameters, the wet film thickness is uniform, without sagging or missed coating, which provides a foundation for the formation of a uniform coating by subsequent sintering.
[0014] After coating, the workpiece is sent into a muffle furnace and baked at a temperature of 300-600℃. The holding time for each sintering is 10-20 minutes, completing one coating-sintering cycle. At high temperature, the precursor undergoes thermal decomposition and oxidation reaction, and the metal ions are converted into iridium-tantalum composite oxide, which at the same time forms a semi-metallurgical bond with the oxide layer on the surface of the titanium substrate. This temperature range can ensure the complete decomposition of the precursor and avoid excessive temperature leading to coarse grains and coating cracking.
[0015] A single cycle yields one layer of iridium-tantalum oxide coating; depending on the target coating thickness, the coating-baking-sintering cycle is repeated 1-20 times to finally obtain an iridium-tantalum active coating with a thickness of 0.1-100μm; after each sintering, the workpiece is cooled to room temperature before the next coating is carried out.
[0016] Furthermore, in step S3, the prepolymer solution is prepared as follows: Dissolve the template metal salt to be plated in a mixed solvent of ethanol and deionized water to prepare a template ion solution; the molar amount of template ions is 0.008-0.012 mol. Add functional monomers at a molar ratio of template ion to functional monomer of 1:3-5; stir at room temperature for 20-40 min to achieve full coordination complexation between template ion and functional monomer. Under this ratio, functional monomer can form a stable coordination complex around template ion, ensuring that the imprinted cavity and template ion are completely matched in spatial configuration and binding sites after subsequent polymerization, avoiding incomplete imprinting due to insufficient monomer or an increase in non-specific binding sites due to excessive monomer. Continue adding crosslinking agent, with a molar ratio of crosslinking agent to functional monomer of 3-5:1; then add initiator, with the initiator accounting for 1%-2% of the mass fraction of crosslinking agent; continue stirring for 15-30 minutes to obtain a homogeneous prepolymer solution. The amount of crosslinking agent can control the crosslinking density of the polymer, ensuring that the imprinted polymer has sufficient mechanical strength and structural rigidity, maintaining the stability of the cavity shape, while avoiding excessive crosslinking leading to excessive cavity rigidity and increased ion mass transfer resistance.
[0017] Furthermore, the preparation method of the composite coating liquid in S3 is as follows: Take a fluorine-based polymer dispersion with a solid content of 0.5%-40%; mix the prepolymer solution and the fluorine-based polymer dispersion at a mass ratio of 1:3-10; Add a nonionic surfactant at a concentration of 0.3%-0.8% of the total mass of the mixture; stir at high speed for 20-40 minutes at a speed of 800-1200 r / min to obtain a uniformly dispersed composite coating solution without precipitation. The surfactant can improve the interfacial compatibility between the polar prepolymer and the nonpolar fluorine dispersion, avoid phase separation, agglomeration and precipitation, and ensure that the polymer precursor is uniformly dispersed in the fluorine matrix. After final curing, the imprinted sites are uniformly distributed inside the coating, giving full play to the selective catalytic effect. This ratio range can ensure the continuity of film formation in the fluorine matrix while retaining sufficient recognition sites.
[0018] Furthermore, in step S3, the composite coating liquid is applied to the outer surface of the iridium-tantalum active coating by brushing, soaking, or spraying, and then kept at an oven temperature of 70-90℃ for 1.5-2.5 hours to generate a polymer encapsulating template ions. Continue heating to 120-400℃ and hold for 8-15 minutes to complete the curing of the fluorine-based polymer film.
[0019] The cured workpiece is immersed in the eluent and ultrasonic-assisted elution is performed until no template metal ions are detected in the eluent. The workpiece is removed, rinsed with deionized water, and dried. After the template ions are released, a specific cavity matching the target ions remains inside the polymer.
[0020] Depending on the target thickness, repeat the coating-in-situ polymerization-baking curing-template washing process 1-10 times to obtain a modified fluorine-based protective coating.
[0021] Furthermore, in step S4, the anode workpiece with all double-layer coatings prepared is placed in a muffle furnace; the post-treatment baking temperature is set to 200-400℃, and the holding time is 10-60 minutes; the medium-temperature baking eliminates the residual internal stress inside the coating, improves the interfacial bonding force between the iridium-tantalum active coating and the modified fluorine protective coating, and improves the overall chemical and electrochemical stability of the coating. The medium-temperature post-treatment can release the residual internal stress caused by temperature difference and polymerization shrinkage during the coating preparation process, reducing the risk of coating cracking; at the same time, it promotes molecular diffusion and physical entanglement at the interface of the two coating layers, improves the interlayer bonding force, and avoids peeling and flaking of the outer coating during long-term use. After the holding time is completed, the workpiece is naturally cooled to room temperature with the furnace to obtain the finished electroplated anode coating.
[0022] Compared with existing technologies, this electroplating anodic coating has the following advantages: This invention constructs a modified fluorine-based protective coating outside a titanium-based iridium-tantalum active coating. The chemical inertness and low surface energy of the fluorine polymer create a dense physical barrier, effectively preventing organic brighteners and leveling agents in the plating bath from directly contacting the highly catalytically active inner oxide layer. This reduces the oxidation consumption rate of the brighteners, decreases the generation and accumulation of organic decomposition byproducts, and reduces quality defects such as pinholes and pitting in the coating. Furthermore, the polymer in situ composited within the coating creates a specific cavity that perfectly matches the target metal ions in terms of spatial size, coordination configuration, and charge distribution. This enables preferential electron transfer catalysis of the target metal ions, selectively suppressing anodic side reactions of impurity ions such as iron, copper, and lead, ensuring a stable and orderly electrodeposition process, and improving the purity and uniformity of the coating.
[0023] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0025] Figure 1 This is a flowchart of a method for preparing an electroplated anodic coating; Figure 2 This is a flowchart of step S3, the preparation of the prepolymer solution, in a method for preparing an electroplated anodic coating. Detailed Implementation
[0026] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0027] Example 1 The titanium substrate used in this embodiment is a 100mm×50mm×2mm TA1 industrial pure titanium plate, such as... Figure 1 As shown, the specific preparation steps are as follows: The titanium plate was completely immersed in a 5% sodium hydroxide aqueous solution, with the liquid level 2 cm above the plate surface. Ultrasonic cleaning was performed for 10 minutes at 200W to remove oil. After removal, it was rinsed three times with flowing deionized water. Then, it was placed in a 10% oxalic acid solution at 80℃ and acid-washed in a water bath for 20 minutes, gently shaking the beaker every 5 minutes to ensure uniform roughening. After removal, it was repeatedly rinsed with flowing deionized water until the pH of the rinsing wastewater was 6.5-7.0. The titanium plate was then placed in a muffle furnace and heated to 500℃ at a rate of 5℃ / min, held at that temperature for 30 minutes, and then allowed to cool naturally to room temperature in a dust-free environment for later use.
[0028] Using chloroiridium acid hydrate (Ir content ≥37%) and n-butoxide tantalum (purity ≥99%) as solutes, weigh them according to the iridium to tantalum metal molar ratio of 7:3, dissolve them in a mixed solvent of n-butanol and concentrated hydrochloric acid in a volume ratio of 9:1, stir until completely dissolved, and prepare a coating solution with a total metal ion concentration of 0.2 mol / L.
[0029] Gravity-driven spray guns were used for coating, with a nozzle diameter of 1.0 mm, a spray gun pressure of 0.3 MPa, a gun distance of 18 cm from the titanium plate surface, and a gun travel speed of 10 cm / s. The spray guns were applied twice in a row to ensure complete wetting of the plate surface. After coating, the plate was immediately placed in a muffle furnace and heated to 500 °C at a rate of 5 °C / min, and sintered and held at that temperature for 15 min. After removal, the plate was allowed to cool naturally to room temperature, completing one coating-sintering cycle. The above cycle was repeated 10 times. Finally, the average thickness of the iridium-tantalum active coating was measured using an eddy current thickness gauge, which showed that the coating thickness was 8 μm.
[0030] like Figure 2 As shown, 0.01 mol of nickel nitrate hexahydrate was weighed and dissolved in a 7:3 volume ratio of ethanol to deionized water; 0.04 mol of methacrylic acid functional monomer was added and stirred at room temperature for 30 min to allow the template ions to fully coordinate with the monomer; then 0.2 mol of ethylene glycol dimethacrylate crosslinking agent and 0.002 mol of azobisisobutyronitrile initiator were added and stirred for another 25 min to obtain a homogeneous and transparent prepolymer solution.
[0031] Take a polytetrafluoroethylene dispersion emulsion with a solid content of 30% and mix it with the above prepolymer liquid at a mass ratio of 4:1; add nonylphenol polyoxyethylene ether nonionic surfactant accounting for 0.5% of the total mass of the mixture system, place it in a high-speed disperser, and stir at 1000 r / min for 30 min to obtain a uniform and stable composite coating liquid.
[0032] The coating was applied by immersion. The titanium plate loaded with iridium-tantalum coating was immersed in the composite coating liquid at a speed of 5 mm / s. After standing for 10 seconds, it was lifted at the same speed to drain the excess liquid from the surface. The plate was first placed in a 40℃ oven for 8 minutes to remove the surface solvent. Then, the temperature was increased to 80℃ at a rate of 2℃ / min and held for 2 hours to initiate in-situ crosslinking polymerization. The temperature was then increased to 380℃ at a rate of 5℃ / min and held for 10 minutes to complete the high-temperature curing and film formation.
[0033] The cured workpiece was immersed in a 0.1 mol / L EDTA-2Na solution (pH adjusted to 8.0), and ultrasonic power was set to 200W for assisted elution. The eluent was replaced with fresh solution every 4 hours, for a total of 3 replacements, with a total elution time of 12 hours. The final eluent was analyzed by atomic absorption spectrometry to determine the Ni content. 2+ A concentration below 0.1 mg / L is considered complete elution; remove the workpiece, rinse it three times with deionized water, and dry it at 60°C.
[0034] The above coating-pre-drying-in-situ polymerization-high temperature curing-template elution process was repeated twice. The final measured average thickness of the modified fluorine protective coating was 2 μm, of which the polymer accounted for approximately 18% by mass.
[0035] The finished workpiece is fed into a muffle furnace and heated to 300°C at a rate of 3°C / min. It is then held at this temperature for 30 minutes for post-processing. After the holding period, the workpiece is allowed to cool naturally to room temperature in the furnace to obtain the final anode sample.
[0036] Example 2 The titanium substrate used in this embodiment is a 100mm×50mm×2mm TA1 industrial pure titanium plate, which is suitable for acidic copper plating system.
[0037] The specific preparation steps are as follows: The titanium plate was completely immersed in a 5% sodium hydroxide aqueous solution, with the liquid level 2 cm above the plate surface. Ultrasonic cleaning was performed for 10 minutes at 200W to remove oil. After removal, it was rinsed three times with flowing deionized water. Then, it was placed in a 10% oxalic acid solution at 80℃ and acid-washed in a water bath for 20 minutes, gently shaking the beaker every 5 minutes to ensure uniform roughening. After removal, it was repeatedly rinsed with flowing deionized water until the pH of the rinsing wastewater was 6.5-7.0. The titanium plate was then placed in a muffle furnace and heated to 500℃ at a rate of 5℃ / min, held at that temperature for 30 minutes, and then allowed to cool naturally to room temperature in a dust-free environment for later use.
[0038] Using chloroiridium acid hydrate (Ir content ≥37%) and n-butoxide tantalum (purity ≥99%) as solutes, weigh them according to the iridium to tantalum metal molar ratio of 7:3, dissolve them in a mixed solvent of n-butanol and concentrated hydrochloric acid in a volume ratio of 9:1, stir until completely dissolved, and prepare a coating solution with a total metal ion concentration of 0.2 mol / L.
[0039] Gravity-driven spray guns were used for coating, with a nozzle diameter of 1.0 mm, a spray gun pressure of 0.3 MPa, a gun distance of 18 cm from the titanium plate surface, and a gun travel speed of 10 cm / s. The spray guns were applied twice in a row to ensure complete wetting of the plate surface. After coating, the plate was immediately placed in a muffle furnace and heated to 400 °C at a rate of 4 °C / min, and sintered and held at that temperature for 15 min. After removal, the plate was allowed to cool naturally to room temperature, completing one coating-sintering cycle. The above cycle was repeated a total of 5 times. Finally, the average thickness of the iridium-tantalum active coating was measured using an eddy current thickness gauge, which showed that the coating thickness was 3.5 μm.
[0040] Weigh 0.01 mol of copper sulfate pentahydrate and dissolve it in a 1:4 volume ratio of ethanol to N-methylpyrrolidone mixed solvent; add 0.04 mol of acrylamide functional monomer and stir at room temperature for 30 min to allow the template ions to fully coordinate and complex with the monomer; then add 0.2 mol of divinylbenzene crosslinking agent and 0.002 mol of benzoyl peroxide initiator and continue stirring for 25 min to obtain a homogeneous and transparent prepolymer solution.
[0041] Take a 20% solid content polyvinylidene fluoride N-methylpyrrolidone solution and mix it with the above prepolymer solution at a mass ratio of 5:1; add 0.6% of the total mass of the mixture of Tween-80 nonionic surfactant, place it in a high-speed disperser, and stir at 900 r / min for 35 min to obtain a uniform and stable composite coating solution.
[0042] Gravity-driven spray guns were used for coating, with a nozzle diameter of 0.8 mm, a spray gun pressure of 0.25 MPa, a gun distance of 20 cm from the titanium plate surface, and a gun travel speed of 12 cm / s. The coating was applied twice in a row to ensure a thin and uniform coating. The plate was first placed in a 35°C oven for 10 min to pre-dry and remove surface solvents. Then, the temperature was increased to 75°C at a rate of 2°C / min and held for 2 h to initiate in-situ crosslinking polymerization. Finally, the temperature was increased to 180°C at a rate of 3°C / min and held for 12 min to complete the curing and film formation.
[0043] The cured workpiece was immersed in a 0.1 mol / L dilute nitric acid solution, and ultrasonic power of 180 W was used for assisted elution. The eluent was replaced with fresh solution every 5 hours, for a total of 2 replacements, with a total elution time of 10 hours. The last eluent was analyzed by atomic absorption spectrometry, and Cu was found to be present. 2+ A concentration below 0.1 mg / L is considered complete elution; remove the workpiece, rinse with deionized water until neutral, and dry at 60°C.
[0044] The above coating-pre-drying-in-situ polymerization-baking curing-template elution process was repeated three times. The final measured average thickness of the modified fluorine-based protective coating was 5 μm, with the polymer accounting for approximately 12% of the total mass.
[0045] The finished workpiece is fed into a muffle furnace and heated to 280°C at a rate of 3°C / min. It is then held at this temperature for 30 minutes for post-processing. After the holding period, the workpiece is allowed to cool naturally to room temperature in the furnace to obtain the final anode sample.
[0046] Example 3 In this embodiment, the titanium substrate used is a 100mm×50mm×2mm TA1 industrial pure titanium plate. The anodic coating is prepared using the following specific steps: The titanium plate was completely immersed in a 5% sodium hydroxide aqueous solution, with the liquid level 2 cm above the plate surface. Ultrasonic cleaning was performed for 10 minutes at 200W to remove oil. After removal, it was rinsed three times with flowing deionized water. Then, it was placed in a 10% oxalic acid solution at 80℃ and acid-washed in a water bath for 20 minutes, gently shaking the beaker every 5 minutes to ensure uniform roughening. After removal, it was repeatedly rinsed with flowing deionized water until the pH of the rinsing wastewater was 6.5-7.0. The titanium plate was then placed in a muffle furnace and heated to 650℃ at a rate of 6℃ / min, held at that temperature for 25 minutes, and then allowed to cool naturally to room temperature in a dust-free environment for later use.
[0047] Using chloroiridium acid hydrate (Ir content ≥37%) and n-butoxide tantalum (purity ≥99%) as solutes, weigh them according to the iridium to tantalum metal molar ratio of 7:3, dissolve them in a mixed solvent of n-butanol and concentrated hydrochloric acid in a volume ratio of 9:1, stir until completely dissolved, and prepare a coating solution with a total metal ion concentration of 0.2 mol / L.
[0048] A soft nylon brush was used to apply a small amount of coating liquid evenly to the surface of the titanium plate in the same direction, ensuring a thin, drip-free, and unspoiled coating. After coating, the plate was immediately placed in a muffle furnace and heated to 550°C at a rate of 5°C / min, and sintered for 12 minutes. After removal, the plate was allowed to cool naturally to room temperature, completing one coating-sintering cycle. The above cycle was repeated 15 times. Finally, the average thickness of the iridium-tantalum active coating was measured to be 12 μm using an eddy current thickness gauge.
[0049] Weigh 0.01 mol of nickel nitrate hexahydrate and dissolve it in a 7:3 volume ratio of ethanol to deionized water. Add 0.04 mol of methacrylic acid functional monomer and stir at room temperature for 30 min to allow the template ions to fully coordinate with the monomer. Then add 0.2 mol of ethylene glycol dimethacrylate crosslinking agent and 0.002 mol of azobisisobutyronitrile initiator and continue stirring for 25 min to obtain a homogeneous and transparent prepolymer solution.
[0050] Take a polytetrafluoroethylene dispersion emulsion with a solid content of 30% and mix it with the above prepolymer liquid at a mass ratio of 9:1; add nonylphenol polyoxyethylene ether nonionic surfactant accounting for 0.4% of the total mass of the mixture system, place it in a high-speed disperser, and stir at 1100 r / min for 25 min to obtain a uniform and stable composite coating liquid; the polymer mass ratio in the final coating is about 8%.
[0051] The coating was applied by immersion. The titanium plate loaded with iridium-tantalum coating was immersed in the composite coating liquid at a speed of 5 mm / s. After standing for 10 seconds, it was lifted at the same speed to drain the excess liquid from the surface. The plate was first placed in a 50℃ oven for 6 minutes to remove the surface solvent. Then, the temperature was increased to 85℃ at a rate of 2℃ / min and held for 2 hours to initiate in-situ crosslinking polymerization. The temperature was then increased to 360℃ at a rate of 5℃ / min and held for 10 minutes to complete the high-temperature curing and film formation.
[0052] The cured workpiece was immersed in a 0.1 mol / L EDTA-2Na solution (pH adjusted to 8.0), and ultrasonic power was set to 200W for assisted elution. The eluent was replaced with fresh solution every 4 hours, for a total of 3 replacements, with a total elution time of 12 hours. The final eluent was analyzed by atomic absorption spectrometry to determine the Ni content. 2+ A concentration below 0.1 mg / L is considered complete elution; remove the workpiece, rinse it three times with deionized water, and dry it at 60°C.
[0053] The above coating-pre-drying-in-situ polymerization-high temperature curing-template elution process was repeated twice, and the final measured average thickness of the modified fluorine-based protective coating was approximately 2.2 μm.
[0054] The finished workpiece is fed into a muffle furnace and heated to 320°C at a rate of 4°C / min. It is then held at this temperature for 20 minutes for post-processing. After the holding period, the workpiece is allowed to cool naturally to room temperature in the furnace to obtain the final anode sample.
[0055] Comparative Example 1 The ordinary iridium-tantalum coated titanium-based anode only prepares the iridium-tantalum active coating, without fluorine-based protective coating and polymer. The titanium substrate pretreatment and iridium-tantalum coating preparation process and parameters are completely consistent with those in Example 1.
[0056] Comparative Example 2 The iridium-tantalum anode with a pure fluorine-based outer coating has the same preparation process as in Example 1 for the iridium-tantalum active coating and the polytetrafluoroethylene outer coating, but without the addition of polymers and corresponding precursors to the outer coating.
[0057] Performance comparison test: The anode samples of Examples 1-3 and Comparative Examples 1-2 were placed in the same bright nickel plating system for a 72-hour continuous energization accelerated test.
[0058] Test conditions: The plating bath composition was 280 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid, and 8 mL / L commercial brightener; artificially added impurity ions: Fe 2+ 50mg / L, Cu 2+ 20 mg / L, Pb 2+ 10 mg / L; current density 2 A / dm 2 The plating solution temperature is 55℃, and the cathode is a pure nickel plate.
[0059] Detection methods: Brightener concentration was quantitatively detected using a UV-Vis spectrophotometer at characteristic wavelengths; impurity ion concentration was determined using an atomic absorption spectrometer; coating purity was detected using an X-ray fluorescence spectrometer (XRF); coating appearance was observed using a stereomicroscope; relative anode lifetime was estimated based on coating weight loss rate from accelerated corrosion tests.
[0060] The test results are shown in the table below:
[0061] In summary, compared with Comparative Example 1, the remaining brightener rate of Comparative Example 2 and Examples 1-3 was significantly improved, indicating that the fluorine-based outer coating can effectively block the contact between the brightener and the iridium-tantalum active layer, reducing the oxidation consumption of the brightener. Compared with Comparative Example 2, the total oxidation rate of impurity ions in Examples 1-3 decreased significantly, and the coating purity was significantly improved, proving that the polymer can selectively catalyze the electron transfer of target metal ions, inhibit the anodic oxidation side reaction of impurity ions such as iron, copper, and lead, and reduce the mixing of impurities into the coating. No cracking or peeling was observed in the coating of any of the samples, indicating that the gradient curing and post-treatment process of the present invention can ensure the interfacial bonding of the double-layer coating. The relative anode life data shows that the composite coating of the present invention can significantly slow down anode loss and extend service life.
[0062] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. An electroplated anodic coating, disposed on the surface of a titanium substrate, characterized in that: Including iridium-tantalum active coatings and modified fluorine-based protective coatings; The iridium-tantalum active coating is laminated onto the surface of the pretreated titanium substrate, with a thickness of 0.1-100 μm; the baking temperature for preparing the iridium-tantalum active coating is 300-600℃. The modified fluorine-based protective coating is uniformly applied to the outer surface of the iridium-tantalum active coating, with a thickness of 0.01-20 μm, and is cured at a baking temperature of 120-400℃; a fluorine-based polymer is used as the film-forming matrix, and the polymer is uniformly dispersed inside the matrix. The polymer uses the metal ions to be plated as template ions and forms imprinted sites with specific recognition cavities through cross-linking polymerization of functional monomers. The imprinted sites match the target metal ions in terms of spatial size, coordination configuration and charge distribution, and have a preferential electron transfer catalytic effect on the target metal ions, while exhibiting electrochemical inertness to iron, copper and lead impurity metal ions.
2. The electroplating anodic coating according to claim 1, characterized in that, The titanium substrate is any one of industrial pure titanium plate, titanium mesh or titanium rod, and the surface is pre-treated by degreasing, pickling and roughening, and then baked at a high temperature of 400-700℃.
3. The electroplating anodic coating according to claim 1, characterized in that, The fluorinated polymer is selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, perfluoroalkoxy resin, and fluorinated ethylene propylene copolymer.
4. The electroplating anodic coating according to claim 1, characterized in that, The template ion is selected from Ni. 2+ Cu 2+ Zn 2+ Cr 3+ Any one of the following; the functional monomer is selected from one or more of methacrylic acid, acrylic acid, acrylamide, and vinylimidazole; the crosslinking agent is selected from divinylbenzene, ethylene glycol dimethacrylate, and trimethylolpropane triacrylate; the initiator is selected from azo or peroxide initiators.
5. A method for preparing an electroplated anodic coating according to any one of claims 1-4, characterized in that, Includes the following steps: S1: The titanium substrate is degreased, pickled and roughened in sequence, rinsed clean and then baked and dried at high temperature to complete the pretreatment of the titanium substrate. S2: Prepare an iridium-tantalum precursor coating solution, coat it onto the surface of the pretreated titanium substrate and bake and sinter it. Repeat the coating-sintering cycle to the target thickness to obtain the inner iridium-tantalum active coating. S3: Prepare a prepolymer solution and mix it with a fluorine-based polymer dispersion to obtain a composite coating solution. Coat the surface of the iridium-tantalum active coating solution with the composite coating solution. After in-situ polymerization, baking and curing and template ion elution, repeat the coating-polymerization-elution cycle until the target thickness is reached to obtain a modified fluorine-based protective coating. S4: The workpiece with the double coating is then baked to eliminate internal stress in the coating and improve the interfacial bonding force. After natural cooling, the finished product is obtained.
6. The method for preparing an electroplated anodic coating according to claim 5, characterized in that, In S1, the high-temperature baking and drying conditions are: baking and holding at 400-700℃ for 20-40 minutes, and then cooling before use.
7. The electroplating anodic coating according to claim 5, characterized in that, In step S2, the coating liquid is applied to the surface of the titanium substrate by brushing, immersion or spraying, and the substrate is kept at 300-600℃ for 10-20 minutes to complete a single coating-sintering cycle. The coating-baking-sintering cycle is repeated 1-20 times to obtain an iridium-tantalum active coating with a thickness of 0.1-100μm.
8. The electroplating anodic coating according to claim 5, characterized in that, In step S3, the prepolymer solution is prepared as follows: Dissolve the template metal salt to be plated in an ethanol-deionized water mixed solvent to prepare a template ion solution; the molar amount of template ions is 0.008-0.012 mol. Add the functional monomer, with a template ion to functional monomer molar ratio of 1:3-5; stir at room temperature for 20-40 min to achieve full coordination and complexation of the template ion and functional monomer. Continue adding crosslinking agent, with a molar ratio of crosslinking agent to functional monomer of 3-5:1; then add initiator, with the initiator accounting for 1%-2% of the mass fraction of crosslinking agent; continue stirring for 15-30 minutes to obtain a homogeneous prepolymer solution.
9. The electroplating anodic coating according to claim 5, characterized in that, The preparation method of the composite coating liquid in S3 is as follows: Take a fluorine-based polymer dispersion with a solid content of 0.5%-40%; mix the prepolymer solution and the fluorine-based polymer dispersion at a mass ratio of 1:3-10; Add a nonionic surfactant at a concentration of 0.3%-0.8% of the total mass of the mixture; stir at high speed for 20-40 minutes at a speed of 800-1200 r / min to obtain a uniformly dispersed composite coating solution without precipitation.
10. The electroplating anodic coating according to claim 5, characterized in that, In step S3, the composite coating liquid is applied to the outer surface of the iridium-tantalum active coating by brushing, soaking, or spraying, and then kept at 70-90℃ in an oven for 1.5-2.5 hours to generate a polymer encapsulating template ions. Continue heating to 120-400℃ and hold for 8-15 minutes to complete the curing of the fluorine-based polymer film. The cured workpiece is immersed in the eluent and ultrasonic-assisted elution is performed until no template metal ions are detected in the eluent. Remove the workpiece, rinse with deionized water, and dry it; after releasing the template ions, a specific cavity matching the target ions remains inside the polymer. Depending on the target thickness, repeat the coating-in-situ polymerization-baking curing-template washing process 1-10 times to obtain a modified fluorine-based protective coating.