A direct X-ray detector of δ-FAPbI3 with ultrasound-pressure synergistic in-plane texture and its fabrication method.
By simultaneously applying ultrasonic vibration during the pressurization process, the in-plane preferred orientation problem in the fabrication of δ-FAPbI3 wafers was solved, which assisted in the orientation rearrangement of powder particles. This resulted in higher yield and signal stability, while reducing the fabrication difficulty and cost.
Patent Information
- Application Number
- CN202611232242.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing δ-FAPbI3 wafers struggle to achieve directional rearrangement and in-plane preferred orientation of powder particles without increasing forming pressure, leading to wafer fragility, internal cracks, and mechanical inhomogeneity.
An ultrasonic-pressure synergistic induction method was adopted, in which ultrasonic vibration was applied simultaneously during the pressurization and holding processes to assist the orientation rearrangement of powder particles and form δ-FAPbI3 wafers with in-plane texture.
This technology enables uniform packing and directional alignment of powder particles under lower forming pressure, reducing wafer cracks and demolding damage, improving detector signal stability and yield, and reducing equipment load and manufacturing costs.
Smart Images

Figure CN123108738A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of X-ray detection technology, specifically a δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method. Background Technology
[0002] Direct-type X-ray detectors can directly convert incident X-rays into electrical signals within a semiconductor absorption layer, offering applications in medical imaging, industrial non-destructive testing, and security inspection. Halide perovskites, with their high X-ray absorption capacity and solution processability, are important candidate materials for the absorption layer of direct-type X-ray detectors. One-dimensional yellow δ-FAPbI3, composed of Pb-I octahedral chains linked along specific crystal orientations, exhibits low ion migration tendency and good environmental stability.
[0003] Existing methods typically involve loading δ-FAPbI3 powder into a mold and then subjecting it to separate hydrostatic pressing or cold isostatic pressing to improve wafer density and mechanical integrity. These methods primarily rely on pressure to compact the powder. However, powder particles are prone to bridging, frictional locking, and random stacking before and during pressurization, resulting in dispersed grain orientation and a lack of active control over the direction of the one-dimensional Pb-I chains relative to the device's operating electric field. Simply increasing the forming pressure can further compact the powder, but this can easily cause wafer edge chipping, internal microcracks, or demolding damage. Even ultrasonic powder distribution before pressurization is insufficient to overcome the slippage and random locking that occur again during pressure establishment.
[0004] Therefore, how to continuously assist particle rearrangement by ultrasonic vibration during the pressure establishment and maintenance process without excessively increasing the forming pressure, so as to obtain δ-FAPbI3 wafers with in-plane preferred orientation, is a technical problem that needs to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to provide a δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method in order to solve the problems mentioned above.
[0006] The technical solution adopted in this invention is as follows: A method for preparing a δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture, comprising the following steps:
[0007] S1. FAI and PbI2 are added to an organic solvent to react, and the resulting yellow precipitate is collected. After washing and drying, δ-FAPbI3 polycrystalline powder is obtained.
[0008] S2. Load the δ-FAPbI3 polycrystalline powder obtained in step S1 into the tableting mold and pre-level the powder in the mold.
[0009] S3. Place the tableting mold containing δ-FAPbI3 polycrystalline powder in a pressurizing device, apply forming pressure along the thickness direction of the tableting mold, and simultaneously apply ultrasonic vibration to the tableting mold or press head during the pressurization and holding process, so that the polycrystalline powder undergoes directional rearrangement under pressure.
[0010] S4. Stop the ultrasonic vibration and unload the forming pressure, and remove the δ-FAPbI3 wafer from the tableting mold;
[0011] S5. Metal electrodes are prepared on opposite sides of the δ-FAPbI3 wafer obtained in step S4 to obtain an in-plane textured δ-FAPbI3 direct X-ray detector.
[0012] In a preferred embodiment, in step 1, the molar ratio of S1FAI to PbI2 is 1:1, the organic solvent is acetonitrile or γ-butyrolactone, and the reaction time is 24-30 h; the resulting precipitate is washed with diethyl ether and dried under vacuum at 40 °C for 10-24 h.
[0013] In a preferred embodiment, in step S2, the amount of δ-FAPbI3 polycrystalline powder is 60-80 mg, and the forming area of the tableting mold is 5 mm × 5 mm.
[0014] In a preferred embodiment, in step S3, ultrasonic vibration and forming pressure are applied simultaneously, and ultrasonic vibration continues at least until the forming pressure reaches a set value.
[0015] In a preferred embodiment, in step S3, ultrasonic vibration is applied continuously or intermittently during the pressure holding process, and the ultrasonic frequency is 20–40 kHz.
[0016] In a preferred embodiment, in step S3, the forming pressure is 0.1–0.3 GPa and the holding time is 10–60 min.
[0017] In a preferred embodiment, in step S3, the ultrasonic transducer is disposed on the side wall, base, or pressure head of the tablet mold.
[0018] In a preferred embodiment, in step S5, the metal electrode is an Au electrode with a thickness of 60-100 nm and an area of 3 mm × 3 mm.
[0019] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0020] 1. In this invention, ultrasonic vibration is introduced simultaneously with pressurization and pressure holding, which can continuously release the mechanical locking and bridging phenomena between powder particles. In traditional static pressing, particles tend to randomly accumulate and become stuck together as pressure increases. However, synchronous ultrasonic action ensures that the particles maintain a certain degree of mobility, allowing them to continuously adjust their position and orientation under pressure, achieving a denser and more uniform packing. This dynamic rearrangement mechanism avoids the structural inhomogeneity problems caused by relying solely on pressure compaction, laying the microscopic foundation for the subsequent formation of texture.
[0021] 2. In this invention, the preferred orientation of the 010 crystal plane is enhanced under relatively low forming pressure, causing the one-dimensional Pb-I octahedral chains to preferentially align along the in-plane direction of the wafer. Due to the ultrasonic vibration-assisted particle rotation and slippage, the grains can complete in-plane directional rotation under lower pressure, without needing to increase the pressure to a level that could easily cause damage. This not only reduces the load on the forming equipment but also makes the control of the texture degree more flexible, avoiding the disadvantage of difficulty in precise control under high pressure.
[0022] 3. In this invention, the in-plane arranged one-dimensional Pb-I chains are perpendicular to the working electric field along the thickness direction of the device. This requires iodine ions to undergo cross-chain transitions when migrating along the electric field direction, which helps suppress ion migration and dark current drift. This structure significantly increases the resistance to long-range ion migration along the thickness direction. The increase in the transition energy barrier is directly reflected in the increase in activation energy and the decrease in leakage current. The baseline drift of the detector is significantly reduced under long-term power-on or continuous irradiation, thus improving signal stability and signal-to-noise ratio.
[0023] 4. In this invention, ultrasonic vibration-assisted particle rearrangement can reduce cracks and demolding damage caused by increasing pressure to obtain texture, thereby improving wafer integrity and fabrication repeatability. Because the forming pressure is controlled within a lower range, the residual stress inside the wafer is significantly reduced, and the probability of edge chipping and internal microcracks during demolding is significantly decreased. Wafers prepared in multiple batches are more similar in thickness, density, and orientation consistency, resulting in a significant improvement in yield and facilitating the transition from small-batch laboratory production to stable production.
[0024] 5. This invention does not alter the electrode configuration on both sides of the wafer or the direct conversion device structure, facilitating compatibility with existing X-ray detection and imaging systems. The method involves only physical processing during the forming stage; electrode fabrication can still employ conventional thermal evaporation or sputtering processes, and the device remains a simple sandwich structure without the need for additional intermediate layers or encapsulation materials. Therefore, existing signal readout circuits and imaging software can be used directly without modification, significantly reducing the barriers to technology integration and promotion costs. Attached Figure Description
[0025] Figure 1 This is a schematic flowchart of the ultrasonic-pressure synergistic preparation method of the present invention;
[0026] Figure 2 A physical image of the in-plane textured δ-FAPbI3 wafer prepared in Example 1;
[0027] Figure 3 XRD comparison images of δ-FAPbI3 wafers obtained in Example 1 and Example 2;
[0028] Figure 4 The (010) polar diagram of the δ-FAPbI3 wafer obtained in Example 1;
[0029] Figure 5 The (010) polar diagram of the δ-FAPbI3 wafer obtained in Example 2;
[0030] Figure 6 The (021) polar diagram of the δ-FAPbI3 wafer obtained in Example 1;
[0031] Figure 7 This is a comparison diagram of the ion migration activation energies of the detectors obtained in Example 1 and Example 2;
[0032] Figure 8 The graph shows the mobility-lifetime product fitting of the detectors obtained in Example 1 and Example 2.
[0033] Figure 9 The sensitivity curves of the detector obtained in Example 1 under different electric fields are shown.
[0034] Figure 10 The signal-to-noise ratio-dose rate curve of the detector obtained in Example 1;
[0035] Figure 11 The graph shows the continuous X-ray switching stability test results of the detector obtained in Example 1.
[0036] Figure 12 This is a photograph of a wafer cracked under excessive pressure, as shown in Example 4. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0038] Reference Figure 1-12 A method for fabricating a δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture includes the following steps:
[0039] S1. FAI and PbI2 are added to an organic solvent to react, and the resulting yellow precipitate is collected. After washing and drying, δ-FAPbI3 polycrystalline powder is obtained.
[0040] S2. Load the δ-FAPbI3 polycrystalline powder obtained in step S1 into the tableting mold and pre-level the powder in the mold.
[0041] S3. Place the tableting mold containing δ-FAPbI3 polycrystalline powder in a pressurizing device, apply forming pressure along the thickness direction of the tableting mold, and simultaneously apply ultrasonic vibration to the tableting mold or press head during the pressurization and holding process, so that the polycrystalline powder undergoes directional rearrangement under pressure.
[0042] S4. Stop the ultrasonic vibration and unload the forming pressure, and remove the δ-FAPbI3 wafer from the tableting mold;
[0043] S5. Metal electrodes are prepared on opposite sides of the δ-FAPbI3 wafer obtained in step S4 to obtain an in-plane textured δ-FAPbI3 direct X-ray detector.
[0044] In step 1, the molar ratio of S1FAI to PbI2 is 1:1, the organic solvent is acetonitrile or γ-butyrolactone, and the reaction time is 24–30 h; the resulting precipitate is washed with diethyl ether and dried under vacuum at 40 °C for 10–24 h.
[0045] In step S2, the amount of δ-FAPbI3 polycrystalline powder is 60-80 mg, and the forming area of the tableting mold is 5 mm × 5 mm.
[0046] In step S3, ultrasonic vibration and forming pressure are applied simultaneously, and ultrasonic vibration continues at least until the forming pressure reaches the set value.
[0047] In step S3, ultrasonic vibration is applied continuously or intermittently during the pressure holding process, and the ultrasonic frequency is 20–40 kHz.
[0048] In step S3, the forming pressure is 0.1–0.3 GPa, and the holding time is 10–60 min.
[0049] In step S3, the ultrasonic transducer is placed on the side wall, base, or pressure head of the tablet mold.
[0050] In step S5, the metal electrode is an Au electrode with a thickness of 60–100 nm and an area of 3 mm × 3 mm.
[0051] Example 1:
[0052] Weigh 1.537 g PbI2 and 0.47 g FAI, mix them, and add them to 15 mL acetonitrile. Stir at high speed for 30 h at room temperature. Collect the resulting yellow precipitate, wash it six times with diethyl ether, and dry it under vacuum at 40 ℃ for 12 h to obtain δ-FAPbI3 polycrystalline powder.
[0053] Weigh 70 mg of the δ-FAPbI3 polycrystalline powder and place it into a tableting mold with a forming area of 5 mm × 5 mm. Pre-level the powder surface. Fix the ultrasonic transducer to the tableting mold base and place the tableting mold in a precision servo pressurizing device.
[0054] While initiating 30 kHz ultrasonic vibration, pressure was applied along the thickness direction of the mold. After the forming pressure reached 0.2 GPa, it was maintained for 60 min, and ultrasonic vibration was continuously applied during the pressure holding period. After the pressure holding period ended, the ultrasonic vibration was stopped first, and then the pressure was slowly unloaded and the mold was demolded to obtain a δ-FAPbI3 wafer with a thickness of approximately 500 μm.
[0055] Au electrodes with a thickness of 80 nm and an area of 3 mm × 3 mm were fabricated on opposite sides of a wafer using a thermal evaporation method to obtain an Au / δ-FAPbI3 / Au direct X-ray detector.
[0056] The XRD and pole figure test results are shown below. Figure 3 , Figure 4 and Figure 6 In Example 1, the diffraction intensity of the (010) crystal plane is significantly enhanced, and the (010) polar density is concentrated in the range of about 5°. The deviation of the crystal plane normal from the preferred out-of-plane direction is about 2.5°. The (021) polar density forms a ring distribution in the range of 20° to 30°, indicating that the one-dimensional Pb-I chain is preferentially arranged along the in-plane direction of the wafer.
[0057] Temperature-dependent conductivity measurements yielded an activation energy of 0.63 eV for ion migration; fitting the modified Hecht equation yielded a μτ of 2.11 × 10⁻⁶. −4 cm 2 ·V −1 The sensitivities at electric fields of 10, 30, 50, 70, and 100 V / mm were 287.7, 467.6, 551.2, 640.7, and 678.3 μC·Gy, respectively. air −1 ·cm −2 The minimum detection limit is 36.2 nGy. air ·s −1 During approximately 5000 seconds of continuous X-ray switching testing, the photocurrent response and baseline remained stable.
[0058] Example 2:
[0059] δ-FAPbI3 polycrystalline powder was prepared according to the method in Example 1. 70 mg of powder was weighed and placed into the same 5 mm × 5 mm tableting mold and pre-leveled.
[0060] Without activating the ultrasonic transducer, a forming pressure of 0.2 GPa was applied along the thickness direction of the mold and held for 60 min, followed by depressurization and demolding. 80 nm Au electrodes were fabricated on opposite sides of the wafer using the same thermal evaporation method as in Example 1 to obtain the control detector.
[0061] The (010) crystal plane density distribution of Example 2 is shown in [reference needed]. Figure 5 Its angular distribution is significantly wider than that of Example 1, indicating that the grain orientation is more dispersed in the absence of synchronous ultrasonic vibration. The modified Hecht equation yields μτ as 1.09 × 10⁻⁶. −4 cm 2 ·V −1 The lowest detection limit, determined with a signal-to-noise ratio of 3, is 81.4 nGy. air ·s −1 All of these results were lower than the corresponding results in Example 1.
[0062] Example 3:
[0063] δ-FAPbI3 polycrystalline powder was prepared according to the method in Example 1. 70 mg of powder was weighed and placed into the same 5 mm × 5 mm tableting mold. The mold was first subjected to ultrasonic vibration at 30 kHz for 10 min without applying forming pressure to pre-level the powder.
[0064] After stopping the ultrasonic vibration, a forming pressure of 0.2 GPa was applied along the thickness direction of the mold and held for 60 min; no ultrasonic vibration was applied during the pressure holding process. Subsequently, the pressure was released, the mold was demolded, and an 80 nm Au electrode was prepared in the same manner as in Example 1.
[0065] Compared with Example 1, the (010) crystal plane diffraction enhancement and polar density concentration of Example 3 are reduced, indicating that ultrasonic powdering before pressurization is insufficient to continuously release particle friction lock during pressure establishment. Simultaneous ultrasonic vibration is beneficial to forming a more obvious in-plane texture.
[0066] Example 4:
[0067] δ-FAPbI3 polycrystalline powder was prepared and filled according to the method in Example 1. Simultaneously, 30 kHz ultrasonic vibration was initiated, and pressure was applied along the thickness direction of the mold to increase the forming pressure to 0.5 GPa and maintain this pressure for 10 min. After the pressure holding period, ultrasonic vibration was stopped, and the mold was released from the pressure.
[0068] The wafer obtained in this embodiment is as follows: Figure 12The presence of cracks and edge damage, along with a reduced complete demolding rate, makes it difficult to use for stable electrode fabrication and X-ray detection. This indicates that excessively high forming pressure cannot replace the ultrasonic-pressure synergistic rearrangement within the preferred pressure window of this invention.
[0069] Example 5:
[0070] δ-FAPbI3 polycrystalline powder was prepared according to the method in Example 1. 70 mg of powder was weighed and placed into the same tableting mold and subjected to ultrasonic vibration at 30 kHz for 60 min, but no forming pressure was applied through a pressurizing device.
[0071] When demolding was attempted directly after ultrasonic vibration was stopped, the powder could not form a dense wafer with a complete self-supporting structure, indicating that ultrasonic vibration, used to promote the rearrangement of compressed particles, still needs to be used in conjunction with the forming pressure during the same processing period.
[0072] From the above, we can conclude that:
[0073] In this invention, ultrasonic vibration is introduced simultaneously with pressurization and pressure holding, which continuously releases the mechanical locking and bridging phenomena between powder particles. In traditional static pressing, particles tend to randomly accumulate and become stuck together as pressure increases. However, synchronous ultrasonic action ensures that the particles maintain a certain degree of mobility, allowing them to continuously adjust their position and orientation under pressure, achieving a denser and more uniform packing. This dynamic rearrangement mechanism avoids the structural inhomogeneity problems caused by relying solely on pressure compaction, laying the microscopic foundation for the subsequent formation of texture.
[0074] In this invention, the preferred orientation of the 010 crystal plane is enhanced under relatively low forming pressure, causing the one-dimensional Pb-I octahedral chains to preferentially align along the in-plane direction of the wafer. Due to the ultrasonic vibration-assisted particle rotation and slippage, the grains can complete in-plane directional rotation under lower pressure, without needing to increase the pressure to a level that could easily cause damage. This not only reduces the load on the forming equipment but also makes the control of the texture degree more flexible, avoiding the disadvantage of difficulty in precise control under high pressure.
[0075] In this invention, the in-plane arranged one-dimensional Pb-I chains are perpendicular to the working electric field along the thickness direction of the device. This requires iodine ions to undergo cross-chain transitions when migrating along the electric field direction, which helps suppress ion migration and dark current drift. This structure significantly increases the resistance to long-range ion migration along the thickness direction. The increased transition energy barrier is directly reflected in the increased activation energy and reduced leakage current. The baseline drift of the detector is significantly reduced under prolonged power-on or continuous irradiation, thus improving signal stability and signal-to-noise ratio.
[0076] In this invention, ultrasonic vibration-assisted particle rearrangement can reduce cracks and demolding damage caused by increasing pressure to obtain texture, thereby improving wafer integrity and fabrication repeatability. Because the forming pressure is controlled within a lower range, the residual stress inside the wafer is significantly reduced, and the probability of edge chipping and internal microcracks during demolding is significantly decreased. Wafers fabricated in multiple batches are more similar in thickness, density, and orientation consistency, resulting in a significant improvement in yield and facilitating the transition from small-batch laboratory production to stable production.
[0077] This invention does not alter the electrode configuration on both sides of the wafer or the direct conversion device structure, facilitating compatibility with existing X-ray detection and imaging systems. The method involves only physical processing during the forming stage; electrode fabrication can still employ conventional thermal evaporation or sputtering processes, and the device remains a simple sandwich structure without the need for additional intermediate layers or encapsulation materials. Therefore, existing signal readout circuits and imaging software can be used directly without modification, significantly reducing the barriers to technology integration and promotion costs.
[0078] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the term "comprising" or any other variations thereof is intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0079] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for fabricating a δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture, characterized in that: Includes the following steps: S1. FAI and PbI2 are added to an organic solvent to react, and the resulting yellow precipitate is collected. After washing and drying, δ-FAPbI3 polycrystalline powder is obtained. S2. Load the δ-FAPbI3 polycrystalline powder obtained in step S1 into the tableting mold and pre-level the powder in the mold. S3. Place the tableting mold containing δ-FAPbI3 polycrystalline powder in a pressurizing device, apply forming pressure along the thickness direction of the tableting mold, and simultaneously apply ultrasonic vibration to the tableting mold or press head during the pressurization and holding process, so that the polycrystalline powder undergoes directional rearrangement under pressure. S4. Stop the ultrasonic vibration and unload the forming pressure, and remove the δ-FAPbI3 wafer from the tableting mold; S5. Metal electrodes are fabricated on opposite sides of the δ-FAPbI3 wafer obtained in step S4 to obtain an in-plane textured δ-FAPbI3 direct X-ray detector.
2. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its fabrication method according to claim 1, characterized in that: In step 1, the molar ratio of S1FAI to PbI2 is 1:1, the organic solvent is acetonitrile or γ-butyrolactone, and the reaction time is 24-30 h; the resulting precipitate is washed with diethyl ether and dried under vacuum at 40 °C for 10-24 h.
3. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its fabrication method according to claim 1, characterized in that: In step S2, the amount of δ-FAPbI3 polycrystalline powder is 60-80 mg, and the forming area of the tableting mold is 5 mm × 5 mm.
4. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method according to claim 1, characterized in that: In step S3, ultrasonic vibration and forming pressure are applied simultaneously, and ultrasonic vibration continues at least until the forming pressure reaches the set value.
5. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method according to claim 1, characterized in that: In step S3, ultrasonic vibration is applied continuously or intermittently during the pressure holding process, and the ultrasonic frequency is 20 to 40 kHz.
6. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method according to claim 1, characterized in that: In step S3, the forming pressure is 0.1–0.3 GPa, and the holding time is 10–60 min.
7. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its fabrication method according to claim 1, characterized in that: In step S3, the ultrasonic transducer is disposed on the side wall, base or pressure head of the tablet mold.
8. The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture and its preparation method according to claim 1, characterized in that: In step S5, the metal electrode is an Au electrode with a thickness of 60–100 nm and an area of 3 mm × 3 mm.
9. A δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture, characterized in that: The δ-FAPbI3 direct X-ray detector with ultrasound-pressure synergistic in-plane texture as described in any one of claims 1 to 8 and the same preparation method are used.