Group III nitride semiconductor epitaxial wafers and electronic devices

By epitaxially growing Al and Ga films on a group III nitride semiconductor substrate and controlling the warpage, the problem of insufficient flatness of group III nitride semiconductor films was solved, and a flat surface and low resistance characteristics of high-frequency electronic devices were achieved.

CN123108731APending Publication Date: 2026-11-17PANASONIC HOLDINGS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610553884.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Group III nitride semiconductor films grown directly on group III nitride semiconductor substrates obtained by HVPE and OVPE methods often do not achieve sufficient flatness.

Method used

By epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on a group III nitride semiconductor substrate, and epitaxially growing a multilayer group III nitride semiconductor film on it, the warpage amount is controlled by the total warpage amount CE and the correction coefficient α to keep it within a reasonable range.

Benefits of technology

It achieves the flatness of the uppermost surface of group III nitride semiconductor epitaxial wafers, making it suitable for high-frequency or high-output electronic devices, and reducing the operating resistance and leakage current of the devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108731A_ABST
    Figure CN123108731A_ABST
Patent Text Reader

Abstract

The group III nitride semiconductor epitaxial wafer of the present invention comprises: a group III nitride semiconductor substrate exhibiting n-type conductivity; a first group III nitride semiconductor film epitaxially grown on the group III nitride semiconductor substrate, comprising Al and Ga as group III elements; and second to Nth group III nitride semiconductor films in which N is a natural number of 2 or more and epitaxially grown on the first group III nitride semiconductor film, wherein the total warpage C of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction. E (μm) satisfies: , and further, when the warpage of the group III nitride semiconductor substrate is set as C, with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following condition is satisfied:
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a group III nitride semiconductor epitaxial wafer having a group III nitride semiconductor substrate, a first group III nitride semiconductor film epitaxially grown thereon, and a second group III nitride semiconductor film epitaxially grown on the first group III nitride semiconductor film, and an electronic device using the group III nitride semiconductor epitaxial wafer. Background Technology

[0002] Group III nitride semiconductors are used in optical devices such as semiconductor lasers and light-emitting diodes, as well as in high-frequency or high-output electronic devices. These semiconductors have attracted particular attention in recent years because they offer the potential for reduced switching losses during power conversion compared to silicon-based devices. To fabricate high-frequency or high-output electronic devices, it is necessary to fabricate devices on high-quality group III nitride semiconductor substrates that can suppress crystal defects generated in the device layers.

[0003] Methods for manufacturing group III nitride crystals include, for example, hydride vapor phase growth (hereinafter also known as HVPE), ammonium thermal method, sodium flux method, and oxide vapor phase growth (hereinafter also known as OVPE).

[0004] In the HVPE process, which is most commonly used for substrate fabrication, hydrogen halide gas is introduced into elemental group III raw materials to generate halide gas, and the resulting group III element halide gas is used as the feed gas for crystal growth. For example, in the case of gallium nitride crystal growth, gallium chloride (e.g., GaCl2) gas is generated by introducing HCl gas into Ga metal, and gallium chloride-containing gas is used as a group III source, thereby achieving high-speed growth of 1 mm / h or higher. In the HVPE process, it is known that group III nitride crystals with N-type conductivity are mainly obtained by adding silicon to the group III nitride crystal.

[0005] In the OVPE method, oxygen is added at a high concentration to a group III nitride crystal using an oxide feed gas to produce the crystal (see, for example, Patent Document 1). In this method, a group III oxide gas is reacted with a nitrogen-containing gas to produce a group III nitride crystal. The substrate obtained by this method has a dislocation density of 10-1. 4 cm -2 With low dislocation density, the OVPE method is one of the means to obtain high-quality group III nitride crystals.

[0006] In addition, a technique for forming multiple group III nitride semiconductor layers with different n-type carrier concentrations on a support substrate is disclosed (for example, see Patent Document 2).

[0007] Existing technical documents Patent documents [Patent Document 1] WO2015 / 053341A1 [Patent Document 2] Japanese Patent No. 6237401 Summary of the Invention

[0008] The problem that the invention aims to solve However, the inventors have discovered the following problem: sometimes the group III nitride semiconductor film grown directly on a group III nitride semiconductor substrate obtained by the HVPE method and the OVPE method does not achieve sufficient flatness.

[0009] Therefore, the purpose of this disclosure is to provide a group III nitride semiconductor epitaxial wafer with the flattest surface, having a group III nitride semiconductor film epitaxially grown on a group III nitride semiconductor substrate.

[0010] means for solving problems The group III nitride semiconductor epitaxial wafer disclosed herein comprises: a group III nitride semiconductor substrate exhibiting n-type conductivity; a first group III nitride semiconductor film epitaxially grown on the group III nitride semiconductor substrate, comprising Al and Ga as group III elements; and second to Nth group III nitride semiconductor films, where N is a natural number of 2 or more, epitaxially grown on the first group III nitride semiconductor film, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), let the composition of Al be a i (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as .

[0011] Furthermore, when the warpage of the group III nitride semiconductor substrate is defined as C, with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), it satisfies .

[0012] The disclosed group III nitride semiconductor epitaxial wafer comprises: a group III nitride semiconductor substrate exhibiting n-type conductivity; a first group III nitride semiconductor film epitaxially grown on the group III nitride semiconductor substrate, comprising Al and Ga as group III elements; and second to Nth group III nitride semiconductor films, where N is a natural number of 2 or more, epitaxially grown on the first group III nitride semiconductor film, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), representing the thickness along the thickness direction of the i-th group III nitride semiconductor film from film thickness 0 (μm) to film thickness t. i Let a be a function of the thickness t in the range of (μm) composed of Al. i (t)(atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0013] Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following is satisfied: .

[0014] The electronic device disclosed herein uses the aforementioned group III nitride semiconductor epitaxial wafer.

[0015] The method for manufacturing a group III nitride semiconductor epitaxial wafer disclosed herein includes: a step of forming a group III nitride semiconductor substrate with n-type conductivity; a step of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and a step of epitaxially growing a second to an Nth group III nitride semiconductor film on the first group III nitride semiconductor film, where N is a natural number of 2 or more, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), let the composition of Al be ai (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0016] Furthermore, when the warpage of the group III nitride semiconductor substrate is defined as C, with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), to satisfy The method enables the epitaxial growth of group III nitride semiconductor films from the first to the Nth.

[0017] The method for manufacturing a group III nitride semiconductor epitaxial wafer disclosed herein includes: a step of forming a group III nitride semiconductor substrate with n-type conductivity; a step of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and a step of epitaxially growing a second to an Nth group III nitride semiconductor film on the first group III nitride semiconductor film, where N is a natural number of 2 or more, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), representing the thickness along the thickness direction of the i-th group III nitride semiconductor film from film thickness 0 (μm) to film thickness t. i Let a be a function of the thickness t in the range of (μm) composed of Al. i (t)(atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0018] Furthermore, when the warpage of the group III nitride semiconductor substrate is defined as C, with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), to satisfy The method enables the epitaxial growth of group III nitride semiconductor films from the first to the Nth.

[0019] Invention Effects According to the group III nitride semiconductor epitaxial wafer disclosed herein, by setting a first group III nitride semiconductor film containing Al and Ga as group III elements as an intermediate layer, the flatness of the uppermost surface of the second to Nth group III nitride semiconductor films can be ensured. Attached Figure Description

[0020] Figure 1 This is a schematic cross-sectional view showing the cross-sectional structure of the group III nitride semiconductor epitaxial wafer of Embodiment 1.

[0021] Figure 2 This is a schematic cross-sectional view showing the amount and depth of warpage of a group III nitride semiconductor epitaxial wafer that warps in the downward convex direction.

[0022] Figure 3 This is a flowchart of a method for manufacturing a group III nitride semiconductor substrate constituting a group III nitride semiconductor epitaxial wafer according to Embodiment 1.

[0023] Figure 4 This is a schematic cross-sectional view showing the cross-sectional structure of the manufacturing apparatus for the group III nitride semiconductor substrate constituting the group III nitride semiconductor epitaxial wafer of Embodiment 1.

[0024] Figure 5 Table 1 shows the composition of each layer of the group III nitride semiconductor epitaxial wafers of Examples 1 to 3, in which the first to Nth group III nitride semiconductor films are epitaxially grown on a group III nitride semiconductor substrate formed by the HVPE method.

[0025] Figure 6 Table 2 shows the 3μm square AFM images and 30μm square AFM images of the surface of the group III nitride semiconductor epitaxial wafers of Examples 1 to 3, as well as the deviation angle and root mean square roughness (RMS) values ​​of the group III nitride semiconductor epitaxial wafers.

[0026] Figure 7 Table 3 shows the composition of each layer of the group III nitride semiconductor epitaxial wafers of Examples 4 to 6, in which the first to Nth group III nitride semiconductor films are epitaxially grown on a group III nitride semiconductor substrate formed by the OVPE method.

[0027] Figure 8 Table 4 shows the 3μm square AFM images and 30μm square AFM images of the surface of the group III nitride semiconductor epitaxial wafers of Examples 4 to 6, as well as the deviation angle and root mean square roughness (RMS) values ​​of the group III nitride semiconductor epitaxial wafers.

[0028] Figure 9A This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 7.

[0029] Figure 9B This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 8.

[0030] Figure 9C This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 9.

[0031] Figure 9D This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 10.

[0032] Figure 10A This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 11.

[0033] Figure 10B This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 12.

[0034] Figure 10C This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 13. Detailed Implementation

[0035] <The Process of Reaching This Publication> As described above, group III nitride semiconductor films grown directly on group III nitride semiconductor substrates sometimes suffer from insufficient flatness. To address this problem, the inventors have developed an insight related to the first technical feature of this disclosure: flatness is achieved by epitaxially growing a group III nitride semiconductor film containing one or more group III elements, Al and Ga, on a group III nitride semiconductor substrate.

[0036] On the other hand, the inventors discovered the following problem: in a Group III nitride semiconductor epitaxial wafer formed by epitaxially growing a first Group III nitride semiconductor film containing Al and Ga, a warping amount in the convex direction caused by the difference in lattice constants between GaN and AlN or AlGaN occurs. Regarding this problem, the inventors conducted in-depth research and found that the warping amount can be estimated by multiplying the product of the thickness t (μm) of the epitaxially grown Group III nitride semiconductor film, the Al composition a (atom%), and the diameter Φ of the Group III nitride semiconductor epitaxial wafer, by a correction factor α. This warping amount can be adjusted to below the upper limit, thereby achieving the second technical feature of this disclosure.

[0037] The following are examples of the various methods disclosed herein.

[0038] The first method involves a group III nitride semiconductor epitaxial wafer comprising: a group III nitride semiconductor substrate exhibiting n-type conductivity; a first group III nitride semiconductor film epitaxially grown on the group III nitride semiconductor substrate, comprising Al and Ga as group III elements; and second to Nth group III nitride semiconductor films, where N is a natural number of 2 or more, epitaxially grown on the first group III nitride semiconductor film. The total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate, with the convex direction as the positive direction, is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), let the composition of Al be a i (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0039] Furthermore, when the warpage of the group III nitride semiconductor substrate is defined as C, with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following is satisfied: .

[0040] The second method involves a group III nitride semiconductor epitaxial wafer comprising: a group III nitride semiconductor substrate exhibiting n-type conductivity; a first group III nitride semiconductor film epitaxially grown on the group III nitride semiconductor substrate, comprising Al and Ga as group III elements; and second to Nth group III nitride semiconductor films, where N is a natural number of 2 or more, epitaxially grown on the first group III nitride semiconductor film, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), representing the thickness along the thickness direction of the i-th group III nitride semiconductor film from film thickness 0 (μm) to film thickness t. i Let a be a function of the thickness t in the range of (μm) composed of Al. i (t)(atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0041] Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following is satisfied: .

[0042] Regarding the III-nitride semiconductor epitaxial wafer involved in the third approach, in the first or second approach described above, the Al composition of the first III-nitride semiconductor film can be 0.1 atm% or more.

[0043] Regarding the group III nitride semiconductor epitaxial wafer involved in the fourth method, in any of the first to third methods described above, the carrier concentration of the group III nitride semiconductor substrate can be 10. 17 cm -3 Above and 10 19 cm -3 the following.

[0044] Regarding the group III nitride semiconductor epitaxial wafer involved in the fifth method, in any of the first to fourth methods mentioned above, the carrier concentration of the group III nitride semiconductor substrate is 10. 20 cm -3 The doping element can be oxygen.

[0045] Regarding the group III nitride semiconductor epitaxial wafer involved in the sixth method, in any of the first to fifth methods described above, the carrier concentration of the first group III nitride semiconductor film can be 10. 17 cm -3 above.

[0046] Regarding the group III nitride semiconductor epitaxial wafer involved in the seventh method, in any of the first to sixth methods described above, the carrier concentration of the i-th group III nitride semiconductor film with i=2 or more epitaxially grown on the first group III nitride semiconductor film can be 10. 17 cm -3 the following.

[0047] Regarding the group III nitride semiconductor epitaxial wafer involved in the eighth method, in any of the first to seventh methods described above, the carrier concentration of the first group III nitride semiconductor film is 10. 17 cm -3 The carrier concentration of the i-th group III nitride semiconductor film with i=2 or more, epitaxially grown on the first group III nitride semiconductor film, can be 10. 17 cm -3 the following.

[0048] Regarding the electronic device involved in the ninth method, the aforementioned group III nitride semiconductor epitaxial wafer involved in any of the first to eighth methods is used.

[0049] The tenth method relates to a method for manufacturing a group III nitride semiconductor epitaxial wafer, comprising: a step of forming a group III nitride semiconductor substrate with n-type conductivity; a step of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and a step of epitaxially growing a second to an Nth group III nitride semiconductor film on the first group III nitride semiconductor film, where N is a natural number of 2 or more, wherein the total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate with the convex direction as the positive direction is defined as C. E (μm), where i is a natural number from 1 to N, and the thickness of the i-th group III nitride semiconductor film is denoted as t. i (μm), let the composition of Al be a i (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction factor is set to α, the total warpage C E (μm) is represented as: .

[0050] Further, let the warpage amount with the downward convex direction defined as the positive direction of the group III nitride semiconductor substrate be C S (μm), and let the upper limit warpage amount of the group III nitride semiconductor epitaxial wafer be C L (μm), the first to N-th group III nitride semiconductor films are epitaxially grown so as to satisfy .

[0051] The method for manufacturing a group III nitride semiconductor epitaxial wafer according to the eleventh aspect includes: a step of forming a group III nitride semiconductor substrate exhibiting n-type conductivity; a step of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and a step of epitaxially growing second to N-th group III nitride semiconductor films on the first group III nitride semiconductor film, wherein N is a natural number of 2 or more, and the total of the warpage amounts with the downward convex direction defined as the positive direction of the first to N-th group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate is defined as C E (μm), i is a natural number from 1 to N, the film thickness of the i-th group III nitride semiconductor film is defined as t i (μm), the function of the Al composition at thickness t in the range from the film thickness of 0 (μm) to the film thickness t along the film thickness direction of the i-th group III nitride semiconductor film is defined as a i (μm), i (t) (atom%), the diameter of the group III nitride semiconductor epitaxial wafer is defined as Φ (cm), and the correction coefficient is defined as α, the total warpage amount C E (μm) is expressed as: .

[0052] Further, let the warpage amount with the downward convex direction defined as the positive direction of the group III nitride semiconductor substrate be C S (μm), and let the upper limit warpage amount of the group III nitride semiconductor epitaxial wafer be C L (μm), the first to N-th group III nitride semiconductor films are epitaxially grown so as to satisfy .

[0053] Hereinafter, the group III nitride semiconductor epitaxial wafer and the manufacturing method thereof according to the embodiments of the present disclosure will be described with reference to the accompanying drawings.

[0054] (Embodiment 1) <Group III Nitride Semiconductor Epitaxial Wafer> Figure 1 FIG. 2 is a schematic cross-sectional view that schematically shows an example of the group III nitride semiconductor epitaxial wafer 10 according to the first embodiment of the present invention.

[0055] The group III nitride semiconductor epitaxial wafer 10 of the present disclosure includes at least three layers, namely a group III nitride semiconductor substrate 2, a first group III nitride semiconductor film 4 including an epitaxial layer epitaxially grown on the substrate, and a second group III nitride semiconductor film 6 epitaxially grown on the first group III nitride semiconductor film 4. The group III nitride semiconductor substrate 2 exhibits n-type conductivity.

[0056] Hereinafter, each component constituting the group III nitride semiconductor epitaxial wafer 10 will be described.

[0057] <Group III Nitride Semiconductor Substrate> The group III nitride semiconductor substrate 2 is doped with impurities serving as n-type dopants to exhibit n-type conductivity, for example, in order to reduce on-resistance during operation, and the carrier concentration thereof may be 10 20 cm -3 or higher.

[0058] The n-type dopant element of the group III nitride semiconductor substrate 2 may include, for example, at least one selected from the group consisting of silicon element, germanium element and oxygen element.

[0059] It is more preferable that the n-type dopant element of the group III nitride semiconductor substrate includes, for example, oxygen element. In this case, particularly when the group III nitride semiconductor substrate for the substrate is produced by the OVPE method, the oxygen element can be easily added into the group III nitride semiconductor substrate.

[0060] In a case where oxygen element is the main element as the n-type dopant element of the group III nitride semiconductor substrate, the oxygen element may be added at a composition level of, for example, 10 20 atoms·cm -3 or higher. This makes it easy to set the carrier concentration of the group III nitride semiconductor substrate to 10 20 cm -3 or higher.

[0061] Note that the group III nitride semiconductor substrate is not limited to GaN obtained by the OVPE method, and may be GaN obtained by the HVPE method.

[0062] <First Group III Nitride Semiconductor Film> The first group III nitride semiconductor film 4 is a group III nitride semiconductor film containing Al and Ga as group III elements, which is epitaxially grown on the group III nitride semiconductor substrate 2. If the total number of group III elements in the first group III nitride semiconductor film is set to 1, the Al composition ratio can be, for example, 0.001 (0.1 atom%) or more and 0.3 (30 atom%) or less.

[0063] The thickness of a group III nitride semiconductor film can be, for example, greater than 0.02 μm and less than 1 μm.

[0064] The thickness of the group III nitride semiconductor film is preferably 0.02 μm or more. When the group III nitride semiconductor film is thinner than 0.02 μm, a stable surface cannot be sufficiently formed when forming an epitaxial layer on the substrate, and sufficient flatness cannot be obtained.

[0065] The thickness of the Group III nitride semiconductor film is preferably less than 1 μm. When it exceeds 1 μm, it may sometimes cause lattice mismatch with the Group III nitride semiconductor film epitaxially grown thereon.

[0066] <Group III nitride semiconductor films from the second to the Nth> N is a natural number greater than or equal to 2, and the second to Nth group III nitride semiconductor films are at least one group III nitride semiconductor film epitaxially grown on a group III nitride semiconductor substrate. The thickness of each group III nitride semiconductor film, from the second to the Nth, can be, for example, 1 μm or more and 30 μm or less. By setting each of the second to Nth group III nitride semiconductor films to 1 μm or more, a sufficiently stable surface can be formed when the epitaxial layer is formed on the substrate, enabling the formation of a device on the uppermost surface. Furthermore, if the thickness is 30 μm or less, it is easier to maintain the planarity of the epitaxial layer.

[0067] The thickness of each of the second to Nth group III nitride semiconductor films is more preferably 1 μm or more and 8 μm or less. If it is 1 μm or more and 8 μm or less, a film with a sufficiently stable surface can be formed, and flatness can be adequately maintained even when the lattice mismatch between the substrate and the epitaxial layer is large.

[0068] The epitaxial layers constituting the second to Nth group III nitride semiconductor films can be one layer or two or more layers.

[0069] The root mean square roughness (RMS) of the Nth group III nitride semiconductor film on the outermost surface of the second to Nth group III nitride semiconductor films is less than 1 nm when measured in a 30 μm square area, indicating sufficient flatness.

[0070] Furthermore, compared to the first group III nitride semiconductor film, the Al composition ratio of group III elements in the second to Nth group III nitride semiconductor films can be lower. When there are two or more epitaxial layers constituting the second to Nth group III nitride semiconductor films, the Al composition ratio can decrease as the film moves upward from the layer closest to the first group III nitride semiconductor film.

[0071] In addition, when used in electronic devices, it is possible to achieve devices with low resistance and low leakage current during operation.

[0072] <Regarding the warpage and warpage depth of group III nitride semiconductor epitaxial wafers> Figure 2 This is a schematic cross-sectional view showing the amount and depth of warpage of a group III nitride semiconductor epitaxial wafer that warps in the downward convex direction.

[0073] In the first group III nitride semiconductor film disposed on a group III nitride semiconductor substrate, since Al and Ga are included as group III elements, the group III nitride semiconductor epitaxial wafer exhibits a bulge warp due to the difference in lattice constants between GaN and AlN. Furthermore, in wafer fabrication processes using 6-inch Φ Si substrates, the limit for the bulge warp of the Si wafer is 60 μm to ensure good yield during focusing by steppers and other processes. That is, as described above, while flatness is achieved in the first group III nitride semiconductor film by including Al and Ga as group III elements, it is necessary to control the upper limit, i.e., the bulge warp C, which is restricted in subsequent wafer fabrication processes. L Within this range. Furthermore, convex wafers cannot be mounted in wafer fabrication processes.

[0074] The warp (μm) of the convexity of the group III nitride semiconductor film formed on the group III nitride semiconductor substrate is considered to be as follows: Figure 2 As shown, the warp of the convexity of the group III nitride semiconductor film increases proportionally to the diameter Φ (mm) of the wafer. Furthermore, it is believed that the warp of the convexity of the group III nitride semiconductor film (μm) increases proportionally to the thickness t (μm) of the group III nitride semiconductor film. Additionally, it is believed that the warp of the convexity of the group III nitride semiconductor film (μm) increases proportionally to the Al composition a (atom%) in the group III nitride semiconductor film.

[0075] If the above circumstances are considered, in the case where first to Nth group III nitride semiconductor films are provided over a group III nitride semiconductor substrate, the downward-convex warpage amount of each of the first to Nth group III nitride semiconductor films can be assumed to be represented by αΦta, which is obtained by multiplying the product of the wafer diameter Φ (mm), the thickness t (μm) of the group III nitride semiconductor film, and the Al composition a (atom%) in the group III nitride semiconductor film by a correction coefficient α. Further, the total C of the downward-convex warpage amounts of the first to Nth group III nitride semiconductor films E (μm) is represented by the sum of the downward-convex warpage amounts of the respective group III nitride semiconductor films. That is, the total C of the downward-convex warpage amounts E (μm) is expressed by the following formula (1): . Here, N is a natural number of 2 or more, and i is a natural number of 1 or more and N or less. In addition, since the downward-convex direction is defined as positive, the total C of the downward-convex warpage amounts E is 0 or more.

[0076] <Case where Al composition in group III nitride semiconductor film varies in thickness direction> In the above description, in the case where the Al composition in the group III nitride semiconductor film varies in the thickness direction, a function of the Al composition with respect to the thickness t in the range from the film thickness 0 (μm) to the film thickness t (μm) along the film thickness direction of the group III nitride semiconductor film is defined as a(t) (atom%). In this case, the downward-convex warpage amount of the group III nitride semiconductor film is represented by . Further, the total C of the downward-convex warpage amounts of the first to Nth group III nitride semiconductor films can be assumed E (μm) is represented by the sum of the downward-convex warpage amounts of the respective group III nitride semiconductor films. That is, the total C of the downward-convex warpage amounts E (μm) is expressed by the following formula (2): . Here, N is a natural number of 2 or more, and i is a natural number of 1 or more and N or less. In addition, since the downward-convex direction is defined as positive, the total C of the downward-convex warpage amounts E is 0 or more.

[0077] Further, the downward-convex warpage amount C which is the upper limit restricted in the wafer process as a subsequent step L (μm), the downward-convex warpage amount C of the group III nitride semiconductor substrate S (μm), and the total C of the downward-convex warpage amounts of the first to Nth group III nitride semiconductor filmsE (μm) needs to satisfy the following relationship (3): C L ≥C S +C E ≥0 (3).

[0078] <Constant Al composition in group III nitride semiconductor films> When the Al composition in a group III nitride semiconductor film is constant, the group III nitride semiconductor films from the first to the Nth need to be constructed in a manner that satisfies the following equation (4) which combines the above equations (1) and (3): .

[0079] <The variation of Al composition along the thickness direction in group III nitride semiconductor films> When the Al composition in a group III nitride semiconductor film varies in the thickness direction, the first to Nth group III nitride semiconductor films need to be constructed in a manner that satisfies the following equation (5) which combines the above equations (2) and (3): .

[0080] <Regarding the correction factor α> Next, the approximate calculation of the correction factor α under the following conditions will be explained.

[0081] As an example, the warpage C of the group III nitride semiconductor substrate before epitaxial growth of the group III nitride semiconductor film is considered. S The value is 0. When a group III nitride semiconductor film with a thickness of approximately 3 μm and an Al composition of 3 atom% is disposed on a 2-inch (50 mm diameter) group III nitride semiconductor substrate without warping, the warping amount of the downward bulge is 30 μm. Based on the above formula (1), it can be expressed as the following formula (6): [Warpage C] E ]30(μm)=[correction coefficient]α×[wafer diameter Φ]50(mm)×[thickness t]3(μm)×[Al composition a]3(atom%) (6).

[0082] According to equation (6) above, the correction coefficient α can be estimated as 0.067 (mm) under the above conditions, for example. -1 ).

[0083] <6 inches (diameter Φ150mm), upper limit of warpage C L For a 60μm case> As an example, in a non-warped 6-inch (diameter Φ150mm, C) S=0 μm) and a group III nitride semiconductor film is provided on the group III nitride semiconductor substrate, it can be expressed as the following formula (7) based on the above formulas (3) and (4): C L ≥C S +C E =C S +αΦta≥0 (7).

[0084] By substituting the above respective numerical values, the following formula (8) can be obtained: 60 (μm)≥0.067 (mm -1 )×150 (mm)×ta≥0 6≥ta (8).

[0085] In the above example, it is found that in order to make the upper limit warpage amount within C L 60 μm, it is sufficient to provide one layer of group III nitride semiconductor film (film thickness t (μm), Al composition a (atom%)) satisfying the above formula (8) on a warp-free 6-inch (diameter Φ150 mm, C S =0 μm) group III nitride semiconductor substrate.

[0086] <Electronic Device> In the electronic device, the above group III nitride semiconductor epitaxial wafer can be used. Thereby, a device with a flat surface, low resistance during operation, and low leakage current can be realized.

[0087] <Method for Manufacturing Group III Nitride Semiconductor Epitaxial Wafer> The method for manufacturing a group III nitride semiconductor epitaxial wafer according to Embodiment 1 includes, for example, the following steps.

[0088] (1) For example, a group III nitride semiconductor substrate exhibiting n-type conductivity and having a carrier concentration of 10 20 cm -3 or more is formed by the OVPE method. Note that the method for manufacturing a group III nitride semiconductor substrate based on the OVPE method will be described later. In addition, the group III nitride semiconductor substrate is not limited to the OVPE method, and may be formed by the HVPE method.

[0089] (2) A first group III nitride semiconductor film containing Al and Ga as group III elements is epitaxially grown on the group III nitride semiconductor substrate. The first group III nitride semiconductor film is, for example, AlGaN. More specifically, when the chemical formula of the first group III nitride semiconductor film is expressed as (Al x Ga 1-x)In the case of N, the Al composition x is, for example, 0.001 or more and 0.3 or less. By setting the Al composition x in the above range, the first group III nitride semiconductor film can obtain sufficient flatness, and generation of lattice strain between the film and the underlying group III nitride semiconductor substrate can be suppressed.

[0090] (3) On the first group III nitride semiconductor film, second to N-th group III nitride semiconductor films where N is a natural number of 2 or more are epitaxially grown. By imparting sufficient flatness to the above first group III nitride semiconductor film, the second to N-th group III nitride semiconductor films can, for example, obtain sufficient flatness with a root mean square roughness RMS value of 1 nm or less in a 30 μm square on the surface.

[0091] Further, in the case where the Al composition in each group III nitride semiconductor film is constant, the first to N-th group III nitride semiconductor films may be configured to satisfy the above formula (4). In addition, in the case where the Al composition in each group III nitride semiconductor film varies in the thickness direction, the first to N-th group III nitride semiconductor films may be configured to satisfy the above formula (5).

[0092] Through the above steps, the group III nitride semiconductor epitaxial wafer of Embodiment 1 can be obtained.

[0093] <Outline of Method for Manufacturing Group III Nitride Semiconductor Substrate> Reference Figure 3 to the flowchart and Figure 3 , an outline of the OVPE-based manufacturing method of the group III nitride semiconductor substrate constituting the group III nitride semiconductor epitaxial wafer of the present Embodiment 1 will be described. Figure 3 (a) is a time-series flowchart showing the manufacturing method. Figure 3 (b) shows each functional unit from the upstream toward the downstream inside the manufacturing apparatus used in the present manufacturing method as a process.

[0094] In the seed crystal substrate preparation step of preparing the seed crystal substrate 116, the seed crystal substrate 116 is placed on the substrate susceptor 117.

[0095] In the temperature raising step, the growth chamber 111 is heated to 100°C or more and less than 500°C in an inert gas atmosphere.

[0096] In the decomposition protection temperature raising step 1, the growth chamber 111 is heated to 500°C or more and less than 1100°C in an NH₃ gas atmosphere.

[0097] In the decomposition protection temperature raising step 2, the growth chamber 111 is heated to 1100°C or more and less than 1500°C in an atmosphere of NH₃ gas and Ga₂O gas.

[0098] In the growth process of growing a group III nitride semiconductor substrate on a seed substrate 116, a group III element oxide gas is generated in the raw material chamber 100 and supplied to the cultivation chamber 111, and a nitrogen-containing gas is supplied to the cultivation chamber 111 to grow a group III nitride semiconductor substrate on the seed substrate 116.

[0099] The growth process also includes a reactive gas supply process, a group III element oxide gas generation process, a group III element oxide gas supply process, a nitrogen-containing gas supply process, a group III nitride semiconductor substrate formation process, and a residual gas removal process. It should be noted that all the steps included in the growth process can be performed simultaneously within the group III nitride semiconductor substrate manufacturing apparatus.

[0100] In the reactive gas supply process, reactive gas is supplied to the raw material reaction chamber 101.

[0101] In the process of generating group III element oxide gas, the starting group III element source is reacted with a reactive gas (a reducing gas when the starting group III element source is an oxide, and an oxidizing gas when it is a metal) to generate group III element oxide gas.

[0102] In the group III element oxide gas supply process, the group III element oxide gas produced in the group III element oxide gas generation process is supplied to the cultivation chamber 111.

[0103] In the nitrogen-containing gas supply process, nitrogen-containing gas is supplied to the cultivation chamber 111.

[0104] In the process of growing a group III nitride semiconductor substrate, the group III element oxide gas supplied to the growth chamber 111 in the process of supplying group III element oxide gas reacts with the nitrogen-containing gas supplied to the growth chamber 111 in the process of supplying nitrogen-containing gas, so that the group III nitride semiconductor substrate grows on the seed substrate.

[0105] In the residual gas removal process, unreacted gases that do not contribute to the formation of the group III nitride semiconductor substrate are discharged outside the chamber.

[0106] In the decomposition protection cooling process, in order to suppress the decomposition of the group III nitride semiconductor substrate grown on the seed crystal substrate 116, the temperature of the raw material chamber 100 and the growth chamber 111 is reduced to 500°C while NH3 gas is supplied.

[0107] In the cooling process, the temperature of the raw material chamber 100 and the incubation chamber 111 is reduced to less than 100°C in an inactive gas atmosphere.

[0108] In the take-out step, the seed crystal substrate 116 on which the group III nitride substrate has been grown is taken out from the growth chamber 111.

[0109] <Outline of Manufacturing Apparatus for Group III Nitride Semiconductor Substrate> Reference Figure 4 An outline of the manufacturing apparatus used in the method for manufacturing the group III nitride semiconductor substrate constituting the group III nitride semiconductor epitaxial wafer of the first embodiment will be described. Figure 4 is a schematic cross-sectional view of the manufacturing apparatus for the group III nitride semiconductor substrate constituting the group III nitride semiconductor epitaxial wafer according to the first embodiment.

[0110] In Figure 4 , the size, ratio, etc. of each component may differ from the actual ones. In the manufacturing apparatus for a group III nitride semiconductor substrate, a source reaction chamber 101 is disposed inside a source chamber 100, and a source boat 104 on which a starting group III element source 105 is placed is disposed inside the source reaction chamber 101. The source reaction chamber 101 is connected to a reactive gas supply pipe 103 that supplies a gas that reacts with the starting group III element source 105. The source reaction chamber 101 has a group III element oxide gas discharge port 107 for discharging the generated group III element oxide gas. When the starting group III source is an oxide, a reducing gas is used as the reactive gas. When the starting group III source is a metal, an oxidizing gas is used as the reactive gas. In addition, the source chamber 100 is connected to a first carrier gas supply port 102 that supplies a first carrier gas. The first carrier gas supplied from the first carrier gas supply port 102 and the group III element oxide gas discharged from the group III element oxide gas discharge port 107 flow from the gas discharge port 108 through the connecting pipe 109 to the growth chamber 111, and are supplied into the growth chamber 111 from the gas supply port 118 connected to the growth chamber 111. The growth chamber 111 has a gas supply port 118, a third carrier gas supply port 112, a nitrogen-containing gas supply port 113, a second carrier gas supply port 114, and an exhaust port 119. The growth chamber 111 is provided with a substrate susceptor 117 on which the seed crystal substrate 116 is placed.

[0111] <Details of Manufacturing Method and Manufacturing Apparatus> Reference Figure 3 and Figure 4 , the method for manufacturing the group III nitride semiconductor substrate of the first embodiment will be described in detail.

[0112] In the first embodiment, metal Ga is used as the starting group III element source 105, but the present invention is not limited thereto, and for example, Al or In may also be used.

[0113] First, a seed substrate 116 is prepared. For example, gallium nitride, gallium arsenide, silicon, sapphire, silicon carbide, zinc oxide, gallium oxide, or ScAlMgO4 can be used as the seed substrate 116. In this embodiment 1, gallium nitride is used as the seed substrate 116.

[0114] based on Figure 3 (a) Provide an explanation.

[0115] In the heating process, the growth chamber is heated to a temperature at which the seed substrate 116 does not decompose under an inert gas atmosphere. In the manufacture of a group III nitride semiconductor substrate using the OVPE method, it is heated to approximately 500°C under an inert gas atmosphere (e.g., N2 gas).

[0116] In the decomposition protection heating step 1, the temperature is increased while suppressing the decomposition of the seed substrate 116 in a nitrogen-containing gas atmosphere. In the manufacture of a Group III nitride semiconductor substrate using the OVPE method, heating is performed in a mixture of an inactive gas and a nitrogen-containing gas (NH3) until the temperature reaches 500°C or higher but is less than 1100°C. The reason for mixing NH3 is to prevent the decomposition of the seed substrate 116 due to the removal of nitrogen atoms. Alternatively, heating can be performed with an additional mixture of H2 gas.

[0117] In the decomposition protection heating step 2, the temperature is increased while suppressing the decomposition of the seed substrate 116 in an atmosphere of Group III oxide gas and nitrogen-containing gas. In the manufacture of Group III nitride semiconductor substrates using the OVPE method, heating is performed in a mixture of H2 gas, inactive gas, Group III oxide gas, and nitrogen-containing gas NH3 gas, up to a temperature above 1100°C and below 1500°C. The reason for mixing the Group III oxide gas is that decomposition cannot be suppressed by nitrogen-containing gas alone. By providing a driving force for the growth of the Group III nitride semiconductor substrate, decomposition can be suppressed.

[0118] In the growth process, group III element oxide gas is generated in the raw material chamber 100 and supplied to the cultivation chamber 111. Nitrogen-containing gas is also supplied to the cultivation chamber 111 to generate a group III nitride semiconductor substrate on the seed substrate 116. Specifically, the growth process includes a reactive gas supply process, a group III element oxide gas generation process, a group III element oxide gas supply process, a nitrogen-containing gas supply process, a group III nitride semiconductor substrate generation process, and a residual gas removal process.

[0119] Next, based on Figure 3 (b) Provide an explanation.

[0120] In the reactive gas supply process, reactive gas is supplied from the reactive gas supply pipe 103 to the raw material reaction chamber 101 within the raw material chamber 100. As described above, either a reducing gas or an oxidizing gas can be used as the reactive gas, depending on the need. In this embodiment 1, since metallic Ga is used as the starting group III element source 105, H2O gas is used as the reactive gas.

[0121] In the Group III element oxide gas generation process, the reactive gas supplied to the raw material reaction chamber 101 in the reactive gas supply process reacts with Ga, which serves as the starting Group III element source 105, to generate Ga₂O gas, which is a Group III element oxide gas. The generated Ga₂O gas is discharged from the raw material reaction chamber 101 to the raw material chamber 100 via the Group III element oxide gas outlet 107. The discharged Ga₂O gas is mixed with the first carrier gas supplied to the raw material chamber from the first carrier gas supply port 102 and supplied to the gas outlet 108. In this embodiment 1, the raw material chamber 100 is heated by the first heater 106. When heating the raw material chamber 100, from the viewpoint of the boiling point of Ga₂O gas, it is preferable to set the temperature of the raw material chamber 100 to 800°C or higher. In addition, it is preferable to set the temperature of the raw material chamber 100 to be lower than that of the incubation chamber 111. When the incubation chamber is heated by the second heater 115 as described later, it is preferable to set the temperature of the raw material chamber 100 to, for example, less than 1800°C. The starting group III element source 105 is placed in a feed boat 104 disposed within the feed reaction chamber 101. The feed boat 104 is preferably shaped to increase the contact area between the reactive gas and the starting group III element source. For example, to prevent the starting group III element source 105 from passing through the feed reaction chamber 101 in a non-contact state with the reactive gas, the feed boat 104 is preferably a multi-segmented disk shape.

[0122] It should be noted that the methods for generating group III element oxide gases can be broadly categorized into methods of reducing the starting group III element source 105 and methods of oxidizing the starting group III element source 105. For example, in the reduction method, an oxide (e.g., Ga₂O₃) is used as the starting group III element source 105, and a reducing gas (e.g., H₂, CO, CH₄, C₂H₆, H₂S, SO₂) is used as the reactive gas. On the other hand, in the oxidation method, a non-oxide (e.g., liquid Ga) is used as the starting group III element source 105, and an oxidizing gas (e.g., H₂O, O₂, CO, CO₂, NO, N₂O, NO₂) is used as the reactive gas. In addition to the starting group III element source 105, In and Al sources can also be used as starting group III elements. Inert gases, H₂, etc., can be used as the first carrier gas.

[0123] In the Group III oxide gas supply process, the Ga2O gas generated in the Group III oxide gas generation process is supplied to the incubation chamber 111 via gas outlet 108, connecting pipe 109, and gas supply port 118. If the temperature of the connecting pipe 109 connecting the raw material chamber 100 and the incubation chamber 111 is lower than the temperature of the raw material chamber 100, a reverse reaction occurs, resulting in the generation of Group III oxide gas, and the initial Ga source 105 precipitates within the connecting pipe 109. Therefore, it is preferable that the connecting pipe 109 is heated by the third heater 110 to a temperature higher than that of the first heater 106, so as not to fall below the temperature of the raw material chamber 100.

[0124] In the nitrogen-containing gas supply process, nitrogen-containing gas is supplied from nitrogen-containing gas supply port 113 to the cultivation chamber 111. Examples of nitrogen-containing gases include NH3 gas, NO gas, NO2 gas, N2O gas, N2H2 gas, and N2H4 gas.

[0125] In the process of growing a group III nitride semiconductor substrate, the raw material gas supplied to the growth chamber reacts through each supply process, causing the group III nitride semiconductor substrate to grow on the seed substrate 116. Preferably, the growth chamber 111 is heated to the temperature at which the group III element oxide gas and the nitrogen-containing gas react by the second heater 115. At this time, in order to prevent the reverse reaction that generates the group III element oxide gas, the temperature of the growth chamber 111 is preferably controlled in a manner that is not lower than the temperature of the raw material chamber 100. The temperature of the growth chamber 111 heated by the second heater 115 is preferably between 1000°C and 1800°C. In addition, for the purpose of suppressing the temperature fluctuation of the growth chamber 111 caused by the Ga2O gas generated in the raw material chamber 100 and the first carrier gas, it is preferable that the temperatures of the second heater 115 and the third heater 110 are the same.

[0126] By mixing the Group III element oxide gas supplied to the growth chamber 111 through the Group III element oxide supply process and the nitrogen-containing gas supplied to the growth chamber 111 through the nitrogen-containing gas supply process upstream of the seed substrate 116, the growth of a Group III nitride semiconductor substrate can be carried out on the seed substrate 116.

[0127] It should be noted that the reactive gas supply process, the group III element oxide gas generation process, the group III element oxide gas supply process, the nitrogen-containing gas supply process, the group III nitride semiconductor substrate generation process, and the residual gas removal process included in the growth process can be carried out simultaneously.

[0128] As a second carrier gas, inert gases or H2 gas can be used, for example. As a third carrier gas, nitrogen, argon, helium, etc., can be used, for example.

[0129] In the residual gas discharge process, unreacted Group III element oxide gas and nitrogen-containing gas, as well as the first carrier gas, the second carrier gas and the third carrier gas are discharged from the exhaust port 119.

[0130] In the decomposition protection cooling process, cooling is performed in a nitrogen-containing gas atmosphere while suppressing the decomposition of the group III nitride semiconductor substrate. In the manufacturing of group III nitride semiconductor substrates using the OVPE method, cooling is performed to below 500°C in a state of mixing inactive gas and nitrogen-containing gas NH3.

[0131] In the cooling process, the temperature is lowered to a level that allows the group III nitride semiconductor substrate to be removed from the incubation chamber under an inactive gas atmosphere.

[0132] In this embodiment 1, after a cooling process, the seed substrate 116 on which the group III nitride semiconductor substrate is grown is taken out from the cultivation chamber 111.

[0133] Thus, a group III nitride semiconductor substrate can be obtained.

[0134] <Group III Nitride Semiconductor Films> The first group III nitride semiconductor film is obtained by epitaxially growing a group III nitride semiconductor film containing Al and Ga as group III elements on a group III nitride semiconductor substrate. The epitaxial growth process of the first group III nitride semiconductor film can be performed by replacing the seed substrate with a group III nitride semiconductor substrate and replacing it with a material containing Al and Ga as the starting group III element source in the aforementioned group III nitride semiconductor substrate manufacturing apparatus and manufacturing method, thereby manufacturing based on the OVPE method. Therefore, after manufacturing the group III nitride semiconductor substrate, the first group III nitride semiconductor film can be continuously epitaxially grown on the group III nitride semiconductor substrate without being removed from the growth chamber. It should be noted that the manufacturing of the aforementioned Group III nitride semiconductor films is not limited to the OVPE-based manufacturing method. For example, it can also be other manufacturing methods such as HVPE (Hydride Vapor Phase Epitaxy), using trimethylgallium (TMG) or triethylgallium (TEG) as Ga raw materials, using trimethylaluminum (TMA) as Al raw materials, or using ammonia (NH3) as nitrogen (N) raw materials.

[0135] <Group III nitride semiconductor films from the second to the Nth> A second to an Nth group III nitride semiconductor film is obtained by epitaxially growing one or more group III nitride semiconductor films on a first group III nitride semiconductor film. The process of epitaxially growing the second to Nth group III nitride semiconductor films can be performed by replacing the seed substrate with a first group III nitride semiconductor substrate in the aforementioned group III nitride semiconductor substrate manufacturing apparatus and manufacturing method, based on the OVPE method. Therefore, after manufacturing the first group III nitride semiconductor film, the second to Nth group III nitride semiconductor films can be continuously epitaxially grown on the first group III nitride semiconductor film without being removed from the growth chamber. It should be noted that the manufacturing of the aforementioned second to Nth group III nitride semiconductor films is not limited to the OVPE-based manufacturing method, but can also be other manufacturing methods such as HVPE (hydride vapor phase epitaxy), MOCVD (metal-organic chemical vapor deposition) using trimethylgallium (TMG) or triethylgallium (TEG) as Ga raw material, trimethylaluminum (TMA) as Al raw material, or ammonia (NH3) as nitrogen (N) raw material.

[0136] This allows for the production of group III nitride semiconductor epitaxial wafers.

[0137] (Examples 1 to 3: Group III nitride semiconductor substrates formed by HVPE method) Figure 5 Table 1 shows the composition of each layer of the group III nitride semiconductor epitaxial wafers of Examples 1 to 3, in which the first to Nth group III nitride semiconductor films are epitaxially grown on a group III nitride semiconductor substrate formed by the HVPE method. Figure 6 Table 2 shows the 3μm square AFM images and 30μm square AFM images of the surface of the group III nitride semiconductor epitaxial wafers of Examples 1 to 3, as well as the deviation angle and root mean square roughness (RMS) values ​​of the group III nitride semiconductor epitaxial wafers.

[0138] like Figure 5 As shown, in the group III nitride semiconductor epitaxial wafers of Examples 1 to 3, the group III nitride semiconductor substrate is GaN formed by the HVPE method. In Examples 1 and 3, first and second group III nitride semiconductor films are provided, and in Example 2, first to third group III nitride semiconductor films are provided.

[0139] like Figure 6As shown, in Examples 1 to 3, the value of the root mean square roughness RMS is 1 nm or less, exhibiting sufficient flatness.

[0140] (Examples 4 to 6: Group III nitride semiconductor substrate formed by OVPE method) Figure 7 is Table 3 showing the composition of each layer of the Group III nitride semiconductor epitaxial wafers of Examples 4 to 6 in which the first to N-th Group III nitride semiconductor films are epitaxially grown on the Group III nitride semiconductor substrate formed by the OVPE method. Figure 8 is Table 4 showing the 3 μm square AFM image and the 30 μm square AFM image of the surface of the Group III nitride semiconductor epitaxial wafers of Examples 4 to 6, and the off-angle and the value of the root mean square roughness RMS of the Group III nitride semiconductor epitaxial wafers.

[0141] The Group III nitride semiconductor epitaxial wafers of Examples 4 to 6 are as Figure 7 shown, the Group III nitride semiconductor substrate is GaN formed by the OVPE method. In Example 4, the first to fourth Group III nitride semiconductor films are provided, and in Examples 5 and 6, the first and second Group III nitride semiconductor films are provided.

[0142] As shown Figure 8 shown, in Examples 4 to 6, the value of the root mean square roughness RMS is 1 nm or less, exhibiting sufficient flatness.

[0143] <Case where the Al composition in the Group III nitride semiconductor film is uniform in the thickness direction> (Example 7) Figure 9A is a schematic cross-sectional view showing the Al composition and thickness of each layer of the Group III nitride semiconductor epitaxial wafer of Example 7.

[0144] As shown Figure 9A shown, the film thickness t1 of the first Group III nitride semiconductor film is 1 μm, the Al composition a1 is 3 atom%, the film thickness t2 of the second Group III nitride semiconductor film is 7 μm, and the Al composition a2 is 0.1 atom%.

[0145] The relational expression for the sum of the warpage amounts including the first and second Group III nitride semiconductor films is: t1×a1 + t2×a2 = (1 μm)×(3 atom%) + (7 μm)×(0.1 atom%) = 3.7 < 6, It is found that the above formula (8) is satisfied, and the warpage amount can be suppressed to not more than the upper limit value.

[0146] (Example 8) Figure 9B This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 8.

[0147] like Figure 9B As shown, the thickness t1 of the first group III nitride semiconductor film is 1 μm and the Al composition a1 is 3 atom%. The thickness t2 of the second group III nitride semiconductor film is 7 μm and the Al composition a2 is 0.2 atom.

[0148] The formula for the total warpage of group I and group II III nitride semiconductor films is as follows: t1×a1+t2×a2=(1μm)×(3atom%)+(7μm)×(0.2atom%)=4.4<6, It can be seen that satisfying the above equation (8) can suppress warping below the upper limit.

[0149] (Example 9) Figure 9C This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 9.

[0150] like Figure 9C As shown, the thickness t1 of the first group III nitride semiconductor film is 1 μm and the Al composition a1 is 5 atom%. The thickness t2 of the second group III nitride semiconductor film is 7 μm and the Al composition a2 is 0.1 atom.

[0151] The formula for the total warpage of group I and group II III nitride semiconductor films is as follows: t1×a1+t2×a2=(1μm)×(5atom%)+(7μm)×(0.1atom%)=5.7<6, It can be seen that satisfying the above equation (8) can suppress warping below the upper limit.

[0152] (Example 10) Figure 9D This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 10.

[0153] like Figure 9D As shown, the thickness t1 of the first group III nitride semiconductor film is 0.2 μm, and the Al composition a1 is 20 atom%. The thickness t2 of the second group III nitride semiconductor film is 0.8 μm, and the Al composition a2 is 0.3 atom%. The thickness t3 of the third group III nitride semiconductor film is 7 μm, and the Al composition a3 is 0.1 atom.

[0154] The relational expression for the total warpage amount of the first to third group III nitride semiconductor films is: t1×a1+t2×a2+t3×a3=(0.2μm)×(20atom%)+(0.8μm)×(0.3atom%)+(7μm)×(0.1atom%)=4.94<6, It is confirmed that the above formula (8) is satisfied, and the warpage amount can be suppressed to be equal to or less than the upper limit value.

[0155] <Case where the Al composition in the group III nitride semiconductor film varies in the thickness direction> In the case where the Al composition in the group III nitride semiconductor film varies in the thickness direction, the above formula (8) can be modified as: .

[0156] (Example 11) Figure 10A is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 11.

[0157] As shown in Figure 10A , the film thickness t1 of the first group III nitride semiconductor film is 1 μm, the Al composition a1 varies linearly from 3 atom% to 0 atom% along the thickness direction, the film thickness t2 of the second group III nitride semiconductor film is 7 μm, and the Al composition a2 is 0.1 atom% (constant).

[0158] The relational expression for the total warpage amount including the first and second group III nitride semiconductor films is expressed as follows, =2.2<6, It is confirmed that the above formula (9) is satisfied, and the warpage amount can be suppressed to be equal to or less than the upper limit value.

[0159] (Example 12) Figure 10B is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 12.

[0160] As shown in Figure 10B , the film thickness t1 of the first group III nitride semiconductor film is 1 μm, the Al composition a1 varies linearly (5.8t+0.2) from 6 atom% to 0.2 atom% along the thickness direction, the film thickness t2 of the second group III nitride semiconductor film is 7 μm, and the Al composition a2 is 0.2 atom% (constant).

[0161] The formula for the total warpage of group I and group II III nitride semiconductor films is as follows: =4.5 < 6, It can be seen that satisfying the above equation (9) can suppress the warping amount below the upper limit.

[0162] (Example 13) Figure 10C This is a schematic cross-sectional view showing the Al composition and thickness of each layer of the group III nitride semiconductor epitaxial wafer of Example 13.

[0163] like Figure 10C As shown, the thickness t1 of the first group III nitride semiconductor film is 0.05 μm, and the Al composition a1 is 30 atom% (constant). The thickness t2 of the second group III nitride semiconductor film is 1 μm, and the Al composition a2 changes linearly from 5 atom% (4.7t + 0.3) to 0.3 atom% along the thickness direction. The thickness t3 of the third group III nitride semiconductor film is 7 μm, and the Al composition a2 is 0.1 atom% (constant).

[0164] The formula for the total warpage of group I to III nitride semiconductor films is as follows: =1.5 + 2.35 + 0.3 + 0.7 = 4.55 < 6, It can be seen that satisfying the above equation (9) can suppress the warping amount below the upper limit.

[0165] Industrial utilization potential According to the group III nitride semiconductor epitaxial wafer disclosed herein, by providing a first group III nitride semiconductor film containing Al and Ga as group III elements as an intermediate layer, the flatness of the group III nitride semiconductor film on the uppermost surface can be ensured. Furthermore, by controlling the thickness and Al composition of the group III nitride semiconductor film at each upper limit, the warpage can be adjusted to be below the upper limit.

[0166] Figure Labels 2. Group III nitride semiconductor substrates 4 Group III Nitride Semiconductor Films 6 Group III Nitride Semiconductor Films 10 Group III nitride semiconductor epitaxial wafer 100 Raw Material Room 101 Raw Material Reaction Chamber 102 First Carrier Gas Supply Port 103 Reactive gas supply pipe 104 Raw Material Boat 105 Initial Group III Elemental Source 106 First Heater 107 Group III element oxide gas exhaust outlet 108 Gas Exhaust Port 109 Connecting pipe 110 Third Heater 111 Cultivation Room 112 Third Carrier Gas Supply Port 113 Nitrogen-containing gas supply port 114 Second Carrier Gas Supply Port 115 Second heater 116 Seed substrate 117 Substrate base 118 Gas supply port 119 Exhaust port

Claims

1. A group III nitride semiconductor epitaxial wafer, comprising: Displaying n-type conductive group III nitride semiconductor substrates; A first group III nitride semiconductor film containing Al and Ga as group III elements, epitaxially grown on the group III nitride semiconductor substrate; and N is a natural number greater than or equal to 2, and second to Nth group III nitride semiconductor films are epitaxially grown on the first group III nitride semiconductor film. in, The total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate, with the convex direction as the positive direction, is denoted as C. E (μm), Let i be a natural number from 1 to N, and let the thickness of the i-th group III nitride semiconductor film be t. i (μm), let Al composition be a i (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction coefficient is set to α, The total amount of warpage C E (μm) is represented as: , Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following is satisfied: 。 2. A group III nitride semiconductor epitaxial wafer, comprising: Displaying n-type conductive group III nitride semiconductor substrates; A first group III nitride semiconductor film containing Al and Ga as group III elements, epitaxially grown on the group III nitride semiconductor substrate; and N is a natural number greater than or equal to 2, and the second to Nth group III nitride semiconductor films are epitaxially grown on the first group III nitride semiconductor film. in, The total warpage of the first to Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate, with the convex direction as the positive direction, is denoted as C. E (μm), Let i be a natural number from 1 to N, and let the thickness of the i-th group III nitride semiconductor film be t. i (μm), representing the thickness along the film thickness direction of the i-th group III nitride semiconductor film from film thickness 0 (μm) to film thickness t. i Let a be a function of the thickness t in the range of (μm) composed of Al. i (t)(atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction coefficient is set to α, The total amount of warpage C E (μm) is represented as: , Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following is satisfied: 。 3. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The Al composition of the first group III nitride semiconductor film is 0.1 atom% or more.

4. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The carrier concentration of the group III nitride semiconductor substrate is 10. 17 cm -3 Above and 10 19 cm -3 the following.

5. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The carrier concentration of the group III nitride semiconductor substrate is 10. 20 cm -3 The doping element is oxygen.

6. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The carrier concentration of the first group III nitride semiconductor film is 10. 17 cm -3 above.

7. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The carrier concentration of the i-th group III nitride semiconductor film with i=2 or more epitaxially grown on the first group III nitride semiconductor film is 10. 17 cm -3 the following.

8. The group III nitride semiconductor epitaxial wafer according to claim 1 or 2, wherein, The carrier concentration of the first group III nitride semiconductor film is 10. 17 cm -3 The carrier concentration of the i-th group III nitride semiconductor film, where i is 2 or more, epitaxially grown on the first group III nitride semiconductor film is 10. 17 cm -3 the following.

9. An electronic device that uses the group III nitride semiconductor epitaxial wafer as described in claim 1 or 2.

10. A method for manufacturing a group III nitride semiconductor epitaxial wafer, comprising: The process of forming a group III nitride semiconductor substrate that exhibits n-type conductivity; The process of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and The process of epitaxially growing second to Nth group III nitride semiconductor films on the first group III nitride semiconductor film, where N is a natural number greater than or equal to 2. Wherein, the total warpage of the first to the Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate, with the convex direction as the positive direction, is defined as C. E (μm), Let i be a natural number from 1 to N, and let the thickness of the i-th group III nitride semiconductor film be t. i (μm), let Al composition be a i (atom%), when the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm) and the correction coefficient is set to α, The total amount of warpage C E (μm) is represented as: , Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following condition is met: The method is used to epitaxially grow the first to the Nth group III nitride semiconductor films.

11. A method for manufacturing a group III nitride semiconductor epitaxial wafer, comprising: The process of forming a group III nitride semiconductor substrate that exhibits n-type conductivity; The process of epitaxially growing a first group III nitride semiconductor film containing Al and Ga as group III elements on the group III nitride semiconductor substrate; and The process of epitaxially growing second to Nth group III nitride semiconductor films on the first group III nitride semiconductor film, where N is a natural number greater than or equal to 2. Wherein, the total warpage of the first to the Nth group III nitride semiconductor films epitaxially grown on the group III nitride semiconductor substrate, with the convex direction as the positive direction, is defined as C. E (μm), Let i be a natural number from 1 to N, and let the thickness of the i-th group III nitride semiconductor film be t. i (μm), representing the thickness along the film thickness direction of the i-th group III nitride semiconductor film from film thickness 0 (μm) to film thickness t. i Let a be a function of the thickness t in the range of (μm) composed of Al. i (t)(atom%), where the diameter of the group III nitride semiconductor epitaxial wafer is set to Φ (cm), and the correction coefficient is set to α, The total amount of warpage C E (μm) is represented as: , Furthermore, C is defined as the warpage of the group III nitride semiconductor substrate with the convex direction as the positive direction. S (μm), the warpage of the upper limit of the group III nitride semiconductor epitaxial wafer is set as C. L In the case of (μm), the following condition is met: The method is used to epitaxially grow the first to the Nth group III nitride semiconductor films.

Citation Information

Patent Citations

  • Repairing of screw nail hole in wooden crosstie

    JP1987037401A

  • Method for producing group iii nitride crystal, group iii nitride crystal, semiconductor device and apparatus for producing group iii nitride crystal

    WO2015053341A1